A method for preparing boron trifluoride sulfate metal salts in the liquid phase

By synthesizing anhydrous metal sulfate salts and boron trifluoride in an organic solvent in the liquid phase, the problems of high energy consumption and numerous impurities in existing lithium/sodium salt synthesis have been solved. This method enables the preparation of high-purity boron trifluoride combined with metal sulfate salts, thereby improving the stability and applicability of the electrolyte.

CN122831363BActive Publication Date: 2026-11-17DONGGUAN UPC IND & TRADE +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611339108.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-17
Estimated Expiration
2046-09-01

AI Technical Summary

Technical Problem

Existing lithium/sodium salt synthesis processes suffer from high energy consumption, residual impurities, complex product composition, low purity, and difficulty in controlling side reactions, resulting in unstable electrolyte quality and making it difficult to meet the requirements of high-energy-density lithium batteries.

Method used

Anhydrous metal sulfate and boron trifluoride are synthesized in a liquid phase in an organic solvent. By controlling the reaction temperature and feed ratio, a suspension liquid phase system is formed to avoid side reactions and directly obtain high-purity boron trifluoride metal sulfate.

Benefits of technology

A low-cost, controllable preparation of boron trifluoride sulfate metal salt has been achieved, which is compatible with lithium/sodium battery electrolytes, improves the stability and electrochemical performance of the electrolyte, simplifies the production process, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122831363B_ABST
    Figure CN122831363B_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium / sodium salt synthesis for lithium / sodium batteries, and discloses a method for liquid-phase preparation of boron trifluoride sulfate metal salt. The method involves reacting anhydrous boron trifluoride metal salt with a gaseous boron trifluoride or a non-gase boron trifluoride organic solvent complex in a liquid-phase organic solvent. The reaction equation includes: [equation missing], where M is any one of lithium atoms or sodium atoms. This invention provides a simple, controllable, and highly stable liquid-phase synthesis method suitable for lithium / sodium battery production lines, achieving low-cost, large-scale preparation of boron trifluoride sulfate metal salt. It overcomes the shortcomings of lithium sulfate's low solubility in organic solvents such as carbonates, which hinders its large-scale application in electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium / sodium salt synthesis for lithium / sodium batteries, and specifically to a method for preparing boron trifluoride sulfate metal salt in the liquid phase. Background Technology

[0002] Lithium / sodium-ion batteries, with their advantages of high energy density, long cycle life, and excellent rate performance, are widely used in new energy vehicles, energy storage devices, and 3C digital products. The electrolyte, as a core component of lithium / sodium batteries, directly determines the battery's cycle stability, thermal stability, and safety performance. Currently, commercially available lithium / sodium batteries generally use lithium hexafluorophosphate / sodium as the main lithium / sodium salt in their electrolytes. However, lithium hexafluorophosphate / sodium has drawbacks such as poor thermal stability, easy hydrolysis to generate acidic impurities like hydrogen fluoride, rapid high-temperature cycle degradation, and a tendency to induce the dissolution of transition metals in the positive electrode. These defects severely restrict the large-scale application of high-energy-density lithium batteries such as high-nickel ternary and silicon-carbon anode batteries.

[0003] To address the performance limitations of traditional lithium / sodium salts, novel lithium / sodium salts have become one of the development directions for electrolyte research and development. Boron trifluoride complex salts have attracted attention due to their high solubility and stable antioxidant and reduction resistance.

[0004] Chinese invention patent CN119340478B discloses a pyrosulfate-boron trifluoride composite metal salt electrolyte additive composition, which uses the reaction of pyrosulfate and boron trifluoride to prepare a composite boron-sulfur lithium salt, which can improve the high and low temperature performance of batteries to a certain extent. However, this technical solution has some inherent defects and technical bottlenecks: Firstly, the core raw material of this patent is pyrosulfate. The industrial preparation of pyrosulfate requires a high-temperature thermal decomposition process of bisulfate. The raw material preparation is energy-intensive, the process is long, and impurities such as sulfur trioxide are easily left behind during the thermal decomposition process. If these impurities are introduced into the electrolyte, they will induce problems such as decomposition of ester solvents, discoloration of the electrolyte, and aggravation of interfacial side reactions, which will seriously affect the quality stability of the electrolyte. Unreacted pyrosulfate is prone to hygroscopic decomposition, producing strong acid, which is detrimental to the stability of electrolyte product quality. Secondly, the patented product is a multi-component complex salt system containing various boron-sulfur complex salt isomers. The product composition is complex and poorly controllable, making it impossible to precisely synthesize a single active component. The consistency of electrochemical performance is difficult to guarantee. Boron trifluoride sulfate metal salt appears as a byproduct, accounting for 0.01%~0.5%, making it difficult to use at high concentrations. Furthermore, the patent does not precisely control the side reactions and lacks a dedicated side-reaction control process. The synthesis process easily generates chain-like and branched polymeric byproducts, significantly increasing the difficulty of product purification and making it unsuitable for the high purity requirements of lithium-ion battery electrolyte raw materials. During the reaction, the boron-sulfur coordination structure is easily disordered, and the solvent is easily decomposed, limiting product purity and stability. Therefore, it is still necessary to develop better lithium / sodium salts based on different anions.

[0005] Lithium sulfate is a lithium salt insoluble in carbonate solvents and cannot be used in lithium battery electrolytes. When boron trifluoride solution reacts with lithium sulfate, the lithium sulfate initially does not dissolve, seemingly indicating no reaction. However, according to further research by the inventors of this application, it was unexpectedly discovered that under specific conditions, boron trifluoride can form a fairly stable complex salt with lithium sulfate, and this complex exhibits good solubility. Furthermore, there are currently no reports on the industrial-scale synthesis process of boron trifluoride combined with lithium sulfate metal salts. Summary of the Invention

[0006] In view of this, the purpose of the present invention is to provide a method for preparing boron trifluoride sulfate metal salt in liquid phase, which provides a simple process, controllable reaction, high product stability, and is suitable for lithium / sodium battery production lines. This method enables low-cost and large-scale preparation of boron trifluoride sulfate metal salt, and overcomes the shortcomings of lithium sulfate in the low solubility of organic solvents such as carbonates, which makes it difficult to apply in electrolytes on a large scale.

[0007] The technical solution adopted in this invention is as follows: A method for preparing boron trifluoride sulfate metal salt in the liquid phase, based on anhydrous metal sulfate salt and a gaseous boron trifluoride or non-gase boron trifluoride organic solvent complex, reacting in a liquid-phase organic solvent, the reaction equation including the following: ; Wherein, M is either lithium atom or sodium atom; the organic solvent in the non-gas phase boron trifluoride organic solvent complex and the liquid phase organic solvent can be the same solvent or different solvents, preferably the same solvent; The reaction product is post-processed to obtain the boron trifluoride sulfate metal salt. It should be noted that the boron trifluoride sulfate metal salt involved in this application can be a boron trifluoride sulfate metal salt solution, or the solvent can be concentrated or distilled to obtain a boron trifluoride sulfate metal salt solid.

[0008] Preferably, the organic solvent in the liquid-phase organic solvent and the non-gas-phase boron trifluoride organic solvent complex is a carbonate or ether organic solvent; more preferably, the carbonate is a chain ester or cyclic ester with 3-7 carbon atoms, including but not limited to dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, propylene carbonate, etc.; the ether organic solvent is a chain ether or cyclic ether with 4-8 carbon atoms, including but not limited to diethyl ether, dipropyl ether, ethylpropyl ether, tetrahydrofuran, etc.

[0009] Preferably, the reaction temperature is set between -20 and 50°C, more preferably between -5 and 20°C.

[0010] Preferably, the molar ratio of boron trifluoride to anhydrous metal sulfate is 2.0-3.5:1, more preferably 2.2-3.2:1, and even more preferably 2.6-3.0:1; the reaction time is 2-10 h, more preferably 4-8 h.

[0011] Preferably, it includes at least the following steps: S1. Pre-preparation of suspension: Under an inert gas protective atmosphere, the dried anhydrous metal sulfate is uniformly dispersed in a liquid-phase ultra-dry organic solvent to form a solid-liquid suspension system; S2. Coordination reaction: Gas-phase boron trifluoride or a non-gas-phase boron trifluoride organic solvent complex is introduced into the solid-liquid suspension system obtained in step S1 to carry out the reaction and obtain a reaction solution; S3. Post-treatment of the reaction solution: The reaction solution obtained in step S2 is filtered, and the filtrate is used as a boron trifluoride sulfate metal salt solution, which can be directly used in lithium / sodium ion batteries; or, the solvent in the reaction solution is concentrated to a viscous state and filtered, or the solvent in the reaction solution is directly distilled to dryness to obtain boron trifluoride sulfate metal salt solid; more preferably, if it is desired to obtain boron trifluoride sulfate metal salt solid, ether solvents with lower boiling points should be preferred in the selection of liquid phase organic solvent.

[0012] Preferably, in step S1, the anhydrous metal sulfate salt includes the following drying process: Anhydrous metal sulfate raw materials are placed in a vacuum drying device and dried for 8-12 hours at 100-150℃ and a vacuum degree ≤-0.095 MPa. The water content of the dried anhydrous metal sulfate salt is ≤20ppm.

[0013] Preferably, in step S1, the solid content of the anhydrous metal sulfate in the solid-liquid suspension system is 2-20 wt%, more preferably 3-8 wt%.

[0014] Preferably, in step S2, the coordination reaction is carried out under an inert gas atmosphere; when the raw material is purged boron trifluoride, the purging time of the purged boron trifluoride gas is controlled to be more than 3 hours, more preferably 4-6 hours; when the raw material is a non-gas-phase boron trifluoride organic solvent complex, the non-gas-phase boron trifluoride organic solvent complex is added to the solid-liquid suspension system in batches, the feeding time is controlled to be 2-5 hours, and stirring is carried out during the feeding process to avoid excessive accumulation of boron trifluoride.

[0015] Preferably, the boron trifluoride sulfate metal salt (solution / solid) has boron trifluoride sulfate metal salt compound as the main active component, and further includes tetrafluoroborate, compound I, and compound II; wherein, The tetrafluoroborate includes the structural formula: ; Compound I comprises the following structural formula: ; The compound II has the following structural formula: ; The total mass percentage of the tetrafluoroborate, compound I, and compound II in the metal salt of boron trifluoride sulfate does not exceed 10%, preferably 2-8%. Suitable for use as a compound electrolyte for lithium / sodium batteries with high-nickel ternary and silicon-carbon anodes.

[0016] It should be noted that the inert gas used throughout this application may be nitrogen or argon.

[0017] The working mechanism of this invention is as follows: using anhydrous metal sulfate and boron trifluoride as core reactants, and an organic solvent (preferably ultra-dry carbonate) as the reaction dispersion medium, a solid-liquid heterogeneous coordination synthesis reaction is carried out in an anhydrous, inert, and sealed atmosphere. At the same time, this invention does not require complex post-processing steps such as crystallization purification, solvent replacement, and distillation purification to obtain a liquid functional lithium / sodium salt composition suitable for lithium / sodium battery formulation systems. The product has multiple functions such as interfacial film formation and inhibition of positive electrode metal ion dissolution. The overall process is simple, highly controllable, and produces few by-products, making it suitable for large-scale industrial production applications.

[0018] Furthermore, this invention achieves precise and controllable coordination reaction by controlling the reaction temperature (firstly, by utilizing a low-temperature environment to weaken the strong Lewis acid activity of boron trifluoride, significantly suppressing the sulfate SO bond cleavage side reaction; and secondly, by using an organic solvent (preferably a carbonate) as a mild coordination solvent, which can moderately complex free boron trifluoride, avoiding side reactions caused by excessive local materials, thus enabling the stable preparation of high-purity, high-stability boron trifluoride sulfate metal salt electrolyte mother liquor) and regulating the molar ratio between anhydrous sulfate metal salt and boron trifluoride. This effectively ensures the forward progress of the main reaction, maximizes the formation ratio of the target product boron trifluoride sulfate metal salt, and simultaneously controls and suppresses subsequent secondary side reactions between metal fluorides and boron trifluoride, reducing the content of tetrafluoroborate byproducts, ultimately ensuring the stability and excellent electrochemical performance of the product electrolyte system.

[0019] The main beneficial effects of this invention are: 1. This invention is the first to use a suspension system formed by an organic solvent (preferably carbonate) and anhydrous metal sulfate to synthesize boron trifluoride sulfate. It can precisely and controllably suppress secondary side reactions, significantly reduce the generation of lithium / sodium tetrafluoroborate and other impurities, and eliminate the need for complex post-processing steps such as crystallization purification, solvent replacement, and distillation purification. The process is extremely simple and can be directly compounded in lithium / sodium battery production lines. 2. By controlling the reaction temperature and limiting the optimal BF3 feed ratio, the sulfate cleavage and BF3-catalyzed solvent decomposition were suppressed, the side reactions were controllable and the product stability was high, effectively solving the pain points of complex by-products and low purity in traditional synthesis processes. 3. The entire process is carried out in a water-free and oxygen-free environment (preferably at low temperatures), with low equipment requirements, high safety, good process tolerance, and easy industrial-scale production. Attached Figure Description

[0020] Appendix Figure 1 This is the NMR characterization image of the product obtained in Example 1 of the present invention. Detailed Implementation

[0021] This embodiment proposes a method for preparing boron trifluoride sulfate metal salt in the liquid phase. The method involves the reaction of anhydrous boron trifluoride metal salt and a gaseous boron trifluoride or non-gase boron trifluoride organic solvent complex in a liquid-phase organic solvent. The reaction equation includes the following: ; Wherein, M is any one of lithium atom and sodium atom; the organic solvent in the non-gas phase boron trifluoride organic solvent complex and the liquid phase organic solvent can be the same solvent or different solvents, preferably the same solvent; The reaction product is post-processed to obtain boron trifluoride sulfate metal salt. The boron trifluoride sulfate metal salt can be a solution (which can be directly used as a liquid additive in lithium / sodium battery electrolytes), or its solvent can be concentrated or distilled to directly obtain solid boron trifluoride sulfate metal salt (which can also be used as a solid additive in lithium / sodium battery electrolytes).

[0022] Preferably, in this embodiment, the organic solvent in the liquid-phase organic solvent and the non-gas-phase boron trifluoride organic solvent complex is a carbonate or ether organic solvent; more preferably, the carbonate is a chain ester or cyclic ester with 3-7 carbon atoms, including but not limited to dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, propylene carbonate, etc.; the ether organic solvent is a chain ether or cyclic ether with 4-8 carbon atoms, including but not limited to diethyl ether, dipropyl ether, ethylpropyl ether, tetrahydrofuran, etc.

[0023] More preferably, in this embodiment, when the boron trifluoride sulfate metal salt is in the state of a boron trifluoride sulfate metal salt solution, the organic solvent in the liquid phase (also serving as the main liquid phase) or the organic solvent in the non-gas phase boron trifluoride organic solvent complex is a carbonate organic solvent (specifically, ultra-dry grade carbonate with a water content ≤50ppm, more preferably ≤20ppm); preferably, in this embodiment, the carbonate is a chain ester or cyclic ester with 3-7 carbon atoms.

[0024] Preferably, in this embodiment, the reaction temperature is set to -20 to 50°C and kept constant, more preferably -5 to 20°C. Implementation verification has shown that this preferred temperature window setting can very effectively suppress SO bond breaking and solvent decomposition, minimize side reactions, and achieve the highest product purity.

[0025] Preferably, in this embodiment, the molar ratio of boron trifluoride to anhydrous metal sulfate is 2.0-3.5:1, more preferably 2.2-3.2:1, and even more preferably 2.6-3.0:1; the reaction time (note: the "reaction time" data involved in this application does not include the feeding time) is 2-10h, more preferably 4-8h.

[0026] Preferably, this embodiment includes at least the following steps: S1. Pre-preparation of suspension: Under an inert gas protective atmosphere, the dried anhydrous metal sulfate salt is uniformly dispersed in a liquid-phase ultra-dry organic solvent to form a solid-liquid suspension system; preferably, in this step S1, the anhydrous metal sulfate salt includes the following drying process: The anhydrous metal sulfate raw material is placed in a vacuum drying device and dried for 8-12 hours at 100-150℃ and a vacuum degree ≤-0.095 MPa to completely remove adsorbed water and trace amounts of crystal water and prevent hydrolysis side reactions caused by moisture. More preferably, in this embodiment, after drying is completed and the material is naturally cooled to room temperature, it is transferred to a glove box with a water and oxygen content of ≤10 ppm and sealed for storage for later use. In this embodiment, the water content of the dried anhydrous metal sulfate is ≤20 ppm.

[0027] Preferably, in step S1, the solid content of the anhydrous metal sulfate in the solid-liquid suspension system is 2-20 wt%, more preferably 3-8 wt%, which balances reaction uniformity and production capacity, avoiding the problems of uneven reaction due to excessive solid content and insufficient production capacity due to excessively low solid content.

[0028] S2. Low-temperature coordination reaction: Gas-phase boron trifluoride or a non-gas-phase boron trifluoride organic solvent complex is introduced into the solid-liquid suspension system obtained in step S1, and the reaction occurs under a preset reaction temperature to obtain a reaction solution. Preferably, in step S2, the coordination reaction is carried out under an inert gas atmosphere; that is, the entire reaction process is conducted under an inert gas atmosphere. Preferably, the oxygen content of the entire reaction system is controlled to be ≤10%. To prevent water vapor and oxygen intrusion that could trigger side reactions, the feed rate should be controlled to ppm. When the raw material is fumed boron trifluoride, the feeding time should be controlled to be more than 3 hours, preferably 4-6 hours, with uniform flow rate being preferred. The feed rate should be calculated based on the flow rate or by weighing. After the gas is introduced, continue the reaction at a constant temperature and uniform rate for 2-10 hours to prevent excessive local accumulation of boron trifluoride. When the raw material is a non-fumed boron trifluoride organic solvent complex, add the non-fumed boron trifluoride organic solvent complex to the solid-liquid suspension system in batches, with the feeding time controlled to 2-5 hours. Stirring should be carried out during the feeding process (stirring speed preferably set to ≥200 rpm) to avoid excessive accumulation of boron trifluoride. After the addition is complete, continue the reaction for 2-10 hours.

[0029] S3. Post-treatment of the reaction solution: The reaction solution obtained in step S2 is filtered, and the resulting filtrate is used as the electrolyte solution of boron trifluoride sulfate metal salt; preferably, in this step S3, a polytetrafluoroethylene (PTFE) filter membrane is used to remove unreacted solid residues and trace amounts of flocculent byproducts, ultimately obtaining a clear, transparent, and highly stable boron trifluoride sulfate metal salt carbonate solution; more preferably, in this embodiment, the PTFE filter membrane has a pore size of 0.22 μm and is kept in a low-temperature inert environment throughout the filtration process; It should be noted that in other embodiments of step S3, the following scheme can also be used to obtain boron trifluoride sulfate metal salt solid: The solvent in the reaction solution is concentrated to a viscous state and then filtered, or the solvent in the reaction solution is directly distilled to dryness.

[0030] Preferably, in this embodiment, the boron trifluoride sulfate metal salt solution is mainly composed of boron trifluoride sulfate metal salt compound, and also includes tetrafluoroborate, compound I, and compound II; wherein, Tetrafluoroborates include the following structural formulas: The corresponding side reaction formula is: ; Compound I includes the following structural formula: The corresponding side reaction formula is: ; Compound II includes the following structural formula: The corresponding side reaction formula is: ; The total mass percentage of tetrafluoroborate, Compound I, and Compound II in the mass of boron trifluoride sulfate metal salt shall not exceed 10%, more preferably 2-8%. The boron trifluoride sulfate metal salt solution prepared in this embodiment is free of solvent decomposition impurities and can be directly used as a compound electrolyte for high-nickel ternary lithium / sodium batteries with silicon-carbon anodes.

[0031] To enable those skilled in the art to better understand the technical solutions of this invention, based on the above implementation schemes, the following embodiments are proposed. Obviously, the described embodiments are merely some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.

[0032] Example 1: Preparation of boron trifluoride sulfate metal salt solution according to the following procedure (1) Raw material pretreatment: Take industrial grade anhydrous lithium sulfate, place it in a vacuum oven, dry it at 130℃ and -0.095 MPa for 10h, cool it naturally to room temperature, and then transfer it to a glove box with water and oxygen content ≤10 ppm for sealed storage for later use; (2) Preparation of suspension: Under the inert atmosphere of nitrogen, take 80g of ultra-dry dimethyl carbonate, add 6g of dried anhydrous lithium sulfate, stir at room temperature and speed for 30 min to form a uniform and stable white solid-liquid suspension. (3) Low temperature coordination reaction: The suspension system was cooled to 10 °C and stirred continuously at a constant speed. Boron trifluoride gas was slowly introduced by constant pressure micro-aeration. The molar ratio of boron trifluoride to anhydrous lithium sulfate was controlled at 2.6:1 (the amount of boron trifluoride introduced was calculated based on the weight gain of the system). The reaction was continuously aerated for 4 h. During the aeration process, local material enrichment was avoided. The reaction was continued for 5 h (i.e., the "reaction time") until the system was basically clear. (4) Filtration and impurity removal: After the reaction is completed, the mixture is kept at 10°C (the principle of setting this aging temperature is to maintain it under the reaction temperature conditions; other examples and comparative examples are set according to this principle) for 1 hour to promote the flocculation and precipitation of trace impurities. The reaction solution is filtered using a 0.22 μm polytetrafluoroethylene filter membrane to remove unreacted solid residues and trace flocculent impurities, resulting in a clear and transparent dimethyl boron trifluoride lithium sulfate carbonate solution, which is the product of Example 1.

[0033] The product obtained in Example 1 was subjected to the following performance tests: Please refer to the above. Figure 1 As shown, through¹ 9F NMR (376MHz) characterization showed a δ (ppm) of -150.96 (main component), with chemical shifts of -151.97ppm, -147.91ppm, and -148.41ppm for other components. The main component of the product was lithium boron sulfate trifluoride, with only small amounts of lithium tetrafluoroborate byproduct, compound I, and compound II. The mass ratio of the four components (lithium boron sulfate trifluoride: lithium tetrafluoroborate: compound I: compound II) was 100:3.5:0.6:0.1, with no carbonate decomposition impurities. The system had a moisture content of ≤20 ppm and excellent electrochemical stability.

[0034] Example 2: The remaining technical solutions of this Example 2 are the same as those of Example 1, except that: in this Example 2, the reaction temperature in the (3) low-temperature coordination reaction is set to -5℃, the solvent is ultra-dry methyl ethyl carbonate, the molar ratio of boron trifluoride to anhydrous lithium sulfate is 2.8:1, and the reaction time is still 5h.

[0035] The results showed that secondary side reactions were further suppressed under lower temperature reaction conditions, the proportion of lithium boron trifluoride sulfate in the system was higher, the impurity content was further reduced, and the ratio of lithium boron trifluoride sulfate, lithium tetrafluoroborate byproduct, compound 1, and compound II was 100:3.0:0.2:0.03. The purity of the product was better than that of Example 1, and it is suitable for the preparation of high-purity electrolyte systems.

[0036] Example 3: The remaining technical solutions of this embodiment 3 are the same as those of embodiment 1, except that: in this embodiment 3, the molar ratio of boron trifluoride to anhydrous lithium sulfate is 3.0:1, the boron trifluoride used is a boron trifluoride-dimethyl carbonate complex, which is added slowly to the suspension system in batches, and the feeding time is controlled at about 4 hours; the reaction time is 3 hours.

[0037] The results show that appropriately increasing the amount of boron trifluoride can improve the conversion rate of lithium sulfate and slightly increase the content of lithium tetrafluoroborate by-product. The overall system still meets the standards for use of lithium battery electrolyte and is suitable for large-scale production.

[0038] Example 4: The remaining technical solutions of this embodiment 4 are the same as those of embodiment 1, except that: in this embodiment 4, the reaction temperature in (3) low-temperature coordination reaction is set to 35°C.

[0039] The results show that the acid activity of boron trifluoride is greatly enhanced under the reaction temperature conditions. This not only causes the breaking of the sulfate SO bond and the decomposition of DMC solvent, but also promotes the continuous reaction of a large amount of lithium fluoride with boron trifluoride. The by-products of lithium tetrafluoroborate increase, the system becomes turbid and yellow, and the impurity content is high, which makes it difficult to meet the requirements of high-quality lithium battery electrolyte. This further verifies the core optimization technology advantage of the present invention in controlling the side reaction at low temperature (-5 to 20°C).

[0040] Example 5: The remaining technical solutions of this embodiment 5 are the same as those of embodiment 1, except that: in this embodiment 5, the molar ratio of boron trifluoride to anhydrous lithium sulfate is 2.0:1, and the reaction time is 20h.

[0041] The results showed that under this material ratio, a large amount of solid remained in the system. The solid components were mainly unreacted lithium sulfate and lithium sulfate that was not fully coordinated with boron trifluoride. This solid was insoluble or sparingly soluble in carbonate solvents, making it difficult to meet the standards for use in electrolytes. This further verified the core technical advantage of this invention, which set the molar ratio of boron trifluoride to anhydrous metal sulfate to 2.2-3.2:1 (more preferably 2.6-3.0:1) as the optimal reaction conditions.

[0042] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

[0043] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A process for the liquid phase preparation of metal salts of bifluoride bisulfate characterized in that, Based on anhydrous metal sulfate salts and fumed or non-fumed boron trifluoride organic solvent complexes, the reaction occurs in a liquid organic solvent, and the equations for this reaction are as follows: ; Where M is either a lithium atom or a sodium atom; The reaction product was post-treated to obtain the boron trifluoride sulfate metal salt. It should include at least the following steps: S1. Pre-preparation of suspension: Under an inert gas protective atmosphere, the dried anhydrous metal sulfate is uniformly dispersed in a liquid-phase ultra-dry organic solvent to form a solid-liquid suspension system; S2. Coordination reaction: Gas-phase boron trifluoride or a non-gas-phase boron trifluoride organic solvent complex is introduced into the solid-liquid suspension system obtained in step S1 to carry out the reaction and obtain a reaction solution; S3. Post-processing of the reaction solution: The reaction solution obtained in step S2 is filtered, and the filtrate is used as a boron trifluoride sulfate metal salt solution, which can be directly used in lithium / sodium ion batteries; or, the solvent in the reaction solution is concentrated to a viscous state and filtered, or the solvent in the reaction solution is directly distilled to dryness to obtain boron trifluoride sulfate metal salt solid. The organic solvent in the liquid-phase organic solvent and the non-gas-phase boron trifluoride organic solvent complex is a carbonate; the carbonate is a chain ester or cyclic ester with 3-7 carbon atoms; the reaction temperature is set at -5 to 20°C; the molar ratio of boron trifluoride to anhydrous metal sulfate is 2.2-3.2:1; the reaction time is 2-10 h.

2. The method for preparing boron trifluoride sulfate metal salt by liquid phase according to claim 1, characterized in that, In step S1, the anhydrous metal sulfate salt includes the following drying process: Anhydrous metal sulfate raw materials are placed in a vacuum drying device and dried for 8-12 hours at 100-150℃ and a vacuum degree ≤-0.095 MPa. The water content of the dried anhydrous metal sulfate salt is ≤20ppm.

3. The method for preparing boron trifluoride sulfate metal salt by liquid phase according to claim 1, characterized in that, In step S1, the solid content of the anhydrous metal sulfate in the solid-liquid suspension system is 2-20 wt%.

4. The method for preparing boron trifluoride sulfate metal salt by liquid phase according to claim 1, characterized in that, In step S2, the coordination reaction is carried out under an inert gas atmosphere. When the raw material is fumed boron trifluoride, the fumed boron trifluoride gas introduction time is controlled to be more than 3 hours. When the raw material is a non-fumed boron trifluoride organic solvent complex, the non-fumed boron trifluoride organic solvent complex is added to the solid-liquid suspension system in batches, and the addition time is controlled to be 2-5 hours. Stirring is carried out during the addition process to avoid excessive boron trifluoride.

5. The method for preparing boron trifluoride sulfate metal salt by liquid phase according to claim 1, characterized in that, The boron trifluoride sulfate metal salt has boron trifluoride sulfate metal salt compound as the main active component, and also includes tetrafluoroborate, compound I, and compound II; wherein... The tetrafluoroborate includes the structural formula: ; Compound I comprises the structural formula: ; The compound II has the following structural formula: ; The total mass of the tetrafluoroborate, Compound I, and Compound II accounts for no more than 10% of the mass of the boron trifluoride sulfate metal salt.

Citation Information

Patent Citations

  • Electrolyte additive composition and use thereof

    CN119340478B

  • Preparation method of lithium difluorosulfate borate

    CN116199230A

  • Electrolyte additive composition and application thereof

    CN119340478A