A laser powder bed melting method for preparing high-performance gradient metal matrix composites.

By setting a separator in the powder supply chamber of the laser powder bed melting equipment and adjusting the powder composition ratio, the equipment limitations in the preparation of gradient metal matrix composites are solved, achieving high-throughput component screening and performance improvement, and applicable to a variety of metal matrix composites.

CN123060118APending Publication Date: 2026-11-10HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611453864.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies require additional powder mixing devices or dual powder bin mechanisms when preparing gradient metal matrix composites, which leads to slow material development progress and increased costs, and makes it impossible to prepare gradient materials with continuously changing composition in ordinary commercial equipment.

Method used

Separators are installed in the powder supply chamber of a laser powder bed melting device to fill different regions with powders of different compositions. By adjusting the angle, position, and shape of the separators, combined with the sample arrangement, the composition ratio can be adjusted to prepare composite materials with continuously varying composition.

Benefits of technology

It enables the simultaneous printing of multiple materials with different composition gradients in ordinary commercial equipment, shortening the material composition screening cycle, reducing costs, and improving the reliability and consistency of material performance. It is applicable to a variety of metal matrix composite systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060118A_ABST
    Figure CN123060118A_ABST
Patent Text Reader

Abstract

This invention discloses a laser powder bed melting method for preparing high-performance gradient metal matrix composites, relating to the field of metal additive manufacturing. The method involves installing separators within the powder supply chamber of a powder bed melting device to separately fill different areas with two or more powders of different compositions. This allows the powders to form mixed powders of varying proportions at different locations within the substrate region during the powder spreading process. Without altering the basic forming principle of the equipment—that is, within ordinary commercial equipment without additional powder mixing devices—this invention enables the preparation of multiple composition gradient material samples within a specific composition range using two or more powders in a single additive manufacturing process. This provides a foundation for high-throughput material composition screening, microstructure and property studies, and the preparation of functionally graded materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal additive manufacturing, and in particular to a laser powder bed melting method for preparing high-performance gradient metal matrix composites. Background Technology

[0002] Metal matrix composites (MMCs) are widely used in aerospace and other fields with extreme service conditions due to their high specific strength, specific modulus, and high-temperature resistance. However, the introduction of reinforcing phases, while improving strength, reduces plasticity and toughness, becoming a major bottleneck limiting the expansion of MMC applications. Gradient metal matrix composites, by retaining the reinforcing phases for strengthening while retaining a portion of the matrix to provide plasticity to the material as a whole, achieve a synergistic improvement in strength and plasticity of MMCs.

[0003] Laser additive manufacturing technology, especially laser powder bed melting (L-PBF), offers numerous advantages such as near-net-shape forming and efficient integrated fabrication of complex structural components. However, due to the limitations of L-PBF processes, the preparation of metal matrix composites requires the pre-preparation of pre-alloyed powders with corresponding compositions, or the use of mechanical mixing devices to pre-mix the two powders to produce composites with a single composition. For the preparation of gradient metal matrix materials with continuously varying compositions, additional powder mixing devices or dual-powder-bin mechanisms are also necessary. These complex processes or additional devices significantly delay the progress of material development and increase the preparation cost of gradient materials. Therefore, if gradient materials with continuously varying compositions could be prepared in a single printing process using a standard commercial metal printer, high-throughput composition screening could be achieved, greatly reducing experimental costs and accelerating the progress of material composition design and gradient material development. Summary of the Invention

[0004] To address the aforementioned technical problems, this invention provides a partitioned powder loading and printing method suitable for laser powder bed melting equipment. Without altering the basic forming principle of the equipment, i.e., in ordinary commercial equipment without additional powder mixing devices, it enables the preparation of multiple material samples with different composition gradients within a certain composition range in a single additive manufacturing process using two or more powders with different compositions. This provides a foundation for high-throughput material composition screening, microstructure and performance research, and the preparation of functionally graded materials.

[0005] To achieve the above objectives, this invention incorporates a separator within the powder supply chamber of a powder bed melting device. This allows two or more powders with different compositions to be loaded into different areas, resulting in mixed powders of varying proportions at different locations on the substrate during the powder spreading process. By altering the angle, position, and shape of the separator, and considering its placement on the forming substrate, the location and range of different local powder ratio areas can be adjusted, thereby obtaining composite material samples with different matrix compositions and a continuous gradient of composition. Specifically, the method for changing the "angle and shape of the separator" is as follows: Figure 8 As shown in the diagram. For a straight baffle, the angle of the baffle is the angle θ between the baffle and the horizontal line of the powder supply hopper, and θ ranges from 0° to 180°. The shape of the baffle can be a straight line or an irregular shape, and the shape of the baffle depends on the designed gradient material composition range. For example, for a gradient composite material with a parabolic variation in composition, a parabolic baffle design as shown in the diagram can be used to form a parabolic component variation function on the forming platform that corresponds one-to-one with the powder hopper area. Obviously, this method can realize single-gradient, dual-gradient, and even arbitrary composition distribution gradient composite materials. For such gradient materials, Example 1 has already illustrated the preparation of high-strength and tough composite materials using this preparation method. Furthermore, the dual-gradient or parabolic composition gradient composite materials obtained using this preparation method will also achieve reliable performance improvements.

[0006] The present invention discloses a laser powder bed melting method for preparing high-performance gradient metal matrix composites, the method being as follows:

[0007] Step 1: Based on the required gradient material composition, the matrix alloy powder and the mixed powder containing the reinforcing phase are respectively designated as end-member powder A and powder B;

[0008] The end-member powder A is titanium and titanium alloys, aluminum and aluminum alloys, nickel and nickel alloys, iron and iron alloys, magnesium and magnesium alloys; the reinforcing phase powder is one or more of TiB2, LaB6, BN, ZrB2, Si, SiC, TiC, and WC.

[0009] Step 2: Add a dividing piece to the powder hopper of the laser powder bed melting equipment to divide the powder hopper into multiple powder loading areas. The dividing piece can be a straight line, a broken line, a curve, or a combination of three. The thickness of the dividing piece is ≤1mm, the horizontal dimension x-axis component is ≤powder hopper length, and the vertical dimension is ≤powder hopper width.

[0010] Step 3: Add the end-member powder A and powder B from Step 1 to the powder loading area divided by the separator in Step 2; the content of the reinforcing phase is 0.1~2 wt.%; when the content of the reinforcing phase is 0.1~1 wt.%, a broken line or curved separator is used; when the content of the reinforcing phase is 1-2 wt.%, a straight line separator is used; set the printing parameters and print to obtain a high-performance gradient metal matrix composite material; during printing, the doctor blade speed is limited to below 5 mm / s, and the preheating temperature is ≥100℃.

[0011] Furthermore, the reinforcing phase is determined based on the selected matrix alloy. If the matrix alloy is titanium or titanium alloys, the reinforcing phase powder is TiB. 2、 The reinforcing phase is LaB6, BN, ZrB2, or Si; if the matrix alloy is aluminum or aluminum alloys or magnesium or magnesium alloys, the reinforcing phase is SiC; if the matrix alloy is nickel or nickel alloys, the reinforcing phase is TiB2; if the matrix alloy is iron or iron alloys, the reinforcing phase is TiC or WC.

[0012] Furthermore, the dividing element is arranged along the diagonal or approximately diagonal of the rectangular powder supply compartment, dividing the powder supply compartment into two triangular or approximately triangular powder loading areas.

[0013] Furthermore, the resin material used for the dividing component is manufactured by a resin printer, and the thickness of the dividing component partition is 0.5~1.5mm.

[0014] Furthermore, the powder hopper is divided into three or more powder loading areas, and each area is filled with three or more powders of different compositions. The three or more powders of different compositions are powders containing three or more different reinforcing phase contents and the same matrix alloy, or powders containing three or more different matrix alloys with the same reinforcing phase content.

[0015] Further, the step of adding the end-member powder A and powder B from step one to the powder-filling area divided by the divider in step two specifically involves:

[0016] 1) Add the end-member powder A and powder B from step one to the powder loading area divided by the divider in step two, so that the types of powder in all areas are different.

[0017] 2) Use a scraper to level the powder in each area to achieve the same or nearly the same filling height;

[0018] 3) After the powder filling is completed, the separator is removed, and each powder is kept in its corresponding area.

[0019] 4) Drive the scraper or powder spreading roller to move in a predetermined direction to spread powder A and powder B in the powder supply hopper to the forming area, so that different local proportions of powder A and powder B are formed at different positions in the forming area.

[0020] Furthermore, when setting the printing parameters and performing printing, the laser power and scanning speed are 120~220W and 700~1300mm / s, respectively, when the base alloy is titanium or titanium alloy.

[0021] Furthermore, when setting the printing parameters and performing printing, the laser power and scanning speed are 180W and 900mm / s when the matrix alloy is TC4 alloy and the reinforcing phase is 1wt.%TiB2; when the TiB2 content is 0.1-2wt.%, the laser power and scanning speed range is 150~210W and 800~1000mm / s.

[0022] Compared with the prior art, the present invention has at least the following beneficial effects:

[0023] (1) The present invention uses two or a few types of end-member powders as raw materials, and uses oblique partitioning powder loading and conventional powder spreading movement to form multiple local powder ratios in the forming area, without the need to weigh and premix powders for each target intermediate component separately.

[0024] (2) The present invention can simultaneously prepare multiple independent samples with different components in one powder loading, one equipment preparation and one printing process, transforming the traditional sample preparation method into one-time preparation, shortening the material component screening cycle and reducing powder consumption.

[0025] (3) Forming multiple samples under the same equipment conditions, atmosphere and similar thermal history conditions is beneficial to reduce batch differences and improve the reliability of comparing the microstructure and properties of samples with different components.

[0026] (4) The present invention only requires the addition of a simple separator to the powder supply hopper of the existing powder bed melting equipment, without the need for a special multi-hopper quantitative powder feeding system, and the equipment modification and post-processing are simple.

[0027] (5) By changing the angle, position, shape, number of powder loading areas, and sample arrangement coordinates of the separators, the number of samples, component ranges, and component intervals can be adjusted, facilitating the formation of a sample library for material screening. The sample arrangement coordinates are achieved by printing on processing platforms for different components.

[0028] (6) This invention is not limited to titanium-based composite materials, but can be extended to various metal-based composite material systems such as aluminum-based, nickel-based, iron-based, cobalt-based, magnesium-based and copper-based, provided that the powder bed melt forming performance and safety are met.

[0029] (7) In the example of TC4 composite powder of pure TC4 powder and 2 wt.% TiB2, samples at different positions obtained by the same printing show different metallographic structures and microhardness. The present invention can simultaneously obtain a variety of gradient metal matrix composite material samples with different compositions within two end-member composition ranges.

[0030] (8) In the comparative example, the room temperature tensile properties of the homogeneous alloy and the composite material were tested, demonstrating that the gradient distribution of the composite material can effectively improve the strength and plasticity of the material.

[0031] (9) This invention can also be applied to the development of functionally graded materials and high-throughput alloy compositions. Attached Figure Description

[0032] Figure 1 This is a macroscopic photograph of the substrate and powder-coating hopper after printing in Example 1.

[0033] Figure 2 Macroscopic photographs of the substrate and printed sample after printing in Example 1;

[0034] Figure 3 These are gradient microstructure images of different sampling locations after printing in Example 1;

[0035] Figure 4 The diagram shows the room temperature tensile mechanical properties of the gradient composite material in Example 1 and the homogeneous composite material in the comparative example.

[0036] Figure 5 This is a schematic diagram of powder placement and printing in the powder-spreading hopper for Example 1;

[0037] Figure 6 This is a schematic diagram of powder placement and printing in the powder-spreading hopper for Example 2;

[0038] Figure 7 This is a linear fit plot of Vickers hardness as a function of the theoretical reinforcing phase content;

[0039] Figure 8 This is a schematic diagram showing the angle and shape of the partition plate of the present invention. Detailed Implementation

[0040] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the spirit of the contents disclosed in the present invention will be described in detail below. After understanding the embodiments of the present invention, any person skilled in the art can make changes and modifications based on the technology taught in the present invention without departing from the spirit and scope of the present invention.

[0041] The illustrative embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention.

[0042] Example 1

[0043] This embodiment utilizes a BLT-S210 laser powder bed melting system, employing pure TC4 powder and a TC4 mixture containing 2 wt.% TiB2 as two end-member powders to prepare multiple independent samples with different nominal TiB2 contents in a single printing process. The specific steps are as follows:

[0044] (1) Preparation of powder A and powder B. Powder A is pure TC4 alloy powder suitable for laser powder bed melting; powder B is a mixed powder with TC4 alloy powder as the matrix and TiB2 mass fraction of 2 wt.%. The mixed powders were mixed in an argon atmosphere using a planetary ball mill at a speed of 180-220 r / min for 4-5 h with a ball-to-powder ratio of 3:1. Both powders were sieved and dried before use to ensure good flowability and spreadability.

[0045] (2) Design and fabrication of the separator plate. The effective planar dimensions of the powder supply chamber and the forming substrate of the metal printer equipment used are both 107 mm × 126 mm. (Reference) Figure 7 A detachable PLA linear baffle is printed along the diagonal of a rectangle inside the powder supply hopper, dividing the hopper into two triangular areas. These two triangular areas are the pre-filling positions for powder A and powder B, determining the mixing ratio of the two powders. The lower edge of the baffle fits into the bottom of the powder supply hopper, and both ends of the baffle fit into the hopper wall to reduce premature cross-mixing during the powder filling process.

[0046] (3) Powder loading. Pure TC4 powder is loaded onto one side of the baffle, and 2 wt.% TiB2 / TC4 composite powder is loaded onto the other side, ensuring both powders reach the same or substantially the same loading height and leveling the powder surface. After loading, the baffle is smoothly removed, allowing the two powders to form an initial distribution diagonally adjacent within the powder supply chamber. Figure 3 ).

[0047] (4) Part design and printing. The parts to be printed are set, and appropriate laser printing parameters are selected for layer-by-layer printing until completion. Preferably, a room temperature tensile test is performed on a gradient composite material with a theoretical TiB2 content range of 0.5-1.5 wt.%, and the stress-strain curve is obtained. Figure 4 The Vickers hardness changes in eight regions along the gradient direction were tested. With increasing nominal B content, the Vickers hardness of the gradient material increased significantly, exhibiting significant gradient material mechanical response characteristics (Table 1). It should be noted that the measured Vickers hardness values ​​basically satisfy a linear relationship with the theoretical composition. Figure 7 Its linear correlation R 2The value reached 0.98. This embodiment not only prepared functionally graded materials, but also quantitatively characterized the effect of TiB2 content on material hardness in a single experiment, saving a lot of experimental steps.

[0048] Table 1

[0049]

[0050] Comparative Example

[0051] In addition to the above-mentioned determination of the effect of TiB2 content on Vickers hardness, the gradient composite material prepared by this invention also has an improved level of strength and toughness. In Example 1, due to the setting of the partition plate angle and the placement of the parts, the composition range of the gradient composite material is limited to 0.5-1.5 wt.%. This comparative example uses a BLT-S210 laser powder bed melting device to print pure TC4 powder, a TC4 mixed powder with high TiB2 content, and a non-gradient homogeneous TC4 mixed powder with low TiB2 content in three stages without partitioned powder loading. The mixed powders are obtained by the same powder mixing process as in Example 1. After printing, printed TC4 pure alloy, high-content titanium-based composite material (1.5 wt.%), and non-gradient homogeneous titanium-based composite material (1.0 wt.%) were obtained.

[0052] The room temperature tensile mechanical properties of the three homogeneous materials were tested. Figure 4 Compared to gradient composites, pure alloys exhibit lower plasticity due to the lack of reinforcing phases. High-TiB / TC4 composites, however, exhibit high strength but low plasticity. While non-gradient homogeneous composites possess strength and plasticity intermediate between the two, gradient composites of the same composition exhibit higher strength and similar plasticity. Therefore, it is evident that the gradient composites obtained in this invention possess superior mechanical properties. Figure 4 ).

[0053] Example 2

[0054] To further illustrate the effects of the present invention, this embodiment changes the spatial angle of the partition, replacing the diagonal partitioned powder loading in Embodiment 1 with V-shaped zigzag area powder loading, thereby achieving a dual-gradient structure of the printing material. Figure 6 As can be seen from the results of Example 1, by designing the partitioned powder loading scheme (multi-linear, wavy, etc.) and the spatial coordinates of the printed sample, it is possible to achieve a non-single gradient change in the content of the reinforcing phase in the composite material, but rather a multi-gradient or even customized functional change. The following is an experimental example of achieving a dual-gradient composite material based on this invention.

[0055] Using a BLT-S210 laser powder bed fusion apparatus, multiple independent samples with different nominal TiB2 contents were prepared in a single printing process, using pure TC4 powder and a TC4 mixture containing 2 wt.% TiB2 as the two end-member powders. The specific steps are as follows:

[0056] (1) Preparation of powder A and powder B. Powder A is pure TC4 alloy powder suitable for laser powder bed melting; powder B is a mixed powder with TC4 alloy powder as the matrix and TiB2 mass fraction of 2 wt.%. The mixed powders were mixed in an argon atmosphere using a planetary ball mill at a speed of 180-220 r / min for 4-5 h with a ball-to-powder ratio of 3:1. Both powders were sieved and dried before use to ensure good flowability and spreadability.

[0057] (2) Design and fabrication of the partition plate. The effective planar dimensions of the powder supply compartment and the forming substrate of the metal printer used are both 107 mm × 126 mm. A detachable PLA zigzag baffle is printed along the diagonal of a rectangle inside the powder supply compartment, dividing the powder supply compartment into three triangular areas. The lower edge of the baffle is attached to the bottom of the powder supply compartment, and the two ends of the baffle are attached to the compartment wall to reduce premature cross-mixing during the powder loading process.

[0058] (3) Powder filling. Pure TC4 powder is filled in the middle of the zigzag baffle, and 2 wt.% TiB2 / TC4 composite powder is filled on the other two sides to make the two powders reach the same or basically the same filling height and level the powder surface. After filling, the baffle is pulled out smoothly to make the two powders distributed in the powder supply hopper.

[0059] (4) Part design and printing. Set the parts to be printed, select appropriate laser printing parameters and print layer by layer until the end.

Claims

1. A method for preparing high-performance gradient metal matrix composites using laser powder bed melting, characterized in that, The method is as follows: Step 1: Based on the required gradient material composition, the matrix alloy powder and the mixed powder containing the reinforcing phase are respectively designated as end-member powder A and powder B; The end-member powder A is titanium and titanium alloys, aluminum and aluminum alloys, nickel and nickel alloys, iron and iron alloys, magnesium and magnesium alloys; the reinforcing phase powder is one or more of TiB2, LaB6, BN, ZrB2, Si, SiC, TiC, and WC. Step 2: Add a dividing piece to the powder hopper of the laser powder bed melting equipment to divide the powder hopper into multiple powder loading areas. The dividing piece can be a straight line, a broken line, a curve, or a combination of three. The thickness of the dividing piece is ≤1mm, the horizontal dimension x-axis component is ≤powder hopper length, and the vertical dimension is ≤powder hopper width. Step 3: Add the end-member powder A and powder B from Step 1 to the powder loading area divided by the separator in Step 2; the content of the reinforcing phase is 0.1~2 wt.%; when the content of the reinforcing phase is 0.1~1 wt.%, a broken line or curved separator is used; when the content of the reinforcing phase is 1-2 wt.%, a straight line separator is used; set the printing parameters and print to obtain a high-performance gradient metal matrix composite material; during printing, the doctor blade speed is limited to below 5 mm / s, and the preheating temperature is ≥100℃.

2. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1, characterized in that, The reinforcing phase is determined based on the selected matrix alloy. If the matrix alloy is titanium or titanium alloys, the reinforcing phase powder is TiB. 2、 The reinforcing phase is LaB6, BN, ZrB2, or Si; if the matrix alloy is aluminum or aluminum alloys or magnesium or magnesium alloys, the reinforcing phase is SiC; if the matrix alloy is nickel or nickel alloys, the reinforcing phase is TiB2; if the matrix alloy is iron or iron alloys, the reinforcing phase is TiC or WC.

3. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1, characterized in that, The dividing element is set along the diagonal or approximately diagonal of the rectangular powder supply compartment, dividing the powder supply compartment into two triangular or approximately triangular powder loading areas.

4. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1 or 3, characterized in that, The dividing component is made of resin material using a resin printer, and the thickness of the dividing component partition is 0.5~1.5mm.

5. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1, characterized in that, The powder hopper is divided into three or more powder loading areas, and each area is filled with three or more powders of different compositions. The three or more powders of different compositions are powders containing three or more different reinforcing phase contents and the same matrix alloy, or powders containing three or more different matrix alloys with the same reinforcing phase content.

6. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1, characterized in that, The step of adding the end-member powder A and powder B from step one to the powder-filling area divided by the divider in step two is specifically as follows: 1) Add the end-member powder A and powder B from step one to the powder loading area divided by the divider in step two, so that the types of powder in all areas are different. 2) Use a scraper to level the powder in each area to achieve the same or nearly the same filling height; 3) After the powder filling is completed, the separator is removed, and each powder is kept in its corresponding area. 4) Drive the scraper or powder spreading roller to move in a predetermined direction to spread powder A and powder B in the powder supply hopper to the forming area, so that different local proportions of powder A and powder B are formed at different positions in the forming area.

7. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1, characterized in that, The printing parameters are set and printing is performed. When the base alloy is titanium or titanium alloy, the laser power and scanning speed are 120~220W and 700~1300mm / s, respectively.

8. The laser powder bed melting method for preparing high-performance gradient metal matrix composites according to claim 1 or 7, characterized in that, The printing parameters are set and printing is performed. When the matrix alloy is TC4 alloy and the reinforcing phase is 1wt.%TiB2, the laser power and scanning speed are 180W and 900mm / s, respectively. When the TiB2 content is 0.1-2wt.%, the laser power and scanning speed ranges from 150 to 210W and 800 to 1000mm / s, respectively.