A black matte aluminum-plastic film and its preparation method

By controlling the cross-linking structure and surface properties of the matte layer, and using hydroxyl-containing resin components and isocyanate curing agents for cross-linking, the balance between inkjet printing compatibility and chemical resistance of black matte aluminum-plastic film was solved, achieving multiple performance improvements for high-end electronic products and lithium battery packaging materials.

CN123060971APending Publication Date: 2026-11-10SHANGHAI ENERGY NEW MATERIALS TECHNOLOGY CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611143421.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The existing matte layer of black matte aluminum-plastic film cannot simultaneously achieve good coding recognition, alcohol resistance, acetone resistance, and electrolyte resistance. Existing solutions cannot achieve a stable balance between coding compatibility and chemical resistance.

Method used

By controlling the crosslinking structure and surface properties of the matte layer, its surface dyne value is maintained between 34 mN/m and 40 mN/m. A hydroxyl-containing resin composition and an isocyanate curing agent are crosslinked at an NCO/OH equivalent ratio of 0.5 < R ≤ 1.5 to form a matte layer with appropriate surface energy and degree of crosslinking.

Benefits of technology

This technology enables black matte aluminum-plastic film to achieve excellent coding recognition, alcohol wiping resistance, acetone wiping resistance, and electrolyte resistance in high-end electronic products and lithium battery packaging materials, thereby improving the chemical stability and service life of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123060971A_ABST
    Figure CN123060971A_ABST
Patent Text Reader

Abstract

This invention discloses a black matte aluminum-plastic film and its preparation method. The black matte aluminum-plastic film comprises at least a heat-sealing layer, an aluminum foil layer, a second adhesive layer, a protective layer, and a matte layer in sequence. When the heat-sealing layer is laminated with an adhesive, a first adhesive layer is also provided between the heat-sealing layer and the aluminum foil layer. The matte layer is the outermost layer of the structure, and its printability, solvent resistance, and electrolyte resistance directly affect the performance of the aluminum-plastic film. When the surface dyne value of the matte layer is 34-40 mN / m, and a crosslinking system formed by a hydroxyl-containing resin composition and an isocyanate curing agent is used, the inkjet-printed graphics can remain identifiable, while simultaneously ensuring solvent resistance and electrolyte resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum-plastic film production technology, specifically to an electrolyte-resistant black matte aluminum-plastic film for lithium battery devices and its preparation method. Background Technology

[0002] Matte black aluminum-plastic film is a subcategory of aluminum-plastic film products, primarily used in high-end electronic products and lithium battery packaging materials. The advantages of matte black aluminum-plastic film include: 1) improved text visibility; 2) enhanced battery scratch and solvent resistance, extending lifespan; and 3) a more distinct appearance compared to ordinary aluminum-plastic film. Matte black aluminum-plastic film achieves its black appearance through three methods: black adhesive, black ink, and black nylon. Finally, a matte layer is applied to the outermost layer. The performance of the matte coating is a key factor affecting the performance of matte black aluminum-plastic film and a core technology for product differentiation.

[0003] Black matte aluminum-plastic film has a matte coating on its surface, making its appearance completely different from the original aluminum-plastic film. While the matte layer can make the aluminum-plastic film look more upscale, improper material use can lead to a decline in surface properties, such as reduced clarity of surface coding, decreased resistance to electrolytes, and reduced resistance to alcohol and ketone solvents.

[0004] Chinese patent CN117106347A discloses a matte black aluminum-plastic film and its preparation method. The patent describes a method that uses a compound of hydroxyl acrylic resin and hyperbranched polyester polyol resin to give the aluminum-plastic film good resistance to wiping with alcohols, esters, and ketones. However, for high-end applications, the performance requirements for the matte black film layer go beyond just resistance to alcohols, esters, and ketones; it also needs to consider properties such as scannable coding, solvent resistance, and electrolyte resistance.

[0005] Chinese patent CN214983907U discloses an improved black matte aluminum-plastic film. The patent uses a black PET film instead of black ink and PA film to give the product better electrolyte resistance. However, the electrolyte resistance of the black matte aluminum-plastic film depends not only on the PET film, but also on the electrolyte resistance of the matte layer coated on the outside of the PET film. If the matte layer is not resistant to electrolyte, it will affect the overall electrolyte resistance of the aluminum-plastic film.

[0006] Chinese patent CN211710243U discloses a corrosion-resistant black matte aluminum-plastic film for digital lithium batteries. The patent uses an integrally molded corrosion-resistant modified black polyester film to be laminated on the nylon surface to improve the corrosion resistance of nylon. However, this method also fails to solve the corrosion resistance problem of the matte layer or does not demonstrate the corrosion resistance capability of the matte layer. Summary of the Invention

[0007] While existing technologies employ methods to improve the surface properties of aluminum-plastic films through single-layer modified films or specific resin formulations, these solutions primarily aim for a single function (such as solvent resistance or corrosion resistance), with a design logic serving passive surface protection. This does not align with the multiple performance requirements of lithium batteries in extreme real-world environments, where the matte layer must simultaneously possess scannable coding capabilities, high solvent resistance, and electrolyte resistance. This indicates that existing solutions still have room for improvement in the synergistic control of the matte layer's coding compatibility, solvent resistance, and electrolyte resistance. Current technologies, such as replacing nylon with PET or relying solely on surface ink modification, often overlook the issue that a lack of corrosion resistance in the matte layer itself will directly lead to the loss of substrate performance. Furthermore, existing testing and preparation methods lack precise control mechanisms for the microstructure and chemical crosslinking degree of the matte layer. This results in improved coding recognition at the expense of coating density and chemical resistance, making it impossible to distinguish the comprehensive protective differences of the matte layer in different application scenarios and hindering comprehensive performance optimization for lithium battery packaging.

[0008] Therefore, there is an urgent need in this field to develop a black matte aluminum-plastic film with excellent inkjet clarity and a matte layer that can simultaneously meet the requirements of resistance to electrolyte corrosion, alcohol and acetone solvent wiping performance, and its preparation method, so as to solve the technical problems of uneven performance of matte layer and difficulty in meeting multiple protection indicators in the existing technology.

[0009] The technical problem this invention aims to solve is that existing matte black aluminum-plastic film technologies only improve a single function, making it difficult to simultaneously address the issues of code readability, solvent resistance, and electrolyte resistance. Furthermore, the surface energy and cross-linking state of the matte layer both affect code compatibility and chemical resistance, and existing solutions struggle to achieve a stable balance between these two aspects. Therefore, current technology lacks a black matte aluminum-plastic film that can simultaneously achieve scannable codes, resistance to alcohol wiping, resistance to acetone wiping, and resistance to electrolytes.

[0010] Accordingly, the present invention provides a black matte aluminum-plastic film and its preparation method. The matte layer of the black matte aluminum-plastic film is formed by crosslinking a hydroxyl-containing resin composition and an isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5. By controlling the crosslinking structure and surface characteristics of the matte layer, the surface dyne value of the matte layer is maintained between 34 mN / m and 40 mN / m to balance ink adhesion and coating crosslinking degree; thus, the resulting black matte aluminum-plastic film simultaneously possesses good inkjet printing recognition, alcohol resistance, acetone resistance, and electrolyte resistance, meeting the application requirements of high-end electronic products and lithium battery packaging materials.

[0011] One object of the present invention is to provide a black matte aluminum-plastic film, comprising an aluminum foil layer, a heat-sealing layer located on one side of the aluminum foil layer, a protective layer located on the other side of the aluminum foil layer, and a matte layer located on the side of the protective layer away from the aluminum foil layer; the protective layer is a black protective layer, or the black matte aluminum-plastic film further comprises a black adhesive layer located between the aluminum foil layer and the protective layer and / or a black ink layer located between the protective layer and the matte layer; and the surface dyne value of the matte layer is 34-40 mN / m. In the aforementioned black matte aluminum-plastic film, the matte layer is formed by crosslinking a hydroxyl-containing resin composition with an isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5.

[0012] As described above, the black matte aluminum-plastic film has a protective layer, a second adhesive layer, an aluminum foil layer, a first adhesive layer, and a heat-sealing layer sequentially disposed on one side of the matte layer in a direction away from the matte layer.

[0013] As described above, the black matte aluminum-plastic film has a 60° gloss level of 1.0 to 3.0.

[0014] As described above, the matte aluminum-plastic film exhibits no exposure, peeling, or significant whitening of the substrate after passing the following two tests: wiping at least 50 times with 95% ethanol (volume fraction) under a 500 g load; and wiping at least 10 times with analytical grade acetone (volume fraction) under a 500 g load. Furthermore, at 23±2℃, 0.10 mL of electrolyte is added to the surface of the matte layer and allowed to stand for 15 min. After wiping away the residual electrolyte, the matte layer is gently wiped with a lint-free cloth soaked in 95% ethanol. The matte layer shows no exposure, peeling, or significant whitening. The electrolyte is a 1 mol / L LiPF6 solution of ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate, with a volume ratio of 1:1:1.

[0015] As described above, the black matte aluminum-plastic film has the following characteristics: the thickness of the heat-sealing layer is 30–50 μm; the thicknesses of the first adhesive layer and the second adhesive layer are 2–5 μm, respectively; the thickness of the aluminum foil layer is 30–50 μm; the thickness of the protective layer is 15–25 μm; and the thickness of the matte layer is 2–5 μm.

[0016] As described above, the black matte aluminum-plastic film, wherein the heat-sealing layer comprises polypropylene resin.

[0017] As described above, the black matte aluminum-plastic film includes a protective layer comprising one or more of nylon resin and PET resin; wherein the nylon resin is a transparent resin or a black resin.

[0018] As described above, the black matte aluminum-plastic film contains hydroxyl-containing resin components, which are one or more of polyurethane resin, polyester polyol resin, and hydroxyl acrylic resin.

[0019] As described above, the black matte aluminum-plastic film has a weight-average molecular weight (Mw) of 5,000 to 20,000, a hydroxyl value of 10 to 100 mg KOH / g based on resin solids, and a glass transition temperature (Tg) of 50 to 100 °C.

[0020] As described above, the black matte aluminum-plastic film contains silica matting powder in the hydroxyl-containing resin composition.

[0021] As described above, the black matte aluminum-plastic film, wherein the isocyanate curing agent is an aliphatic isocyanate, an aromatic isocyanate, or a mixture thereof.

[0022] Another aspect of the present invention is to provide a method for preparing a black matte aluminum-plastic film, which includes the following steps: surface treating an aluminum foil; bonding a protective layer to one side of the surface-treated aluminum foil with a second adhesive layer; directly extruding a heat-sealing layer to the other side, or bonding a heat-sealing layer with a first adhesive layer, to form an aluminum-plastic film substrate; coating a matte coating composition on the side of the protective layer away from the aluminum foil and curing it to form a matte layer; wherein the method further satisfies at least one of the following conditions: the protective layer is black; the second adhesive layer is black; a black ink layer is formed between the protective layer and the matte layer; the matte layer is formed by crosslinking a hydroxyl-containing resin composition and an isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5.

[0023] The preparation method described above, wherein the surface treatment is a double-sided passivation treatment.

[0024] The preparation method described above, wherein the matte coating composition comprises silica matting powder.

[0025] As described above, the surface dyne value of the matte layer is 34 ~ 40 mN / m.

[0026] As described above, the matte layer has a 60° gloss level of 1.0 to 3.0.

[0027] The preparation method described above, wherein the protective layer comprises nylon resin, PET resin, or a combination thereof; wherein the nylon resin is transparent nylon resin or black nylon resin.

[0028] As described above, the matte coating composition comprises a hydroxyl-containing resin composition, which includes one or more of polyurethane resin, polyester polyol resin, and hydroxyl acrylic resin.

[0029] As described above, the hydroxyl-containing resin composition has a weight-average molecular weight (Mw) of 5,000 to 20,000, a hydroxyl value of 10 to 100 mg KOH / g based on resin solids, and a glass transition temperature (Tg) of 50 to 100 °C.

[0030] The preparation method described above, wherein the matte coating composition further includes an isocyanate curing agent, wherein the isocyanate curing agent includes aliphatic isocyanates, aromatic isocyanates or mixtures thereof.

[0031] As described above, the prepared black matte aluminum-plastic film is wiped back and forth at least 50 times with 95% ethanol under a 500 g load, and the matte layer does not show any exposed substrate, peel off, or turn obviously white.

[0032] As described above, in the preparation method, after the obtained black matte aluminum-plastic film is wiped back and forth with analytical grade acetone at least 10 times under a load of 500 g, the matte layer does not show any exposed substrate, peel off, or turn obviously white.

[0033] As described above, in the preparation method, 0.10 mL of electrolyte is dropped onto the surface of the matte layer at 23±2℃ and allowed to stand for 15 min. After wiping away the residual electrolyte, the matte layer is gently wiped with a lint-free cloth soaked in 95% ethanol. The matte layer does not show any exposed substrate, peel off, or turn obviously white. The electrolyte is a mixed solution of ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate in 1 mol / L LiPF6, with a volume ratio of 1:1:1.

[0034] The advantage of this invention over prior art is that by controlling the R value and the dyne value of the matte layer surface, it can achieve both coding recognition, solvent resistance and electrolyte resistance under the conditions shown in the examples.

[0035] This invention proposes a design paradigm for a black matte aluminum-plastic film that balances coding legibility, solvent resistance, and electrolyte resistance. It is formed by crosslinking a hydroxyl-containing resin component with an isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5, thus establishing a matte layer structure with appropriate surface energy and crosslinking degree. This differs from existing technologies that only focus on improving a single performance aspect. The R value is defined as: R = n(NCO) / n(OH). n(NCO) is the number of moles of isocyanate groups in the isocyanate curing agent, and n(OH) is the number of moles of hydroxyl groups in the hydroxyl-containing resin component. n(NCO) is calculated based on the solid mass of the isocyanate curing agent and the NCO mass fraction stated in its Certificate of Analysis (COA); n(OH) is calculated based on the resin solid mass of the hydroxyl-containing resin component and the hydroxyl value based on resin solids. Solvents and non-reactive additives are not included in the R value calculation; all components are calculated on a solids basis.

[0036] Existing technical solutions mostly rely on specific resin formulations, black inks, black PET films, or single solvent-resistant modification technologies to improve a certain performance index, but it is difficult to simultaneously achieve good coding recognition, alcohol resistance, acetone resistance, and electrolyte resistance.

[0037] Therefore, the black matte aluminum-plastic film and its preparation method provided by this invention establish a comprehensive performance design standard that takes into account the scannability of inkjet printing, solvent resistance, and electrolyte resistance, breaking through the limitation of traditional black matte aluminum-plastic films that can only improve a single performance index. Through a specific cross-linking reaction system and surface dyne value control mechanism, not only can the clarity of inkjet printing and print readability be effectively improved, but the chemical stability and durability of the coating can also be enhanced, reducing the risk of performance degradation caused by electrolyte penetration, solvent erosion, and coating deterioration. This improves the reliability and service life of lithium battery packaging materials in high-end electronic product applications and meets the demand for a black matte appearance in high-end consumer electronics battery packaging.

[0038] This invention proposes a matte layer structure with a dyne value of 34 to 40 mN / m, an R-value greater than 0.5 and less than or equal to 1.5, and a high degree of cross-linking. This upgrades the performance design of matte layers from the traditional approach of relying on a single chemical resistance or printing performance to a multi-performance synergistic design mechanism that considers both surface energy control and cross-linking structure control. By controlling the surface dyne value and cross-linking degree of the matte layer, the adhesion and recognition effect of inkjet printing can be improved simultaneously, while maintaining excellent resistance to alcohol, acetone, and electrolyte corrosion. This resolves the inherent contradiction in black matte aluminum-plastic films between the requirements for "high inkjet printing clarity" and "high requirements for the matte layer's solvent and electrolyte resistance."

[0039] The black matte aluminum-plastic film provided by this invention possesses excellent overall surface performance. By controlling the surface dyne value of the matte layer between 34 and 40 mN / m and forming a crosslinking reaction product with an appropriate degree of crosslinking between the hydroxyl-containing resin component and the isocyanate curing agent, the matte layer maintains a black, low-gloss appearance while achieving good inkjet printing clarity, barcode recognition, and chemical resistance. Simultaneously, by crosslinking the hydroxyl-containing resin component and the isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5, the density and chemical stability of the matte layer can be improved, effectively reducing the risk of corrosion from alcohol, acetone, and electrolytes, and minimizing problems such as whitening, peeling, or appearance deterioration after wiping.

[0040] This invention provides a black matte aluminum-plastic film and its preparation method, establishing a quantitative design standard for the industry that balances appearance, processing suitability, and packaging protection. The comprehensive performance evaluation system established by this invention has a clear structure and intuitive data, providing process optimization guidance for the production of high-end products. Manufacturers of black matte aluminum-plastic films only need to optimize based on key parameters such as "surface dyne value," "isocyanate to hydroxyl molar ratio (R value)," and "coating crosslinking degree" to accurately achieve product upgrades and quality control. This breaks free from the limitations of traditional trial-and-error development, significantly improving the industrialization efficiency and application reliability of lithium battery packaging materials, and meeting the demand for a black matte appearance in high-end consumer electronics battery packaging. Attached Figure Description

[0041] Figure 1 This is a schematic diagram illustrating the structure of a black matte aluminum-plastic film; Figure 2 A flowchart illustrating the preparation method of black matte aluminum-plastic film. Detailed Implementation

[0042] The following examples, illustrated with figures, illustrate specific embodiments of the present invention.

[0043] The present invention will be described in detail below with reference to specific embodiments. It should be noted that the embodiments are only used to illustrate the present invention and are not intended to limit the scope of protection of the present invention.

[0044] The first embodiment of the present invention provides a black matte aluminum-plastic film (100), which includes at least a heat-sealing layer (6), an aluminum foil layer (4), a second adhesive layer (3), a protective layer (2), and a matte layer (1) in sequence; when the heat-sealing layer (6) is laminated with an adhesive, a first adhesive layer (5) is also provided between the heat-sealing layer (6) and the aluminum foil layer (4). The matte layer (1) is disposed on the surface side of the black matte aluminum-plastic film and is used to give the aluminum-plastic film a low-gloss appearance, inkjet printing recognition, solvent resistance, and electrolyte resistance. The matte layer (1) includes a crosslinking reaction product of a hydroxyl-containing resin composition and an isocyanate curing agent, wherein the hydroxyl-containing resin composition and the isocyanate curing agent are crosslinked at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5. Through the above crosslinking reaction system, the matte layer can have an appropriate degree of crosslinking, thereby taking into account both the adhesion state of the inkjet printing ink on the surface of the matte layer and the tolerance of the matte layer to chemical media such as alcohol, acetone, and electrolyte.

[0045] In some embodiments, the surface dyne value of the matte layer (1) is 34 to 40 mN / m. Controlling the surface dyne value within the above range is beneficial for the inkjet ink to spread appropriately on the surface of the matte layer and to maintain clear boundaries of the graphics or QR codes; at the same time, in conjunction with the crosslinking system formed by the hydroxyl-containing resin composition and the isocyanate curing agent, both inkjet compatibility and solvent resistance can be taken into account.

[0046] In some embodiments, the gloss of the matte layer at 60° of the black matte aluminum-plastic film, measured according to the method described in the specification, is 1.0 to 3.0, preferably 1.3 to 2.0. By controlling the gloss within the above range, the black matte aluminum-plastic film can have a surface effect with low reflectivity, good appearance and texture, and high visual distinction, and can meet the requirements of high-end consumer electronics battery packaging for a black matte appearance.

[0047] In some embodiments, if the thickness of the matte layer (1) is too thin, it may result in insufficient matte effect and chemical resistance; if the thickness of the matte layer (1) is too thick, it may affect the uniformity of coating curing, flexibility and subsequent molding performance. By controlling the thickness of the matte layer within the above range, the matte appearance, coding effect and solvent resistance can be simultaneously achieved. The thickness is 2μm to 5μm, preferably 3μm.

[0048] In some embodiments, the hydroxyl-containing resin composition includes one or more of polyurethane resin, polyester polyol resin, and hydroxyl acrylic resin. The weight-average molecular weight (Mw) of the hydroxyl-containing resin composition is 5,000 to 20,000, the hydroxyl value based on resin solids is 10 to 100 mg KOH / g, and the glass transition temperature (Tg) is 50°C to 100°C. The setting of the weight-average molecular weight (Mw) is mainly related to the solvent resistance of the matte layer (1); when the hydroxyl-containing resin composition has an appropriate weight-average molecular weight (Mw), the alcohol resistance and acetone resistance of the matte layer (1) can be improved. The hydroxyl value based on resin solids is used to provide reaction sites with the isocyanate curing agent, so that a cross-linked network is formed after the coating is cured; the glass transition temperature helps to balance the hardness, flexibility, and chemical resistance of the coating. In this invention, the weight-average molecular weight (Mw) is determined by gel permeation chromatography, with tetrahydrofuran as the mobile phase, polystyrene as the calibration standard, a column temperature of 35°C, and a flow rate of 1.0 mL / min. The hydroxyl value based on resin solids was determined using the acetic anhydride-pyridine method and converted according to the resin solids mass, with units of mg KOH / g. The glass transition temperature Tg was determined using differential scanning calorimetry, with the temperature increased at 10℃ / min under a nitrogen atmosphere, and the midpoint temperature of the baseline shift of the second heating curve was taken as Tg.

[0049] In some embodiments, the hydroxyl-containing resin composition further includes silica matting powder. The silica matting powder can be dispersed in the hydroxyl-containing resin composition and is used to reduce the gloss of the coating surface, so that the matte layer (1) forms a low-gloss surface. By combining silica matting powder with the hydroxyl-containing resin composition and isocyanate curing agent, the matte effect can be maintained while avoiding excessive roughness of the coating surface that would affect the clarity of the inkjet printing.

[0050] In some embodiments, the isocyanate curing agent is an aliphatic isocyanate, an aromatic isocyanate, or a mixture thereof. The isocyanate curing agent can react with the hydroxyl groups in the hydroxyl-containing resin composition to form a crosslinking reaction product. When the R value is greater than 0.5, the matte layer (1) can achieve a better degree of crosslinking, thereby improving its resistance to alcohol wiping, acetone wiping, and electrolyte wiping. Preferably, the R value is from 0.6 to 1.5, more preferably 0.8.

[0051] In some embodiments, the protective layer (2) is one or more of nylon resin or PET resin, with a thickness of 15 μm to 25 μm. The nylon resin can be transparent nylon resin or black nylon resin, preferably black nylon resin. When the protective layer is transparent, the second adhesive layer is a black adhesive, or a black ink layer is disposed between the protective layer and the matte layer. By using black nylon resin as the protective layer, a black appearance can be given to the aluminum-plastic film, and the adverse effects of an additional black ink layer or black adhesive layer on interlayer adhesion and chemical resistance can be reduced.

[0052] In some embodiments, the first adhesive layer (5) is used to connect the aluminum foil layer (4) and the heat-sealing layer (6), and the second adhesive layer (3) is used to connect the aluminum foil layer (4) and the protective layer (2), with a thickness of 2 μm to 5 μm. By setting the above adhesive layer, the interlayer composite strength of the black matte aluminum-plastic film can be improved, and the risk of interlayer peeling, blistering or delamination during subsequent battery manufacturing or use can be reduced. In some embodiments, the aluminum foil layer (4) can be a surface-treated aluminum foil, preferably a double-sided passivated aluminum foil, to improve the bonding stability between the aluminum foil layer and the adjacent adhesive layer, and to enhance the aluminum foil layer's resistance to electrolyte, with a thickness of 30 μm to 50 μm.

[0053] In some embodiments, the heat-sealing layer (6) is used for heat sealing during battery encapsulation and provides good sealing and electrolyte resistance, and has a thickness of 30 μm to 50 μm.

[0054] The second embodiment of the present invention provides a method for preparing a black matte aluminum-plastic film, which includes the following steps: surface treatment of aluminum foil (S1); composite of the surface-treated aluminum foil with a protective layer (2) and a heat-sealing layer (6) to form an aluminum-plastic film substrate (S2); and forming a matte layer on the side of the protective layer (2) away from the aluminum foil (S3). The matte layer (1) is formed by crosslinking a hydroxyl-containing resin composition with an isocyanate curing agent, and the hydroxyl-containing resin composition and the isocyanate curing agent are crosslinked at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5.

[0055] In some embodiments, the surface treatment is a double-sided passivation treatment, which can improve the corrosion resistance and composite stability of both sides of the aluminum foil layer (4). Subsequently, the aluminum foil can be laminated with a nylon resin layer or a PET resin layer and cured to form a semi-finished product containing a protective layer (2) and an aluminum foil layer (4). The nylon resin layer can be a transparent nylon layer or a black nylon layer, preferably a black nylon layer.

[0056] In some embodiments, a matte coating solution is applied to the protective layer side, and the matte layer (1) is formed after drying and cross-linking curing. The matte coating solution includes a hydroxyl-containing resin composition, an isocyanate curing agent, and a silica matting agent. By controlling the ratio of the molar number of isocyanate to the molar number of hydroxyl groups in the matte coating solution, the formed matte layer (1) can possess appropriate surface dyne value, low gloss, and chemical resistance.

[0057] In some embodiments, a heat-sealing layer (6) may be formed on the side of the aluminum foil layer (4) away from the protective layer. The heat-sealing layer (6) may be formed by hot extrusion composite polypropylene resin or by adhesive composite polypropylene resin; a slip agent layer may also be coated on the surface of the heat-sealing layer (6) away from the aluminum foil layer (4) to improve the surface slipness and subsequent processing performance of the aluminum-plastic film. Several embodiments are provided below to illustrate the technical effects achieved by the present invention. However, these embodiments are not intended to limit the implementation of the present invention, and the interpretation of the scope of the claims shall still be based on the content of the claims.

[0058] Example of Performance Testing for Black Matte Aluminum-Plastic Film

[0059] Example 1:

[0060] Raw materials and structural parameters: The black matte aluminum-plastic film comprises, from the inside out, a heat-sealing layer (6), an aluminum foil layer (4), a second adhesive layer (3), a protective layer (2), and a matte layer (1). The outermost matte layer (1) has a thickness of 3 μm, the protective layer (2) is black nylon resin with a thickness of 15 μm, the second adhesive layer (3) has a thickness of 3 μm, the aluminum foil layer (4) has a thickness of 35 μm, and the heat-sealing layer (6) is a 35 μm thick polypropylene layer. The matte layer (1) is made by crosslinking a hydroxyl-containing resin composition with an aromatic isocyanate curing agent, wherein the isocyanate molar ratio (R value) to hydroxyl molar ratio is 0.8. The mass ratio of polyurethane resin to hydroxyl acrylic resin is 2:1, and the hydroxyl-containing resin composition also includes silica matting powder; the weight-average molecular weight (Mw) of the hydroxyl-containing resin is 15,000, the hydroxyl value based on resin solids is 60 mg KOH / g, and the glass transition temperature (Tg) is 50 °C.

[0061] The value of R is defined as: R = n(NCO) / n(OH); n(NCO) represents the number of moles of isocyanate groups in the isocyanate curing agent, and n(OH) represents the number of moles of hydroxyl groups in the hydroxyl-containing resin composition. n(NCO) is calculated based on the solid mass of the isocyanate curing agent and the NCO mass fraction stated in its product inspection report (COA). n(OH) is calculated based on the resin solid mass of the hydroxyl-containing resin composition and the hydroxyl value based on resin solids. Solvents and non-reactive additives are not included in the R value calculation, and all components are calculated on a solids basis.

[0062] Specifically, n(OH) and n(NCO) can be calculated using the following formulas: n(OH) = Mass of hydroxyl-containing resin solids × Hydroxyl value / 56100; n(NCO) = Solid mass of isocyanate curing agent × NCO mass fraction listed in COA / 42.02; Wherein, 56100 is the molar mass of KOH converted to mg / mol, and 42.02 is the molar mass of the NCO group; after substituting the amount of each component in Example 1 on a solid basis into the above formula, R = 0.8 is obtained.

[0063] Preparation method: Double-sided passivation of aluminum foil; The aluminum foil from step a is then laminated and cured with nylon.

[0064] A composite polypropylene layer is extruded from the aluminum foil side of the semi-finished product obtained in step b to form a heat-sealing layer (6). In step c, a matte coating is applied to the nylon side of the semi-finished product, followed by curing. A black matte aluminum-plastic film with a total thickness of 91 μm was prepared by applying a slip agent.

[0065] Example 2:

[0066] The raw materials, preparation process, and process parameters used are basically the same as those in Example 1. The difference is that a first adhesive layer (5) is further provided between the aluminum foil layer (4) and the heat-sealing layer (6). Among them, the outermost matte layer (1) has a thickness of 3 μm, the protective layer (2) is black nylon resin with a thickness of 22 μm, the first adhesive layer (5) and the second adhesive layer (3) are both 3 μm thick, the aluminum foil layer (4) has a thickness of 40 μm, and the heat-sealing layer (6) is a polypropylene layer with a thickness of 31 μm.

[0067] Example 3:

[0068] The raw materials, preparation process, and process parameters used are basically the same as those in Example 2. The difference is that the mass ratio of polyurethane resin to hydroxyl acrylic resin in the matte layer (1) is 1:1, and its glass transition temperature (Tg) is 70℃. Among them, the outermost matte layer (1) has a thickness of 3μm, the protective layer (2) is black nylon resin with a thickness of 25μm, the first adhesive layer (5) and the second adhesive layer (3) are both 2μm thick, the aluminum foil layer (4) has a thickness of 40μm, and the heat-sealing layer (6) is made of polypropylene resin with a thickness of 40μm.

[0069] Comparative Example 1: The raw materials, preparation process, and process parameters used are basically the same as those in Example 2. The difference is that the amount of isocyanate curing agent added in the matte layer (1) is reduced so that the R value is 0.3.

[0070] Comparative Example 2: The raw materials, preparation process, and process parameters used are basically the same as those in Example 2. The difference is that the weight average molecular weight Mw of the hydroxyl-containing resin composition of the matte layer (1) is 25,000, and the mass ratio of polyurethane resin to hydroxyl acrylic resin is 4:1.

[0071] Comparative Example 3: The raw materials, preparation process, and process parameters used are basically the same as those in Example 2. The difference is that the weight average molecular weight Mw of the hydroxyl-containing resin composition of the matte layer (1) is 3,000, and the mass ratio of polyurethane resin to hydroxyl acrylic resin is 1:2.

[0072] Comparative Example 4: The raw materials, preparation process, and process parameters used are basically the same as those in Example 2. The difference is that the glass transition temperature (Tg) of the hydroxyl-containing resin composition of the matte layer (1) is 40°C.

[0073] Comparative Example 5: The raw materials, preparation process and process parameters used are basically the same as those in Example 2. The difference is that the hydroxyl value of the hydroxyl-containing resin composition of the matte layer (1) is 5 mg KOH / g based on resin solids.

[0074] Comparative Example 6: The preparation process and main process parameters used were basically the same as those in Example 2. The difference was that the resin system containing hydroxyl resin components in the matte layer (1) was adjusted so that its hydroxyl value, calculated based on resin solids, was 120 mg KOH / g, and the mass ratio of polyurethane resin to hydroxyl acrylic resin was 0:1, with a glass transition temperature (Tg) of 100℃. This comparative example was used to evaluate the comprehensive influence of the above-mentioned high hydroxyl value pure hydroxyl acrylic resin system on the basic properties of the matte layer (1).

[0075] Basic Performance Testing Basic performance tests were conducted on the black matte aluminum-plastic films provided in Examples 1 to 3 and Comparative Examples 1 to 6. Table 1 lists the main formulation and structural parameters of Examples 1 to 3 and Comparative Examples 1 to 6. The differences in raw materials or parameters of each comparative example relative to Example 2 are shown in Table 1 to evaluate the influence of the corresponding formulation or parameter combinations on the performance of the black matte aluminum-plastic film.

[0076] The test items include aluminum-plastic film thickness, inkjet printing recognition capability, alcohol wiping resistance, acetone wiping resistance, electrolyte resistance test time, and the 60° gloss and dyne value of the matte layer. Specifically, the aluminum-plastic film thickness test: the total thickness of the sample was determined according to GB / T6672. After the sample was placed in an environment of 23±2℃ and 50%±5% relative humidity for 24 hours, five measuring points were selected at equal intervals along the transverse direction for measurement. The arithmetic mean of the five measurements was taken as the thickness of the sample. Three samples were tested in each group. The inkjet printing recognition capability, alcohol wiping resistance, acetone wiping resistance, electrolyte resistance test, and the 60° gloss and dyne value of the matte layer were used to characterize the appearance, texture, processing and printing suitability, and long-term chemical protection performance of the matte layer. The specific test processes and methods for each test item are described below, and the final test data for each embodiment and comparative example are detailed in Table 2 below.

[0077] Coding test: The sample was placed in an environment of 23±2℃ and 50%±5% relative humidity for 24 h. Characters and QR codes were printed on the matte surface using an IMAS inkjet printer and MW133 white ink. The character height was 5.0 mm, and the distance between the printhead and the film surface was 10±1 mm. After printing, the sample was placed in the above environment for 10 min. A Honeywell 1900GHD / 1902 barcode scanner was used to scan the sample 10 times consecutively at a distance of 100±10 mm and a scanning angle of 0°~30°. If all 10 scans were successful, the sample was considered "scannable"; otherwise, it was considered "unscannable". Three samples were tested in each group, and the worst result among the three samples was taken as the result for that group.

[0078] Alcohol resistance test: Cut a 100 mm × 50 mm sample, wrap a lint-free cloth around a 20 mm × 20 mm friction head, and thoroughly wet it with 95% ethanol (by volume). Under a load of 500 g, wipe the matte surface at a speed of 30 times / min with a reciprocating stroke of 50 mm. One reciprocating stroke counts as one cycle. Wipe until any of the following phenomena occur: exposure of the substrate, peeling, or obvious whitening of the matte layer, or until 50 cycles are reached, and stop. Record the number of wiping cycles. Test 3 samples per group, and take the lowest number of wiping cycles as the test result; if no of the above phenomena occur after 50 cycles, it is recorded as ≥50 cycles.

[0079] Acetone resistance rubbing test: Except that the rubbing liquid is replaced with analytically pure acetone and the maximum number of rubbing cycles is adjusted to 10, the remaining conditions and judgment methods are the same as those of the alcohol resistance rubbing test; if no substrate exposure, peeling or significant whitening occurs after 10 rubbing cycles, the result is recorded as ≥10 cycles.

[0080] Electrolyte resistance test: The test electrolyte is a mixed solution of 1 mol / L LiPF6 in ethylene carbonate, ethyl methyl carbonate and diethyl carbonate, with a volume ratio of 1:1:1 for the three components. A test specimen with an area of 100 mm×100 mm is cut out, 0.10 mL of the electrolyte is added dropwise to the center of the matte surface at 23±2°C, and the specimen is left to stand for 15 min. The residual electrolyte is first wiped off with a dry dust-free cloth, and then the area where the electrolyte was added dropwise is gently wiped again with a dust-free cloth dipped in ethanol with a volume fraction of 95%. The test is judged as qualified when the matte layer shows no substrate exposure, peeling or significant whitening. Three test specimens are tested for each group, and the group is judged to pass the 15-minute electrolyte resistance test only when all three specimens are qualified; otherwise, the group is judged as unqualified. Dyne value test: The test specimen is placed in an environment at 23±2°C with a relative humidity of 50%±5% for 24 h. Using Arcotest dyne pens, continuous ink lines with a length of 100 mm are drawn on the matte surface in sequence from low to high nominal value, and the interval between adjacent nominal values of the dyne pens is 2 mN / m. If the ink line remains continuous without shrinking, breaking or beading within 5 s, the corresponding nominal value is judged to pass; the highest nominal value of the dyne pen that passes the test is taken as the surface dyne value of the measurement point, in mN / m. Three points are tested in the transverse direction and three points in the longitudinal direction for each test specimen, and the arithmetic mean of the 6 measurement points is taken as the surface dyne value of the test specimen; three test specimens are tested for each group.

[0081] 60° gloss test of the matte layer: The test specimen is placed in an environment at 23±2°C with a relative humidity of 50%±5% for 24 h. A 60° glossmeter calibrated with a standard black glass plate is used, with the matte surface facing the measurement window, measurements are taken at 5 different positions no less than 20 mm away from the edge of the test specimen, and the arithmetic mean of the 5 measurement results is taken as the 60° gloss of the test specimen. Three test specimens are tested for each group, and the arithmetic mean of the three test specimens is reported.

[0082] Table 1

[0083] Table 2

[0084] Based on the data in Tables 1 and 2, the specific analysis of each black matte aluminum-plastic film is as follows: The black matte aluminum-plastic films prepared in Examples 1 to 3 can all achieve 5.0 mm height inkjet scanning capability, indicating that the matte layer formed by the present invention has good inkjet recognition and ink compatibility; at the same time, the alcohol wiping resistance of Examples 1 to 3 is not less than 50 times, the acetone wiping resistance is not less than 10 times, and the 15-minute electrolyte resistance test is qualified, indicating that the matte layer of the present invention can maintain excellent solvent resistance and electrolyte resistance under different film thicknesses and different dyne values.

[0085] The black matte aluminum-plastic film of Example 1 has a thickness of 91 μm, a surface dyne value of 36 mN / m, and a 60° gloss of 2.0. It can achieve 5.0 mm height coding and is resistant to alcohol wiping for no less than 50 times, acetone wiping for no less than 10 times, and passes the 15-minute electrolyte resistance test. This shows that under low dyne value conditions, the present invention can still take into account both coding recognition and chemical resistance.

[0086] The black matte aluminum-plastic film of Example 2 has a thickness of 102 μm, a dyne value of 38 mN / m on the surface of the matte layer, and a gloss of 1.5 at 60°. It can also achieve 5.0 mm height inkjet printing and scanning. Moreover, its resistance to alcohol wiping, acetone wiping and electrolyte wiping all meet the requirements. This shows that when the dyne value is in the preferred intermediate range of the present invention, the matte layer can obtain good inkjet printing adaptability, low gloss appearance and solvent resistance.

[0087] The black matte aluminum-plastic film of Example 3 has a thickness of 112 μm, a dyne value of 40 mN / m on the surface of the matte layer, and a gloss of 1.3 at 60°. It can achieve inkjet scanning and maintains resistance to alcohol wiping for no less than 50 times, acetone wiping for no less than 10 times, and passes the electrolyte resistance test for 15 minutes. This indicates that the dyne value is close to the upper limit range of the present invention, and the matte layer can still maintain good overall performance.

[0088] As can be seen from Examples 1 to 3, under their respective formulations and structural conditions, the aluminum-plastic film thickness in Examples 1 to 3 is 91–112 μm, the dyne value of the matte layer surface is 36–40 mN / m, and the 60° gloss of the matte layer is 1.3–2.0, all exhibiting satisfactory chemical resistance. That is, within the dyne value range defined by this invention, the matte layer can simultaneously maintain a low-gloss appearance and good inkjet printing readability. Therefore, by controlling the dyne value of the matte layer surface between 34 mN / m and 40 mN / m, and combining it with the cross-linked structure formed by the hydroxyl-containing resin composition and the isocyanate curing agent, the black matte aluminum-plastic film can simultaneously possess a low-gloss appearance, scannable inkjet printing, resistance to alcohol wiping, resistance to acetone wiping, and resistance to electrolytes, achieving a synergistic balance of multiple surface properties.

[0089] Comparative Example 1: Compared with Example 2, the main difference in Comparative Example 1 is that the R value is 0.3. The test results show that although Comparative Example 1 can still achieve scannable coding at a height of 5.0 mm, with a dyne value of 40 mN / m and a 60° gloss of 1.4 for the matte layer, its resistance to alcohol wiping is ≤20 times, its resistance to acetone wiping is ≤3 times, and it fails the 15-minute electrolyte resistance test. Therefore, when the R value is below 0.5, the cross-linking density of the matte layer is insufficient. Although it can maintain a certain level of coding legibility and a low-gloss appearance, its solvent resistance and electrolyte resistance are significantly reduced.

[0090] Comparative Example 2: Compared with Example 2, the main difference in Comparative Example 2 is that the weight-average molecular weight of the hydroxyl-containing resin is 25,000, and the mass ratio of polyurethane resin to hydroxyl acrylic resin is adjusted to 4:1. Test results show that Comparative Example 2 can achieve 5.0 mm height inkjet scanning capability, withstands ≥50 alcohol wipes, passes the 15-minute electrolyte resistance test, and has a dyne value of 36 mN / m and a 60° gloss of 1.5 for the matte layer; however, its resistance to acetone wipes is ≤3 times. Therefore, when the weight-average molecular weight of the hydroxyl-containing resin is higher than the range of this invention and the resin ratio deviates from the optimal conditions, the film-forming state and solvent resistance of the matte layer may be affected, resulting in insufficient resistance to strong solvents such as acetone.

[0091] Comparative Example 3: Compared with Example 2, the main difference in Comparative Example 3 is that the weight-average molecular weight of the hydroxyl-containing resin is 3,000, and the mass ratio of polyurethane resin to hydroxyl acrylic resin is adjusted to 1:2. The test results show that although Comparative Example 3 can achieve 5.0 mm height coding and the matte layer has a 60° gloss of 1.4, its dyne value increases to 42 mN / m, exceeding the 34 to 40 range specified in this invention. Simultaneously, its resistance to alcohol wiping is ≤10 times, its resistance to acetone wiping is ≤3 times, and it fails the 15-minute electrolyte resistance test. Therefore, when the weight-average molecular weight of the hydroxyl-containing resin is lower than the range of this invention and the resin ratio deviates from the optimal conditions, the alcohol resistance, acetone resistance, and electrolyte resistance of the matte layer significantly decrease.

[0092] Comparative Example 4: Compared with Example 2, the main difference in Comparative Example 4 is its glass transition temperature (Tg) of 40°C. The test results show that while Comparative Example 4 can achieve 5.0 mm height coding, and its dyne value of 38 mN / m and 60° gloss of the matte layer of 1.5 are all within the optimal surface performance range, its resistance to alcohol wiping is ≤20 times, its resistance to acetone wiping is ≤3 times, and it fails the 15-minute electrolyte resistance test. Therefore, when Tg is below 50°C, the hardness, wiping resistance, and chemical stability of the matte layer are insufficient. Even if its surface dyne value and 60° gloss of the matte layer are still within the optimal range, it is still difficult to simultaneously meet the requirements for alcohol resistance, acetone resistance, and electrolyte resistance.

[0093] Comparative Example 5: Compared with Example 2, the main difference of Comparative Example 5 is that the hydroxyl value based on resin solids is 5 mgKOH / g. The test results show that although Comparative Example 5 can achieve 5.0 mm height coding, with a dyne value of 34 mN / m and a 60° gloss of 2.0 for the matte layer, its resistance to alcohol wiping is only ≤10 times, its resistance to acetone wiping is only ≤3 times, and it fails the 15-minute electrolyte resistance test. Therefore, when the hydroxyl value based on resin solids is less than 10 mg KOH / g, the number of hydroxyl reaction sites in the hydroxyl-containing resin composition that can participate in the cross-linking reaction is insufficient, the cross-linking structure and chemical stability of the matte layer decrease, and thus the resistance to alcohol, acetone, and electrolytes is significantly reduced.

[0094] Comparative Example 6: Compared with Example 2, the main difference in Comparative Example 6 is the use of a high hydroxyl value resin system, which increases the hydroxyl value by resin solids to 120 mg KOH / g. The mass ratio of polyurethane resin to hydroxyl acrylic resin is adjusted to 0:1, and the glass transition temperature (Tg) is 100℃. Test results show that Comparative Example 6 has an alcohol resistance of ≥50 wipes, an acetone resistance of ≥10 wipes, and passes the 15-minute electrolyte resistance test. The matte layer has a 60° gloss of 2.0. However, its dyne value is 44 mN / m, exceeding the 34 to 40 mN / m range specified in this invention, resulting in unscannable 5.0 mm high coding. Therefore, while a high hydroxyl value resin system can maintain good alcohol resistance, acetone resistance, and electrolyte resistance in the matte layer, its high surface dyne value affects the spreading and recognition stability of the coding ink on the matte layer surface, leading to a decrease in coding recognition capability.

[0095] In summary, as shown in Comparative Examples 1 to 6, the surface energy state, film-forming state, cross-linking structure, and chemical stability of the matte layer all affect the inkjet printing compatibility, solvent resistance, and electrolyte resistance of the black matte aluminum-plastic film. Specifically, when the surface dyne value deviates from the range of 34 mN / m to 40 mN / m, it easily affects the spreading, adhesion, and recognition stability of the inkjet printing ink on the matte layer surface. Meanwhile, parameters such as the R-value, the weight-average molecular weight of the hydroxyl-containing resin, the hydroxyl value based on resin solids, the resin mass ratio, and the glass transition temperature (Tg) affect the film-forming state, cross-linking structure, and chemical resistance of the matte layer. In contrast, Examples 1 to 3 achieve a better balance between surface energy state and cross-linked structure by controlling the surface dyne value of the matte layer between 34 mN / m and 40 mN / m, and by combining appropriate resin molecular weight, hydroxyl value, R value and glass transition temperature (Tg) based on resin solids. This results in a combination of features such as scannable coding, low gloss appearance, resistance to alcohol wiping, resistance to acetone wiping and resistance to electrolyte.

[0096] Based on the above test results, the beneficial effects of the black matte aluminum-plastic film provided by this invention can be summarized as follows: Improved coding clarity: The black matte aluminum-plastic film provided by this invention controls the dyne value of the matte layer surface between 34 mN / m and 40 mN / m, which can regulate the spreading state of the coding ink on the matte layer surface. This avoids poor ink adhesion due to excessively low surface energy or excessive ink diffusion due to excessively high surface energy, thereby improving the clarity and scanning recognition rate of the coded text and QR codes, and solving the problems of blurry coding and unstable recognition of traditional black matte aluminum-plastic film.

[0097] Improved solvent resistance: In the black matte aluminum-plastic film provided by this invention, the matte layer is formed by cross-linking a hydroxyl-containing resin composition with an isocyanate curing agent. The hydroxyl-containing resin composition and the isocyanate curing agent are cross-linked at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.5, which can form a denser and more stable cross-linked network. This gives the matte layer excellent resistance to alcohol and acetone wiping. The alcohol wiping resistance can reach no less than 50 times, and the acetone wiping resistance can reach no less than 10 times, thereby reducing the risk of discoloration, whitening, or peeling when wiping, cleaning, or in contact with solvents during the manufacturing process.

[0098] Electrolyte resistance optimization: The black matte aluminum-plastic film provided by this invention controls the resin composition, crosslinking degree and surface dyne value of the matte layer, so that the matte layer maintains a matte appearance and coding compatibility while still having good resistance to electrolyte corrosion. It can pass a 15-minute electrolyte resistance test, thereby effectively reducing the problems of matte layer peeling, corrosion or appearance deterioration caused by electrolyte contact with the aluminum-plastic film surface, and improving the durability and reliability of lithium battery outer packaging materials.

[0099] Balancing Appearance and Overall Performance: The black matte aluminum-plastic film provided by this invention, measured according to the method described in the instruction manual, has a 60° gloss level that can be controlled between 1.0 and 3.0, giving the product a black matte effect with low reflectivity, high texture, and high visual distinctiveness. Simultaneously, through a combination design of a dyne value of 34 mN / m to 40 mN / m and an R value greater than 0.5 and less than or equal to 1.5, the matte layer also possesses properties such as scannable coding, resistance to alcohol wiping, resistance to acetone wiping, and resistance to electrolytes. This fundamentally solves the problem that traditional black matte aluminum-plastic films struggle to simultaneously achieve good coding readability, solvent resistance, electrolyte resistance, and appearance stability.

[0100] The above content involving common knowledge will not be described in detail, as those skilled in the art will understand.

[0101] The embodiments described above are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A black matte aluminum-plastic film, characterized in that, The film includes an aluminum foil layer, a heat-sealing layer on one side of the aluminum foil layer, a protective layer on the other side of the aluminum foil layer, and a matte layer on the side of the protective layer away from the aluminum foil layer; the protective layer is a black protective layer, or the black matte aluminum-plastic film further includes a black adhesive layer between the aluminum foil layer and the protective layer and / or a black ink layer between the protective layer and the matte layer; and the surface dyne value of the matte layer is 34 to 40 mN / m.

2. The black matte aluminum-plastic film according to claim 1, characterized in that, The matte layer is formed by crosslinking a hydroxyl-containing resin composition with an isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.

5.

3. The black matte aluminum-plastic film according to claim 1, characterized in that, On one side of the matte layer, a protective layer, a second adhesive layer, an aluminum foil layer, a first adhesive layer, and a heat-sealing layer are sequentially disposed in a direction away from the matte layer.

4. The black matte aluminum-plastic film according to claim 1, characterized in that, The gloss level of the matte layer at 60° is 1.0 to 3.

0.

5. The black matte aluminum-plastic film according to claim 1, characterized in that, The matte layer showed no signs of exposure, peeling, or significant whitening after undergoing the following two tests: wiping with 95% ethanol (volume fraction) at least 50 times under a 500 g load; and wiping with analytical grade acetone at least 10 times under a 500 g load.

6. The black matte aluminum-plastic film according to claim 1, characterized in that, At 23±2℃, 0.10 mL of electrolyte was dropped onto the surface of the matte layer and allowed to stand for 15 min. After wiping away the residual electrolyte, the matte layer was gently wiped with a lint-free cloth soaked in 95% ethanol. The matte layer showed no exposed substrate, peeling, or obvious whitening. The electrolyte was a mixed solution of ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate in 1 mol / L LiPF6, with a volume ratio of 1:1:

1.

7. The black matte aluminum-plastic film according to claim 3, characterized in that, The thickness of the heat-sealing layer is 30–50 μm, the thickness of the first adhesive layer and the second adhesive layer are 2–5 μm, the thickness of the aluminum foil layer is 30–50 μm, the thickness of the protective layer is 15–25 μm, and the thickness of the matte layer is 2–5 μm.

8. The black matte aluminum-plastic film according to claim 1, characterized in that, The heat-sealing layer comprises polypropylene resin.

9. The black matte aluminum-plastic film according to claim 1, characterized in that, The protective layer comprises one or more of nylon resin and PET resin; wherein the nylon resin is a transparent resin or a black resin.

10. The black matte aluminum-plastic film according to claim 2, characterized in that, The hydroxyl-containing resin composition is one or more of polyurethane resin, polyester polyol resin, and hydroxyl acrylic resin.

11. The black matte aluminum-plastic film according to claim 2, characterized in that, The weight-average molecular weight (Mw) of the hydroxyl-containing resin composition is 5,000 to 20,000, the hydroxyl value based on resin solids is 10 to 100 mg KOH / g, and the glass transition temperature (Tg) is 50 to 100 °C.

12. The black matte aluminum-plastic film according to claim 2, characterized in that, The hydroxyl-containing resin composition includes silica matting powder.

13. The black matte aluminum-plastic film according to claim 2, characterized in that, The isocyanate curing agent is an aliphatic isocyanate, an aromatic isocyanate, or a mixture thereof.

14. A method for preparing a black matte aluminum-plastic film as described in any one of claims 1 to 13, characterized in that, Includes the following steps: Surface treatment of aluminum foil; A protective layer is laminated onto one side of the surface-treated aluminum foil via a second adhesive layer; And directly extruding a composite heat-sealing layer on the other side, or compositing a heat-sealing layer through a first adhesive layer, to form an aluminum-plastic film substrate; coating a matte coating composition on the side of the protective layer away from the aluminum foil and curing it to form a matte layer; wherein the method also satisfies at least one of the following conditions: the protective layer is black; the second adhesive layer is black; a black ink layer is formed between the protective layer and the matte layer; the matte layer is formed by crosslinking a hydroxyl-containing resin composition and an isocyanate curing agent at an NCO / OH equivalent ratio of 0.5 < R ≤ 1.

5.

15. The preparation method according to claim 14, characterized in that, The surface treatment is a double-sided passivation treatment.

16. The preparation method according to claim 14, characterized in that, The matte coating composition includes silica matting powder.

17. The preparation method according to claim 14, characterized in that, The surface dyne value of the matte layer is 34~40 mN / m.

18. The preparation method according to claim 14, characterized in that, The gloss level of the matte layer at 60° is 1.0 to 3.

0.

19. The preparation method according to claim 14, characterized in that, The protective layer comprises nylon resin, PET resin, or a combination thereof; wherein the nylon resin is transparent nylon resin or black nylon resin.

20. The preparation method according to claim 14, characterized in that, The matte coating composition includes a hydroxyl-containing resin composition, which comprises one or more of polyurethane resin, polyester polyol resin, and hydroxyl acrylic resin.

21. The preparation method according to claim 20, characterized in that, The weight-average molecular weight (Mw) of the hydroxyl-containing resin composition is 5,000 to 20,000, the hydroxyl value based on resin solids is 10 to 100 mg KOH / g, and the glass transition temperature (Tg) is 50 to 100 °C.

22. The preparation method according to claim 20, characterized in that, The matte coating composition further includes an isocyanate curing agent, which includes aliphatic isocyanates, aromatic isocyanates, or mixtures thereof.

23. The preparation method according to claim 14, characterized in that, The resulting black matte aluminum-plastic film was wiped back and forth at least 50 times with 95% ethanol under a 500 g load, and the matte layer showed no exposure of the substrate, peeling, or obvious whitening.

24. The preparation method according to claim 14, characterized in that, After the prepared black matte aluminum-plastic film was wiped back and forth with analytical grade acetone at least 10 times under a load of 500 g, the matte layer showed no exposure of the substrate, peeling, or obvious whitening.

25. The preparation method according to claim 14, characterized in that, At 23±2℃, 0.10 mL of electrolyte was dropped onto the surface of the matte layer and allowed to stand for 15 min. After wiping away the residual electrolyte, the matte layer was gently wiped with a lint-free cloth soaked in 95% ethanol. The matte layer showed no exposed substrate, peeling, or obvious whitening. The electrolyte was a mixed solution of ethylene carbonate, methyl ethyl carbonate, and diethyl carbonate in 1 mol / L LiPF6, with a volume ratio of 1:1:1.

Citation Information

Patent Citations

  • Matte varnish, black matte aluminum-plastic film and preparation method thereof

    CN117106347A

  • Corrosion-resistant black matte aluminum-plastic film for digital lithium battery

    CN211710243U

  • Improved black matte aluminum-plastic film

    CN214983907U