In-situ growth of molybdenum disulfide foam nickel self-supporting hydrogen evolution electrode and preparation method thereof

By cross-weaving metal wires on the hydrogen evolution electrode to form a mesh structure and combining it with magnetic field regulation, a MoS2 catalytically active coating is grown in situ, which solves the problem of small specific surface area of ​​nickel wire mesh and achieves efficient electrolytic hydrogen production and improved catalytic effect of hydrogen evolution electrode.

CN123063802APending Publication Date: 2026-11-10LUOYANG NEW ENERGY TECHNOLOGY DEVELOPMENT GROUP CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611235549.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The nickel wire mesh of the existing magnetic field-loaded hydrogen evolution electrode device has a small specific surface area, resulting in low hydrogen production efficiency in the electrolyzer. There is an urgent need to improve the specific surface area and catalytic effect of the hydrogen evolution electrode.

Method used

A self-supporting hydrogen evolution electrode using in-situ grown MoS2 foam nickel is employed. This is achieved by cross-weaving metal wires into a mesh structure on a foam nickel substrate, and by using permanent magnets and soft magnetic materials to adjust the magnitude and direction of the magnetic field, combined with an electrochemical reaction to grow a MoS2 catalytically active coating in situ.

Benefits of technology

It significantly improved the specific surface area and catalytic effect of the hydrogen evolution electrode, enhanced the efficiency of hydrogen production by electrolysis, and improved the catalytic effect by optimizing the reaction conditions through an adjustable magnetic field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063802A_ABST
    Figure CN123063802A_ABST
Patent Text Reader

Abstract

This invention relates to the field of water electrolysis for hydrogen production, specifically to an in-situ grown MoS2 foamed nickel self-supporting hydrogen evolution electrode and its preparation method. The electrode includes an anode electrolyzer, a counter electrode and a reference electrode, and a foamed nickel substrate. A wire weaving device is installed inside the foamed nickel substrate. In this in-situ grown MoS2 foamed nickel self-supporting hydrogen evolution electrode and its preparation method, the anode electrolyzer stores an electrolyte, and the foamed nickel substrate is immersed in the electrolyte. By weaving the foamed nickel substrate into a mesh structure formed by multiple first and second metal wires, it is equivalent to filling the pores of the mesh structure with the foamed nickel substrate. This increases the specific surface area of ​​the hydrogen evolution electrode, thereby increasing its contact area with the electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of water electrolysis for hydrogen production technology, specifically to an in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method. Background Technology

[0002] In response to the increasingly serious global warming caused by excessive consumption of fossil fuels, innovative energy carriers to reduce greenhouse gas emissions from power plants have received great attention in recent years. Hydrogen is considered an excellent candidate for renewable energy carriers because it can provide high energy density without producing carbon emissions. For hydrogen production, water electrolysis is a promising and environmentally friendly method. Highly efficient electrocatalysts are crucial for improving hydrogen production efficiency. The activity of electrocatalysts can be improved through two strategies: one is to increase the active sites on the electrode surface by increasing the loading mass or adjusting the structure to expose more active sites; the other is to improve the inherent activity of each active site.

[0003] A magnetic field-loaded hydrogen evolution electrode device is disclosed in Chinese patent CN220550237U. This device uses a permanent magnet moving device placed in the hydrogen evolution electrolyte, driven by a drive device to move or rotate the permanent magnet back and forth, and adjusts the magnetic field strength by changing the distance between the permanent magnet and the working electrode surface. The direction of the magnetic field applied to the electrode is changed by rotating the bar permanent magnet. The magnetic field variation is adjustable within a certain range and only affects the hydrogen evolution reaction, achieving a significant improvement in catalytic effect. However, this magnetic field-loaded hydrogen evolution electrode device has the following drawbacks: Although the magnetic field variation is adjustable within a certain range and only affects the hydrogen evolution reaction, achieving a significant improvement in catalytic effect, the hydrogen evolution electrode is usually a metal mesh woven from nickel wire. However, due to the smooth surface and low roughness of the nickel wire, the specific surface area of ​​the nickel wire mesh is small, which affects the hydrogen production efficiency of the electrolyzer. Therefore, there is an urgent need for an in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method to solve the above problems. Summary of the Invention

[0004] The purpose of this invention is to at least address one of the aforementioned technical deficiencies.

[0005] Therefore, one objective of this invention is to propose an in-situ grown MoS2 nickel foam self-supporting hydrogen evolution electrode and its preparation method, so as to solve the problems mentioned in the background art and overcome the shortcomings of the prior art.

[0006] To achieve the above objectives, one aspect of the present invention provides an in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method, comprising an anodic electrolytic cell, a counter electrode installed inside the anodic electrolytic cell, a reference electrode installed inside the anodic electrolytic cell, a foam nickel substrate installed inside the reference electrode, and a metal wire weaving device disposed inside the foam nickel substrate.

[0007] The metal wire braiding device includes a first metal wire and a second metal wire. The first metal wire is woven laterally inside the nickel foam matrix, and the second metal wire is woven vertically inside the nickel foam matrix. The first metal wire and the second metal wire are cross-woven to form a cross joint.

[0008] The present invention is further configured such that: flow holes are formed on the surface of the nickel foam substrate, the flow holes penetrate the interior of the nickel foam substrate, and the flow holes are uniformly distributed on the surface of the nickel foam substrate.

[0009] The present invention is further configured such that: a cathode electrolytic cell is provided on the left side of the anode electrolytic cell, a working electrode is installed inside the cathode electrolytic cell, and three support frames are installed near the circumference of the cathode electrolytic cell.

[0010] The present invention is further configured such that: a drive motor is fixedly installed at the upper end of the three support frames, and a rotating shaft is fixedly installed at the output end of the drive motor.

[0011] The invention is further configured such that: a container is fixedly connected to the lower end of the rotating shaft, and a soft magnetic material is fixedly installed on the surface of the container.

[0012] The present invention is further configured such that: a guide slide rod is fixedly connected to the surface of the container, a permanent magnet is slidably installed on the surface of the container, a guide groove is formed on the surface of the permanent magnet, and the guide slide rod is slidably engaged in the inside of the guide groove.

[0013] The present invention is further configured such that: an electric cylinder is fixedly installed on the top of the container, a connecting block is fixedly connected to the upper end of the permanent magnet, and the output end of the electric cylinder is fixedly installed on the surface of the connecting block.

[0014] The present invention is further configured as follows: an in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method, comprising the following steps:

[0015] S1, substrate structure modification, using a mesh structure woven from the first and second metal wires, filling the mesh pores with the nickel foam substrate, and opening uniformly penetrating flow holes on the surface of the nickel foam substrate to increase the specific surface area of ​​the electrode and the contact area with the electrolyte.

[0016] S2, Substrate cleaning pretreatment: The modified nickel foam substrate is ultrasonically cleaned to remove surface impurities and oil stains, and then dried to ensure that the substrate is clean and free of contaminants for subsequent assembly and use.

[0017] S3, Electrolytic cell basic assembly, build a dual electrolytic cell system, assemble the counter electrode, reference electrode and foamed nickel substrate inside the anode electrolytic cell, and fix the working electrode inside the cathode electrolytic cell.

[0018] S4, magnetic field mechanism assembly: a support frame is installed on the outside of the cathode electrolytic cell to fix the drive motor and the rotating shaft. The lower end of the rotating shaft is connected to the container. Soft magnetic material is fixed on the surface of the container, and permanent magnets are assembled through the guide structure.

[0019] S5, Installation and debugging of the adjustment mechanism: Install an electric cylinder on the top of the container, fix its output end to the connecting block of the permanent magnet, and rely on the guide slide rod and guide slot for limit to ensure that the permanent magnet can slide smoothly;

[0020] S6, Electrolyte preparation and filling: Prepare an electrolyte suitable for in-situ growth of MoS2, and inject it into the anodic and cathodic electrolytic cells respectively to completely immerse the foamed nickel substrate, and let it stand for 10~20 minutes to stabilize.

[0021] S7, magnetic field direction control, starts the drive motor, drives the container to rotate synchronously with the permanent magnet through the rotating shaft, and adjusts the direction of the magnetic field applied by the electrode by taking into account the magnetic response characteristics of the soft magnetic material;

[0022] S8, magnetic field strength control, starts the electric cylinder, drives the permanent magnet to slide horizontally along the guide slide, adjusts the distance between the permanent magnet and the working electrode, and precisely controls the strength of the auxiliary magnetic field;

[0023] S9, in-situ growth of catalytic coating, starts the electrolysis system, and uses an adjustable and controllable auxiliary magnetic field to optimize reaction conditions, and grows MoS2 catalytically active coating in-situ on the surface of nickel foam substrate through electrochemical reaction.

[0024] S10, electrode post-processing and shaping, after the reaction is completed, the equipment is shut down, the electrode semi-finished product is taken out, the residual electrolyte is rinsed with deionized water, and the finished self-supporting hydrogen evolution electrode is obtained by low temperature vacuum drying.

[0025] In summary, the beneficial technical effects of the present invention are as follows:

[0026] 1. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method: The inside of the anolyte contains an electrolyte, and the foam nickel substrate is immersed in the electrolyte. By weaving the foam nickel substrate into a mesh structure formed by multiple first metal wires and multiple second metal wires, it is equivalent to filling the pores of the mesh structure formed by the first metal wires and second metal wires with the foam nickel substrate. The specific surface area of ​​the hydrogen evolution electrode is increased by means of the foam nickel substrate, which increases the contact area with the electrolyte, thereby improving the electrolytic hydrogen production efficiency of the hydrogen evolution electrode.

[0027] 2. This in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method utilize a magnetic field provided by a permanent magnet to magnetize a sheet-like soft magnetic material. The sheet-like soft magnetic material can change the magnitude and direction of its own magnetic field according to the movement and rotation of the bar permanent magnet, thereby providing a magnetic field of different magnitudes and directions to the working electrode. By placing a permanent magnet moving device in the hydrogen evolution electrolyte, a drive motor is used to rotate the permanent magnet, and the magnitude of the magnetic field is adjusted by changing the distance between the permanent magnet and the surface of the working electrode. The direction of the magnetic field applied to the electrode is changed by rotating the bar permanent magnet. The change of the magnetic field is adjustable within a certain range and only affects the hydrogen evolution reaction, thereby achieving a significant improvement in catalytic effect. Attached Figure Description

[0028] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:

[0029] Figure 1 This is a schematic diagram of the overall structure of the present invention;

[0030] Figure 2 This is a schematic diagram of the surface structure of the nickel foam matrix of the present invention;

[0031] Figure 3 This is a schematic diagram of the surface structure of the container in Embodiment 1 of the present invention;

[0032] Figure 4 This is a schematic diagram of the surface structure of the permanent magnet of the present invention;

[0033] Figure 5 This is a schematic diagram of the surface structure of the container in Embodiment 2 of the present invention.

[0034] In the diagram: 1. Anode electrolytic cell; 2. Counter electrode; 3. Reference electrode; 4. Nickel foam substrate; 5. First metal wire; 6. Second metal wire; 7. Cross joint; 8. Flow hole; 9. Cathode electrolytic cell; 10. Working electrode; 11. Support frame; 12. Drive motor; 13. Rotating shaft; 14. Container; 15. Soft magnetic material; 16. Permanent magnet; 17. Guide slot; 18. Guide slide rod; 19. Electric cylinder; 20. Connecting block. Detailed Implementation

[0035] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0036] Example 1

[0037] Reference Figure 1 , Figure 2 , Figure 3 , Figure 4 This invention discloses an in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method, comprising an anolyte 1, a counter electrode 2 installed inside the anolyte 1, a reference electrode 3 installed inside the anolyte 1, a foam nickel substrate 4 installed inside the reference electrode 3, and a wire braiding device disposed inside the foam nickel substrate 4. The wire braiding device includes a first wire 5 and a second wire 6. The first wire 5 is horizontally braided inside the foam nickel substrate 4, and the second wire 6 is vertically braided inside the foam nickel substrate 4. The first wire 5 and the second wire 6 are cross-braided to form a cross joint 7. Flow holes 8 are formed on the surface of the foam nickel substrate 4, penetrating the interior of the foam nickel substrate 4, and are uniformly distributed on the surface of the foam nickel substrate 4.

[0038] The anodic electrolytic cell 1 contains an electrolyte. The nickel foam substrate 4 is immersed in the electrolyte. By weaving the nickel foam substrate 4 into a mesh structure formed by multiple first metal wires 5 and multiple second metal wires 6, it is equivalent to filling the pores of the mesh structure formed by the first metal wires 5 and the second metal wires 6 with the nickel foam substrate 4. The specific surface area of ​​the hydrogen evolution electrode is increased by means of the nickel foam substrate 4, which increases the contact area with the electrolyte, thereby improving the electrolytic hydrogen production efficiency of the hydrogen evolution electrode.

[0039] A cathode electrolytic cell 9 is provided on the left side of the anode electrolytic cell 1. A working electrode 10 is installed inside the cathode electrolytic cell 9. Three support frames 11 are installed near the circumference of the cathode electrolytic cell 9. A drive motor 12 is fixedly installed on the upper end of the three support frames 11. A rotating shaft 13 is fixedly installed on the output end of the drive motor 12. A container 14 is fixedly connected to the lower end of the rotating shaft 13. A soft magnetic material 15 is fixedly installed on the surface of the container 14. A guide slide rod 18 is fixedly connected to the surface of the container 14. A permanent magnet 16 is slidably installed on the surface of the container 14. A guide slot 17 is opened on the surface of the permanent magnet 16. The guide slide rod 18 is slidably engaged in the inside of the guide slot 17.

[0040] The permanent magnet 16 is mounted on the surface of the container 14 and is fixed by the engagement of the guide slide rod 18 and the guide slot 17. After the operator starts the drive motor 12, the output end of the drive motor 12 rotates, which drives the rotating shaft 13 to rotate. The rotation of the rotating shaft 13 drives the container 14 and the permanent magnet 16 to rotate simultaneously. The permanent magnet 16 is the simplest and most effective way to generate a magnetic field. Because the electrons in the permanent magnet 16 move in a directional circular motion around the atomic nucleus, they can form a small ring current, which manifests as a neat molecular current. Therefore, it can generate a strong and stable magnetic field without an external current, making it an excellent energy-saving magnetic field source. In order to obtain a uniform magnetic field with variable intensity, a magnetic field needs to be applied between the permanent magnet 16 and other magnetic materials. The magnetic material 15 has low coercivity and narrow hysteresis loop, enabling it to respond quickly to changes in the external magnetic field. The sheet-like soft magnetic material 15 is magnetized by the magnetic field provided by the permanent magnet 16. The sheet-like soft magnetic material 15 can change the magnitude and direction of its own magnetic field according to the movement and rotation of the bar permanent magnet 16, thereby providing the working electrode 10 with magnetic fields of different magnitudes and directions. By placing a permanent magnet moving device in the electrolyte of hydrogen evolution, the permanent magnet 16 is driven to rotate by the drive motor 12, and the magnitude of the magnetic field is adjusted by changing the distance between the permanent magnet 16 and the surface of the working electrode 10. The direction of the magnetic field applied to the electrode is changed by rotating the bar permanent magnet 16. The change of the magnetic field is adjustable within a certain range and only affects the hydrogen evolution reaction, thereby achieving a significant improvement in catalytic effect.

[0041] Example 2

[0042] Reference Figure 5 An electric cylinder 19 is fixedly installed on the top of the container 14, and a connecting block 20 is fixedly connected to the upper end of the permanent magnet 16. The output end of the electric cylinder 19 is fixedly installed on the surface of the connecting block 20.

[0043] After the operator starts the electric cylinder 19, the output end of the electric cylinder 19 slides left and right, which drives the connecting block 20 and the permanent magnet 16 to slide left and right, thereby adjusting the distance between the permanent magnet 16 and the working electrode 10. The permanent magnet 16 slides and acts on the surface of the guide slide rod 18 through the guide slot 17. The guide slide rod 18 limits and fixes the permanent magnet 16, improving the stability of the left and right sliding of the permanent magnet 16. By adjusting the distance between the permanent magnet 16 and the working electrode 10, the magnitude of its own magnetic field is adjusted. Similarly, the change of the magnetic field is adjustable within a certain range and only affects the hydrogen evolution reaction, thereby achieving a significant improvement in catalytic effect.

[0044] The implementation principle of this embodiment is as follows:

[0045] By weaving the nickel foam matrix 4 into a mesh structure formed by multiple first metal wires 5 and multiple second metal wires 6, it is equivalent to filling the pores of the mesh structure with the nickel foam matrix 4. This increases the specific surface area of ​​the hydrogen evolution electrode, enlarging its contact area with the electrolyte, thereby improving the electrolytic hydrogen production efficiency of the hydrogen evolution electrode. Rotation of the output end of the drive motor 12 drives the rotating shaft 13 to rotate, which in turn drives the container 14 and the permanent magnet 16 to rotate simultaneously. The magnetic field strength is adjusted by changing the distance between the permanent magnet 16 and the surface of the working electrode 10, thus significantly improving the catalytic effect. Sliding the output end of the electric cylinder 19 left and right drives the connecting block 20 and the permanent magnet 16 to slide left and right, thereby adjusting the distance between the permanent magnet 16 and the working electrode 10. The distance between the working electrodes 10, the permanent magnet 16 slides and acts on the surface of the guide rail 18 through the guide slot 17, the guide rail 18 limits and fixes the permanent magnet 16, improving the stability of the permanent magnet 16 sliding left and right, the magnitude of its own magnetic field is adjusted by adjusting the distance between the permanent magnet 16 and the working electrode 10, similarly, the change of the magnetic field is adjustable within a certain range and only affects the hydrogen evolution reaction, thereby achieving a significant improvement in catalytic effect, and an in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method, the steps are as follows: S1, substrate structure modification, the first metal wire 5 and the second metal wire 6 are cross-woven into a mesh structure, the foam nickel substrate 4 is filled into the mesh pores, and uniform through-flow holes 8 are opened on the surface of the foam nickel substrate 4 to increase the electrode specific surface area and the contact area with the electrolyte; S2, Substrate cleaning pretreatment: The modified nickel foam substrate 4 is ultrasonically cleaned to remove surface impurities and oil stains, and then dried to ensure the substrate is clean and free of contaminants for subsequent assembly; S3, Electrolytic cell basic assembly: A dual electrolytic cell system is built. The counter electrode 2, reference electrode 3, and nickel foam substrate 4 are assembled inside the anode electrolytic cell 1, and the working electrode 10 is fixedly installed inside the cathode electrolytic cell 9; S4, Magnetic field mechanism assembly: A support frame 11 is installed on the outside of the cathode electrolytic cell 9 to fix the drive motor 12 and the rotating shaft 13. The lower end of the rotating shaft 13 is connected to the container 14. Soft magnetic material 15 is fixed on the surface of the container 14, and a permanent magnet 16 is assembled through a guide structure; S5, Gap adjustment mechanism installation and debugging: An electric cylinder 19 is installed on the top of the container 14, and its output end is fixed to the connecting block 20 of the permanent magnet 16. The guide slide rod 18 and guide slot 17 limit the movement to ensure that the permanent magnet 16 can slide smoothly; S6, Electrolyte preparation and filling: Prepare an electrolyte suitable for in-situ growth of MoS2 and inject it into the anodic electrolytic cell 1 and the cathode electrolytic cell 9 respectively, completely immersing the nickel foam substrate 4, and let it stand for 10~20 minutes to stabilize; S7, Magnetic field direction adjustment: Start the drive motor 12, and drive the container 14 and the permanent magnet 16 to rotate synchronously through the rotating shaft 13. Combined with the magnetic response characteristics of the soft magnetic material 15, adjust the direction of the magnetic field applied to the electrode;S8, Magnetic field strength adjustment: The electric cylinder 19 is activated, driving the permanent magnet 16 to slide horizontally along the guide rod 18, adjusting the distance between the permanent magnet 16 and the working electrode 10, and precisely controlling the strength of the auxiliary magnetic field; S9, In-situ growth of the catalytic coating: The electrolysis system is turned on, and the adjustable and controllable auxiliary magnetic field is used to optimize the reaction conditions, growing a MoS2 catalytically active coating in-situ on the surface of the nickel foam substrate 4 through electrochemical reaction; S10, Electrode post-treatment and shaping: After the reaction is completed, the equipment is shut down, the electrode semi-finished product is removed, the residual electrolyte is rinsed with deionized water, and then dried under low temperature vacuum to obtain the finished self-supporting hydrogen evolution electrode.

[0046] Furthermore, the following precautions should be taken during the preparation process: 1. When braiding the first metal wire 5 and the second metal wire 6, they must be evenly arranged, and the opening specifications of the flow holes 8 must be consistent to avoid uneven local structure of the foamed nickel substrate 4, which would affect the uniformity of electrolyte contact; 2. The pretreatment of the foamed nickel substrate 4 must thoroughly remove oil and impurities, and after drying, there must be no residual moisture to prevent impurities and moisture from interfering with the in-situ growth quality of the MoS2 coating; 3. When assembling the electrolytic cell, it is necessary to ensure that the positions of the counter electrode 2, reference electrode 3, and working electrode 10 are regular, and the equipment wiring is secure to ensure stable electrolytic reaction; 4. When assembling and sliding the permanent magnet 16, it is necessary to ensure that the guide slide rod 18 and the guide slot 17 are precisely matched, and that the sliding is smooth and without jamming or deviation. 5. The operating parameters of the electric cylinder 19 and the drive motor 12 must be smoothly controlled, and high-speed start-stop is strictly prohibited to avoid sudden changes in the displacement and speed of the permanent magnet 16, which could affect the stability of the magnetic field; 6. The electrolyte filling amount must be strictly controlled to completely immerse the foamed nickel substrate 4 and allow it to stand for stabilization before starting the reaction to ensure uniform concentration and state of the electrolytic system; 7. During the magnetic field control process, the magnitude and direction of the magnetic field must be adjusted gradually, and the hydrogen evolution reaction should be optimized only to avoid excessive parameter fluctuations that could affect the growth of the electrode catalytic coating; 8. The drying temperature of the electrode post-treatment must be controlled within the low-temperature range, and high-temperature baking is strictly prohibited to prevent damage to the MoS2 coating structure and performance degradation, and to ensure the quality of the finished electrode.

Claims

1. An in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method, characterized in that: It includes an anode electrolytic cell (1), a counter electrode (2) is installed inside the anode electrolytic cell (1), a reference electrode (3) is installed inside the anode electrolytic cell (1), a nickel foam substrate (4) is installed inside the reference electrode (3), and a wire weaving device is provided inside the nickel foam substrate (4).

2. The metal wire braiding device includes a first metal wire (5) and a second metal wire (6). The first metal wire (5) is woven laterally inside the nickel foam substrate (4), and the second metal wire (6) is woven vertically inside the nickel foam substrate (4). The first metal wire (5) and the second metal wire (6) are cross-woven to form a cross joint (7).

3. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 1, characterized in that: The surface of the nickel foam substrate (4) has flow holes (8) that penetrate the interior of the nickel foam substrate (4) and are evenly distributed on the surface of the nickel foam substrate (4).

4. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 2, characterized in that: A cathode electrolytic cell (9) is provided on the left side of the anode electrolytic cell (1). A working electrode (10) is installed inside the cathode electrolytic cell (9). Three support frames (11) are installed near the circumference of the cathode electrolytic cell (9).

5. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 3, characterized in that: A drive motor (12) is fixedly installed on the upper end of the three support frames (11), and a rotating shaft (13) is fixedly installed on the output end of the drive motor (12).

6. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 4, characterized in that: The lower end of the rotating shaft (13) is fixedly connected to a container (14), and a soft magnetic material (15) is fixedly installed on the surface of the container (14).

7. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 5, characterized in that: The surface of the container (14) is fixedly connected to a guide slide rod (18), and a permanent magnet (16) is slidably installed on the surface of the container (14). A guide slot (17) is opened on the surface of the permanent magnet (16), and the guide slide rod (18) is slidably engaged in the inside of the guide slot (17).

8. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 6, characterized in that: An electric cylinder (19) is fixedly installed on the top of the container (14), and a connecting block (20) is fixedly connected to the upper end of the permanent magnet (16). The output end of the electric cylinder (19) is fixedly installed on the surface of the connecting block (20).

9. The in-situ grown MoS2 foam nickel self-supporting hydrogen evolution electrode and its preparation method according to claim 7, characterized in that, The steps are as follows: S1, substrate structure modification, using the first metal wire 5 and the second metal wire 6 to cross-weave into a mesh structure, filling the mesh pores with the foamed nickel substrate 4, and opening uniformly penetrating flow holes 8 on the surface of the foamed nickel substrate 4 to increase the specific surface area of ​​the electrode and the contact area with the electrolyte. S2, Substrate cleaning pretreatment: The modified nickel foam substrate 4 is ultrasonically cleaned to remove surface impurities and oil stains, and then dried to ensure that the substrate is clean and free of contaminants for subsequent assembly and use. S3, Electrolytic cell basic assembly, build a dual electrolytic cell system, assemble counter electrode 2, reference electrode 3 and foamed nickel substrate 4 inside the anode electrolytic cell 1, and fix the working electrode 10 inside the cathode electrolytic cell 9. S4, magnetic field mechanism assembly: a support frame 11 is installed on the outside of the cathode electrolytic cell 9 to fix the drive motor 12 and the rotating shaft 13. The lower end of the rotating shaft 13 is connected to the container 14. The surface of the container 14 is fixed with soft magnetic material 15 and a permanent magnet 16 is assembled through a guide structure. S5, Installation and debugging of the adjustment mechanism: Install an electric cylinder 19 on the top of the container 14 and fix its output end to the connecting block 20 of the permanent magnet 16. Relying on the guide slide rod 18 and the guide slot 17 for limiting, the permanent magnet 16 can slide smoothly. S6, Electrolyte preparation and filling: Prepare an electrolyte suitable for in-situ growth of MoS2, and inject it into the anodic electrolytic cell 1 and the cathode electrolytic cell 9 respectively, completely immersing the nickel foam substrate 4, and let it stand for 10~20 minutes to stabilize. S7, magnetic field direction adjustment, start drive motor 12, drive container 14 and permanent magnet 16 to rotate synchronously through rotating shaft 13, and adjust the direction of magnetic field applied by electrode in combination with the magnetic response characteristics of soft magnetic material 15; S8, magnetic field strength adjustment, start electric cylinder 19, drive permanent magnet 16 to slide horizontally along guide slide rod 18, adjust the distance between permanent magnet 16 and working electrode 10, and precisely control the strength of auxiliary magnetic field; S9, In-situ growth of catalytic coating, the electrolysis system is turned on, and the reaction conditions are optimized by an adjustable and controllable auxiliary magnetic field. MoS2 catalytic active coating is grown in-situ on the surface of nickel foam substrate 4 through electrochemical reaction. S10, electrode post-processing and shaping, after the reaction is completed, the equipment is shut down, the electrode semi-finished product is taken out, the residual electrolyte is rinsed with deionized water, and the finished self-supporting hydrogen evolution electrode is obtained by low temperature vacuum drying.

Citation Information

Patent Citations

  • Magnetic field loading hydrogen evolution electrode device

    CN220550237U