A negative electrode plate, a secondary battery
By using high-temperature crosslinking additives and compound binder systems in high-silicon anode sheets to form a continuous protective film and conductive network, the volume expansion problem of high-silicon anode systems is solved, the high-temperature cycle stability and safety of batteries are improved, and room-temperature cycle and rate performance are also improved.
Patent Information
- Application Number
- CN202611241142.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies cannot effectively solve the problems of electrode cracking, repeated SEI film rupture, and high-temperature side reactions caused by volume expansion during the charging and discharging process of high-silicon anode systems, which affect the room temperature cycle stability and high temperature safety of batteries.
A continuous protective film and conductive network are formed by using a high-temperature crosslinking additive 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane and a compound binder system, combined with inorganic fillers and conductive agents, to buffer the expansion stress of silicon particles and suppress high-temperature side reactions.
It improves the high-temperature cycle stability and safety performance of the battery, enhances the room-temperature cycle performance and rate performance, and reduces the probability of micro-short circuits.
Smart Images

Figure SMS_3 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] This invention belongs to the field of battery technology, specifically relating to a negative electrode sheet and a secondary battery. Background Technology
[0002] With the increasing demand for energy density in lithium-ion batteries, silicon-based materials, due to their extremely high theoretical specific capacity (approximately 4200 mAh / g), are considered an important development direction for next-generation high-energy-density lithium-ion battery anode materials. To meet the stringent requirements of high energy density, silicon-carbon anode systems with high silicon content (effective silicon ≥ 30%) have gradually become a focus of industry research. However, silicon materials exhibit a volume expansion effect of up to 200%~300% during charge-discharge cycles. This significant volume change leads to serious problems such as electrode cracking, repeated rupture of the solid electrolyte interphase (SEI) film, and uncontrolled high-temperature side reactions, greatly limiting the commercial application of high-silicon anodes.
[0003] To address the above problems, existing technologies typically employ the following improvement schemes, but these schemes also present some challenges.
[0004] Method 1: Adding film-forming additives to the electrolyte, such as fluoroethylene carbonate (FEC) and vinylene carbonate (VC), forms an SEI film on the silicon anode surface to inhibit the continuous decomposition of the electrolyte. However, the SEI film formed by these traditional additives often exhibits significant brittleness and cannot adapt to the large volume deformation of anode particles in high-silicon systems. During long-term charge-discharge cycles, the brittle SEI film continuously breaks and rebuilds, failing to provide stable protection and instead continuously consuming limited electrolyte and active lithium, leading to a sharp decline in battery cycle life.
[0005] Method 2: Using siloxane additives as electrolyte additives, but their application has significant limitations. Firstly, the addition amount is extremely low (usually less than 1%), and it is only suitable for low-silicon systems (effective silicon < 15%). This is because those skilled in the art generally believe that the polymerization reaction of siloxanes on the negative electrode surface significantly increases the interfacial impedance of the battery. Secondly, increasing the addition amount of siloxane additives in high-silicon systems will damage the conductive network of the electrode, leading to a sharp increase in internal resistance and deterioration of electrochemical performance.
[0006] Method 3: Modify the negative electrode binder, such as with polyacrylic acid (PAA) or polyurethane (PUD), to reduce expansion by improving adhesion. However, binder modification can only partially improve the mechanical properties of the electrode at the mechanical and physical level. Once the battery is in a high-temperature environment, it still cannot fundamentally solve the problem of severe side reactions caused by the thermal decomposition of the SEI film.
[0007] In summary, due to the unique ultra-large volume expansion effect and high temperature characteristics of high-silicon anodes (effective silicon ≥30%), existing single technical means cannot effectively control them.
[0008] There is an urgent need for a technical solution that can simultaneously ensure room temperature cycling stability, high temperature safety, and electrode structure integrity in high-silicon anode systems. Summary of the Invention
[0009] In response to the problems of poor room temperature cycling stability, poor high temperature safety, and electrode cracking in existing silicon-carbon anode systems with a silicon content of 30% to 50%, this application provides an anode sheet and a secondary battery.
[0010] The technical solution adopted by the present invention to solve the above-mentioned technical problems is as follows: In a first aspect, the present invention provides a negative electrode sheet comprising a negative electrode active material layer, the negative electrode active material layer comprising a negative electrode active material, a negative electrode binder, a negative electrode conductive agent, an inorganic filler, and a high-temperature crosslinking additive, wherein the negative electrode active material comprises silicon; the high-temperature crosslinking additive comprises 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane; and the negative electrode binder comprises a first binder and a second binder, wherein the first binder comprises modified polyacrylic acid. The second adhesive includes at least one of rubber-based adhesives, polyurethane-based adhesives, polyimide-based adhesives, and polyvinyl alcohol-based adhesives; The negative electrode sheet satisfies Equations 1 and 2; 7×W1≤W2≤9×W1, Equation 1; and 30%≤W1≤50%; 5.4 + 4.8 × (W1 - 0.3) ≤ W3 ≤ 5.6 + 5.2 × (W1 - 0.3) (Equation 2) Wherein, W1 is the mass percentage of silicon in the negative electrode active material, in % (%). W2 represents the mass percentage of the high-temperature crosslinking additive in the negative electrode active material layer, expressed in % (%). W3 represents the mass percentage of the negative electrode binder in the negative electrode active material layer, in units of %.
[0011] Preferably, the mass ratio of the first adhesive to the second adhesive is (2~3):1.
[0012] Preferably, 2.4%≤W2≤4%.
[0013] Preferably, 5.5% ≤ W3 ≤ 6.5%.
[0014] Preferably, the negative electrode conductive agent includes a first conductive agent and a second conductive agent, and the negative electrode sheet also satisfies formula 3: Equation 3; Where W4 is the mass ratio of the first conductive agent to the second conductive agent.
[0015] Preferably, the first conductive agent comprises a one-dimensional conductive carbon material, and the second conductive agent comprises a zero-dimensional conductive carbon material; the one-dimensional conductive carbon material comprises at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanofibers, and vapor-grown carbon fibers; the zero-dimensional conductive carbon material is selected from at least one of conductive carbon black SP, acetylene black, and Ketjen black. 1≤W4≤2.
[0016] Preferably, the negative electrode material layer comprises the following mass contents: 83%~88% negative electrode active material, 3.5%~5% negative electrode conductive agent, and 1%~1.5% inorganic filler.
[0017] Preferably, the inorganic filler includes at least one selected from aluminum oxide, silicon dioxide, TiO2, ZrO2, MgO, TiN, BN, and SiC; And / or, the D50 particle size of the inorganic filler is 50~200nm.
[0018] Preferably, the rubber-based adhesive includes at least one of hydrogenated nitrile rubber and styrene-butadiene rubber; The polyurethane adhesive includes at least one of oil-based polyurethane and water-based polyurethane; The polyimide adhesive includes at least one of oil-based polyimide and water-soluble polyimide; Polyvinyl alcohol adhesives include at least one of polyvinyl alcohol and modified polyvinyl alcohol; The modifying groups in the modified polyacrylic acid include at least one of sulfonic acid groups and amide groups; The modified polyvinyl alcohol contains at least one of the following modified groups: -COOH, -NH2, and silane groups.
[0019] Secondly, this application provides a secondary battery, including a positive electrode, a separator, and the aforementioned negative electrode.
[0020] The negative electrode sheet provided in this application has the following effects: 1) It contains a high-temperature crosslinking additive, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, which is dispersed in the negative electrode sheet in a solid nano-form at room temperature. It has electrochemical inertness and does not participate in the lithium intercalation / deintercalation electrochemical reaction. It forms a discontinuous film at room temperature and does not have the problem of interface impedance deterioration. It satisfies Formula 1, which limits the amount of high-temperature crosslinking additive to 7 to 9 times the effective silicon content. The higher the effective silicon content, the greater the expansion range of silicon particles and the greater the risk of high-temperature heat release. Correspondingly, the amount of high-temperature crosslinking additive is increased. It forms a continuous protective film on the surface of silicon particles by relying on the island aggregation-high-temperature spreading mechanism, which blocks the high-temperature side reaction between the electrolyte and silicon and improves the high-temperature cycle stability and safety performance of the battery. The upper limit of 9 times the effective silicon content can avoid excessive accumulation of high-temperature crosslinking additive, prevent the obstruction of lithium-ion conduction at room temperature and the increase of interface impedance, ensure the long cycle capacity retention rate of the battery at room temperature and high temperature, and improve the high-temperature safety performance of the battery. 2) With the increase of effective silicon, the expansion stress of silicon-carbon particles during charge and discharge increases simultaneously. Therefore, the total amount of binder increases with the increase of effective silicon. The negative electrode binder includes a first binder and a second binder. The negative electrode sheet satisfies Formula 2. The binder is compounded. Modified polyacrylic acid has high adhesion, and the second binder has high elasticity. The combination of the first binder and the second binder takes into account both the bonding strength and elastic deformation ability, which can effectively buffer the expansion stress of silicon during charge and discharge, reduce electrode powder shedding, cracking, and local lithium plating, and improve the cycle performance and safety performance of the battery. The lower limit of the range ensures the minimum bonding strength and prevents the electrode structure from collapsing during long cycles. The upper limit of the range limits the maximum proportion of binder to avoid excessive blockage of ion channels by organic polymers and increase of polarization voltage, thus ensuring the rate discharge performance. 3) The inorganic filler contained in the negative electrode fills the micro-pores inside the electrode, assists in heat conduction and heat dissipation, isolates the micro-burrs and protrusions of the electrode, reduces the probability of micro-short circuits, and improves the battery safety performance; the negative electrode conductive agent contained therein builds a long-range continuous conductive framework, fills the micro-gap, and can maintain the continuity of the conductive network even after the silicon particles expand significantly, thus synergistically improving the cycle performance of the battery. Detailed Implementation
[0021] To make the technical problems solved, the technical solutions, and the beneficial effects of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0022] An embodiment of the present invention provides a negative electrode sheet, comprising a negative electrode active material layer, the negative electrode active material layer comprising a negative electrode active material, a negative electrode binder, a negative electrode conductive agent, an inorganic filler, and a high-temperature crosslinking additive; the negative electrode active material comprising silicon; the high-temperature crosslinking additive comprising 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane; the negative electrode binder comprising a first binder and a second binder, the first binder comprising modified polyacrylic acid; The second adhesive includes at least one of rubber-based adhesives, polyurethane-based adhesives, polyimide-based adhesives, and polyvinyl alcohol-based adhesives; The negative electrode sheet satisfies Equations 1 and 2; 7×W1≤W2≤9×W1, Equation 1; and 30%≤W1≤50%; 5.4 + 4.8 × (W1 - 0.3) ≤ W3 ≤ 5.6 + 5.2 × (W1 - 0.3) (Equation 2) Wherein, W1 is the mass percentage of silicon in the negative electrode active material, in % (%). W2 represents the mass percentage of the high-temperature crosslinking additive in the negative electrode active material layer, expressed in % (%). W3 represents the mass percentage of the negative electrode binder in the negative electrode active material layer, in units of %.
[0023] The negative electrode sheet provided in this application has the following effects: 1) Contains a high-temperature crosslinking additive, 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, which is dispersed in the negative electrode in solid nano-form at room temperature. It is electrochemically inert and does not participate in the lithium intercalation / deintercalation electrochemical reaction. It forms a discontinuous film at room temperature and does not have the problem of interface impedance deterioration. It satisfies Formula 1, limiting the amount of high-temperature crosslinking additive to 7 to 9 times the effective silicon content. The higher the effective silicon content, the greater the expansion of silicon particles and the greater the risk of high-temperature exothermic reaction. Correspondingly, the amount of high-temperature crosslinking additive is increased. It forms a continuous protective film on the surface of silicon particles by relying on the island aggregation-high-temperature spreading mechanism, blocking the high-temperature side reaction between the electrolyte and silicon, and improving the high-temperature cycle stability and safety performance of the battery. The upper limit of the mass percentage of high-temperature crosslinking additive is 9 times the effective silicon content, which can avoid excessive accumulation of high-temperature crosslinking additive, prevent the obstruction of lithium-ion conduction at room temperature and the increase of interface impedance, ensure the long-term cycle capacity retention rate of the battery in room temperature and high-temperature cycles, and improve the high-temperature safety performance of the battery.
[0024] 2) With the increase of effective silicon, the expansion stress of silicon-carbon particles during charge and discharge increases simultaneously. Therefore, the total amount of binder increases with the increase of effective silicon. The negative electrode binder includes a first binder and a second binder. The negative electrode sheet satisfies Formula 2. The binder is compounded. Modified polyacrylic acid has high adhesion, and the second binder has high elasticity. The combination of the first binder and the second binder takes into account both the bonding strength and elastic deformation ability, which can effectively buffer the expansion stress of silicon during charge and discharge, reduce electrode powder shedding, cracking, and local lithium plating, and improve the cycle performance and safety performance of the battery. The lower limit of the mass percentage range of the negative electrode binder ensures the minimum bonding strength and prevents the long-cycle electrode structure from collapsing. The upper limit of the mass percentage range of the negative electrode binder limits the maximum proportion of binder, avoiding excessive blockage of ion channels by organic polymers and increasing polarization voltage, and ensuring rate discharge performance.
[0025] 3) The inorganic filler contained in the negative electrode fills the micro-pores inside the electrode, assists in heat conduction and heat dissipation, isolates the micro-burrs and protrusions of the electrode, reduces the probability of micro-short circuits, and improves the battery safety performance; the negative electrode conductive agent contained therein builds a long-range continuous conductive framework, fills the micro-gap, and can maintain the continuity of the conductive network even after the silicon particles expand significantly, thus synergistically improving the cycle performance of the battery.
[0026] The above-mentioned island aggregation-high temperature spreading film formation mechanism is as follows: When the negative electrode is heated, the silicon particles expand and expand the nanoclusters. The high temperature crosslinking additive can spread on the surface of the silicon particles. When the temperature rises to 90℃~120℃, ring-opening in-situ polymerization occurs to generate a dense organic-inorganic hybrid protective film, which blocks the electrolyte from contacting the active silicon and inhibits the high temperature SEI decomposition and side reactions from the source.
[0027] If the amount of high-temperature crosslinking additive added does not satisfy Equation 1, and W2 is less than 7 × W1, the content is too low, and a continuous protective film cannot be formed on the surface of silicon particles. The high-temperature side reaction between the electrolyte and silicon will still exist, reducing the battery's high-temperature cycle performance and safety. If W2 is greater than 9 × W1, the content is too high, lithium-ion conduction is hindered, interfacial impedance increases, and the battery's room-temperature cycle performance decreases.
[0028] If the amount of negative electrode binder added does not satisfy Equation 2, and W3 is less than 5.4 + 4.8 × (W1 - 0.3), the content of negative electrode binder is too low, the peel strength of the negative electrode sheet is reduced, it cannot effectively buffer the expansion stress of silicon during charging and discharging, and it is prone to problems such as electrode powder shedding, cracking, and local lithium plating, which reduces the battery's room temperature cycle performance, high temperature cycle performance, and safety. If W3 is greater than 5.6 + 5.2 × (W1 - 0.3), the content of negative electrode binder is too high, the binder ratio is high, and too much organic polymer blocks ion channels, increases polarization voltage, increases battery impedance, reduces rate performance, and reduces cycle performance.
[0029] In some embodiments, the mass ratio of the first adhesive to the second adhesive is (2~3):1.
[0030] Specifically, the mass ratio of the first binder to the second binder is in the range of (2~3):1. The first binder has a high content and high adhesion, ensuring that the negative electrode sheet has a good bonding effect. The second binder has high elasticity, which can improve the flexibility of the negative electrode sheet, so that the negative electrode sheet can take into account both bonding strength and elastic deformation ability, buffer the silicon charging and discharging expansion stress, and prevent the electrode sheet from cracking and shedding powder.
[0031] If the proportion of the first binder is too low and the proportion of the second binder is too high, the adhesion and peel strength of the negative electrode sheet will decrease, making it prone to powder shedding. As the number of charge-discharge cycles increases, the negative electrode material layer is more likely to detach, reducing the battery's cycle performance and safety. If the proportion of the first binder is too high and the proportion of the second binder is too low, the elastic deformation capacity of the negative electrode sheet will decrease, failing to effectively buffer the expansion stress of silicon during charge-discharge. This makes the negative electrode sheet prone to cracking, reducing battery safety and cycle performance.
[0032] In specific embodiments, the mass ratio of the first adhesive to the second adhesive can be 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.8:1, 3:1, or any two of the above.
[0033] In some embodiments, 2.4% ≤ W2 ≤ 4%.
[0034] Specifically, W2 satisfies 2.4%≤W2≤4%, meaning that the mass content of the high-temperature crosslinking additive in the negative electrode active material layer is in the range of 2.4%~4%. This can form a dense organic-inorganic hybrid continuous protective film on the surface of silicon particles, which can block the contact between the electrolyte and the active silicon, block the high-temperature side reactions between the electrolyte and the active silicon, effectively suppress the high-temperature SEI decomposition and side reactions, and at the same time, not significantly reduce the battery energy density.
[0035] In a specific embodiment, the value of W2 can be 2.4%, 2.5%, 2.8%, 2.9%, 3%, 3.3%, 3.4%, 3.5%, 3.7%, 3.9%, 4%, or any two of the above.
[0036] In some embodiments, 5.5% ≤ W3 ≤ 6.5%.
[0037] Specifically, the mass content of the negative electrode binder is in the range of 5.5% to 6.5%, which takes into account both bonding strength and elastic deformation capability. It can effectively buffer the expansion stress of silicon during charging and discharging, reduce electrode powder shedding, cracking, and local lithium plating, effectively improve the bonding strength and peel strength of the negative electrode, and has high elastic buffer deformation, thereby improving the cycle stability and safety of the battery.
[0038] In a specific embodiment, the value of W3 can be 5.5%, 5.8%, 5.9%, 6%, 6.3%, 6.4%, 6.5%, or any two of the above.
[0039] In some embodiments, the negative electrode conductive agent includes a first conductive agent and a second conductive agent, and the negative electrode sheet also satisfies formula 3: Equation 3; Where W4 is the mass ratio of the first conductive agent to the second conductive agent.
[0040] Specifically, the negative electrode sheet satisfies Equation 3. The mass ratio of the first conductive agent and the second conductive agent is calculated through the silicon content. In the negative electrode sheet, the first conductive agent builds a long-range continuous conductive framework, and the second conductive agent fills the micro gaps. This ensures that even if the silicon particles expand significantly and the conductive framework is stretched, the second conductive agent can still maintain local conductive contact, forming an effective conductive network. This maintains the continuity of the conductive network, effectively improves the conductivity of the negative electrode sheet, reduces the contact internal resistance and charge transfer impedance of the electrode sheet, and improves the rate performance and cycle performance of the battery.
[0041] In some embodiments, the first conductive agent comprises a one-dimensional conductive carbon material, and the second conductive agent comprises a zero-dimensional conductive carbon material; the one-dimensional conductive carbon material comprises at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanofibers, and vapor-grown carbon fibers; the zero-dimensional conductive carbon material is selected from at least one of conductive carbon black SP, acetylene black, and Ketjen black. 1≤W4≤2.
[0042] Specifically, the first conductive agent is selected from the above types and can build a long-range continuous conductive framework. The second conductive agent is selected from the above types and can fill the micro gaps. Even after the silicon particles expand significantly, the continuity of the conductive network can still be maintained, effectively reducing the impedance of the negative electrode and improving the cycle performance of the battery.
[0043] Specifically, 1≤W4≤2 means that the mass ratio of the first conductive agent to the second conductive agent is in the range of (1~2):1, which can effectively improve the conductivity of the negative electrode, reduce the contact internal resistance and charge transfer impedance of the electrode, and improve the rate performance and cycle performance of the battery.
[0044] In specific embodiments, the mass ratio of the first conductive agent and the second conductive agent can be 1:1, 1.1:1, 1.2:1, 1.4:1, 1.5:1, 1.6:1, 1.8:1, 1.9:1, 2:1, or any two of the above.
[0045] In some embodiments, the negative electrode material layer comprises the following mass contents: 83%~88% negative electrode active material, 3.5%~5% negative electrode conductive agent, and 1%~1.5% inorganic filler.
[0046] Specifically, the mass content of the negative electrode conductive agent ranges from 3.5% to 5%, effectively reducing the impedance of the negative electrode and improving the battery's cycle performance and rate performance. The mass content of the inorganic filler ranges from 1% to 1.5%, which fills the micropores of the electrode, assists in heat conduction and dissipation, and isolates the electrode burrs to prevent micro-short circuits. The mass content of the negative electrode active material ranges from 83% to 88%, ensuring the battery's energy density and other electrical properties.
[0047] In specific embodiments, the mass content of the negative electrode conductive agent can be 3.5%, 3.8%, 4%, 4.3%, 4.5%, 4.7%, 5%, or any two of the above. The mass content of the inorganic filler can be 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, or any two of the above. The mass content of the negative electrode active material can be 83%, 84%, 85%, 86%, 87%, 88%, or any two of the above.
[0048] In some embodiments, the negative electrode active material includes at least one of silicon material, silicon-carbon composite material, and carbon material.
[0049] In some preferred embodiments, the negative electrode active material includes silicon-carbon composite material and carbon material. In the negative electrode active material layer, the mass content of silicon-carbon composite material is 60% to 80%, and the mass content of carbon material is 8% to 23%.
[0050] In a specific embodiment, the mass content of the silicon-carbon composite material in the negative electrode active material layer can be 60%, 62%, 64%, 65%, 68%, 69%, 70%, 73%, 75%, 77%, 80%, or any two of the above. The mass content of the carbon material in the negative electrode active material layer can be 8%, 10%, 13%, 15%, 17%, 20%, 22%, 23%, or any two of the above.
[0051] In some embodiments, the carbon material includes at least one of natural graphite, hard carbon, soft carbon, and artificial graphite.
[0052] Silicon materials include at least one of elemental silicon and silicon oxide.
[0053] Silicon-carbon composite materials include nano-silicon / graphite composite materials, silicon oxide / graphite composite materials, silicon-carbon core-shell materials, and silicon oxide-carbon core-shell materials.
[0054] In some embodiments, the inorganic filler includes at least one selected from aluminum oxide, silicon dioxide, TiO2, ZrO2, MgO, TiN, BN, and SiC; And / or, the D50 particle size of the inorganic filler is 50nm~200nm.
[0055] Specifically, the inorganic fillers are selected from the above types and can assist in heat conduction and dissipation.
[0056] When the D50 particle size of the inorganic filler is within the above range, it is beneficial for the inorganic filler to fill the micropores of the electrode and effectively isolate the electrode burrs to prevent micro-short circuits.
[0057] In a specific embodiment, the D50 particle size of the inorganic filler can be 50nm, 60nm, 80nm, 100nm, 120nm, 150nm, 170nm, 190nm, 200nm, or any two of the above.
[0058] In some preferred embodiments, the inorganic filler includes one or both of aluminum oxide and silicon dioxide.
[0059] In some embodiments, the rubber-based adhesive includes at least one of hydrogenated nitrile rubber and styrene-butadiene rubber; The polyurethane adhesive includes at least one of oil-based polyurethane and water-based polyurethane; The polyimide adhesive includes at least one of oil-based polyimide and water-soluble polyimide; Polyvinyl alcohol adhesives include at least one of polyvinyl alcohol and modified polyvinyl alcohol; The modifying groups in the modified polyacrylic acid include at least one of sulfonic acid groups and amide groups; The modified polyvinyl alcohol contains at least one of the following modified groups: -COOH, -NH2, and silane groups.
[0060] Specifically, the modifying groups in the modified polyacrylic acid are selected from the above-mentioned types. The amide group has extremely strong polarity and the ability to form hydrogen bonds, which can form multiple high-strength hydrogen bond networks and coordination bonds with silicon materials and negative electrode current collectors (such as copper foil). This "dynamically reversible" strong interaction greatly improves the peel strength of the electrode. The sulfonic acid group is a strongly hydrophilic group with large steric hindrance. Its introduction can effectively disrupt the regular stacking of the original PAA molecular chains and significantly improve the solubility and dispersibility of the binder in aqueous slurry. More importantly, the introduction of the sulfonic acid group can improve the flexibility of the polymer chain and improve the wettability of the electrode to the electrolyte, thereby accelerating the conduction rate of lithium ions in the micropores of the electrode and reducing polarization without reducing the adhesion.
[0061] Rubber-based binders have high elastic deformation capacity, polyurethane-based binders can improve the flexibility of the electrode, polyimide-based additives can improve the rigidity of the electrode, and polyvinyl alcohol-based binders have a large number of hydroxyl groups, which can react with the modified groups in the first binder to construct a dense and high-strength three-dimensional interpenetrating network structure in the electrode, preventing electrode powder from falling off.
[0062] Oil-based polyurethane refers to polyurethane compounds that can dissolve in organic solvents such as acetone, ethyl acetate, and DMF. Water-based polyurethane refers to polyurethane compounds that can dissolve in water.
[0063] Similarly, oil-soluble polyimides refer to polyimide compounds that can dissolve in organic solvents, while water-soluble polyimides refer to polyimide compounds that can dissolve in water.
[0064] In some embodiments, oily polyurethane includes at least one of polyester-type oily polyurethane, polyether-type oily polyurethane, and polycarbonate-type oily polyurethane.
[0065] In some embodiments, the waterborne polyurethane includes at least one of anionic waterborne polyurethane, cationic waterborne polyurethane, and nonionic waterborne polyurethane.
[0066] The negative electrode sheet provided in this application abandons the traditional approach of modifying a single raw material and simple physical compounding of multiple components. Instead, it constructs a precise synergistic modification system of four components: high-temperature cross-linking functional component, compound elastic binder, binary composite conductive agent, and nano-inorganic filler. Each component has a clear division of labor and synergistic effect, which can simultaneously achieve the effects of no performance loss at room temperature, self-protection at high temperature, and long-term stability of electrode structure, thereby improving the cycle performance and safety performance of the battery.
[0067] Secondly, this application provides a method for preparing a negative electrode sheet, comprising the following steps: A composite powder is obtained by uniformly mixing a high-temperature crosslinking additive with an inorganic filler. The negative electrode active material, negative electrode conductive agent, negative electrode binder, solvent and the composite powder are mixed evenly to obtain a negative electrode slurry. The negative electrode slurry is coated on the surface of the negative electrode current collector and dried to obtain a negative electrode sheet.
[0068] The method for preparing the negative electrode sheet provided in this application is simple, easy to operate, and can be mass-produced.
[0069] In some embodiments, the high-temperature crosslinking additive is uniformly mixed with the inorganic filler to obtain a composite powder, including the following steps: High-temperature crosslinking additives and inorganic fillers are added to a grinding equipment and ground for 5 to 30 minutes to obtain composite powder.
[0070] The grinding method includes at least one of ball milling, air jet milling, and high shear dispersion grinding.
[0071] In some embodiments, the negative electrode active material, negative electrode conductive agent, negative electrode binder, solvent, and the composite powder are mixed uniformly to obtain a negative electrode slurry, including the following steps: The negative electrode binder includes a first binder and a second binder; A first adhesive and a portion of solvent are mixed evenly to obtain a first mixed solution, and a second adhesive and another portion of solvent are mixed evenly to obtain a second mixed solution; The negative electrode active material, negative electrode conductive agent, and the composite powder are added to a stirring device and dispersed evenly. First, a first mixed solution is added and mixed evenly, and then a second mixed solution is added and mixed evenly to obtain a negative electrode slurry.
[0072] In some embodiments, a negative electrode slurry is coated onto the surface of a negative electrode current collector and dried to obtain a negative electrode sheet, comprising the following steps: coating the negative electrode slurry onto the surface of a negative electrode current collector with a coating thickness of 80-120 μm, and drying at 60°C-130°C to obtain a negative electrode sheet.
[0073] In some embodiments, drying at 60℃ to 130℃ includes a first stage drying and a second stage drying. The first stage drying temperature T1 is 60℃≤T1<90℃, and the first stage drying time t1 is 15min≤t1≤30min. The second stage drying temperature T2 is 90℃≤T2≤130℃, and the second stage drying time t2 is 20min≤t2≤120min.
[0074] The drying process is divided into two stages. The first stage drying temperature T1 meets the requirement of 60℃≤T1<90℃, and the first stage drying time t1 is 15min≤t1≤30min, providing preliminary drying of the negative electrode sheet to avoid high-temperature sublimation loss of the high-temperature crosslinking additive. The second stage drying temperature T2 meets the requirement of 90℃≤T2≤130℃, and the second stage drying time t2 is 20min≤t2≤120min. This facilitates the ring-opening in-situ polymerization of the high-temperature crosslinking additive at 90℃~120℃, forming a dense organic-inorganic hybrid protective film that blocks contact between the electrolyte and active silicon, suppressing high-temperature SEI decomposition and side reactions from the source.
[0075] In a specific embodiment, the value of T1 can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 89°C, or within any two of the above. The value of t1 can be 15 min, 18 min, 20 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 30 min, or within any two of the above.
[0076] The value of T2 can be 90℃, 95℃, 100℃, 105℃, 110℃, 115℃, 120℃, 125℃, 130℃, or within any two of the above. The value of t2 can be 20min, 30min, 40min, 50min, 70min, 80min, 90min, 100min, 110min, 120min, or within any two of the above.
[0077] The solvent is deionized water.
[0078] Thirdly, this application provides a secondary battery, including a positive electrode, a separator, and the aforementioned negative electrode.
[0079] The secondary battery provided in this application, including the aforementioned negative electrode sheet, has the following effects: 1) It satisfies Formula 1, where the high-temperature crosslinking additive forms a continuous protective film on the surface of silicon particles, blocking the high-temperature side reactions between the electrolyte and silicon, improving the battery's room temperature cycle stability and high-temperature cycle stability, and enhancing the battery's high-temperature cycle performance and safety performance; 2) It satisfies Formula 2, where the binder compound, the modified polyacrylic acid has high adhesion, and the second binder has high elasticity. The first binder combined with the second binder balances bonding strength and elastic deformation capability, effectively buffering the silicon charge and discharge expansion stress, reducing electrode powder shedding, cracking, and local lithium plating, and improving the battery's room temperature cycle performance and high-temperature cycle performance. 3) The inorganic filler contained in the negative electrode sheet fills the microscopic pores inside the electrode sheet, assists in heat conduction and dissipation, isolates the microscopic burrs and protrusions of the electrode sheet, and reduces the probability of micro-short circuits; the contained negative electrode conductive agent builds a long-range continuous conductive framework, fills the microscopic gaps, and can maintain the continuity of the conductive network even after the silicon particles expand significantly, ensuring the conductivity of the electrode sheet and synergistically improving the battery's cycle performance and safety performance.
[0080] In some embodiments, the positive electrode sheet includes a positive current collector and a positive electrode material layer disposed on at least one side surface of the positive current collector, wherein the positive electrode material layer includes a positive electrode active material, a positive electrode conductive agent, and a positive electrode binder.
[0081] The positive electrode conductive agent includes at least one of carbon nanotubes, graphene, conductive carbon black, carbon fiber, and mesophase carbon microspheres.
[0082] The positive electrode binder includes at least one of polyacrylic acid, polyvinylidene fluoride, polyvinyl fluoride-hexafluoropropylene copolymer, polyimide, and polyurethane.
[0083] The positive electrode active material includes at least one of lithium-containing active materials and sodium-containing active materials.
[0084] Lithium-containing active materials include lithium cobalt oxide, lithium manganese oxide, ternary materials, lithium iron phosphate, lithium manganese iron phosphate, lithium-rich manganese-based materials, lithium nickel cobalt oxide, and lithium vanadium phosphate.
[0085] The battery cell, which is made by winding or stacking positive electrode plates, separators and negative electrode plates, needs to be baked before liquid filling. The baking temperature is 70℃~85℃.
[0086] The present invention will be further illustrated by the following examples.
[0087] Example 1 This embodiment is used to illustrate the negative electrode sheet and secondary battery disclosed in this invention.
[0088] S1. Preparation of negative electrode sheet S11: Raw materials: The negative electrode active material is selected from silicon-carbon composite material + graphite; the first binder is selected from modified polyacrylic acid, and the modifying group is selected from sulfonic acid group + amide group; the second binder is selected from hydrogenated nitrile rubber; the mass ratio of the first binder and the second binder is 2:1; The first conductive agent is selected from single-walled carbon nanotubes; the second conductive agent is selected from conductive carbon black SP; and the inorganic filler is selected from aluminum oxide with a D50 particle size of 100 nm.
[0089] S12: 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane and inorganic nanofillers are fed into a grinding equipment and ball-milled for 30 minutes to obtain composite powder.
[0090] S13: Mix the first adhesive and a portion of deionized water evenly to obtain a first mixed solution, and mix the second adhesive and another portion of deionized water evenly to obtain a second mixed solution; The negative electrode active material, negative electrode conductive agent, and composite powder obtained in step S11 were added to a vacuum mixer and dispersed at high speed for 10 minutes at a speed of 1400 rpm / min until uniformly dispersed. First, the first mixed solution was added and stirred at low speed for 15 minutes at a speed of 550 rpm / min until uniformly dispersed. Then, the second mixed solution was added and stirred at low speed for 15 minutes at a speed of 550 rpm / min until uniformly dispersed. Finally, high-speed dispersion was performed for 60 minutes at a speed of 1500 rpm / min. This step-by-step addition prevented local agglomeration of the binder, resulting in a stable negative electrode slurry.
[0091] S14: Coat the negative electrode slurry obtained in step S13 onto the surface of the negative electrode current collector copper foil with a coating thickness of 100 μm. Perform the first stage drying at T1=80℃ for 25 min, and then perform the second stage drying at T2=110℃ for 30 min.
[0092] S15: The negative electrode sheet dried in step S14 is rolled, slit, and dusted.
[0093] In the negative electrode active material layer, the mass content of silicon-carbon composite material is 76.3%, the mass content of graphite is 10%, the mass content of the first binder is 4%, the mass content of the second binder is 1.7%, the mass content of the first conductive agent is 2.5%, the mass content of the second conductive agent is 1.5%, the mass content of inorganic filler is 1.2%, and the mass content of high-temperature crosslinking additive is 2.8%.
[0094] W1=35%, W2=2.8%; W3=5.7%; W4=1.667.
[0095] S2, Preparation of positive electrode sheet The positive electrode active materials lithium cobalt oxide, PVDF, and SP are mixed evenly at a mass ratio of 98:1:1. Then, NMP solvent is added and mixed evenly to obtain a positive electrode slurry. The positive electrode slurry is coated on both sides of the positive electrode current collector aluminum foil and dried to form a positive electrode material layer on the surface of the aluminum foil, thus obtaining a positive electrode sheet.
[0096] S3, Lithium-ion battery manufacturing The positive electrode sheet, separator, and negative electrode sheet prepared above are wound sequentially into a battery cell. Care is taken to align the electrodes and control the tension to prevent separator damage or internal short circuits. The wound battery cell is placed in a soft-pack aluminum-plastic film casing and baked at 80°C. The separator is a PP separator. Purchased electrolyte is then injected to assemble a lithium-ion battery.
[0097] Examples 2-16 and Comparative Examples 1-12 Examples 2-16, Comparative Examples 1-12 and Example 1 are mostly the same in terms of steps, except that the specific values of W1, W2, W3 and W4 are different, as shown in Table 1; the rest are the same as in Example 1.
[0098] Table 1 Examples 17-32 Examples 17-32 are largely the same as Example 1, with the following differences: the mass ratio of the first binder to the second binder is different, the type of the second binder is different, the type of inorganic filler is different, the D50 particle size of the inorganic filler is different, and the mass content of the inorganic filler in the negative electrode active material layer is different, as detailed in Table 2. After changing the mass content of the inorganic filler, the mass content of the negative electrode active material is adjusted so that the sum of the total mass content of the negative electrode active material, the negative electrode conductive agent, the negative electrode binder, and the inorganic filler is 100%; the rest is the same as in Example 1.
[0099] Table 2 Performance testing I. The following performance tests were performed on the batteries obtained in the above embodiments and comparative examples: 1. Cyclic performance test at 25℃ The battery was left to stand at 25±2℃ for 2 hours, then charged at a constant current of 1C to 4.2V, and then charged at a constant voltage to 0.05C. After standing for 10 minutes, it was discharged at a constant current of 1C to 3.0V. This charging and discharging process was repeated 500 times. The capacity retention rate after 500 cycles at 25℃ was calculated as: (500th discharge capacity / 1st discharge capacity) * 100%.
[0100] Test the temperature change T3 of the battery during the first charge and discharge. T3 = maximum temperature of the battery surface during the first charge and discharge - surface temperature of the battery before charge and discharge.
[0101] 2. 45℃ Cyclic Performance Test The battery was left to stand at 45℃ for 2 hours, then charged at a constant current of 1C to 4.2V, and then charged at a constant voltage to a current of 0.05C. After standing for 10 minutes, it was discharged at a constant current of 1C to 3.0V. The above charge and discharge steps were repeated 500 times. The capacity retention rate after 500 cycles at 45℃ was calculated as: (500th discharge capacity / 1st discharge capacity) * 100%.
[0102] 3. Battery impedance growth rate after being placed at 100℃ for 4 hours; Test the internal resistance R1 of the battery at 100% SOC, then place it in a 100℃ constant temperature chamber for 4 hours, remove it and cool it to room temperature, then test the internal resistance R2 of the battery. The impedance growth rate = (R2-R1) / R1*100%.
[0103] 4. 130℃ Hot Box Test Five battery samples were tested for each embodiment and comparative example. The sample batteries were charged to 4.2V, heated to 130±1℃ at 5±2℃ / min, and held at that temperature for 30 minutes. The pass / fail status was recorded, and the highest surface temperature of the battery was tested using ARC.
[0104] 5. Electrode cracking test: Place the coated and dried negative electrode in an oven at 120℃ for 5 minutes, then take it out and record the number of cracks in the negative electrode (area 10*10cm).
[0105] The test results are shown in Table 3.
[0106] Table 3 Continued from Table 3 Continued from Table 3 As shown in Tables 1-3, comparing Examples 1-10 and Comparative Examples 1-12, the actual value of W2 in Comparative Examples 1-6 does not satisfy Equation 1, 7×W1≤W2≤9×W1. The battery's capacity retention rate during both room temperature and high temperature cycling is low, and the value of T3 is relatively large, indicating that the battery's charging and discharging temperature changes greatly, the battery's high-temperature storage impedance growth rate at 100℃ is large, the number of negative electrode cracks is large, the surface temperature of the 130℃ hot box test is high, the pass rate is low, and the battery's safety performance is low. This indicates that Equation 1 is satisfied, limiting the amount of high-temperature crosslinking additive to 7 to 9 times the effective silicon content. The higher the effective silicon content, the greater the expansion of silicon particles and the greater the risk of high-temperature heat release. Correspondingly, the amount of high-temperature crosslinking additive should be increased to form a continuous protective film on the surface of silicon particles by relying on the island aggregation-high-temperature spreading mechanism, blocking the high-temperature side reaction between the electrolyte and silicon, and improving the high-temperature cycling stability and safety performance of the battery. In Comparative Examples 7-12, the actual value of W3 does not satisfy Equation 2: 5.4 + 4.8 × (W1 - 0.3) ≤ W3 ≤ 5.6 + 5.2 × (W1 - 0.3). The battery's capacity retention rates during both room temperature and high temperature cycles are low, and the value of T3 is relatively large, indicating that the battery's charge and discharge temperature changes significantly, the battery's high-temperature storage impedance growth rate at 100℃ is large, the number of negative electrode cracks is high, the surface temperature of the 130℃ hot box test is high, the pass rate is low, and the battery's safety performance is low. This indicates that Equation 2 is satisfied. The binder is compounded, the modified polyacrylic acid has high adhesion, and the second binder has high elasticity. The combination of the first binder and the second binder takes into account both the bonding strength and elastic deformation ability, which can effectively buffer the silicon charge and discharge expansion stress, reduce electrode powder shedding, cracks, and local lithium plating, and improve the battery's cycle performance and safety performance.
[0107] Comparing Examples 1-10 and Examples 11-12, although Examples 11-12 satisfy Equations 1 and 2, W2 does not meet the range of 2.4% ≤ W2 ≤ 4%. In Example 11, the negative electrode active material layer contains too few high-temperature crosslinking additives, resulting in reduced density of the formed protective film and inability to effectively block the high-temperature side reactions between the electrolyte and active silicon. In Example 12, the high-temperature crosslinking additives are too numerous, increasing impedance. The batteries of Examples 11-12 have poor cycle performance at both room temperature and high temperature, with cracking of the negative electrode and reduced safety performance. This indicates that W2 meeting the range of 2.4% ≤ W2 ≤ 4% can form a dense organic-inorganic hybrid continuous protective film on the surface of silicon particles, which can block the contact between the electrolyte and active silicon, block the high-temperature side reactions between the electrolyte and active silicon, effectively suppress high-temperature SEI decomposition and side reactions, improve the cycle performance and safety performance of the battery, reduce impedance, and reduce cracking of the negative electrode.
[0108] Comparing Examples 1-10 and Examples 13-14, although they satisfy Equations 1 and 2, W3 does not satisfy 5.5%≤W3≤6.5%. The battery's room temperature cycle performance and high temperature cycle performance deteriorate, the charge and discharge temperature is high, the high temperature storage impedance growth rate increases, the negative electrode sheet cracks, and the hot box test has a 10% failure rate, resulting in reduced safety performance. This indicates that the negative electrode sheet satisfies Equations 1 and 2, and simultaneously satisfies W3 within the range of 5.5%≤W3≤6.5%. This balances bonding strength and elastic deformation capability, effectively buffers silicon charge and discharge expansion stress, reduces electrode powder shedding, cracking, and local lithium plating, effectively improves the bonding strength and peel strength of the negative electrode sheet, has high elastic buffer deformation, and improves the cycle stability and safety of the battery.
[0109] Comparing Examples 1-10 and Examples 15-16, the negative electrode sheet does not satisfy Equation 3. In Example 15, the mass ratio of the first conductive agent to the second conductive agent is too low, resulting in numerous cracks in the negative electrode sheet. In Example 16, the mass ratio of the first conductive agent to the second conductive agent is too high, leading to cracking of the negative electrode sheet. The cycle performance and safety performance of the batteries in Examples 15-16 are both poor, and the high-temperature storage impedance growth rate is high, indicating that the negative electrode sheet satisfies Equation 3. In the negative electrode, the first conductive agent builds a long-range continuous conductive framework, and the second conductive agent fills the micro gaps. This ensures that even if the silicon particles expand significantly and the conductive framework is stretched, the second conductive agent can still maintain local conductive contact, forming an effective conductive network. This maintains the continuity of the conductive network, effectively improves the conductivity of the negative electrode, reduces the contact internal resistance and charge transfer impedance of the electrode, and improves the rate performance and cycle performance of the battery.
[0110] Comparing Examples 1, 22-23 and Examples 24-25, when the mass content of inorganic filler is less than 1%, it cannot effectively assist in heat dissipation, resulting in high charging and discharging temperature changes in the battery. When the mass content of inorganic filler is greater than 1.5%, excessive inorganic filler reduces safety performance, but also leads to poor battery cycle performance due to excessive filling of micropores in the negative electrode. This indicates that when the mass content of inorganic filler is in the range of 1% to 1.5%, the inorganic filler fills the micropores of the electrode on one hand, assists in heat conduction and heat dissipation on the other hand, and isolates the burrs on the electrode to prevent micro-short circuits.
[0111] Comparing Examples 1, 26-27, and 28-29, in Example 26, the D50 particle size of the inorganic filler was less than 50 nm. The excessively small particle size of the inorganic filler blocked the pores of the negative electrode, affecting the battery's cycle performance and increasing impedance. In Example 27, the D50 particle size of the inorganic filler was greater than 50 nm. The excessively large particle size of the inorganic filler resulted in uneven distribution, reduced battery safety performance, worse cycle performance, and high impedance during high-temperature storage. This indicates that a D50 particle size of 50 nm to 200 nm is beneficial for the inorganic filler to fill the micropores of the electrode, effectively isolate electrode burrs to prevent micro-short circuits, and synergistically improve the battery's cycle performance and safety performance.
[0112] Comparing Examples 1 and 30-32, changing the type of inorganic filler and the type of the second binder, as long as they meet the types specified in this application, can improve the battery's room temperature cycle performance, high temperature cycle performance, reduce impedance, and improve battery safety performance.
[0113] In this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Additionally, in this application, the character " / " generally indicates that the preceding and following related objects have an "and" relationship.
[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A negative electrode sheet, characterized in that, The device includes a negative electrode active material layer, which comprises a negative electrode active material, a negative electrode binder, a negative electrode conductive agent, an inorganic filler, and a high-temperature crosslinking additive. The negative electrode active material includes silicon. The high-temperature crosslinking additive includes 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane. The negative electrode binder comprises a first binder and a second binder, wherein the first binder comprises modified polyacrylic acid. The second adhesive includes at least one of rubber-based adhesives, polyurethane-based adhesives, polyimide-based adhesives, and polyvinyl alcohol-based adhesives; The negative electrode sheet satisfies Equations 1 and 2; 7×W1≤W2≤9×W1, Equation 1; and 30%≤W1≤50%; 5.4 + 4.8 × (W1 - 0.3) ≤ W3 ≤ 5.6 + 5.2 × (W1 - 0.3) (Equation 2) Wherein, W1 is the mass percentage of silicon in the negative electrode active material, in % (%). W2 represents the mass percentage of the high-temperature crosslinking additive in the negative electrode active material layer, expressed in % (%). W3 represents the mass percentage of the negative electrode binder in the negative electrode active material layer, in units of %.
2. The negative electrode sheet according to claim 1, characterized in that, The mass ratio of the first adhesive to the second adhesive is (2~3):
1.
3. The negative electrode sheet according to claim 1, characterized in that, 2.4%≤W2≤4%。 4. The negative electrode sheet according to claim 1, characterized in that, 5.5%≤W3≤6.5%。 5. The negative electrode sheet according to claim 1, characterized in that, The negative electrode conductive agent includes a first conductive agent and a second conductive agent, and the negative electrode sheet also satisfies formula 3: Equation 3; Where W4 is the mass ratio of the first conductive agent to the second conductive agent.
6. The negative electrode sheet according to claim 5, characterized in that, The first conductive agent comprises a one-dimensional conductive carbon material, and the second conductive agent comprises a zero-dimensional conductive carbon material; the one-dimensional conductive carbon material comprises at least one of single-walled carbon nanotubes, multi-walled carbon nanotubes, carbon nanofibers, and vapor-grown carbon fibers; the zero-dimensional conductive carbon material is selected from at least one of conductive carbon black SP, acetylene black, and Ketjen black. 1≤W4≤2。 7. The negative electrode sheet according to claim 1, characterized in that, The negative electrode material layer comprises the following mass contents: 83%~88% negative electrode active material, 3.5%~5% negative electrode conductive agent, and 1%~1.5% inorganic filler.
8. The negative electrode sheet according to claim 1, characterized in that, The inorganic filler includes at least one of aluminum oxide, silicon dioxide, TiO2, ZrO2, MgO, TiN, BN, and SiC; And / or, the D50 particle size of the inorganic filler is 50~200nm.
9. The negative electrode sheet according to claim 1, characterized in that, The rubber-based adhesive includes at least one of hydrogenated nitrile rubber and styrene-butadiene rubber; The polyurethane adhesive includes at least one of oil-based polyurethane and water-based polyurethane; The polyimide adhesive includes at least one of oil-based polyimide and water-soluble polyimide; Polyvinyl alcohol adhesives include at least one of polyvinyl alcohol and modified polyvinyl alcohol; The modifying groups in the modified polyacrylic acid include at least one of sulfonic acid groups and amide groups; The modified polyvinyl alcohol contains at least one of the following modified groups: -COOH, -NH2, and silane groups.
10. A secondary battery, characterized in that, It includes a positive electrode, a separator, and a negative electrode as described in any one of claims 1-9.