Electrolyte for carbon fluoride battery based on quaternary sulfur fluoride and its preparation method and application

By introducing tetravalent sulfur fluoride into the electrolyte of fluorinated carbon batteries, an energy storage system in which SF bonds and CF bonds synergistically participate is established, solving the problem of improving the energy density and capacity of fluorinated carbon batteries in the existing technology, realizing the simultaneous improvement of battery performance, and applicable to a variety of metal battery systems.

CN123073086APending Publication Date: 2026-11-10QINGDAO INST OF BIOENERGY & BIOPROCESS TECH CHINESE ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611293614.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-25
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously improve the energy density and capacity of lithium batteries by introducing another type of active component without changing the composition and preparation process of fluorinated carbon cathode materials.

Method used

Introducing tetravalent sulfur fluoride as a liquid-phase active material into the electrolyte of a carbon fluoride battery allows for the construction of a dual-active-center energy storage system with SF and CF bonds participating synergistically. The tetravalent sulfur fluoride contributes to the capacity in the high-voltage range, while carbon fluoride provides the main capacity in the low-voltage range.

Benefits of technology

It achieves an increase in the total discharge capacity and energy density of lithium batteries, and the process is simple, compatible with existing fluorinated carbon battery manufacturing processes, and applicable to various metal primary battery systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The application belongs to the technical field of chemical power supply and electrochemical energy storage, and particularly relates to an electrolyte of a fluorocarbon battery based on capacity increase of tetravalent sulfur fluorides, a preparation method and application thereof. The electrolyte has tetravalent sulfur fluorides as active substances dissolved therein; wherein the concentration of the tetravalent sulfur fluorides in the electrolyte is 0.01-5 M, and the tetravalent sulfur fluorides contain at least one high-valence sulfur center and at least one S-F bond. The tetravalent sulfur fluorides contain high-valence sulfur centers and sulfur fluorine (S-F) bonds, and can participate in battery discharge reaction as liquid-phase active substances. By directly introducing the tetravalent sulfur fluorides into the electrolyte, the liquid-phase active components and the solid-phase fluorocarbon positive electrode are cooperatively discharged without changing the composition and preparation process of the fluorocarbon positive electrode material. The tetravalent sulfur fluorides provide capacity contribution in a higher voltage interval, and the fluorocarbon subsequently provides main capacity, thereby establishing a dual-active-center energy storage system in which S-F bonds and C-F bonds jointly participate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical power source and electrochemical energy storage technology, specifically relating to an electrolyte for a fluorinated carbon battery based on tetravalent sulfur fluoride for capacity enhancement, its preparation method, and its application. Background Technology

[0002] Primary lithium batteries are widely used in smart meters, medical devices, IoT devices, aerospace, and defense industries due to their high energy density, low self-discharge rate, long storage life, and excellent environmental adaptability. Among them, lithium-fluorinated carbon (Li / CF4) batteries... x With its extremely high theoretical specific capacity and excellent storage performance, the fluorocarbon battery has become one of the highest energy density systems among commercially available primary lithium batteries. Fluorocarbon materials are typically represented as CF₂. x (0 < x ≤ 1.3), its discharge process mainly involves the electrochemical reduction reaction of carbon-fluorine bonds: CF x + xLi+ + xe - → C + xLiF When x=1, CF x The theoretical specific capacity can reach 865 mAh / g, and the theoretical energy density is 2180 Wh / kg. Therefore, Li / CF x Batteries have significant application value in the field of high-energy-density primary power supplies.

[0003] However, the energy storage mechanism of fluorinated carbon materials mainly relies on the electrochemical reduction reaction of CF bonds, and their theoretical specific capacity and discharge voltage are determined by the degree of fluorination and material composition. Once the degree of fluorination is determined, the theoretical capacity and theoretical energy density of the cathode material are essentially fixed. Existing technologies mainly improve the utilization rate of active materials and reaction kinetics by controlling the microstructure of fluorinated carbon, constructing conductive networks, optimizing electrolytes, and improving interfacial reactions. However, these methods primarily improve actual discharge performance, and have limited potential for increasing the theoretical capacity and energy density determined by the energy storage mechanism of fluorinated carbon materials themselves. Therefore, if another type of high-energy-density active component that can participate in the electrochemical discharge reaction can be introduced while maintaining the main energy storage reaction of fluorinated carbon, allowing it to discharge synergistically with fluorinated carbon and provide additional capacity contribution, it is expected to further improve the energy density of primary lithium batteries.

[0004] Sulfur-fluorine bonded tetravalent sulfur fluorides, due to the integration of a high-oxidation-state sulfur center (+4 valence) and multiple strongly polar SF bonds within a single molecule, possess excellent high-potential electrochemical reactivity (3.5-3.7 V) and intrinsically high energy density, providing a sound material basis for their use as electrochemically active components. Therefore, how to fully utilize the high-potential electrochemical reactivity of these compounds and combine them with the high-capacity energy storage characteristics of fluorinated carbon to overcome the limitations of traditional single-energy storage mechanisms of fluorinated carbon and achieve simultaneous improvement in capacity and energy density remains a challenge that requires further investigation. Summary of the Invention

[0005] The purpose of this invention is to provide an electrolyte for a fluorinated carbon battery based on tetravalent sulfur fluoride for capacity enhancement, as well as its preparation method and application.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: An electrolyte for a capacity-enhancing fluorinated carbon battery, wherein a tetravalent sulfur fluoride is dissolved in the electrolyte as an active material; wherein the concentration of the tetravalent sulfur fluoride in the electrolyte is 0.01-5 M (preferably 0.1 M-2 M), and the tetravalent sulfur fluoride contains at least one high-valence sulfur center and at least one SF bond.

[0007] The tetravalent sulfur fluoride is selected from one or more of diethylamino sulfur trifluoride (DAST), sulfur trifluoride morpholine (Morpho-DAST), [bis(2-methoxyethyl)amine] sulfur trifluoride (Deoxo-Fluor), morpholine difluorosulfonium tetrafluoroborate (XtalFluor-M), (diethylamino) difluoride sulfur tetrafluoroborate (XtalFluor-E), and 4-tert-butyl-2,6-dimethylphenyl sulfur trifluoride (Fluolead).

[0008] The electrolyte is an organic solvent, an electrolyte salt, and a tetravalent sulfur fluoride; wherein the organic solvent is selected from one or more of the following: carbonate solvents (e.g., ethylene carbonate (EC), dimethyl carbonate (DMC), propylene carbonate (PC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC)), ether solvents (e.g., 1,3-dioxolane (DOL), 1,2-dimethoxyethane (DME), diethylene glycol dimethyl ether (DEGDME), tetraethylene glycol dimethyl ether (TEGDME), tetrahydrofuran (THF)), nitrile solvents (e.g., acetonitrile (AN), succinate (SN), propionitrile, glutaronitrile), sulfone solvents (e.g., sulfolane (TMS), dimethyl sulfone (DMS)), and fluorocarbonate solvents (e.g., fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC)).

[0009] The electrolyte salt is selected from one or more of LiPF6, LiBF4, LiFSI, LiTFSI, LiClO4, NaPF6, NaFSI, NaTFSI, and Mg(TFSI)2.

[0010] The application of an electrolyte in a capacity-enhancing fluorinated carbon battery, wherein the electrolyte is used as an electrolyte in a primary fluorinated carbon battery to achieve capacity enhancement.

[0011] A fluorinated carbon primary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the electrolyte is the aforementioned electrolyte.

[0012] The negative electrode is selected from lithium, sodium, potassium, magnesium, calcium, aluminum, and alloys of the aforementioned metals.

[0013] A method for preparing the battery: (1) Preparation of a positive electrode containing fluorinated carbon active material; (2) Prepare the electrolyte containing tetravalent sulfur fluoride; (3) Assemble the positive electrode, separator and negative electrode to form a battery; (4) Inject the electrolyte into the battery and complete the encapsulation.

[0014] In step (2), the tetravalent sulfur fluoride is added to the solution of organic solvent and electrolyte salt and mixed well, and then directly injected into the battery.

[0015] The fluorocarbon ratio x of the fluorocarbon material satisfies 0 < x ≤ 1.3.

[0016] In the electrolyte, tetravalent sulfur fluoride acts as a liquid-phase active fluorine source, first undergoing a discharge reaction in the high-voltage range, followed by a discharge reaction of fluorinated carbon, thus forming a staged discharge process and improving the average discharge voltage and capacity of the battery.

[0017] During discharge, tetravalent sulfur fluoride in the electrolyte preferentially undergoes reduction reactions in the higher voltage range, releasing capacity; subsequently, carbon fluoride continuously undergoes CF bond reduction reactions and provides the bulk capacity. This establishes a dual-active-center energy storage system involving both CF and SF bonds, achieving synergistic energy release from different active centers.

[0018] Compared with the prior art, the present invention has the following beneficial effects: This invention introduces soluble tetravalent sulfur fluoride containing sulfur-fluorine bonds as a liquid-phase active component into the electrolyte of a fluorinated carbon battery. By constructing an energy storage system in which the liquid-phase active component and the solid-phase fluorinated carbon cathode synergistically participate in the discharge reaction, the aim is to improve the capacity and energy density of primary batteries; specifically: 1. While maintaining the main energy storage mechanism of fluorinated carbon, tetravalent sulfur fluoride active components are introduced to provide additional capacity contribution to the battery system and improve the total discharge capacity; 2. In the electrolyte of this invention, the tetravalent sulfur fluoride can undergo an electrochemical reduction reaction during battery discharge, and participate in the discharge together with the fluorinated carbon active material, thereby forming a synergistic energy storage system in which SF bonds and CF bonds are involved, realizing synergistic energy storage of multiple fluorine-containing active centers; 3. This invention utilizes the high discharge potential of tetravalent sulfur fluoride in the electrolyte to release capacity in the high voltage range, thereby improving the average discharge voltage and energy density of the battery; 4. The primary battery assembled using the electrolyte of this invention does not require changes to the existing fluorinated carbon cathode formulation, coating process and battery manufacturing process. The capacity can be improved simply by adjusting the electrolyte composition, which has good prospects for industrial application. 5. The electrolyte of this invention is suitable for primary battery systems of lithium, sodium, potassium and multivalent metals, and has good versatility and scalability. Attached Figure Description

[0019] Figure 1 Example 1, Comparative Example 1, and Comparative Example 2 were measured at 0.1 mA cm⁻¹. -2 Specific capacity-voltage curve under constant current discharge conditions; Figure 2 Examples 1, 2, and 3 are at 0.1 mA cm -2 Specific capacity-voltage curve under constant current discharge conditions; Figure 3 Examples 7 and 8 are at 0.1 mA cm -2 Specific capacity-voltage curve under constant current discharge conditions. Detailed Implementation

[0020] The following specific embodiments further illustrate the fluorinated carbon battery based on tetravalent sulfur fluoride active electrolyte for capacity enhancement according to the present invention. It should be noted that the following embodiments are only used to explain the technical solution of the present invention and do not constitute a limitation on the scope of protection of the present invention. Equivalent substitutions or modifications made by those skilled in the art without departing from the concept of the present invention should all fall within the scope of protection of the present invention.

[0021] This invention utilizes tetravalent sulfur fluoride, which contains a high-valence sulfur center and a sulfur-fluorine (SF) bond, to participate in the battery discharge reaction as a liquid-phase active material. By directly introducing tetravalent sulfur fluoride into the electrolyte, synergistic discharge of the liquid-phase active component and the solid-phase fluorinated carbon cathode is achieved without altering the composition and preparation process of the fluorinated carbon cathode material. Specifically, the tetravalent sulfur fluoride contributes capacity in the higher voltage range, while the fluorinated carbon subsequently provides the bulk capacity, thus establishing a dual-active-center energy storage system involving both SF and CF bonds, improving the battery's total discharge capacity, average discharge voltage, and energy density. This invention offers advantages such as simple process, compatibility with existing fluorinated carbon battery manufacturing processes, and wide applicability, and can be applied to primary battery systems of lithium, sodium, potassium, magnesium, calcium, and aluminum.

[0022] Example 1: Lithium-carbon fluoride primary battery with capacity enhanced by solvent-based DAST active electrolyte A basic electrolyte was prepared by dissolving 1.0 M LiPF6 in a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio 1:1). Diethylaminosulfur trifluoride (DAST) was added to the basic electrolyte under argon protection and stirred thoroughly for 12 h to ensure uniform dissolution, with a final concentration of 1.0 M, thus obtaining the DAST active electrolyte.

[0023] Using commercial CF x (x≈1.0) is used as the positive electrode active material, according to CF x A positive electrode was prepared using Super P and PVDF in a mass ratio of 85:10:5. A lithium metal sheet was used as the negative electrode, and Celgard 2400 was used as the separator. CR2032 coin cells were assembled in a glove box, and the DAST active electrolyte prepared above was injected. After assembly, the cells were allowed to stand for 24 hours.

[0024] Comparative Example 1: Traditional lithium-carbon fluoride primary batteries Commercial fluorinated carbon was used as the positive electrode active material, in accordance with CF x The positive electrode was prepared using Super P and PVDF in a mass ratio of 85:10:5. A lithium metal sheet was used as the negative electrode, and a Celgard 2400 membrane was used as the separator. A conventional electrolyte was prepared by dissolving 1.0 M LiPF6 in a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio 1:1). CR2032 coin cells were assembled using this method.

[0025] Comparative Example 2: Tetravalent sulfide fluoride active electrolyte system alone The same electrolyte system as in Example 1 was used, namely, 1.0 M diethylaminosulfur trifluoride (DAST) was added to a 1.0 M LiPF6EC / DMC (volume ratio 1:1) base electrolyte. Porous carbon paper was used as the conductive carrier for the positive electrode, and no fluorinated carbon active material was introduced; lithium metal sheet was used as the negative electrode, and the remaining assembly conditions were the same as in Example 1.

[0026] Batteries were obtained by assembling the above-described Examples 1, 1, and 2, and then subjected to a test at 25 °C with a flow rate of 0.1 mA / cm². 2 Perform constant current discharge test (see) Figure 1 ).Depend on Figure 1 Test results show that the battery in Example 1 exhibits obvious graded discharge characteristics, initially showing a high-voltage discharge plateau in the 3.5-3.7 V range, corresponding to the electrochemical reduction reaction related to the SF bond in DAST; subsequently, it enters a fluorinated carbon-based discharge plateau at approximately 2.5 V. Comparative Example 1 uses a conventional Li / CF system. x The battery exhibits only the characteristic discharge plateau of fluorinated carbon, with a discharge voltage of approximately 2.5 V, corresponding to the electrochemical reduction reaction of the CF bonds in fluorinated carbon. Compared with Comparative Example 1, Example 1 shows an increase of approximately 35% in total discharge capacity and a significant improvement in battery energy density.

[0027] In contrast, the constant current discharge test of Example 2 showed a significant high-voltage discharge plateau in the 3.5-3.7 V range, demonstrating that DAST can participate in the discharge reaction as an independent electrochemical active material. However, due to the absence of a fluorinated carbon cathode in the system, its total discharge capacity was significantly lower than that of Example 1. This result indicates that the increased battery capacity of the present invention originates from the synergistic energy storage effect of tetravalent sulfur fluoride and fluorinated carbon, rather than the capacity contribution of tetravalent sulfur fluoride alone.

[0028] Example 2: Lithium-carbon fluoride primary battery with capacity enhanced by ionic XtalFluor-E active electrolyte A basic electrolyte was prepared by dissolving 1.0 M LiTFSI in a mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME) (volume ratio 1:1). XtalFluor-E was then added to the solution and stirred thoroughly to dissolve it, resulting in a final concentration of 1 M, thus obtaining the active electrolyte.

[0029] Using the same CF as in Example 1 x A coin cell is assembled using a positive electrode and a lithium negative electrode system, and the aforementioned active electrolyte is injected.

[0030] Example 3: Lithium-carbon fluoride primary battery with capacity-enhanced aryl-stabilized Fluolead active electrolyte 1.0 M LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) (volume ratio 1:1) to form a basic electrolyte. Fluolead was added to the electrolyte and the mixture was stirred continuously until a uniform dispersion was achieved, resulting in a final concentration of 0.5 M. CF was prepared using the same method as in Example 1. x The positive electrode is then assembled into a button cell.

[0031] The batteries assembled in Examples 1-3 above were subjected to a temperature of 25 °C and a flow rate of 0.1 mA / cm². 2 Perform constant current discharge test (see) Figure 2 In this system, all embodiments of the battery exhibit a high voltage capacity plateau in the 3.55-3.75 V range, followed by a high voltage capacity plateau with CF. x The main discharge platform is smoothly connected. Compared with Comparative Example 1, Example 1 shows an increase of approximately 35% in total discharge capacity and a significant improvement in battery energy density; compared with Comparative Example 1, Example 2 shows an increase of approximately 50% in total discharge capacity, indicating that XtalFluor-E can participate in discharge as a liquid-phase active component and contribute additional capacity; in Example 3, due to the good chemical stability of Fluolead in the electrolyte system, the battery exhibits a lower self-discharge tendency during storage, and the overall energy density is higher than that of Comparative Example 1.

[0032] Example 4: Lithium-carbon fluoride primary battery with synergistic capacity enhancement by multiple tetravalent sulfur fluorides DAST and Fluolead were added to the electrolyte as composite active components, with DAST concentration of 0.5 M and Fluolead concentration of 0.5 M. The base electrolyte consisted of 1.0 M LiPF6 dissolved in a mixed solvent of propylene carbonate (PC) and diethyl carbonate (DEC) (volume ratio 1:1). A lithium-carbon fluoride primary battery was assembled using the same method as in Example 1.

[0033] Test results show that the composite system combines the high reactivity of DAST with the high stability of Fluolead, forming a longer and more stable high-voltage discharge plateau in the 3.5-3.8 V range. Subsequently, the fluorinated carbon continues to release its bulk capacity. Compared with the single active component system, the composite system has a higher total discharge capacity and energy density, indicating a synergistic energy storage effect among different tetravalent sulfur fluorides.

[0034] Example 5: Low-concentration DAST active electrolyte system Using the same basic electrolyte system as in Example 1, only the DAST concentration was adjusted to 0.05 M to prepare a low-concentration DAST active electrolyte. A lithium-carbon fluoride primary battery was assembled using the same method as in Example 1.

[0035] The discharge curves show that a high-voltage discharge plateau can still be observed near 3.5 V, but the capacity contribution is relatively small. Compared with Comparative Example 1, the total energy density is increased by about 3%-5%, indicating that even under low concentration conditions, tetravalent sulfur fluorides can still participate in the discharge reaction and play a capacity-enhancing role.

[0036] Example 6: High-concentration DAST active electrolyte system A mixed solvent of acetonitrile (AN) and sulfolane (SL) (volume ratio 1:1) was used as the base system. 1.0 M LiTFSI was added, followed by the addition of DAST for dissolution, bringing the final DAST concentration to 5 M, resulting in a high-concentration active electrolyte. The same CF444 solution as in Example 1 was used. x The positive electrode and lithium negative electrode are used to assemble the battery.

[0037] Discharge test results show a relatively long high-voltage discharge plateau in the 3.5-3.7 V range, indicating that liquid-phase DAST can provide a significant additional capacity contribution. After the high-voltage plateau ends, CF x The main discharge reaction continued. Compared with Comparative Example 1, the total discharge capacity increased by more than 60%, verifying the effectiveness of high-concentration active electrolyte in improving battery energy density.

[0038] Example 7: Verification of the universality of solvent-based DAST active electrolyte for capacity enhancement in sodium-fluorinated carbon primary battery systems A Na / CF4 assembly was performed using commercially available fluorinated carbon cathode sheets as the positive electrode, sodium metal foil as the negative electrode, and ceramic-coated polyolefin as the separator. x Primary battery. 1.0 M NaPF6 was dissolved in a mixed solvent of propylene carbonate (PC) and diethyl carbonate (DEC) (volume ratio 1:1) to form a basic electrolyte. Diethylaminosulfur trifluoride (DAST) was added to the electrolyte under argon protection to bring the final concentration to 1.0 M, thus obtaining a sodium battery electrolyte containing a liquid-phase active fluorine source.

[0039] Using the electrolytes obtained above, Na / CF were assembled separately. x A primary battery was used, and constant current discharge tests were conducted at room temperature. The results show that the system exhibits obvious graded discharge characteristics. Figure 3 In the initial stage of discharge, the voltage is approximately 3.2-3.5 V (vs. Na / Na). + The voltage plateau first appears in the 2.2 V range, corresponding to the electrochemical reduction reactions related to the high-valence sulfur centers and SF bonds in the DAST. Subsequently, the voltage transitions to the approximately 2.2 V range, where the CF bond reduction reaction continues at the fluorinated carbon cathode, providing the bulk capacity. These results demonstrate that the liquid-phase active fluorine source capacity enhancement strategy proposed in this invention is applicable not only to lithium systems but also to sodium metal primary battery systems, exhibiting good system versatility.

[0040] Example 8: Verification of the universality of solvent-based DAST active electrolyte for capacity enhancement in magnesium-carbon fluoride primary battery systems A commercially available fluorinated carbon positive electrode was used as the positive electrode, a magnesium metal sheet as the negative electrode, and glass fiber as the separator. The basic electrolyte consisted of 0.5 M Mg(TFSI)₂ dissolved in a mixed solvent of 1,2-dimethoxyethane (DME) and tetraethylene glycol dimethyl ether (TEGDME) (volume ratio 1:1). Under an inert atmosphere, the DAST active component was added to the basic electrolyte to achieve a final concentration of 0.5 M, resulting in an active electrolyte suitable for magnesium systems.

[0041] The Mg / CF electrolytes obtained above were used to assemble the following solutions. x A primary battery was tested and subjected to a constant current discharge test. The results showed that ( Figure 3 ), approximately 2.5 V in the initial stage of discharge (vs. Mg / Mg). 2+ The battery initially exhibits a high voltage capacity plateau contributed by DAST in the range of approximately 1.5 V, followed by a sustained discharge phase where the bulk capacity is provided by the fluorinated carbon cathode. Due to the multi-electron transfer characteristics of the electrochemical reactions involving magnesium ions, the battery demonstrates a high energy output capacity per unit volume.

[0042] The above results demonstrate that the tetravalent sulfur fluoride described in this invention contains a high-valence sulfur center and a sulfur-fluorine (SF) bond, enabling it to participate in the battery discharge reaction as a liquid-phase active material. By directly introducing the tetravalent sulfur fluoride into the electrolyte, synergistic discharge of the liquid-phase active component and the solid-phase fluorinated carbon cathode is achieved without altering the composition and preparation process of the fluorinated carbon cathode material. Specifically, the tetravalent sulfur fluoride contributes capacity in the higher voltage range, while the fluorinated carbon subsequently provides the bulk capacity, thus establishing a dual-active-center energy storage system involving both SF and CF bonds, thereby improving the total battery discharge capacity, average discharge voltage, and energy density. This invention offers advantages such as simple process, compatibility with existing fluorinated carbon battery manufacturing processes, and wide applicability. It is evident that the method proposed in this invention for constructing a liquid-phase active fluorine source by introducing soluble tetravalent sulfur fluoride into the electrolyte is applicable not only to monovalent lithium and sodium systems but also to multivalent metal systems, proving the good universality and scalability of this capacity enhancement strategy.

[0043] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An electrolyte for a capacity-enhancing fluorinated carbon battery, characterized in that: The electrolyte contains a tetravalent sulfur fluoride as an active substance; wherein the concentration of the tetravalent sulfur fluoride in the electrolyte is 0.01-5 M, and the tetravalent sulfur fluoride contains at least one high-valence sulfur center and at least one SF bond.

2. The electrolyte of the capacity-enhanced fluorinated carbon battery according to claim 1, characterized in that: The tetravalent sulfur fluoride is selected from one or more of diethylamino sulfur trifluoride (DAST), sulfur trifluoride morpholine (Morpho-DAST), [bis(2-methoxyethyl)amine] sulfur trifluoride (Deoxo-Fluor), morpholine difluorosulfonium tetrafluoroborate (XtalFluor-M), (diethylamino) difluoride sulfur tetrafluoroborate (XtalFluor-E), and 4-tert-butyl-2,6-dimethylphenyl sulfur trifluoride (Fluolead).

3. The electrolyte of the capacity-enhanced fluorinated carbon battery according to claim 1 or 2, characterized in that: The electrolyte is an organic solvent, an electrolyte salt, and a tetravalent sulfur fluoride; wherein the organic solvent is selected from one or more of carbonate solvents, ether solvents, nitrile solvents, sulfone solvents, and fluorocarbonate solvents.

4. The electrolyte of the capacity-enhanced fluorinated carbon battery according to claim 3, characterized in that: The electrolyte salt is selected from one or more of LiPF6, LiBF4, LiFSI, LiTFSI, LiClO4, NaPF6, NaFSI, NaTFSI, and Mg(TFSI)2.

5. The application of the electrolyte in the capacity-enhancing fluorinated carbon battery according to claim 1, characterized in that: The electrolyte is used in fluorinated carbon primary batteries to increase capacity.

6. A primary fluorinated carbon battery, comprising a positive electrode, a negative electrode, a separator, and an electrolyte, characterized in that, The electrolyte is the electrolyte as described in claim 1.

7. The fluorinated carbon primary battery according to claim 6, characterized in that, The negative electrode is selected from one or more of lithium, sodium, potassium, magnesium, calcium, aluminum, and alloys of the aforementioned metals.

8. A method for preparing the battery according to claim 6, characterized in that: (1) Preparation of a positive electrode containing fluorinated carbon active material; (2) Prepare the electrolyte containing tetravalent sulfur fluoride as described in claim 1; (3) Assemble the positive electrode, separator and negative electrode to form a battery; (4) Inject the electrolyte into the battery and complete the encapsulation.

9. The method for preparing the battery according to claim 8, characterized in that: In step (2), the tetravalent sulfur fluoride is added to the solution of organic solvent and electrolyte salt and mixed well, and then directly injected into the battery.