Non-aqueous secondary batteries
By using an electrolyte consisting of LiFSI, SN, and a specific solvent combination in non-aqueous secondary batteries, the problem of metal leaching was solved, resulting in improved battery performance and durability.
Patent Information
- Application Number
- CN202610337488.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-03-19
- Publication Date
- 2026-11-10
AI Technical Summary
In existing non-aqueous secondary batteries, the leaching of metals from the current collector foil and active materials leads to a decrease in battery performance and durability, especially when using LiFSI and lithium manganese iron phosphate (LMFP), where the leaching of Mn and Fe is particularly significant.
A non-aqueous electrolyte containing lithium bis(fluorosulfonyl)imide (LiFSI) as the lithium salt, succinate (SN) as the additive, and cyclic carbonate and ester compounds as solvents is used to suppress metal leaching by combining appropriate lithium salt concentration and additive ratio.
It effectively inhibits the leaching of metal from the current collector foil and active material, improves the lithium-ion diffusion and metal corrosion inhibition capabilities of the battery, and maintains the battery's high performance and durability.
Smart Images

Figure CN123073124A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to non-aqueous secondary batteries. Background Technology
[0002] Various technologies have been proposed for non-aqueous secondary batteries using non-aqueous electrolytes, as disclosed in International Patent Publication No. 2023 / 219102 and Japanese Patent Publication No. 2016-536776. Summary of the Invention
[0003] To obtain non-aqueous secondary batteries with high battery performance, various non-aqueous electrolytes have been proposed. These non-aqueous electrolytes include, for example, electrolytes containing lithium salts and non-aqueous solvents.
[0004] Lithium bis(fluorosulfonyl)imide (LiFSI) is known to have excellent lithium diffusion properties as a lithium salt constituting a non-aqueous electrolyte, but it corrodes the Al foil used as a current collector.
[0005] In the non-aqueous secondary battery described in International Publication No. 2023 / 219102, a non-aqueous electrolyte composed of a mixture of cyclic carbonate compounds and ester compounds is used. However, if the ester compounds decompose, acid is generated, which may promote the dissolution of Al from the current collector foil. In addition, if lithium manganese iron phosphate (LMFP) is used as the positive electrode active material, Mn and Fe may dissolve.
[0006] The leaching of metals from the current collector foil and active materials is the cause of reduced battery performance and durability.
[0007] This invention provides a non-aqueous secondary battery capable of suppressing the leaching of metal from the current collector foil and active material.
[0008] That is, the present invention includes the following methods.
[0009] A non-aqueous secondary battery comprises a positive electrode foil, a positive electrode layer containing a positive electrode active material, an electrolyte layer containing a separator and a non-aqueous electrolyte, a negative electrode layer, and a negative electrode foil. In the non-aqueous secondary battery, the positive electrode active material is lithium manganese iron phosphate (LMFP), and the weight per unit area of the positive electrode layer is 20 mg / cm³. 2 The above-mentioned non-aqueous electrolyte contains lithium bis(fluorosulfonyl)imide (LiFSI) as a lithium salt, a dinitrile compound as an additive, and a cyclic carbonate compound and an ester compound as a solvent. The concentration of the lithium salt in the above-mentioned non-aqueous electrolyte is 1.4 M or more, and the dinitrile compound is succinic anionyl (SN).
[0010] In the non-aqueous secondary battery of the above-described manner, the volume ratio of the cyclic carbonate compound to the ester compound is 0.17 or more, the cyclic carbonate compound is at least one of ethylene carbonate (EC) and propylene carbonate (PC), and the ester compound is at least one selected from the group consisting of methyl acetate (MA), methyl propionate (MP), ethyl acetate (EA), vinyl propionate (EP), and propyl propionate (PP).
[0011] In the non-aqueous secondary battery described above, the non-aqueous electrolyte further includes vinylene carbonate (VC) as an additive, with 1.0% by mass or more of the vinylene carbonate as an additive, and 1.0% by mass or more of the dinitrile compound as an additive.
[0012] In the non-aqueous secondary battery described above, the non-aqueous electrolyte further includes LiX as the lithium salt, wherein the LiX is at least one of LiPF6 and LiBF4.
[0013] In the non-aqueous secondary battery described above, the concentration ratio (LiFSI / LiX) of the LiFSI contained in the non-aqueous electrolyte is 2.5 or higher.
[0014] According to the present invention, a non-aqueous secondary battery capable of suppressing the leaching of metal from the current collector foil and active material can be provided. Attached Figure Description
[0015] The features, advantages, and technical and industrial significance of exemplary embodiments of the present invention will be described below with reference to the accompanying drawings, in which the same reference numerals denote the same elements. Figure 1 This is a graph showing the aging loss voltage of the embodiments and comparative examples.
[0016] Figure 2 This is a diagram showing the initial capacity of the embodiments and comparative examples.
[0017] Figure 3 This is a graph showing the relationship between elapsed time and convergence current in the float charge test of the embodiments and comparative examples.
[0018] Figure 4 This is a graph showing the cumulative convergence current values of the embodiments and comparative examples.
[0019] Figure 5 This is a graph showing the Al dissolution amounts of the examples and comparative examples.
[0020] Figure 6 This is a graph showing the amount of Fe leaching in the examples and comparative examples.
[0021] Figure 7 This is a graph showing the amount of Mn leached in the examples and comparative examples. Detailed Implementation
[0022] The embodiments of the present invention will be described below. It should be noted that matters necessary for the implementation of the present invention, other than those specifically mentioned in this specification (e.g., the general structure and manufacturing process of non-aqueous secondary batteries not characteristic of the present invention), can be understood by those skilled in the art based on prior art. The present invention can be implemented based on the disclosures in this specification and common technical knowledge in the field.
[0023] In this invention, unless otherwise specified, the average particle size is the particle size at which the cumulative value of the particle size distribution of the volume reference, measured by laser diffraction / scattering particle size distribution determination, is 50%, i.e., the median particle size (D50).
[0024] This invention provides a non-aqueous secondary battery comprising a positive electrode current collector foil, a positive electrode layer containing a positive electrode active material, an electrolyte layer containing a separator and a non-aqueous electrolyte, a negative electrode layer, and a negative electrode current collector foil. The positive electrode active material is lithium manganese iron phosphate (LMFP), and the weight per unit area of the positive electrode layer is 20 mg / cm³. 2 The above-mentioned non-aqueous electrolyte contains lithium bis(fluorosulfonyl)imide (LiFSI) as a lithium salt, a dinitrile compound as an additive, and a cyclic carbonate compound and an ester compound as a solvent. The concentration of the lithium salt in the above-mentioned non-aqueous electrolyte is 1.4 M or more, and the dinitrile compound is succinic anionyl (SN).
[0025] In the non-aqueous secondary battery of the present invention, by using a non-aqueous electrolyte composed of LiFSI as a lithium salt, the aforementioned specific dinitrile compound as an additive, and cyclic carbonate and ester compounds as solvents, the dissolution of metal from the current collector foil and the active material is successfully suppressed. Although the non-aqueous secondary battery of the present invention uses LiFSI, which is known to dissolve Al foil as a current collector, it is able to suppress metal dissolution, exhibiting excellent characteristics that balance high lithium-ion diffusion and suppression of metal corrosion.
[0026] The electrolyte layer, positive electrode current collector foil, positive electrode layer, negative electrode current collector foil, and negative electrode layer constituting the non-aqueous secondary battery of the present invention will be described in sequence below. It should be noted that the non-aqueous secondary battery of the present invention has a structure in which a positive electrode having a positive electrode having a positive electrode current collector foil and a positive electrode layer, an electrolyte layer, and a negative electrode having a negative electrode layer and a negative electrode current collector foil are sequentially stacked, with the electrolyte layer disposed between the positive electrode layer and the negative electrode layer.
[0027] 1. Electrolyte layer
[0028] The electrolyte layer is a layer that includes a membrane and a non-aqueous electrolyte.
[0029] The separator is impregnated with a non-aqueous electrolyte and prevents contact between the positive and negative electrode layers. There are no particular limitations on the separator material, as long as it is a porous membrane; examples include resins such as polyethylene (PE), polypropylene (PP), polyester, polyvinyl alcohol, cellulose, and polyamide. Furthermore, the separator can be a single-layer or multi-layer structure. Examples of multi-layer separators include two-layer PE / PP structures, or three-layer PP / PE / PP or PE / PP / PE structures.
[0030] The diaphragm can be made of nonwoven fabrics such as resin nonwoven fabric and glass fiber nonwoven fabric.
[0031] In the non-aqueous secondary battery of the present invention, the non-aqueous electrolyte comprises LiFSI as a lithium salt, a specific dinitrile compound as an additive, and a cyclic carbonate compound and an ester compound as a solvent.
[0032] The non-aqueous electrolyte contains LiFSI (chemical formula LiN(SO2F)2) as an essential component of the lithium salt. The non-aqueous electrolyte may contain only LiFSI as an imide salt, or it may contain other lithium salts besides LiFSI. Examples of other lithium salts include lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium bis(pentafluoroethanesulfonyl)imide (LiBETI). Furthermore, examples include organic lithium salts such as LiCF3SO3 and LiC(SO2CF3)3. In addition, inorganic lithium salts (LiX) such as LiPF6, LiBF4, LiClO4, and LiAsF6 can also be used as lithium salts. Other lithium salts may be at least one LiX selected from LiPF6 and LiBF4. In non-aqueous secondary batteries containing LMFP as the positive electrode active material, LiPF6 sometimes promotes the dissolution of Mn and Fe from LMFP, but in the non-aqueous secondary battery of the present invention, the dissolution of Mn and Fe is suppressed even when using LiPF6. Other lithium salts can be used alone or in combination of two or more.
[0033] Non-aqueous electrolytes may contain LiFSI as the main lithium salt. Here, "containing LiFSI as the main lithium salt" means that the concentration of LiFSI in the non-aqueous electrolyte is greater than the combined concentration of other lithium salts in the non-aqueous electrolyte. For example, when LiFSI is used in combination with at least one of LiX, LiPF6 and LiBF4, as the lithium salt, the concentration ratio of LiFSI to LiX in the non-aqueous electrolyte (LiFSI / LiX) may be 2.5 or more. Furthermore, the concentration ratio of LiFSI to LiX in the non-aqueous electrolyte (LiFSI / LiX) may be 100.0 or less, or 10.0 or less.
[0034] The concentration of lithium salt in the non-aqueous electrolyte can be 1.4 M or higher, 2.0 M or higher, 6.0 M or lower, or 4.0 M or lower. A non-aqueous electrolyte with excellent ionic conductivity can be obtained by using a lithium salt concentration of 1.4 M or higher. If the lithium salt concentration increases, the viscosity of the non-aqueous electrolyte increases, and the ionic conductivity may decrease. However, in the non-aqueous secondary battery of the present invention, by combining cyclic carbonate compounds and ester compounds as solvents, the decrease in ionic conductivity can be suppressed.
[0035] The non-aqueous electrolyte of this invention contains succinate (SN), a dinitrile compound. It is believed that by including succinate in the non-aqueous electrolyte, metal leaching from the current collector foil and the positive electrode active material can be suppressed. This is presumably due to the metal chelating effect of succinate. Besides succinate, other dinitrile compounds such as adiponitrile (AdN) can also be used, but considering battery performance beyond metal leaching suppression, succinate is used as an essential dinitrile compound in the non-aqueous secondary battery of this invention.
[0036] There is no particular limitation on the content of succinic anion as a dinitrile compound. When the total mass of the non-aqueous electrolyte is set to 100%, the non-aqueous electrolyte may contain more than 1.0% by mass of succinic anion, less than 5.0% by mass, or less than 2.0% by mass.
[0037] The non-aqueous electrolyte contains a cyclic carbonate compound and an ester compound as solvents. The cyclic carbonate can be, for example, at least one of ethylene carbonate (EC) and propylene carbonate (PC), or ethylene carbonate (EC). The ester compound can be at least one selected from the group consisting of methyl acetate (MA), methyl propionate (MP), ethyl acetate (EA), vinyl propionate (EP), and propyl propionate (PP). Methyl propionate (MP) can also be used as the ester compound.
[0038] The mixing ratio of the cyclic carbonate compound to the ester compound is not particularly limited. For example, the volume ratio of the cyclic carbonate compound to the ester compound (cyclic carbonate compound / ester compound) can be 0.17 or more. Furthermore, the aforementioned volume ratio can be 9.00 or less, 6.00 or less, or 1.00 or less. It is believed that when the volume ratio of the cyclic carbonate compound to the ester compound is 0.17 or more, the metal dissolution inhibition effect brought about by succinate, as a dinitrile compound, is improved.
[0039] Non-aqueous electrolytes can also further include vinylene carbonate (VC) as an additive. This is because the presence of vinylene carbonate promotes the formation of a film called SEI (Solid Electrolyte Interface) on the surface of the negative electrode. SEI protects the negative electrode and inhibits solvent decomposition, thus stabilizing battery performance.
[0040] There is no particular limitation on the content of vinylene carbonate in non-aqueous electrolytes. When the total mass of the non-aqueous electrolyte is set to 100%, it can be above 1.0% by mass, below 5.0% by mass, or below 2.0% by mass.
[0041] Non-aqueous electrolytes can contain ionic liquids. Ionic liquids can include, for example, sulfonium salts, ammonium salts, and pyridine. Salt, piperidine Salt, pyrrolidine Salt, Morpholine Salt, Salt, imidazole At least one of the group consisting of salts and their derivatives.
[0042] 2. Positive electrode
[0043] The positive electrode has a positive current collector foil and a positive electrode layer containing positive active material.
[0044] Materials used for the positive electrode current collector foil include, for example, SUS, Cr, Au, Pt, Zn, aluminum, copper, nickel, iron, titanium, and carbon. The thickness of the positive electrode current collector foil is, for example, 0.1 μm or more and 100 μm or less. The top-view shape of the positive electrode current collector foil is not particularly limited; for example, it can be circular, elliptical, rectangular, or any polygonal shape. The positive electrode current collector foil can also be composed of a buffer layer, an elastic layer, or a PTC (Positive Temperature Coefficient) thermistor layer disposed on its surface.
[0045] The positive electrode layer contains lithium manganese iron phosphate (LMFP) as the positive electrode active material. LMFP is usually in particulate form, with an average particle size of, for example, greater than 1 μm or less than 30 μm.
[0046] The positive electrode active material contained in the positive electrode layer can be LMFP alone, or it can be a combination of LMFP and other positive electrode active materials other than LMFP. However, from the point of view of durability, it can be LMFP alone.
[0047] Other known positive electrode active materials can be used as positive electrode active materials for lithium secondary batteries. Examples include lithium metal composite oxides such as LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, and Li(NiCoAl)O2. Here, "(NiCoMn)" in "Li(NiCoMn)O2" and "(NiCoAl)" in "Li(NiCoAl)O2" indicate that the sum of the composition ratios within the parentheses is 1. As long as the sum is 1, the composition ratio of each element is arbitrary. For example, Li(NiCoMn)O2 can be Li(Ni... 1 / 3 Co 1 / 3 Mn 1 / 3 O2, Li(Ni) 0.5 Co 0.2 Mn 0.3 O2, Li(Ni) 0.8 Co 0.1 Mn 0.1 Li(NiCoAl)O2, for example, can be Li(Ni)O2, etc. 0.81 Co 0.15 Al 0.04 O2, etc.
[0048] When the total mass of the positive electrode layer is set to 100%, the proportion of positive electrode active material in the positive electrode layer can be, for example, 20% or more by mass, 30% or more by mass, or 40% or more by mass, or on the other hand, 95% or less by mass, or 70% or less by mass.
[0049] The positive electrode layer may contain at least one of conductive material, binder, dispersant and electrolyte as needed.
[0050] Examples of conductive materials include carbon-based conductive materials, metal particles, and conductive polymers. Examples of carbon-based conductive materials include particulate materials such as acetylene black (AB) and Ketjen black (KB), and fibrous materials such as vapor-phase carbon fiber (VGCF), carbon nanotubes (CNTs), and carbon nanofibers (CNFs).
[0051] When the overall mass of the positive electrode layer is set to 100%, the proportion of conductive material in the positive electrode layer can be, for example, more than 0.1% by mass or less than 5% by mass.
[0052] Examples of adhesives include styrene-butadiene rubber (SBR), polyimide (PI), polyacrylic acid (PAA), acrylonitrile-butadiene rubber (NBR), butadiene rubber (BR), polyvinylidene fluoride (PVdF), carboxymethyl cellulose (CMC), polytetrafluoroethylene (PTFE), styrene-isoprene-styrene block copolymer (SIS), and ethylene-propylene-diene copolymer (EPDM).
[0053] When the overall mass of the positive electrode layer is set to 100%, the proportion of binder in the positive electrode layer can be, for example, more than 0.5% by mass or less than 15% by mass.
[0054] There are no particular limitations on the dispersant used; any known dispersant can be used. When the total mass of the positive electrode layer is set to 100%, the proportion of the dispersant in the positive electrode layer can be, for example, 0.1% by mass or more, or 1% by mass or less.
[0055] The electrolyte can be, for example, an inorganic solid electrolyte such as a sulfide solid electrolyte, a halide solid electrolyte, an oxide solid electrolyte, or a complex hydride solid electrolyte, or an organic solid electrolyte such as a gel electrolyte. The proportion of solid electrolyte in the positive electrode layer can be, for example, 0 to 1% by mass.
[0056] The thickness of the positive electrode layer can be, for example, 0.1 μm or more and 1000 μm or less, 1 μm or more and 500 μm or less, or 30 μm or more and 100 μm or less.
[0057] The positive electrode layer can be disposed on one side of the positive electrode current collector foil or on both sides of the positive electrode current collector foil.
[0058] There are no particular limitations on the manufacturing method of the positive electrode layer. For example, LMFP, a conductive material, a binder, a dispersant, and a solvent can be mixed to prepare a positive electrode slurry. This positive electrode slurry can then be coated onto a positive electrode current collector foil and dried to form a positive electrode layer on the foil. A pressing process can be performed to press the positive electrode layer along its thickness direction. Examples of pressing processes include roll pressing and flat pressing. Examples of solvents for the positive electrode slurry include N-methylpyrrolidone (NMP), tetrahydronaphthalene, diisobutyl ketone, butyl butyrate, mesitylene, heptane, dibutyl ether, decane, dodecane, isodecane, and toluene. Furthermore, two or more of these components may be included.
[0059] The positive electrode layer of the non-aqueous secondary battery of the present invention has a unit area weight of 20 mg / cm².2 The above describes a positive electrode layer with a high weight per unit area. When such a positive electrode layer has a high weight per unit area, side reactions other than the discharge and charging reactions are more likely to occur, leading to material degradation and potentially reducing battery performance. However, in the non-aqueous secondary battery of this invention, side reactions accompanying metal dissolution can be suppressed, thus stabilizing battery performance.
[0060] The surface area weight of the positive electrode layer is 20 mg / cm². 2 That's sufficient; for example, it could be 100 mg / cm³. 2 The following can also be 50 mg / cm³ 2 the following.
[0061] 3. Negative electrode
[0062] The negative electrode has a negative electrode current collector foil and a negative electrode layer containing negative electrode active material.
[0063] Materials used for the negative electrode current collector foil include, for example, SUS, aluminum, copper, nickel, iron, titanium, and carbon. Furthermore, the thickness of the negative electrode current collector foil can range from, for example, 1 μm to 50 μm. The top-view shape of the negative electrode current collector foil is not particularly limited; for example, it can be circular, elliptical, rectangular, or any polygonal shape. The negative electrode current collector foil can be composed of a buffer layer, an elastic layer, or a PTC thermistor layer disposed on its surface.
[0064] The negative electrode layer is a layer containing at least a negative electrode active material. Additionally, the negative electrode layer may contain at least one of a conductive material, a binder, and an electrolyte, depending on requirements.
[0065] The negative electrode active material can be in particle or sheet form. The average particle size of the negative electrode active material can be, for example, 1 μm or more. Alternatively, the average particle size of the negative electrode active material can be, for example, 30 μm or less.
[0066] The negative electrode active material may include at least one selected from the group consisting of carbon-based active materials, Li-based active materials, Si-based active materials, Si-C composite materials, and lithium titanate. The carbon-based active material may include at least one selected from the group consisting of graphite, soft carbon, and hard carbon. "Graphite" is a general term for both natural and artificial graphite. Examples of Li-based active materials include Li, Li silicate, and Li alloys. Examples of Si-based active materials include Si, SiO, and Si alloys. Si-C composite materials refer to composite materials of carbon-based active materials (such as graphite) and Si-based active materials (such as Si).
[0067] Regarding the conductive materials, binders, and electrolytes used in the negative electrode layer, examples can be made of the same substances described in "2. Positive Electrode" above. Additionally, the negative electrode layer may contain a dispersant.
[0068] The negative electrode layer can be disposed on one side or both sides of the negative electrode current collector foil. There is no particular limitation on the manufacturing method of the negative electrode layer. For example, a negative electrode active material, a conductive material, a binder and water (solvent) can be mixed to prepare a negative electrode slurry, which is then coated onto the negative electrode current collector foil and dried to form a negative electrode layer on the negative electrode current collector foil.
[0069] There is no particular limitation on the weight per unit area of the negative electrode layer; for example, it can be 8.0 mg / cm³. 2 The above can be 8.9 mg / cm³ 2 The above can be 100.0 mg / cm³ 2 The following can be 50.0 mg / cm³ 2 the following.
[0070] 4. Non-aqueous secondary batteries
[0071] The type of non-aqueous secondary battery used in this invention is not particularly limited, but is typically a lithium-ion battery. The shape of the battery is not particularly limited; for example, it can be coin-shaped, cylindrical, square, sheet-shaped, button-shaped, flat, or stacked. In the case of a battery stack containing two or more batteries, the battery stack can be unipolar or bipolar.
[0072] Batteries are used in various applications, including as power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), battery electric vehicles (BEVs), gasoline vehicles, and diesel vehicles. Specifically, they can be used as power sources for driving hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), or battery electric vehicles (BEVs). Furthermore, batteries can be used as power sources for mobile bodies other than vehicles (such as rail vehicles, ships, and aircraft), and also as power sources for electrical products such as information processing devices.
[0073] Example 1
[0074] Preparation of non-aqueous electrolytes
[0075] Prepare the components of the non-aqueous electrolyte shown in Table 1. Specifically, prepare LiFSI (imide salt) as a lithium salt. Weigh the LiFSI according to the condition that the LiFSI concentration in the non-aqueous electrolyte is 1.4M.
[0076] Additionally, EC (cyclic carbonate compound) and MP (ester compound) are prepared as solvents. EC and MP are weighed separately such that EC becomes 15% and MP becomes 85% when the total volume of EC and MP is set to 100%. At this point, the volume ratio (A / B) of the cyclic carbonate compound (here, A) to the ester compound (here, B) is 0.176.
[0077] In addition, SN (dianitronidazole compound) and VC are prepared as additives. SN and VC are weighed to a weight of 1.0% by mass when the total mass of the non-aqueous electrolyte is set to 100%.
[0078] Mix the above components to prepare a non-aqueous electrolyte.
[0079] (Table 1)
[0080] Fabrication of battery cells (non-aqueous secondary batteries)
[0081] Prepare LMFP (positive electrode active material), CNT (conductive material), PVdF (binder), and dispersant. Disperse them in NMP at a mass ratio of LMFP:CNT:PVdF:dispersant = 94.32%:1.40%:4.00%:0.28% to prepare a positive electrode slurry. The positive electrode slurry is prepared at a weight per unit area of 20 mg / cm³. 2 The coating is applied to Al foil (positive electrode current collector foil) and dried to create a positive electrode with a positive electrode layer formed on the positive electrode current collector foil.
[0082] On the other hand, artificial graphite (negative electrode active material), CNT (conductive material), CMC (binder), and SBR (binder) were prepared and dispersed in water in a mass ratio of artificial graphite:CNT:CMC:SBR = 97.170%:0.125%:0.405%:2.300% to prepare a negative electrode slurry. The negative electrode slurry was prepared with a unit area weight of 8.9 mg / cm³. 2 The coating is applied to Cu foil (negative electrode current collector foil) and dried to create a negative electrode with a negative electrode layer formed on the negative electrode current collector foil.
[0083] Next, Al tabs are ultrasonically welded to the positive electrode, and Ni tabs are ultrasonically welded to the negative electrode. Then, a laminate with a separator sandwiched between the positive and negative electrodes is fabricated. The laminate is then packaged in a laminated outer casing and dried at 80°C.
[0084] The non-aqueous electrolyte prepared above is injected into the laminated outer casing in a glove box. Then, the laminated outer casing is sealed with a heat sealer to produce a battery cell (non-aqueous secondary battery).
[0085] Comparative Example 1
[0086] As shown in Table 1, the battery cells were fabricated using a non-aqueous electrolyte prepared in the same manner as in Example 1, without the use of SN (dianitronic compounds).
[0087] Comparative Example 2
[0088] As shown in Table 1, a non-aqueous electrolyte was prepared using LiFSI (imide salt) and LiPF6 as lithium salts, and SN (dianitronidium compound) was not used. Otherwise, the battery cell was fabricated in the same manner as in Example 1. It should be noted that the non-aqueous electrolyte was prepared with a LiFSI concentration of 1.0 M and a LiPF6 concentration of 0.4 M. At this point, the LiFSI / LiX concentration ratio was 2.5.
[0089] Evaluation of battery cells
[0090] The battery cells of Example 1 and Comparative Examples 1-2 fabricated above were evaluated as follows. The results are shown in Table 2.
[0091] Initial adjustment
[0092] As an initial adjustment, the following process is performed: First, the battery cell is CC-charged to 4.3V at 0.05C at 25°C. Then, the battery cell is left to stand at 60°C for 20 hours. Next, the battery cell is CC-charged to 4.3V at 0.1C at 25°C, and CC-discharged to 2.5V at 0.2C.
[0093] Evaluation of aging loss voltage
[0094] Before and after the initial settling treatment (60°C, 20 hours) described above, the voltage was measured, and the voltage difference before and after the settling treatment was calculated using the following formula.
[0095] (Aging loss voltage) = (Voltage before static treatment) - (Voltage after static treatment)
[0096] Figure 1 This is a graph showing the aging loss voltage of the embodiments and comparative examples.
[0097] Evaluation of initial discharge capacity
[0098] For the battery cells that underwent initial adjustments, the discharge capacity was measured as follows: The cells were charged at 0.1C at 25°C to 4.3V using a CCCV method, then discharged at 0.1C to 2.5V using a CC method, and the discharge capacity was measured. The initial capacities of Examples 1 and 2 were normalized to 100% of the initial capacity of Comparative Example 1. Figure 2 This is a diagram showing the initial capacity of the embodiments and comparative examples.
[0099] float test
[0100] For the battery cells that have undergone initial adjustments, a float charge test was conducted at 60°C for one week, maintaining a voltage of 4.3V through CV charging using an external power source. During the float charge test, the current value of the battery cells was measured.
[0101] Figure 3 This is a graph showing the relationship between elapsed time and convergence current (mA) in the float charge test of the embodiments and comparative examples. It should be noted that... Figure 3 The results are shown from the start of the float charge test to 600,000 seconds later.
[0102] In addition, the convergence current values measured during the float charge test are accumulated. Figure 4 This is a graph showing the cumulative convergence current (mA) of the embodiments and comparative examples.
[0103] Evaluation of metal leaching
[0104] For battery cells that underwent float charging tests, the leaching of metals (Al, Fe, and Mn) was determined as follows: The battery cell was disassembled after the float charging test. First, only the negative electrode layer was removed and weighed. Next, the removed negative electrode layer was heated together with hydrochloric acid and nitric acid. After heating, the metal concentration of the filtrate was analyzed by ICP. Figure 5 This is a graph showing the Al dissolution amounts of the examples and comparative examples. Figure 6 This is a graph showing the amount of Fe leaching in the examples and comparative examples. Figure 7 This is a graph showing the amount of Mn leached in the examples and comparative examples.
[0105] (Table 2)
[0106] As shown in Table 2 and Figure 1 As shown, compared to Comparative Examples 1 and 2, the battery cell (non-aqueous secondary battery) of Example 1 exhibits a lower aging loss voltage. In particular, when comparing the battery cell of Example 1, which differs only in the presence or absence of succinic anionizer, with that of Comparative Example 1, the aging loss voltage of Example 1 is approximately one-quarter that of Comparative Example 1. It is believed that the lower aging loss voltage of the battery cell of Example 1 is due to the absence of side reactions in the battery cell of Example 1 during the initial settling treatment.
[0107] On the other hand, as shown in Table 2 and Figure 2 As shown, Example 1 and Comparative Examples 1 and 2 exhibit the same initial capacity.
[0108] Additionally, as shown in Table 2 and Figure 4 As shown, compared to Comparative Examples 1 and 2, the cumulative convergence current of the battery cell in Example 1 is significantly smaller. In the comparison between Comparative Example 1 and Example 1, the cumulative convergence current of Example 1 is half that of Comparative Example 1. This means that the battery cell in Example 1 experiences less discharge due to side reactions during the float charge test compared to the battery cells in Comparative Examples 1 and 2. In other words, it can be said that even under harsh conditions such as 60°C, the battery cell in Example 1 is less prone to side reactions.
[0109] Additionally, as shown in Table 2 and Figures 5-7 As shown, the amount of metal leaching from the battery cell of Example 1 is less than that of the battery cells of Comparative Examples 1 and 2 in any of the Al, Fe, and Mn elements. In particular, the comparison with Comparative Example 1 shows that the Al leaching suppression effect of Example 1 is particularly high. It is assumed that Al originates from the positive electrode current collector foil, and Fe and Mn originate from the positive electrode active material; the Al, Fe, and Mn dissolved in the positive electrode are deposited in the negative electrode layer, respectively. Figures 5-7 Evaluation of metal leaching amount and Figure 1 Aging loss voltage and Figure 4 The results of the cumulative convergence current were also studied. It can be said that the battery cell of Example 1 can suppress side reactions, especially the dissolution of metals from the current collector foil and active material, even in a harsh environment such as 60°C.
[0110] It should be noted that, as Figure 6 and Figure 7 As shown, the battery cell of Comparative Example 2 exhibits significantly higher levels of Fe and Mn dissolution compared to the battery cells of Comparative Example 1 and Example 1. This is believed to be because, in the battery cell of Comparative Example 2, both LiFSI and LiPF6 were used as lithium salts. Figure 3 In the time variation of the convergence current shown, Comparative Example 2 also exhibited behavior different from that of Example 1 and Comparative Example 1, suggesting that a side reaction accompanied by the dissolution of Mn and Fe occurred compared to Example 1 and Comparative Example 1.
Claims
1. A non-aqueous secondary battery, comprising a positive electrode current collector foil, a positive electrode layer containing a positive electrode active material, an electrolyte layer containing a separator and a non-aqueous electrolyte, a negative electrode layer, and a negative electrode current collector foil, wherein in the non-aqueous secondary battery, The positive electrode active material is lithium manganese iron phosphate (LMFP). The weight per unit area of the positive electrode layer is 20 mg / cm³. 2 above, The non-aqueous electrolyte comprises lithium bis(fluorosulfonyl)imide (LiFSI) as a lithium salt, a dinitrile compound as an additive, and cyclic carbonate and ester compounds as solvents. The concentration of the lithium salt in the non-aqueous electrolyte is 1.4 M or higher. The dinitrile compound is butadionitrile SN.
2. The non-aqueous secondary battery according to claim 1, wherein, The volume ratio of the cyclic carbonate compound to the ester compound is 0.17 or higher. The cyclic carbonate compound is at least one of ethylene carbonate (EC) and propylene carbonate (PC). The ester compound is at least one selected from the group consisting of methyl acetate (MA), methyl propionate (MP), ethyl acetate (EA), vinyl propionate (EP), and propyl propionate (PP).
3. The non-aqueous secondary battery according to claim 1, wherein, The non-aqueous electrolyte also contains vinylene carbonate (VC) as an additive. The non-aqueous electrolyte contains 1.0% by mass or more of the vinylene carbonate as an additive, and the non-aqueous electrolyte contains 1.0% by mass or more of the dinitrile compound as an additive.
4. The non-aqueous secondary battery according to claim 1, wherein, The non-aqueous electrolyte also contains LiX as the lithium salt. The LiX is at least one of LiPF6 and LiBF4.
5. The non-aqueous secondary battery according to claim 4, wherein, The concentration ratio of LiFSI to LiX in the non-aqueous electrolyte is 2.5 or higher (LiFSI / LiX).
Citation Information
Patent Citations
High voltage lithium ion battery electrolyte and high voltage lithium ion battery
JP2016536776A