A battery and electrical device

By controlling the particle size distribution, specific surface area, and electrolyte ionic conductivity of the cathode material in lithium iron phosphate batteries, the problem of balancing dynamic performance and energy density in traditional lithium iron phosphate batteries has been solved, achieving a balance between high energy density and excellent dynamic performance.

CN123073129APending Publication Date: 2026-11-10CALB GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611239831.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the process of increasing electrode compaction density and energy density, traditional lithium iron phosphate batteries suffer a significant decrease in kinetic performance and fast charging performance, making it difficult to achieve a balance.

Method used

By synergistically controlling the particle size distribution, specific surface area of ​​the cathode material, and the ionic conductivity of the electrolyte, the relationship between the peak intensity ratio of ultra-small particles and small particles, the specific surface area of ​​the cathode material, and the geometric mean of the high and low temperature ionic conductivity of the electrolyte is adjusted, thereby optimizing the battery composition to improve lithium-ion transport capacity and reaction kinetics.

Benefits of technology

This approach achieves the goal of improving electrode compaction density and energy density while maintaining excellent lithium-ion transport capability and reaction kinetics performance, thereby enhancing the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073129A_ABST
    Figure CN123073129A_ABST
Patent Text Reader

Abstract

This invention provides a battery and an electrical device. The battery includes a positive electrode and an electrolyte. The positive electrode includes a positive electrode material, which is lithium iron phosphate. The lithium iron phosphate includes a first particle, a second particle, and a third particle. The particle size A2 corresponding to the apex of the first peak is 20~100nm, the particle size B2 corresponding to the apex of the second peak is 120~800nm, and the particle size C2 corresponding to the apex of the third peak is 1~4μm. The peak intensity corresponding to the apex of the first peak is A1%, the peak intensity corresponding to the apex of the second peak is B1%, and A1 / B1=a. The specific surface area of ​​the positive electrode material is bm². 2 / g; the ionic conductivity of the electrolyte at 40℃ is n mS / cm, and the ionic conductivity of the electrolyte at -10℃ is m mS / cm, (m×n) 1 / 2 =c; where a×b / c ranges from 0.015 to 2.4. The battery provided by this invention can balance kinetic performance and energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of battery technology, and particularly relates to a battery and an electrical device. Background Technology

[0002] Lithium iron phosphate (LFP) materials possess advantages such as stable cycle performance, high safety, and low cost, making them the most widely used cathode material in the lithium-ion battery field. However, LFP materials themselves have low electronic conductivity, slow lithium-ion diffusion rate, and poor kinetic performance. To improve battery energy density, it is usually necessary to increase electrode compaction density and active material loading. However, high compaction and high loading further prolong the transport path of lithium ions and electrons, exacerbating electrode polarization and leading to a significant decrease in rate performance and fast charging performance.

[0003] Therefore, in traditional lithium iron phosphate batteries, there is a mutual constraint between dynamic performance and energy density, making it difficult to achieve an effective balance. This has become a key technical problem restricting their high-performance application. Summary of the Invention

[0004] The main objective of this invention is to provide a battery and electrical device that can achieve both excellent dynamic performance and high energy density.

[0005] In a first aspect, the present invention provides a battery comprising a positive electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode material, the positive electrode material comprises lithium iron phosphate, and the lithium iron phosphate comprises a first particle, a second particle, and a third particle.

[0006] The particle size distribution curve of the cathode material has particle size on the x-axis and peak intensity on the y-axis. The particle size distribution curve includes the first peak of the first particle, the second peak of the second particle, and the third peak of the third particle. The particle size A2 corresponding to the vertex of the first peak is 20~100nm, the particle size B2 corresponding to the vertex of the second peak is 120~800nm, and the particle size C2 corresponding to the vertex of the third peak is 1~4μm.

[0007] The peak intensity corresponding to the vertex of the first peak is A1%; the peak intensity corresponding to the vertex of the second peak is B1%; A1 / B1 = a;

[0008] The specific surface area of ​​the positive electrode material is bm 2 / g;

[0009] The electrolyte has an ionic conductivity of n mS / cm at 40℃ and an ionic conductivity of m mS / cm at -10℃; (m×n) 1 / 2 =c;

[0010] The range of a×b / c is 0.015 to 2.4.

[0011] Secondly, the present invention provides an electrical device including the battery as described above.

[0012] The battery provided by this invention can achieve a balance between battery dynamic performance and energy density by limiting the relationship between the peak intensity ratio of ultra-small particles and small particles in the cathode material, the specific surface area of ​​the cathode material, and the geometric mean of the high and low temperature ionic conductivity of the electrolyte. Attached Figure Description

[0013] To more clearly illustrate the technical solutions in the embodiments of the present invention or related technologies, the accompanying drawings used in the description of the embodiments of the present invention or related technologies are briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0014] Figure 1 A particle size distribution curve of lithium iron phosphate provided by the present invention. Detailed Implementation

[0015] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions in the embodiments of this invention will be clearly and completely described below in conjunction with the embodiments of this invention. Obviously, the described embodiments are only some embodiments of this invention, not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this invention.

[0016] In existing technologies, cathode materials typically employ a combination of large and ultra-small particles. The ultra-small particles fill the gaps between the large particles, effectively increasing the electrode's compaction density and thus improving the battery's energy density. However, ultra-small particles have a large specific surface area, making them prone to agglomeration during slurry preparation. This necessitates the addition of significant amounts of dispersant to achieve proper dispersion. A large amount of dispersant remaining at the electrode interface and coating the particle surface forms a barrier layer, hindering the rapid transport of lithium ions and leading to a decline in battery kinetic performance.

[0017] The inventors of this application discovered through research that controlling the specific surface area of ​​the cathode material can reduce the dependence on dispersants and mitigate their adverse effects on lithium-ion transport. However, an excessively low specific surface area reduces the effective active area of ​​the electrode reaction, thus decreasing electrode reaction kinetics. Therefore, by further regulating the ionic conductivity of the electrolyte, the ion transport efficiency within the system is improved, compensating for the kinetic deficiencies caused by an excessively low specific surface area.

[0018] In summary, by synergistically controlling the three key parameters of cathode material particle size distribution, specific surface area, and electrolyte ionic conductivity, it is possible to improve electrode compaction density and energy density while taking into account excellent ion transport capability and reaction kinetics, thereby achieving a balance between the kinetic performance and energy density of lithium iron phosphate batteries.

[0019] Based on this, in a first aspect, the present invention provides a battery comprising a positive electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode material, the positive electrode material comprises lithium iron phosphate, and the lithium iron phosphate comprises a first particle, a second particle, and a third particle; as shown Figure 1 As shown, the particle size distribution curve of the cathode material has particle size on the x-axis and peak intensity on the y-axis, representing the volume percentage of particles of that size. The particle size distribution curve includes the first peak of the first particle, the second peak of the second particle, and the third peak of the third particle. The particle size A2 corresponding to the vertex of the first peak is 20~100nm, the particle size B2 corresponding to the vertex of the second peak is 120~800nm, and the particle size C2 corresponding to the vertex of the third peak is 1~4μm. The peak intensity corresponding to the vertex of the first peak is A1%; the peak intensity corresponding to the vertex of the second peak is B1%; A1 / B1=a; the specific surface area of ​​the cathode material is bm. 2 / g; the ionic conductivity of the electrolyte at 40℃ is n mS / cm; the ionic conductivity of the electrolyte at -10℃ is m mS / cm; (m×n) 1 / 2 =c; where a×b / c ranges from 0.015 to 2.4.

[0020] For example, A2 can be a range consisting of 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, or any two of them; B2 can be a range consisting of 120nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, or any two of them; C2 can be a range consisting of 1μm, 2μm, 2.5μm, 3μm, 4μm, or any two of them; and the range of a×b / c can be 0.015, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 2, 2.2, 2.4, or any two of them.

[0021] The battery provided by this invention achieves both excellent kinetic performance and high energy density by limiting the relationship between the particle size distribution, specific surface area of ​​the cathode material, and the geometric mean of the high and low temperature ionic conductivity of the electrolyte. This is because this invention can adjust the relative content of ultra-small particle size first particles by controlling the peak intensity ratio A1 / B1 of the first and second peaks. As this ratio increases, more first particles can fill the gaps between third particles and between third and second particles, which is beneficial to improving the compaction density of the electrode sheet, thereby increasing the energy density of the battery. However, an excessively high proportion of first particles will increase the risk of particle agglomeration during the slurry mixing process, requiring the addition of more dispersant, which is prone to forming an impedance layer at the electrode interface, adversely affecting lithium-ion transport performance. Therefore, this invention reduces the dependence on dispersant and the obstruction of lithium-ion transport by controlling the specific surface area of ​​the cathode material; however, if the specific surface area is too small, it will reduce the active sites of electrode reactions and reduce reaction kinetics. Therefore, this invention further improves the lithium-ion transport efficiency in the system by regulating the ionic conductivity of the electrolyte, compensating for the kinetic loss caused by the control of specific surface area. Ultimately, by synergistically controlling the relationship between the three parameters—peak intensity ratio, specific surface area, and electrolyte ionic conductivity—it is possible to improve electrode compaction density and energy density while ensuring excellent lithium-ion transport capability and reaction kinetics, thereby achieving a balance between battery kinetic performance and energy density.

[0022] In this invention, particle size selection is essentially a synergy of three dimensions: diffusion kinetics, packing mechanics, and processing feasibility. Specifically, A2 is 20~100nm: the rigid requirement of ion diffusion kinetics (<100 nm) combined with the constraint of agglomeration control (cannot be too small), the upper boundary is jointly defined by carbon coating uniformity and agglomeration threshold; B2 is 120~800nm: the geometric constraint of void filling (needs to fill the pores of the micron-scale framework) + functional transition requirements, the lower boundary is driven by the continuous connection with the first peak, and the upper boundary is constrained by the filling ability of large particle gaps; C2 is 1~4μm: the mechanical requirement of high compaction framework (>1μm) and the limitation of transport polarization (<4μm), the upper and lower boundaries are determined by the trade-off between compaction density and rate performance.

[0023] It's important to note that room-temperature conductivity cannot reflect the battery's bottleneck under real-world operating conditions. Room temperature (typically 25°C) is the optimal range for electrolyte performance. Almost all solvents exhibit peak ion dissociation and migration capabilities at this temperature. If only room-temperature conductivity is considered, even a mediocre electrolyte system may perform well.

[0024] -10℃ is a common temperature for cold starts and low-temperature charging of electric vehicles in winter. Below -10℃, the discharge capacity of lithium iron phosphate batteries will decrease sharply, and charging is more likely to cause lithium plating (lithium dendrites pierce the separator, creating serious safety hazards). 40℃ represents the warning line for "high-temperature stability". When the battery is charged and discharged at high rates or the ambient temperature is high (such as the battery pack inside a car or on the ground after being exposed to the summer sun), the internal temperature can easily reach 40℃ or even higher. 40℃ is the temperature at which the interfacial side reactions of lithium iron phosphate materials (especially nanoparticles) begin to accelerate significantly. LiPF6 in the electrolyte will decompose more rapidly, producing HF and corroding the positive electrode, leading to iron dissolution and damage to the SEI film.

[0025] Therefore, the battery provided by the present invention can achieve a balance between battery dynamic performance and energy density by limiting the relationship between the peak intensity ratio of ultra-small particles and small particles in the cathode material, the specific surface area of ​​the cathode material and the geometric mean of high and low temperature ionic conductivity of the electrolyte.

[0026] In some embodiments of the present invention, the range of a×b / c is 0.1 to 1.8. For example, it can be a range consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.5, 1.8 or any two of them, preferably 0.2 to 1.2.

[0027] As a preferred option, the battery can further achieve both excellent dynamic performance and high energy density.

[0028] In some embodiments of the present invention, a is 0.05 to 0.6, for example, it can be a range of 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6 or any two of them, preferably 0.4 to 0.6.

[0029] In some embodiments, b is 6~30m 2 / g, for example, can be 6m 2 / g、8m 2 / g, 10m 2 / g, 15m 2 / g、20m 2 / g、25m 2 / g、30m 2 The range of / g or any two thereof is preferably 12~14m. 2 / g.

[0030] In some embodiments, c is 6~30mS / cm, for example, it can be a range of 6mS / cm, 8mS / cm, 10mS / cm, 15mS / cm, 20mS / cm, 25mS / cm, 30mS / cm or any two of them, preferably 10~12mS / cm.

[0031] By controlling the peak intensity ratio α within the range of 0.1 to 1, the ratio of the first ultra-small particle to the second small particle can be reasonably controlled. This ensures that the ultra-small particles fill the gaps between the large particles, thereby increasing the compaction density and energy density of the electrode, while also preventing excessive ultra-small particles from causing slurry agglomeration and excessive addition of dispersant, thus reducing interfacial impedance and ensuring lithium-ion transport.

[0032] The specific surface area b is controlled between 6 and 30 m². 2 / g can achieve a balance between active surface area and dispersant requirements. With a moderate specific surface area, it can provide sufficient reactive sites to ensure good reaction kinetics, while reducing the amount of dispersant adsorption and usage, and reducing the obstacle to lithium-ion transport.

[0033] By controlling c to 6~30 mS / cm, the electrolyte can have suitable ionic conductivity over a wide temperature range: effectively improving the migration rate of lithium ions in the electrolyte, compensating for possible transport resistance in the electrode system, further improving the rate performance and kinetics of the battery, while not degrading the battery stability and safety.

[0034] By controlling a, b, and c synergistically within the above range, it is possible to improve the electrode compaction density and energy density while ensuring excellent lithium-ion transport efficiency and reaction kinetics, ultimately achieving an effective balance between energy density and kinetic performance of lithium iron phosphate batteries.

[0035] In this invention, the ionic conductivity *m* of the electrolyte at -10°C can be increased by increasing the content of carboxylic acid esters in the electrolyte; the ionic conductivity *n* of the electrolyte at 40°C can be increased by adjusting the content of diboronate ester additives in the electrolyte. Peak intensity *A1* can be controlled by adjusting the number of milling cycles in the slurry; the more milling cycles, the larger *A1*. Peak intensity *B1* can be controlled by adjusting the sintering temperature; the higher the sintering temperature, the larger *B1*.

[0036] In some embodiments of the present invention, the electrolyte includes an additive selected from at least one of diboronate compounds, cyclic sulfate compounds, and cyclic sulfonate compounds.

[0037] The electrolyte of this invention uses an additive containing at least one of diboronate compounds, cyclic sulfate compounds, and cyclic sulfonate compounds, which can form a dense, stable interfacial film (CEI or SEI) with excellent ionic conductivity on the electrode surface, which is beneficial to further improve the battery's kinetic performance and cycle stability.

[0038] The aforementioned additives preferentially undergo oxidative polymerization on the cathode surface, forming a uniform interfacial film with low impedance. This suppresses side reactions between the electrolyte and the cathode material, reduces active lithium loss, and improves battery cycle life and safety. Simultaneously, the formed interfacial film exhibits excellent lithium-ion transport capabilities, reducing interfacial polarization and improving lithium-ion insertion / extraction kinetics.

[0039] In some embodiments of the present invention, the additive is selected from diboronate compounds.

[0040] Choosing diboron ester compounds as electrolyte additives offers a core advantage: leveraging the synergistic effect of the "two borons" in their molecular structure to precisely control the interface and simultaneously address two major challenges faced by lithium-ion batteries in pursuing high energy density—building a robust and stable electrode interface and reducing interfacial impedance. On one hand, the synergistic effect of the "two borons" groups makes the film-forming process of the additive more intelligent and stable. The diboron structure preferentially undergoes coordination polymerization on the electrode surface, forming a dense, uniform, and mechanically superior interfacial film (CEI). Compared to single-boron structure additives, it has higher film-forming efficiency and a more robust film layer, effectively isolating the active material from the electrolyte, suppressing interfacial side reactions, reducing active lithium loss, and improving battery cycle stability and safety, thus ensuring the long-term stable operation of high-energy-density batteries. On the other hand, the interfacial film constructed by this type of additive has low impedance characteristics, providing a rapid transport channel for lithium-ion migration. The molecular design of the double boron structure enables the interface film formed to have both good lithium-ion conductivity and electronic insulation. It can prevent side reactions caused by electron shuttle and reduce the transport resistance of lithium ions at the interface, improve the battery dynamics performance, and solve problems such as excessive interface polarization and poor rate performance that are common in high energy density batteries.

[0041] In addition, diboronate compounds have the advantages of multifunctional integration and high molecular design flexibility. They can be modified to optimize film formation performance and ion transport efficiency according to the needs of the battery system, thereby further enhancing the balance between high energy density and excellent kinetic performance of the battery.

[0042] In some embodiments of the present invention, the diboronate compounds include at least one of lithium dioxaborate, lithium di(trifluoromethyloxarate)borate, and lithium bis(malonic acid)borate.

[0043] Using at least one of the aforementioned diboronate compounds as a diboronate additive can form a stable, dense interfacial film with excellent lithium-ion conductivity on the electrode surface. This type of boron-containing structure preferentially undergoes electropolymerization and coordination on the positive electrode surface, inhibiting electrolyte decomposition, reducing side reactions, and improving battery cycle stability and safety. Simultaneously, the resulting interfacial film exhibits low impedance and strong lithium-ion transport capability, reducing electrode interface polarization and improving rate performance and kinetic performance.

[0044] In some embodiments of the present invention, the mass percentage of the additive is 0.05 to 2.5% based on the total mass of the electrolyte, for example, it can be a range of 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5% or any two of these; preferably 0.1 to 2%.

[0045] When the additive content is too low, it is difficult to form a sufficient, continuous and stable interface film on the electrode surface, and the interface modification and impedance optimization effects cannot be fully utilized. When the additive content is too high, it is easy to cause the electrolyte viscosity to increase and the ionic conductivity to decrease. At the same time, excess additives are prone to side reactions, increasing the interface impedance and hindering lithium-ion transport.

[0046] By controlling the additive content within the above range, a uniform, dense, and low-resistance interfacial film can be formed on the electrode surface, effectively suppressing side reactions and improving kinetic performance, without adversely affecting the electrolyte ionic conductivity and slurry dispersibility. This can further improve the battery kinetic performance while ensuring high electrode compaction and high energy density, achieving a balance between the two.

[0047] In some embodiments of the present invention, the electrolyte further includes a solvent, which includes a carboxylic acid ester. The mass percentage of the carboxylic acid ester is 5% to 30% based on the total mass of the electrolyte. For example, it can be a range of 5%, 8%, 10%, 15%, 20%, 25%, 30%, or any two of these.

[0048] Carboxylic acid esters have low viscosity and strong solubility, which can effectively reduce electrolyte viscosity, increase electrolyte ionic conductivity, and improve the migration rate of lithium ions in electrolyte and electrode pores, thus improving battery dynamic performance.

[0049] Meanwhile, carboxylic acid esters have good compatibility with the above-mentioned diboronate ester additives, which can promote the uniform film formation of additives on the electrode surface and further reduce interfacial impedance.

[0050] By controlling the content of carboxylic acid esters within the above-mentioned range, it is possible to ensure that the electrolyte has excellent ion transport capabilities, while avoiding side reactions at the solvent-cathode interface and affecting the cycle stability of the battery due to excessive content. This approach can improve lithium-ion transport and reaction kinetics while ensuring high electrode compaction and high energy density, thus achieving a balance between energy density and kinetic performance.

[0051] In some embodiments of the present invention, the electrolyte further includes carbonate, wherein the number of carbon atoms in the carbonate is 2 to 6, for example, it can be a range of 2, 3, 4, 5, 6 or any two of them.

[0052] In this invention, the electrolyte also includes carbonates with 2 to 6 carbon atoms. These carbonates possess characteristics such as moderate dielectric constant, low viscosity, and good electrochemical stability. Using them as the main solvent of the electrolyte ensures sufficient dissociation of lithium salts, improves the ionic conductivity of the electrolyte, and provides a good medium for rapid lithium ion migration. Furthermore, their moderate molecular size ensures good compatibility with the electrode interface, allowing them to synergistically work with carboxylic esters and diboronate additives to form a stable and low-impedance interfacial film on the electrode surface.

[0053] Meanwhile, carbonates with 2 to 6 carbon atoms have moderate volatility and strong structural stability, which can improve the overall cycle stability and safety performance of the battery while ensuring good electrolyte wettability and ion transport capability, and further balance the battery's kinetic performance and energy density.

[0054] In some embodiments of the present invention, the range of B2 / A2 is 1.2 to 40, for example, it can be a range of 1.2, 5, 10, 15, 20, 30, 35, 40 or any two of them.

[0055] The appropriate particle size ratio between the second and first particles allows the first particle (ultra-small particle) to effectively fill the gaps between the second (small particle) and third (large particle), significantly improving the electrode compaction density and battery energy density. Simultaneously, this particle size ratio effectively reduces the agglomeration tendency of ultra-small particles, decreases the amount of dispersant used during slurry mixing, lowers interfacial impedance, and ensures rapid lithium-ion transport.

[0056] If the ratio is too small, the first and second particles will have similar sizes, resulting in poor gap filling and limited improvement in energy density. If the ratio is too large, the particle size difference will be too great, which will easily aggravate particle segregation and agglomeration and degrade kinetic performance.

[0057] Therefore, by controlling the B2 / A2 ratio between 1.2 and 40, a balance can be achieved between gap filling, compaction density, slurry dispersion, and ion transport, thus balancing the dynamic performance and energy density of lithium iron phosphate batteries.

[0058] In some embodiments of the present invention, the range of C2 / B2 is 1.25 to 35, for example, it can be a range of 1.25, 2, 5, 10, 15, 20, 30, 35 or any two of them.

[0059] This particle size ratio allows for a reasonable gradient of large and small particles, facilitating the effective filling of gaps between third particles by the second particle, and further filling of microscopic voids by the first particle, which is beneficial for improving electrode compaction density and battery energy density.

[0060] Meanwhile, a reasonable particle size ratio can avoid segregation, sedimentation and local agglomeration caused by excessive particle size differences, ensuring uniform electrode structure and moderate pore distribution, which is conducive to electrolyte wetting and lithium ion transport.

[0061] If the ratio is too small, the small and large particles are close in size, resulting in limited gap filling and insufficient energy density improvement; if the ratio is too large, particle stratification and agglomeration are likely to occur, increasing interfacial impedance and deteriorating kinetic performance.

[0062] Therefore, controlling the C2 / B2 ratio between 1.25 and 35 can achieve a good balance between graded filling, compaction density, structural uniformity, and ion transport, thus taking into account both the kinetic performance and energy density of lithium iron phosphate batteries.

[0063] In some embodiments of the present invention, A1 is 0.5 to 5%, for example, it can be a range of 0.5%, 0.7%, 1%, 1.2%, 1.5%, 1.7%, 2%, 3%, 4%, 5% or any two of them, preferably 0.5 to 2%.

[0064] In some embodiments, B1 is 2 to 12.5%, for example, it can be a range of 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 12.5% ​​or any two of them, preferably 2 to 5%.

[0065] A1 enables an appropriate amount of ultra-small particles to effectively fill the gaps between small and large particles, improving electrode compaction density and increasing battery energy density; B1 enables large particles to provide a stable electrode framework while avoiding excessive particle accumulation, resulting in a reasonable internal pore structure of the electrode, which is beneficial for electrolyte wetting and lithium-ion transport.

[0066] By controlling A1 and B1 within the above range, we can avoid the agglomeration problem caused by too many ultra-small particles, reduce the use of dispersants and reduce interfacial impedance, and ensure sufficient filling effect and compaction density, so as to achieve a balance between energy density and kinetic performance, and ultimately take into account both battery kinetic performance and energy density.

[0067] In some embodiments of the present invention, the peak intensity corresponding to the apex of the third peak is C1, expressed as a percentage; A1 < C1.

[0068] This invention controls the peak intensity A1 of the first peak to be less than the peak intensity C1 of the third peak (i.e., A1 < C1), indicating that the large third particle is the main phase and the ultra-small first particle is an auxiliary filler phase. Using large particles as the electrode framework helps ensure that the cathode material has a high tap density and electrode compaction density, thereby improving the battery energy density. At the same time, the higher proportion of large particles can reduce the overall specific surface area, reduce the adsorption and use of dispersants during the slurry mixing process, reduce interfacial impedance, and facilitate lithium-ion transport. Ultra-small particles exist only as an appropriate amount of filler phase, which can fully fill the interparticle gaps to further improve the compaction density, without causing serious agglomeration due to excessive amount, thus avoiding the degradation of kinetic performance.

[0069] Therefore, controlling A1 < C1 can achieve better gap filling effect and slurry dispersion while ensuring high energy density, effectively balancing the battery's kinetic performance and energy density.

[0070] In some embodiments of the present invention, the range of A1 / C1 is 0.1 to 0.5, for example, it can be a range consisting of 0.1, 0.2, 0.3, 0.4, 0.5 or any two of them.

[0071] By controlling the ratio of the peak intensity of the first peak to the peak intensity of the third peak, A1 / C1, within the range of 0.1 to 0.5, the relative proportion of ultra-small particles (first peak) to large particles (third peak) can be reasonably controlled. If this ratio is too low, the amount of ultra-small particles is insufficient, the inter-electrode gap filling effect is limited, and the improvement in compaction density and energy density is not significant. If this ratio is too high, the proportion of ultra-small particles is too large, which easily leads to agglomeration during the slurry mixing process, requiring more dispersant, increasing interfacial impedance, and deteriorating lithium-ion transport and kinetic performance.

[0072] By controlling A1 / C1 within the above range, it is possible to ensure that sufficient ultra-small particles effectively fill the gaps between large particles, improve the electrode compaction density, and increase the battery energy density; at the same time, it is possible to avoid the agglomeration problem caused by excessive ultra-small particles, reduce the amount of dispersant, reduce interfacial impedance, and ensure the battery's excellent kinetic performance.

[0073] In some embodiments of the present invention, C1 is 4 to 8%, for example, it can be a range of 4%, 5%, 6%, 7%, 8% or any two of them.

[0074] Controlling the peak intensity C1 of the third peak within the range of 4-8% indicates that the large-diameter third particles are the main components in the cathode material, which can provide a stable skeleton structure for the electrode. This is beneficial to improving the tap density and electrode compaction density of the cathode material, thereby significantly improving the energy density of the battery.

[0075] Meanwhile, using large particles as the main component can effectively reduce the overall specific surface area, reduce the adsorption and addition of dispersants during the mixing process, reduce the electrode interface impedance, ensure rapid lithium-ion transport, and improve kinetic performance.

[0076] Therefore, controlling C1 within the above range can ensure a sufficient proportion of large particles to achieve high compaction and high energy density, while also forming a reasonable gradient with the first and second particles, avoiding problems such as agglomeration, sedimentation, or poor wettability caused by particle ratio imbalance, thus achieving a balance between the dynamic performance and energy density of lithium iron phosphate batteries.

[0077] In some embodiments of the present invention, lithium iron phosphate further includes a fourth particle, and the particle size distribution curve further includes a fourth peak of the particle size of the fourth particle. The particle size D2 corresponding to the vertex of the fourth peak is 4~35μm, for example, it can be a range of 4μm, 5μm, 10μm, 15μm, 20μm, 25μm, 30μm, 35μm or any two of them.

[0078] By introducing this ultra-large diameter fourth particle, the present invention can construct a more stable multi-level skeleton structure inside the electrode, further improving the tap density of the cathode material and the compaction density of the electrode sheet, thereby significantly improving the energy density of the battery.

[0079] Meanwhile, the ultra-large fourth particle has a small specific surface area, which reduces the overall system's adsorption and demand for dispersant, decreases the dispersant's obstruction of lithium-ion transport, and improves electrode kinetic performance. With a four-level particle size gradient composite of the first, second, third, and fourth particles, particles of different sizes can sequentially fill the gaps, resulting in a denser particle arrangement and more uniform pore distribution within the electrode. This ensures high energy density while facilitating electrolyte wetting and lithium-ion transport.

[0080] In some embodiments of the present invention, a carbon coating layer is provided on the surface of lithium iron phosphate, and the thickness of the carbon coating layer is 0.5~120nm, for example, it can be a range of 0.5nm, 1nm, 5nm, 10nm, 30nm, 50nm, 70nm, 100nm, 120nm or any two of them.

[0081] Carbon coating can construct a continuous and efficient electronic conductive network on the surface of lithium iron phosphate particles, improving the electronic conductivity of the active material, accelerating electron transport rate, and enhancing battery rate performance and kinetic performance. Simultaneously, the carbon coating can isolate the active material from the electrolyte, suppressing interfacial side reactions and improving battery cycle stability and safety.

[0082] By controlling the thickness of the carbon coating layer within the above-mentioned range, sufficient electronic conductivity can be ensured without the coating layer being too thick, which would block lithium-ion transport channels and increase ion diffusion resistance, or the coating layer being too thin, which would prevent the formation of a complete conductive network.

[0083] In some embodiments of the present invention, the battery further includes a negative electrode sheet, which includes a negative electrode material, including at least one of graphite and silicon-carbon materials.

[0084] Graphite has the characteristics of stable layered structure, low lithium intercalation potential, excellent cycle performance and low cost, which can ensure the long-term cycle stability and safety performance of batteries.

[0085] Silicon-carbon materials have extremely high theoretical specific capacity, which can significantly improve the overall energy density of batteries.

[0086] In some embodiments of the present invention, the Dv50 of the negative electrode material is 5~20μm, for example, it can be a range of 5μm, 7μm, 10μm, 12μm, 15μm, 17μm, 20μm or any two of them.

[0087] This particle size range allows the negative electrode to possess both high compaction density and a reasonable pore structure, which is beneficial for improving the overall energy density of the battery. Simultaneously, it ensures sufficient electrolyte wetting and rapid lithium-ion transport, improving battery kinetic performance. A moderate particle size can reduce side reactions on the negative electrode surface, improve cycle stability, and effectively balance battery kinetic performance and energy density.

[0088] The battery of the present invention can be prepared using conventional methods in the art. Specifically, the positive electrode, separator and negative electrode can be stacked in sequence, and the cell can be obtained by stacking or winding. Then, the battery can be obtained by baking, liquid injection, formation and packaging.

[0089] The battery of the present invention can be a single cell, a battery pack, a battery stack, or a cylindrical cell formed by connecting single cells. These cells can be electrically connected by conventional methods in the art, such as series connection, parallel connection, or a hybrid connection including these connection methods, etc., without particular limitation.

[0090] Secondly, the present invention provides an electrical device including the battery as described above, which has advantages corresponding to the battery described above, and will not be elaborated further.

[0091] The electrical equipment of the present invention can be conventional electrical equipment in the art, such as power equipment (e.g., electric vehicles), electronic equipment (e.g., computers, mobile phones, digital cameras, printers, fax machines, etc.), wearable devices (e.g., watches, wristbands, VR glasses, etc.), and home appliances (e.g., air conditioners, refrigerators, washing machines, microwave ovens, etc.), etc., and there are no particular limitations.

[0092] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0093] Example 1

[0094] The battery preparation method of this embodiment includes the following steps:

[0095] Preparation of positive electrode

[0096] 1) Preparation method of the first particle:

[0097] ① Lithium hydroxide monohydrate, ferrous sulfate heptahydrate, 85wt% phosphoric acid, and ultrapure water were mixed in a mass ratio of 0.167:1:0.433:2.4 to obtain the first slurry;

[0098] ② The first slurry was transferred to a hydrothermal reactor and reacted at 200℃ for 3 hours to obtain the first lithium iron phosphate powder;

[0099] ③ The first lithium iron phosphate powder is mixed with glucose, polyethylene glycol, vanadium pentoxide and ultrapure water in a mass ratio of 100:7:4.5:0.7:166 to obtain the second slurry;

[0100] ④ After the second slurry was milled 8 times, a third slurry with a Dv50 of 250nm was obtained;

[0101] ⑤ The third slurry undergoes spray drying with an inlet air temperature of 200℃ and a feed rate of 50m. 3 / h, with an outlet air temperature of 100℃, the solvent is evaporated to obtain the first raw material;

[0102] ⑥ The first raw material is subjected to a first high-temperature sintering under a nitrogen atmosphere. The first high-temperature sintering temperature is 730℃ and the holding time is 8h to obtain the first sintered material.

[0103] ⑦ The first sintered material is subjected to air jet milling with a milling pressure of 460 MPa and a classification frequency of 60 Hz to obtain lithium iron phosphate containing the first particles.

[0104] 2) Preparation methods of the second and third particles:

[0105] ① Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:3.5:4.5:0.35:0.8:204 to obtain the fourth slurry;

[0106] ②After sand milling the fourth slurry, a fifth slurry with a Dv50 of 400nm is obtained;

[0107] ③ The fifth slurry is spray-dried at an inlet air temperature of 200℃ and a feed rate of 50m. 3 / h, with an outlet air temperature of 100℃, after evaporating the solvent, a second raw material with a Dv50 of 40μm is obtained;

[0108] ④ The second raw material is subjected to a second high-temperature sintering under a nitrogen atmosphere. The second high-temperature sintering temperature is 810℃ and the holding time is 8h to obtain the second sintered material.

[0109] ⑤ The second sintered material is crushed and depolymerized. The crushing pressure is 0.46 MPa and the grading frequency is 60 Hz to obtain lithium iron phosphate containing the second and third particles.

[0110] 3) Preparation method of the fourth particle:

[0111] ① Ferric phosphate, lithium carbonate, glucose, polyethylene glycol, titanium dioxide, vanadium pentoxide, phosphoric acid, and ultrapure water were mixed and dispersed in a mass ratio of 100:25:6:4:0.75:0.35:0.3:204 to obtain the sixth slurry;

[0112] ② After sand milling the sixth slurry, a seventh slurry with a Dv50 of 250nm was obtained;

[0113] ③ The seventh slurry is sprayed through a multi-fluid sprayer with an inlet air temperature of 200℃ and a feed rate of 50m. 3 / h, with an outlet air temperature of 100℃, after the solvent is evaporated, a third raw material with a Dv50 of 10μm is obtained;

[0114] ④ The third raw material is subjected to a third high-temperature sintering under a nitrogen atmosphere. The third high-temperature sintering temperature is 790℃ and the holding time is 8h to obtain the third sintered material.

[0115] ⑤ Vibrate and sieve the third sintering material to remove the caking material and obtain lithium iron phosphate containing the fourth particle.

[0116] 4) Mix the first particle, the second particle, the third particle, and the fourth particle in a mass ratio of 0.255:0.595:0.15 to obtain lithium iron phosphate.

[0117] Lithium iron phosphate (LFP) comprises four particles: a first particle, a second particle, a third particle, and a fourth particle. The particle size distribution curve of the LFP material represents particle size on the x-axis and peak intensity on the y-axis. The curve includes the first peak of the first particle, the second peak of the second particle, the third peak of the third particle, and the fourth peak of the fourth particle. The particle size corresponding to the vertex of the first peak is A2, and the corresponding peak intensity is A1. The particle size corresponding to the vertex of the second peak is B2, and the corresponding peak intensity is B1. The particle size corresponding to the vertex of the third peak is C2, and the corresponding peak intensity is C1. The particle size corresponding to the vertex of the fourth peak is D2. A1 / B1 = a. The surface of the LFP is coated with a carbon layer, and the specific surface area of ​​LFP is b.

[0118] The prepared lithium iron phosphate, conductive agent SP, binder PVDF, and dispersant polyvinylpyrrolidone were mixed at a mass ratio of 97.78:0.5:1.6:0.12. NMP solvent was added, and the mixture was stirred under vacuum until homogeneous to obtain a positive electrode slurry. The positive electrode slurry was coated onto the upper and lower surfaces of the positive electrode current collector aluminum foil, air-dried at room temperature, and then transferred to an oven for further drying. After cold pressing and slitting, positive electrode sheets with an areal density of 400 g / m³ were obtained. 2 The compacted density is 2.65 g / cm³. 3 .

[0119] Preparation of negative electrode

[0120] Graphite, conductive carbon black (SP), carboxymethyl cellulose (CMC), and dispersant polyvinylpyrrolidone (PVP) were mixed and dispersed in deionized water to obtain a negative electrode slurry. The mass percentages of graphite, conductive agent (SP), binder (CMC), and dispersant PVP were 96.4:2:0.6:1. The negative electrode slurry was coated on the upper and lower surfaces of the negative electrode current collector, and after drying, rolling, and slitting, a negative electrode sheet was obtained with an areal density of 93 g / m³. 2 Compacted density 1.6 g / cm³ 3 .

[0121] Preparation of electrolyte

[0122] Ethyl carbonate (EC), diethyl carbonate (DEC), and ethyl acetate (EA) were mixed in a volume ratio of 4:4:2 to obtain an organic solvent. Then, thoroughly dried lithium salts LiPF6 and LiFSI were dissolved in the mixed organic solvent to prepare an electrolyte with a concentration of 1 mol / L. 1.7% lithium dioxaborate was added as an additive. The ionic conductivity of the electrolyte at 40℃ is n, and the ionic conductivity of the electrolyte at -10℃ is m, (m×n). 1 / 2 =c.

[0123] Preparation of diaphragm

[0124] PP is selected as the diaphragm.

[0125] Assembly, formation

[0126] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrode sheets. Then, they are wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained.

[0127] Example 2

[0128] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 12 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:5.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 0.6% lithium dioxalate borate is added to the electrolyte as an additive.

[0129] Example 3

[0130] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 8 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:0.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 1.7% lithium dioxalate borate is added to the electrolyte as an additive.

[0131] Example 4

[0132] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 12 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:3.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 0.1% lithium dioxalate borate is added to the electrolyte as an additive.

[0133] Example 5

[0134] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 10 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:0.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 1.2% lithium dioxalate borate is added to the electrolyte as an additive.

[0135] Example 6

[0136] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 7 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:15.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 0.1% lithium dioxalate borate is added to the electrolyte as an additive.

[0137] Example 7

[0138] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled twice; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:1.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 2% lithium dioxalate borate is added to the electrolyte as an additive.

[0139] Example 8

[0140] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 20 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:10.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 0.8% lithium dioxalate borate is added to the electrolyte as an additive.

[0141] Example 9

[0142] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled once; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:6.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 0.05% lithium dioxalate borate is added to the electrolyte as an additive.

[0143] Example 10

[0144] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 24 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:1.5:1.5:0.35:0.8:204 to obtain the fourth slurry; 1.1% lithium dioxalate borate is added to the electrolyte as an additive.

[0145] Example 11

[0146] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 22 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:19.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 1.5% lithium dioxalate borate is added to the electrolyte as an additive.

[0147] Example 12

[0148] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 5 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:4:4.5:0.35:0.8:204 to obtain the fourth slurry; 1.9% lithium dioxalate borate is added to the electrolyte as an additive.

[0149] Example 13

[0150] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled 11 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:15:4.5:0.35:0.8:204 to obtain the fourth slurry; 0.2% lithium dioxalate borate is added to the electrolyte as an additive.

[0151] Example 14

[0152] The preparation method of the battery in this embodiment is basically the same as that in Example 1, except that in step 1), the second slurry is milled once; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:1:4.5:0.35:0.8:204 to obtain the fourth slurry; 1.6% lithium dioxalate borate is added to the electrolyte as an additive.

[0153] Comparative Example 1

[0154] The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step 1), the second slurry is milled 4 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:1.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 1.5% lithium dioxalate borate is added to the electrolyte as an additive.

[0155] Comparative Example 2

[0156] The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step 1), the second slurry is milled 20 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:7.5:4.5:0.35:0.8:204 to obtain the fourth slurry; 2% lithium dioxalate borate is added to the electrolyte as an additive.

[0157] Comparative Example 3

[0158] The preparation method of the battery in this comparative example is basically the same as that in Example 1, except that in step 1), the second slurry is milled 6 times; in step 2), iron phosphate, lithium carbonate, glucose, polyethylene glycol, vanadium pentoxide, phosphoric acid, and ultrapure water are mixed and dispersed in a mass ratio of 100:25:2.5:1.5:0.35:0.8:204 to obtain the fourth slurry; 1.3% lithium dioxalate borate is added to the electrolyte as an additive.

[0159] Experimental example:

[0160] 1. Particle size distribution curve:

[0161] Pretreatment: Discharge the battery at 0.33C to the lower limit voltage of 2.5V, remove the empty battery, disassemble the positive electrode, soak the positive electrode in dimethyl carbonate (DMC) solution for 4 hours, air dry, and then scrape off the powder from the positive electrode for later use.

[0162] A certain amount of positive electrode material sample was placed on the sample stage and observed using a scanning electron microscope (SEM). First, the magnification was adjusted to low magnification (5000~10000 times) to observe the overall dispersion state of the sample and exclude areas with severe agglomeration. Then, the magnification was adjusted to high magnification (50000~80000 times) to clearly distinguish the particle size difference between the first and second particles. The image was saved for subsequent statistical analysis.

[0163] Open the relevant particle size analysis software and import the SEM image to be analyzed. Use the diagonal line method to measure the particle size in the image, selecting 5 different non-overlapping regions (to avoid local bias). Take a clear SEM image of each region, avoiding edges and agglomerates, ensuring that the particles in the image are independently dispersed and without significant overlap. Convert the statistically analyzed particle size and quantity percentages into a particle size-volume percentage distribution map. The specific conversion method is as follows: ① For the i-th particle size class, take the median particle size of that class as Di, and the quantity percentage of that class as Ni; ② The corresponding volume weight of that particle size class is: Vi' = Ni × Di³; ③ Normalize to obtain the volume percentage Vi = Vi' / ∑Vi'. Generate a particle size-volume percentage map for parameter reading and calculation.

[0164] 2. Specific surface area:

[0165] In an environment of 25℃ and 60% humidity, weigh the empty small test tube and load 1g of positive electrode material powder sample into the sample tube; turn on the degassing station, place the small test tube in the degassing station at 200℃, vacuum heat for 120min, backfill with nitrogen, remove the sample tube and weigh it to calculate the sample mass; conduct the test on the instrument in an environment of 25℃ and 60% humidity; select the multi-point BET test method, set the P / P0 range to 0.05~0.3, select 6 pressure points, input the mass parameters, and the equipment will automatically analyze and read the test results.

[0166] 3. Additive content:

[0167] The electrolyte used in the test was a finished product, and its component content was determined directly by comparing it with standard GC-MS spectra.

[0168] 4. Ionic conductivity of the electrolyte:

[0169] 1) Electrolyte Collection: If the electrolyte of the test object is in a secondary battery, use a battery charge-discharge device to discharge the secondary battery under the following conditions: current 0.3C, cutoff lower limit voltage 2.5V. Disassemble the battery and collect the electrolyte in a glove box (H2O≤0.1ppm, O2≤0.1ppm). There are three methods for collecting the electrolyte: After removing the battery cover, ① if there is free electrolyte, collect it into a 5mL sample tube using a pipette and seal it with sealing tape to prevent leakage. ② if there is no free electrolyte, use a hydraulic press (Beijing Heng'ao Technology Co., Ltd.'s FY-30 hydraulic press) to continuously pressurize until free electrolyte appears, collect it into a sample tube, and seal it. ③ Add an appropriate amount of dichloromethane extractant to the battery and record the dichloromethane content. After adding dichloromethane, put the battery into an aluminum-plastic bag and seal it with a heat sealer. Transfer it to an ultrasonic oscillator and oscillate for 12 hours to allow the electrolyte in the electrode to mix thoroughly with the dichloromethane. Then, use a pipette to draw the mixture of dichloromethane and electrolyte into a 5mL sample tube and seal the sample tube with sealing glue.

[0170] 2) Electrolyte conductivity testing: The electrolytes prepared in each example and comparative example were tested using a Mettler conductivity meter (model: S230) under normal atmospheric pressure at 25°C. The conductivity meter consists of conductivity electrodes and an electronic unit. High-frequency alternating current is used to measure the resistance of the solution between two parallel electrodes. The electronic unit uses an AC signal of appropriate frequency to amplify and process the signal before converting it into conductivity. The testing steps are as follows:

[0171] The electrolyte must be handled under an inert atmosphere throughout the pretreatment process. Sampling and dispensing should be completed in a high-purity argon glove box, controlling the water content to <0.1 ppm and the oxygen content to <0.1 ppm. The conductivity cell or test container used should be dry and sealed; if necessary, vacuum grease should be applied to the interface to achieve a good seal. Air bubbles should be avoided during dispensing to prevent affecting the accuracy of impedance testing.

[0172] The pretreated electrolyte must be verified to meet the moisture content requirements. The moisture content of the LiPF6-based electrolyte should be ≤20ppm; otherwise, the sample is deemed unqualified and must be prepared again. Moisture content is determined by coulometric Karl Fischer titration (refer to GB / T 6324.8), with the sample volume controlled at 1-2mL.

[0173] Inside the glove box, inject the qualified electrolyte (with moisture content verified) into the conductivity cell. The test cell uses inert metal electrodes (platinum or stainless steel). During assembly, ensure that the electrode spacing is fixed and the electrodes are completely submerged in liquid. After assembly, remove the conductivity cell from the glove box and immediately transfer it to the temperature control device.

[0174] Pretreatment for ionic conductivity testing at 40℃: Place the sealed conductivity cell in a constant temperature chamber or water bath, controlling the temperature accuracy to ±10℃. After heating to 40℃, the sample must be left to stand at this temperature for at least 30 minutes to ensure uniform temperature distribution of the electrolyte within the conductivity cell and eliminate any temperature gradients.

[0175] Pretreatment for -10℃ ionic conductivity testing: Place the sealed conductivity cell in a low-temperature constant temperature bath (such as a conductivity testing system equipped with a low-temperature circulating bath). The cooling rate should be controlled at 1-2℃ / min to avoid local solidification of the solvent or the formation of bubbles due to rapid cooling. After reaching -10℃, the sample needs to stand at this temperature for at least 60 minutes.

[0176] Electrode calibration

[0177] Take approximately 10 mL of a conductivity standard solution with a conductivity of 12.88 mS / cm and place it in a centrifuge tube. Incubate the solution in a water bath at 25°C for 30 minutes. If the temperature of the conductivity standard solution measured by the temperature electrode is 25.0 ± 0.2°C, then calibration begins. If the conductivity of the standard solution is 12.88 ± 0.15 mS / cm, then the calibration is successful.

[0178] Sample preparation

[0179] Take approximately 100 mL of sample into a dry, clean fluorinated bottle and seal it. Place the sample in a constant temperature water bath at 25.0 ± 0.2 °C for 30 min.

[0180] test

[0181] Install the conductivity electrode and clean it with ethanol, then wipe it dry with filter paper. Open the sampling bottle, immerse the conductivity electrode in the sample to be tested, select "automatic measurement mode", click the "measure" button to start the measurement, and after hearing a "beep" sound, the value remains unchanged. Record the current value, which is the conductivity.

[0182] 5. Solvent content: The test method is the same as that for additive content.

[0183] 6. Test method for carbon coating thickness:

[0184] 1) Pretreatment: Discharge the battery to 2.5V at 0.33C. Take the positive electrode sheet of the lithium-ion battery in the empty state and soak it in dimethyl carbonate (DMC) solution at room temperature for 4 hours. After soaking, take out the positive electrode sheet and dry it in a vacuum environment. Use a ceramic knife to scrape off the active material powder on the surface of the electrode sheet.

[0185] 2) Take a small amount of active material powder sample and place it in a sample tube. Add anhydrous ethanol and sonicate for 40 minutes. Use a pipette to take a small amount of solution and drop it onto a copper grid. Finally, dry the sample completely in a vacuum drying oven. Place the sample on the test stage and transfer it to the cavity. Use TEM to measure the thickness of the coating layer at a suitable high magnification for different coating layer thicknesses. Select 5 regions for measurement and take the average value.

[0186] 7. Dv50 of the negative electrode material: The volume median particle size (Dv50) of the negative electrode material was determined using a laser particle size analyzer (refer to GB / T 19077) in wet dispersion mode. The specific steps are as follows:

[0187] (1) Sampling and drying

[0188] Take about 0.1~0.5g of the negative electrode material sample to be tested, place it in a vacuum drying oven, dry it at 120±5℃ for 2~4h, and then place it in a desiccator to cool to room temperature.

[0189] (2) Dispersion medium and dispersant

[0190] The dispersion medium is deionized water (resistivity ≥18.2 mΩ·cm, filtered through a 0.45 μm filter membrane) or anhydrous ethanol; the dispersant is selected from one or more of sodium hexametaphosphate, sodium pyrophosphate, or Triton X-100, and the amount added is 0.05~0.2% of the volume of the dispersion medium. Add the dispersant to the dispersion medium and stir magnetically at 200~300 rpm for 1~2 min.

[0191] (3) Sample dispersion

[0192] Add the dried sample to the dispersion medium described above, stir with a glass rod for 30 seconds, and then place it in an ultrasonic cleaner for ultrasonic dispersion. The ultrasonic power is 100-200W, and the ultrasonic time is 3-10 minutes (not exceeding 15 minutes). Control the initial water temperature to be <18℃ and the final water temperature to be <24℃. Perform the test immediately after ultrasonication, with an interval of no more than 5 minutes.

[0193] (4) Test conditions

[0194] The test environment temperature is 20~25℃, and the relative humidity is ≤60%. Before testing, the instrument's circulation system should be turned on for 5~10 minutes to warm up. The instrument should be verified using standard particles (Dv50 deviation ≤±3%). The optical model adopts Mie theory. The optical parameters of the negative electrode material are set according to the material type: graphite refractive index 1.5~2.0, absorptivity 0.01~0.5; the refractive index of the dispersion medium is 1.33 for water and 1.36 for ethanol. The light-blocking rate is controlled at 5~15% (preferably 8~12%), the pump speed is 2000~3000 rpm, and the single acquisition time is 5~15s.

[0195] (5) Data collection

[0196] Each sample was tested in parallel three times, and the average value of Dv50 was taken as the test result. The relative standard deviation (RSD) of the three results should be ≤3%.

[0197] 8. Methods for testing energy density:

[0198] Weigh the battery and record the weight as m. Place the battery in a fixture, apply a force of 3000N, charge it at a constant voltage of 0.33C to 3.65V, then charge it at a constant voltage to the cutoff current of 0.05C, let it rest for 30 minutes, discharge it at a constant current of 0.33C to 2.5V, let it rest for 30 minutes, and repeat the cycle 3 times. Obtain the discharge capacity (in Ah) and energy E (average of three cycles). Discharge energy density = E / m (in Wh / kg).

[0199] 9. Test methods for charge / discharge performance:

[0200] 1) Place the battery at room temperature until it reaches thermal equilibrium;

[0201] 2) In a 25℃ constant temperature chamber, the lithium-ion battery was subjected to charge-discharge cycle test. The charge-discharge regime was as follows: charge at a constant current of 0.33C to the upper limit voltage of 3.65V, then charge at a constant voltage until the current drops to 0.05C. After standing for 5 minutes, discharge the battery at a constant current of 0.33C to the lower limit voltage of 2.5V. This is one cycle. After three cycles, the discharge capacity of the third cycle was used as the standard capacity of the battery.

[0202] 3) Adjust to the test temperature in the following order (25℃ / -10℃) until thermal equilibrium is reached;

[0203] 4) Adjust the battery charge to 50% SOC at a 1 / 3C discharge rate;

[0204] 5) Discharge at a 1C rate current for 18s, record the battery voltage U2, current I before the discharge stops and the battery voltage U1 after the battery voltage stabilizes. Calculate the DC internal resistance R1 according to the formula R1=(U2-U1) / I.

[0205] Table 1

[0206]

[0207] As shown in Table 1, compared with the comparative example, the battery provided by the present invention can achieve a balance between battery dynamic performance and energy density by limiting the relationship between the peak intensity ratio of ultra-small particles and small particles in the cathode material, the specific surface area of ​​the cathode material and the geometric mean of high and low temperature ionic conductivity of the electrolyte.

[0208] As can be seen from Examples 1-11 and Comparative Examples 1-3, when the range of a×b / c is 0.1~1.8, the energy density and impedance performance of the battery are excellent. Specifically, the energy density of the battery is greater than or equal to 153Wh / kg, and the resistance is below 0.73mΩ. Further controlling the range of a×b / c to 0.2~1.2 can further improve the energy density of the battery and reduce the resistance.

[0209] Based on Examples 1-11 and Comparative Examples 1-3, it can be seen that when the range of a is 0.1~1 and the range of b is 6~30m... 2 When the range of / g and c is 6~30mS / cm, the energy density and impedance performance of the battery are better; further controlling the range of a to 0.4~0.6 and the range of b to 12~14mS / cm 2 When the range of / g and c is 10~12mS / cm, the energy density and impedance performance of the battery can be further improved.

[0210] Finally, it should be noted that other embodiments of the invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention disclosed herein. This invention is intended to cover any variations, uses, or adaptations of the invention that follow the general principles of the invention and include common knowledge or customary techniques in the art not disclosed herein, and is not limited to the precise structures described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of the invention is limited only by the appended claims.

Claims

1. A battery, characterized in that, The device includes a positive electrode sheet and an electrolyte, wherein the positive electrode sheet includes a positive electrode material, the positive electrode material includes lithium iron phosphate, and the lithium iron phosphate includes a first particle, a second particle, and a third particle. The particle size distribution curve of the cathode material has particle size on the x-axis and peak intensity on the y-axis. The particle size distribution curve includes the first peak of the first particle, the second peak of the second particle, and the third peak of the third particle. The particle size A2 corresponding to the vertex of the first peak is 20~100nm, the particle size B2 corresponding to the vertex of the second peak is 120~800nm, and the particle size C2 corresponding to the vertex of the third peak is 1~4μm. The peak intensity corresponding to the vertex of the first peak is A1%; the peak intensity corresponding to the vertex of the second peak is B1%; A1 / B1 = a; The specific surface area of ​​the positive electrode material is bm 2 / g; The electrolyte has an ionic conductivity of n mS / cm at 40℃ and an ionic conductivity of mmS / cm at -10℃; (m×n) 1 / 2 =c; The range of a×b / c is 0.015 to 2.

4.

2. The battery according to claim 1, characterized in that, The range of a×b / c is 0.1 to 1.

8.

3. The battery according to claim 1, characterized in that, a is 0.05~0.6; And / or, b is 6~30m 2 / g; And / or, c is 6~30mS / cm.

4. The battery according to claim 1, characterized in that, The electrolyte includes an additive selected from at least one of diboronate compounds, cyclic sulfate compounds, and cyclic sulfonate compounds.

5. The battery according to claim 4, characterized in that, The additive is selected from diboronate compounds.

6. The battery according to claim 5, characterized in that, The diboronic acid ester compounds include at least one of lithium dioxaborate, lithium di(trifluoromethyloxarate)borate, and lithium bis(malonic acid)borate.

7. The battery according to claim 4, characterized in that, Based on the total mass of the electrolyte, the mass percentage of the additive is 0.05~2.5%.

8. The battery according to claim 1, characterized in that, The electrolyte also includes a solvent, which includes a carboxylic acid ester, and the carboxylic acid ester accounts for 5-30% of the total mass of the electrolyte.

9. The battery according to claim 1, characterized in that, The electrolyte also includes carbonates, wherein the number of carbon atoms in the carbonates is 2 to 6.

10. The battery according to claim 1, characterized in that, The range of B2 / A2 is 1.2 to 40.

11. The battery according to claim 1, characterized in that, The C2 / B2 ratio ranges from 1.25 to 35.

12. The battery according to claim 1, characterized in that, A1 is 0.5%~5%; And / or, B1 is 2~12.5%.

13. The battery according to claim 1, characterized in that, The peak intensity corresponding to the apex of the third peak is C1, expressed as a percentage; A1 < C1.

14. The battery according to claim 13, characterized in that, The range of A1 / C1 is 0.1 to 0.

5.

15. The battery according to claim 13, characterized in that, C1 is 4-8%.

16. The battery according to claim 1, characterized in that, The lithium iron phosphate also includes a fourth particle, and the particle size distribution curve also includes the fourth peak of the fourth particle, the particle size D2 corresponding to the vertex of the fourth peak is 4~35μm.

17. The battery according to claim 1, characterized in that, The lithium iron phosphate has a carbon coating layer on its surface, and the thickness of the carbon coating layer is 0.5~120nm.

18. The battery according to any one of claims 1-17, characterized in that, The battery also includes a negative electrode sheet, which includes a negative electrode material, and the negative electrode material includes at least one of graphite and silicon-carbon materials.

19. The battery according to claim 18, characterized in that, The Dv50 of the negative electrode material is 5~20μm.

20. An electrical appliance, characterized in that, Includes the battery as described in any one of claims 1-19.