Secondary batteries, their preparation methods and electrical devices

By adding ternary and quaternary nitrogen heterocyclic compounds to the electrolyte to form a polymer skeleton, the problem of insufficient cycle performance of high-nickel ternary lithium-ion batteries was solved. This achieved the binding of transition metal ions and the reduction of HF generation, thereby improving the cycle stability of the battery.

CN123073154APending Publication Date: 2026-11-10CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510588059.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-08
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

High-nickel ternary lithium-ion batteries have poor cycle performance and cannot meet the needs of daily life. This is mainly due to crosstalk problems caused by the dissolution and free migration of transition metal ions, as well as interface corrosion problems caused by the reaction of fluorine-containing lithium salts with water to generate HF.

Method used

Adding ternary and quaternary nitrogen heterocyclic compounds as polymer monomers to the electrolyte forms a polymer skeleton with a three-dimensional network structure. By binding the solvent and inhibiting the migration of transition metal ions through the polymer skeleton, the amount of HF generated is reduced, the direct contact between the positive electrode and the electrolyte is reduced, and the cycle performance of the battery is improved.

Benefits of technology

It effectively suppressed the crosstalk problem of ternary materials and the interface corrosion problem of HF, and improved the cycle performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073154A_ABST
    Figure CN123073154A_ABST
Patent Text Reader

Abstract

This application relates to a secondary battery, a method for preparing the same, and an electrical device thereof. The secondary battery includes a gel electrolyte comprising a polymer backbone and an electrolyte solution located within the polymer backbone. The electrolyte solution contains a fluorinated lithium salt. The polymer backbone is made from polymer monomers, which include one or more of ternary and quaternary nitrogen heterocyclic compounds. This secondary battery exhibits improved cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of secondary battery technology, and further to secondary batteries, their preparation methods, and electrical devices. Background Technology

[0002] In recent years, lithium-ion batteries have been used in a wide range of applications, including energy storage systems in hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, and electric vehicles. High-nickel ternary materials are increasingly being used in lithium-ion batteries due to their high energy density.

[0003] Currently, the cycle performance of high-nickel ternary lithium-ion batteries is poor and cannot meet people's daily needs. Summary of the Invention

[0004] In view of the above problems, this application provides a secondary battery with excellent cycle performance, a method for preparing the same, and an electrical device thereof.

[0005] In a first aspect, this application provides a secondary battery comprising a gel electrolyte, the gel electrolyte comprising a polymer backbone and an electrolyte located within the polymer backbone, the electrolyte comprising a fluorinated lithium salt, and the polymer backbone comprising polymer monomers, the polymer monomers comprising one or more of ternary nitrogen heterocyclic compounds and quaternary nitrogen heterocyclic compounds.

[0006] Therefore, selecting one or more of ternary and quaternary nitrogen heterocyclic compounds for polymerization is beneficial for forming a polymer framework with a three-dimensional network structure. The polymer framework in the gel electrolyte of this secondary battery then possesses a liquid-binding function, reducing direct contact between the electrolyte and the positive electrode and lowering the risk of oxidative decomposition. Simultaneously, the three-dimensional network structure of the polymer framework can bind the solvent to a certain extent. Since the solvent is a carrier for the migration of transition metal ions, a slower solvent movement also slows down the movement of transition metal ions. Thus, the gel electrolyte can significantly inhibit the dissolution and free migration of transition metal ions in the positive electrode active material. Through these combined effects, the crosstalk problem of ternary materials can be effectively reduced. The raw material monomers of the polymer framework are amine compounds. Since the binding energy of amine compounds with H2O is higher than that between fluorinated lithium salts and H2O, the reaction between fluorinated lithium salts and H2O can be effectively inhibited. Therefore, the amount of HF generated can be effectively reduced, thus reducing the corrosion of the solid electrolyte interface film formed on the negative electrode surface by HF. Therefore, by adding a polymer backbone formed by one or more monomers of ternary and quaternary nitrogen heterocyclic compounds to the electrolyte, the crosstalk problem of ternary materials and the interfacial corrosion problem of HF can be effectively reduced, thereby effectively improving the cycle performance of the ternary system.

[0007] In any embodiment of this application, the polymer monomer includes one or more of aziridine, 2-methylaziridine, trimethylolpropane-tris[3-(2-methylaziridine)propionate], trimethylolpropane-tris(3-aziridine)propionate, 1-hydroxyethylaziridine, and aziridine and its derivatives.

[0008] In any embodiment of this application, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine.

[0009] In any embodiment of this application, the polymer monomer comprises trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.5:1.5-4:1. This mass ratio ensures a suitable polymer backbone network density, guaranteeing both liquid retention and normal lithium-ion conduction.

[0010] In any embodiment of this application, the polymer monomers include trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine.

[0011] In any embodiment of this application, the polymer monomer comprises trimethylolpropane tris(3-acridinylpropionate) and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine is 3.5:1.5-4:1. This mass ratio ensures a suitable polymer backbone network density, guaranteeing both liquid retention and normal lithium-ion conduction.

[0012] In any embodiment of this application, the polymer backbone comprises a cross-linked polymer with a degree of cross-linking of 0.4-0.8. Thus, the polymer backbone network density is moderate, ensuring both liquid retention and normal lithium-ion conduction.

[0013] In any embodiment of this application, the fluorinated lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium difluorophosphate.

[0014] In any embodiment of this application, the secondary battery is a lithium-ion secondary battery.

[0015] In any embodiment of this application, the secondary battery further includes a positive electrode and a negative electrode. The positive electrode includes a positive active material layer containing lithium nickel cobalt manganese oxide. The negative electrode includes a negative active material layer containing graphite.

[0016] In any embodiment of this application, the molar percentage of nickel in the lithium nickel cobalt manganese oxide is ≥0.6% of all metal elements except lithium.

[0017] In any embodiment of this application, the chemical formula of the lithium nickel cobalt manganese oxide is Li. 1+d [Ni x Co y Mn z M w O 2+f Wherein, -0.2≤d≤0.2, x+y+z+w=1, 0.5≤x<1, 0≤y<0.3, 0.5≤z<1, 0≤w<0.3, -0.5≤f≤0.5, and M includes one or more of Zr, Al, Ti, Sb, Nb, Te, Mg, B, Ca, V, Ta or Sr.

[0018] Secondly, this application provides a method for preparing a secondary battery, comprising the following steps:

[0019] An electrolyte comprising a polymer monomer is prepared, the electrolyte comprising a fluorinated lithium salt; the polymer monomer comprising one or more of ternary nitrogen heterocyclic compounds and quaternary nitrogen heterocyclic compounds;

[0020] The electrolyte is injected into the electrode assembly and left to stand so that the polymer monomers form a polymer skeleton with a three-dimensional network structure, thereby preparing the secondary battery.

[0021] In any embodiment of this application, the settling time is 24h-36h. Therefore, reasonably controlling the settling time is beneficial to complete the wetting of the electrode sheet by the electrolyte before the formation of the polymer skeleton.

[0022] In any embodiment of this application, the electrolyte includes a solvent, and the mass percentage of the polymer monomer relative to the mass of the solvent is 0.5%-2%. Therefore, by reasonably controlling the mass percentage of the polymer monomer relative to the mass of the solvent contained in the electrolyte, a suitable polymer backbone network density can be ensured, guaranteeing both the liquid retention capacity of the polymer backbone and the normal conduction of lithium ions.

[0023] In any embodiment of this application, the electrolyte comprises a solvent, and the mass percentage of the polymer monomer relative to the mass of the solvent is 1%-2%.

[0024] In any embodiment of this application, the polymer monomer includes one or more of aziridine, 2-methylaziridine, trimethylolpropane-tris[3-(2-methylaziridine)propionate], trimethylolpropane-tris(3-aziridine)propionate, 1-hydroxyethylaziridine, and aziridine and its derivatives.

[0025] In any embodiment of this application, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine.

[0026] In any embodiment of this application, the polymer monomer comprises trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.5:1.5-4:1. This mass ratio ensures a suitable polymer backbone network density, guaranteeing both liquid retention and normal lithium-ion conduction.

[0027] In any embodiment of this application, the polymer monomers include trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine.

[0028] In any embodiment of this application, the polymer monomer comprises trimethylolpropane tris(3-acridinylpropionate) and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine is 3.5:1.5-4:1. This ensures a suitable polymer backbone network density, guaranteeing both liquid retention and normal lithium-ion conduction.

[0029] In any embodiment of this application, the fluorinated lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium difluorophosphate.

[0030] Thirdly, this application provides an electrical device, including at least one of the secondary battery of the first aspect and the semi-solid battery prepared by the preparation method of the secondary battery of the second aspect. Attached Figure Description

[0031] To better describe and illustrate the implementation methods, embodiments, or examples provided in this application, reference may be made to one or more accompanying drawings. Additional details or examples used to describe the drawings should not be considered as limiting the scope of any of the disclosed applications, the currently described implementation methods, embodiments, or examples, or the best mode of these applications as currently understood.

[0032] In the attached diagram:

[0033] Figure 1This is a schematic diagram of a battery cell according to one embodiment of this application.

[0034] Figure 2 for Figure 1 An exploded view of a battery cell according to one embodiment of this application is shown.

[0035] Figure 3 This is a schematic diagram of a battery device according to one embodiment of this application.

[0036] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0037] Figure 5 for Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.

[0038] Figure 6 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.

[0039] Figure 7 The image shows a cross-linked network diagram obtained by nuclear magnetic resonance testing of the polymer skeleton obtained from the disassembly of the secondary battery in Example 1.

[0040] Explanation of reference numerals in the attached figures:

[0041] 1. Battery pack; 2. Upper casing; 3. Lower casing; 4. Battery assembly; 5. Individual battery cell; 51. Housing; 52. Solid-state battery cell; 53. Cover plate; 6. Electrical device. Detailed Implementation

[0042] The following describes in detail, with appropriate reference to the accompanying drawings, some embodiments of the secondary battery, its preparation method, and its electrical device of this application. However, some unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0043] The "range" disclosed in this application can be defined in the form of a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints. Any endpoint can be included or excluded independently and can be combined arbitrarily; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​1 and 2 are listed, and maximum range values ​​3, 4, and 5 are also listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0" and "5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when describing a parameter as an integer ≥ 2, it is equivalent to listing integers such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 for that parameter. For instance, when describing a parameter as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0044] In this application, unless otherwise specified, "about" means within a reasonable range above and below the stated number, and the range of fluctuation may vary depending on the type and value of the stated number. For example, a range of ±10%, ±5%, ±2%, ±1% is permissible. For instance, taking "about 20°C" as an example, where the approximation is ±1°C, approximate values ​​such as 19°C and 19.5°C within the approximation range indicated by "about 20°C" should also be included in the range indicated by "about 20°C".

[0045] In this application, the terms "multiple," "various," "multiple items," "several," etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more (greater than or equal to) two. It can be understood that when "any number of" items are involved, it refers to any suitable combination of multiple items, that is, a combination of "any number of" items in a manner that does not conflict and enables the implementation of this application.

[0046] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0047] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment or implementation of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. The term "implementation" as used herein has a similar understanding.

[0048] Those skilled in the art will understand that the order in which the steps are written in the methods of various embodiments or examples does not imply a strict execution order and does not constitute any limitation on the implementation process. The detailed execution order of each step should be determined by its function and possible internal logic. Unless otherwise specified, all steps of this application may be performed sequentially or randomly, but are preferably performed sequentially. For example, if method M includes steps (a) and (b), it means that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, method M may also include step (c), meaning that step (c) can be added to method M in any order. For example, method M may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0049] In this application, unless otherwise specified, M (e.g., m1) means that m1 is a non-limiting example of M, and it is understood that M is not limited to m1.

[0050] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it is selected from either "with" or "without." If multiple "options" appear in a technical solution, unless otherwise specified and there are no contradictions or mutual constraints, each "option" is independent. Unless otherwise specified, the descriptions such as "optionally include" and "optionally contain" in this application, taking "optionally include" as an example, mean "may include or not include."

[0051] In this document, the term "suitable" in phrases such as "suitable combination," "suitable method," and "any suitable method" refers to the technical solution that enables the implementation of this application.

[0052] In this application, the exemplary descriptions such as "in some implementations (or embodiments)" and "in one implementation (or embodiment)" may cover, but are not limited to, the following meanings: these solutions can be combined with other solutions in a suitable manner to form new technical solutions.

[0053] During the cycling process of ternary lithium-ion batteries, high-nickel ternary materials (NCM) undergo delithiation, specifically the transformation from a layered structure to a spinel structure, involving the transition metal ion Mn. 2+ Ni 2+ The lithium will dissolve in the electrolyte, generating byproducts. These byproducts migrate to the negative electrode, causing insufficient lithium insertion into the negative electrode and leading to performance degradation. This is the crosstalk problem in the ternary system. Furthermore, the fluorinated lithium salts in the electrolyte system react with H₂O to produce HF, causing interfacial corrosion and resulting in interfacial instability. The crosstalk problem and the HF-induced interfacial corrosion in the ternary system result in poor cycle performance of ternary lithium-ion batteries, failing to meet the needs of daily life.

[0054] In related technologies, in-situ solidification is often used to form gel electrolytes to improve crosstalk problems in ternary systems. Traditional in-situ solidification mainly includes free radical polymerization and cationic polymerization to form gel electrolytes. Free radical polymerization often uses AIBN as an initiator, which will react to produce N2, resulting in an increase in gas production in the system. Cationic polymerization mainly uses epoxy monomers. Epoxy monomers have low binding energy with H2O and do not have acid suppression function, so they cannot effectively suppress the interfacial corrosion problem caused by HF.

[0055] To address the aforementioned issues, this application adds one or more polymer monomers from ternary and quaternary nitrogen heterocyclic compounds to the electrolyte. After electrolyte injection into the battery assembly, H2O is generated in HF produced by the reaction of fluorinated lithium salt and H2O. + Under the influence of [the catalyst], polymer monomers polymerize to form a polymer skeleton, thereby effectively reducing the crosstalk problem of ternary materials and the interface corrosion problem of HF, and thus effectively improving the cycle performance of the ternary system.

[0056] One or more embodiments of this application provide a secondary battery comprising a gel electrolyte, the gel electrolyte comprising a polymer backbone and an electrolyte located within the polymer backbone, the electrolyte comprising a fluorinated lithium salt, and the raw material of the polymer backbone comprising polymer monomers, the polymer monomers comprising one or more of ternary nitrogen heterocyclic compounds and quaternary nitrogen heterocyclic compounds.

[0057] It should be noted that, in the context of this article, three-membered nitrogen heterocyclic compounds refer to compounds containing a three-membered nitrogen heterocyclic structure; and four-membered nitrogen heterocyclic compounds refer to compounds containing a four-membered nitrogen heterocyclic structure.

[0058] Understandably, selecting one or more of ternary and quaternary nitrogen heterocyclic compounds for polymerization is beneficial for forming a polymer framework with a three-dimensional network structure. The polymer framework in the gel electrolyte of this secondary battery then possesses a liquid-binding function, reducing direct contact between the electrolyte and the positive electrode and lowering the risk of oxidative decomposition. Simultaneously, the three-dimensional network structure of this polymer framework can confine the solvent, which is a carrier for the migration of transition metal ions. Slowing down the solvent movement slows down the movement of transition metal ions, thus the gel electrolyte can significantly inhibit the dissolution and free migration of transition metal ions in the positive electrode active material. Through these combined effects, the crosstalk problem of ternary materials can be effectively reduced. The raw material monomers of the polymer framework are amine compounds. Since the binding energy of amine compounds with H2O is higher than that between fluorinated lithium salts and H2O, the reaction between fluorinated lithium salts and H2O can be effectively inhibited. Therefore, the amount of HF generated can be effectively reduced, thus reducing the corrosion of the solid electrolyte interface film formed on the negative electrode surface by HF. Therefore, by adding a polymer backbone formed by one or more monomers of ternary and quaternary nitrogen heterocyclic compounds to the electrolyte, the crosstalk problem of ternary materials and the interfacial corrosion problem of HF can be effectively reduced, thereby effectively improving the cycle performance of the ternary system.

[0059] Without limitation, the structural characteristics of the polymer skeleton, the types of raw material monomers forming the polymer skeleton, and the mass ratio between different types of monomers mentioned in the context can be determined by nuclear magnetic resonance (NMR). The specific method is as follows: the secondary battery is disassembled to obtain a membrane with the polymer skeleton attached. The membrane with the polymer skeleton is centrifuged in ethanol. Since the electrolyte contained in the polymer skeleton is soluble in ethanol, and the polymer skeleton and membrane are insoluble in ethanol, the polymer skeleton and membrane can be separated by centrifugation in ethanol. Furthermore, since the polymer skeleton and membrane have different shapes, the polymer skeleton can be easily separated from the membrane, thus obtaining the polymer skeleton. The polymer skeleton is characterized by NMR testing and thermal decomposition GC-MS, for example, by determining the different NMR peak positions of different functional groups to identify the types of raw material monomers forming the polymer skeleton and the mass ratio between different types of monomers. The polymer skeleton is then tested by scanning electron microscopy (SEM) to observe its microstructure. In some embodiments, the polymer monomer includes one or more of aziridine, 2-methylaziridine, trimethylolpropane-tris[3-(2-methylaziridine)propionate], trimethylolpropane-tris(3-aziridine)propionate, 1-hydroxyethylaziridine, and aziridine and its derivatives.

[0060] In some of these embodiments, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine.

[0061] In some exemplary embodiments, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.4:1.6-4.1:0.9.

[0062] In some optional embodiments, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, with a mass ratio of 3.5:1.5 to 4:1. This mass ratio ensures a suitable polymer backbone network density, guaranteeing both liquid retention and proper lithium-ion conduction. Specifically, the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine can be, but is not limited to, 3.5:1.5, 4:1.5, 4.5:1.5, 5:1.5, 5.5:1.5, 6:1.5, or any range between two of the above ratios.

[0063] As one possible implementation, the polymer monomers include trimethylolpropane tris(3-acrylidinylpropionate) and 1-hydroxyethylaziridine.

[0064] In some alternative embodiments, the polymer monomers include trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane tris(3-acrididinylpropionate) to 1-hydroxyethylaziridine is 3.4:1.6-4.1:0.9.

[0065] In some embodiments, the polymer monomers include trimethylolpropane tris(3-acridinylpropionate) and 1-hydroxyethylaziridine, with a mass ratio of 3.5:1.5 to 4:1. By appropriately controlling the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine, a suitable polymer backbone network density can be ensured, guaranteeing both liquid retention and normal lithium-ion conduction. Specifically, the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine can be, but is not limited to, 3.5:1.5, 4:1.5, 4.5:1.5, 5:1.5, 5.5:1.5, 6:1.5, or any range between two of the above ratios.

[0066] As one possible implementation, the polymer monomers include 2-methylaziridine and trimethylolpropane-tris[3-(2-methylaziridine)propionate] (TTMAP).

[0067] In some alternative embodiments, the polymer monomers include 2-methylaziridine and trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP), wherein the mass ratio of 2-methylaziridine to trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) is (1-1.5):(1-3); for example, it can be, but is not limited to, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, or any range between two of the above ratios.

[0068] In some embodiments, the polymer backbone includes a cross-linked polymer with a degree of cross-linking of 0.4-0.8. When the degree of cross-linking of the cross-linked polymer is within the above range, the polymer backbone network density is moderate, ensuring both liquid retention and normal lithium-ion conduction. Specifically, the degree of cross-linking of the cross-linked polymer can be, but is not limited to, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, or any range between two of the above values.

[0069] As an example, the degree of crosslinking of the crosslinked polymer mentioned in the context can be determined using nuclear magnetic resonance (NMR). The specific method is as follows: The secondary battery is disassembled to obtain a membrane with a polymer backbone attached. The membrane with the polymer backbone is centrifuged in ethanol. Since the electrolyte contained in the polymer backbone is soluble in ethanol, and the polymer backbone and membrane are insoluble in ethanol, centrifugation in ethanol can separate the polymer backbone and membrane. Furthermore, because the polymer backbone and membrane have different shapes, the polymer backbone can be easily separated from the membrane, thus obtaining the polymer backbone. NMR testing is performed on the polymer backbone. Different components within the polymer backbone have different relaxation kinetics; for example, monomer or solvent components are highly mobile and decay the slowest. Non-crosslinked segments have certain molecular motion characteristics and decay relatively slowly. Crosslinked segments are more bound and have less molecular motion characteristics, decaying faster. Therefore, by acquiring the signal of the entire polymer and calculating the proportion of the crosslinked portion, the degree of crosslinking of the polymer backbone can be obtained.

[0070] As one possible implementation, the fluorinated lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium difluorophosphate.

[0071] In some embodiments, the solvent may include fluoroethylene carbonate (FEC), ethylene carbonate (EC), ), propylene carbonate (PC, One or more of the following: ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and 1,4-butyrolactone (GBL).

[0072] The electrolyte also contains an electrolyte salt, including a fluorinated lithium salt. In some alternative embodiments, the concentration of the fluorinated lithium salt is typically 0.5-5 mol / L.

[0073] In some embodiments, the electrolyte may optionally include other additives. For example, it may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.

[0074] In some embodiments, the additives in the electrolyte may include, but are not limited to, one or more of fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethyl ethylene carbonate (TFPC), etc.

[0075] As one possible implementation method, the secondary battery is a lithium-ion secondary battery.

[0076] In some embodiments, the secondary battery further includes a positive electrode sheet, which includes a positive active material layer comprising lithium nickel cobalt manganese oxide.

[0077] In some embodiments, the secondary battery further includes a negative electrode sheet, which includes a negative electrode active material layer containing graphite.

[0078] In some embodiments, the secondary battery further includes a positive electrode and a negative electrode. The positive electrode includes a positive active material layer containing lithium nickel cobalt manganese oxide. The negative electrode includes a negative active material layer containing graphite.

[0079] Non-limiting examples of lithium nickel cobalt manganese oxides may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 )wait.

[0080] As one possible implementation, the chemical formula of the lithium nickel cobalt manganese oxide is Li 1+d [Ni x Co y Mn z M w O 2+f Wherein, -0.2≤d≤0.2, x+y+z+w=1, 0.5≤x<1, 0≤y<0.3, 0.5≤z<1, 0≤w<0.3, -0.5≤f≤0.5, and M includes one or more of Zr, Al, Ti, Sb, Nb, Te, Mg, B, Ca, V, Ta or Sr.

[0081] Understandably, lithium (Li) is intercalated and deintercalated during the charging and discharging process of a battery, and the Li content in the positive electrode varies depending on the state of discharge. In the examples of positive electrode active materials listed in this application, unless otherwise specified, the Li content refers to the initial state of the material. When positive electrode active materials are applied to the positive electrode in a battery system, the Li content in the positive electrode active material typically changes after charge-discharge cycles. The Li content can be measured using molar content, but is not limited to this. Regarding "Li content refers to the initial state of the material," the initial state of the material refers to its state before being added to the positive electrode slurry. It is understood that new materials obtained by appropriately modifying the listed positive electrode active materials are also within the scope of positive electrode active materials. The aforementioned appropriate modification refers to acceptable modification methods for the positive electrode material; non-limiting examples include coating modification.

[0082] In the examples of positive electrode active materials in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause changes in the molar content of oxygen, and the actual O content will fluctuate. The O content can be measured in molar content, but is not limited to this.

[0083] One or more embodiments of this application provide a method for preparing a secondary battery, which can be used to prepare the aforementioned secondary battery. The preparation method includes the following steps: preparing an electrolyte containing polymer monomers, the electrolyte containing a fluorinated lithium salt; injecting the electrolyte into an electrode assembly, and allowing it to stand to allow the polymer monomers to form a polymer skeleton with a three-dimensional network structure, thereby preparing the secondary battery; wherein the polymer monomers include one or more of ternary nitrogen heterocyclic compounds and quaternary nitrogen heterocyclic compounds.

[0084] In the above preparation method, after the electrolyte is injected into the electrode assembly, H is generated in HF produced by the reaction of fluorine-containing lithium salt and H2O. + Under the influence of [the specific chemical process], polymer monomers can polymerize to form a polymer skeleton with a three-dimensional network structure. This polymer skeleton has a liquid binding function, reducing direct contact between the electrolyte and the positive electrode and lowering the risk of oxidative decomposition. Simultaneously, the three-dimensional network structure of this polymer skeleton can bind the solvent to a certain extent. Since the solvent is a carrier for the migration of transition metal ions, slowing down the solvent movement also slows down the movement of transition metal ions. Therefore, the gel electrolyte can significantly inhibit the dissolution and free migration of transition metal ions. Through these combined effects, the crosstalk problem of ternary materials can be effectively reduced. Furthermore, the polymer monomers in the electrolyte are amine compounds. Since the binding energy of amine compounds with H₂O is higher than that between fluorinated lithium salts and H₂O, the reaction between fluorinated lithium salts and H₂O can be effectively inhibited. This can effectively reduce the amount of HF generated and reduce the corrosion of the solid electrolyte interfacial film on the negative electrode surface by HF. In summary, by adding polymer monomers to the electrolyte, the crosstalk problem of ternary materials and the interfacial corrosion problem of HF can be effectively reduced, thereby effectively improving the cycle performance of the ternary system.

[0085] As a non-limiting example, the polymerization mechanism of polymer monomers is as follows:

[0086]

[0087] Understandably, the secondary battery prepared by this method has similar technical solutions and advantages to the aforementioned secondary batteries, and will not be repeated here.

[0088] As one possible implementation, the fluorinated lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium difluorophosphate.

[0089] In some embodiments, the settling time is 24-36 hours. Appropriately controlling the settling time facilitates the wetting of the electrode by the electrolyte before the formation of the polymer skeleton. Specifically, the settling time can be, but is not limited to, 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, 36 hours, or any range between two of the above times.

[0090] As one possible implementation, the polymer monomer includes one or more of aziridine, 2-methylaziridine, trimethylolpropane-tris[3-(2-methylaziridine)propionate], trimethylolpropane-tris(3-aziridine)propionate, 1-hydroxyethylaziridine, and aziridine and its derivatives.

[0091] In an alternative embodiment, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine.

[0092] In some embodiments, the polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.4:1.6-4.1:0.9.

[0093] Furthermore, the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.5:1.5-4:1. This mass ratio ensures a suitable polymer backbone network density, guaranteeing both liquid retention and proper lithium-ion conduction. Specifically, the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine can be, but is not limited to, 3.5:1.5, 4:1.5, 4.5:1.5, 5:1.5, 5.5:1.5, 6:1.5, or any range between two of the above ratios.

[0094] In some embodiments, the polymer monomers include trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine.

[0095] In some alternative embodiments, the polymer monomers include trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane tris(3-acrididinylpropionate) to 1-hydroxyethylaziridine is 3.4:1.6-4.1:0.9.

[0096] Furthermore, the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine is 3.5:1.5-4:1. Reasonably controlling the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine ensures a moderate polymer backbone network density, guaranteeing both liquid retention and normal lithium-ion conduction. Specifically, the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine can be, but is not limited to, 3.5:1.5, 4:1.5, 4.5:1.5, 5:1.5, 5.5:1.5, 6:1.5, or any range between two of the above ratios.

[0097] In some embodiments, the polymer monomers include 2-methylaziridine and trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP). Further, the mass ratio of 2-methylaziridine to trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) is (1-1.5):(1-3); for example, it can be, but is not limited to, 1:3, 1:2.5, 1:2, 1:1.5, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, or any range between two of the above ratios.

[0098] In one possible implementation, the electrolyte includes a solvent, and the percentage of the polymer monomer's mass relative to the solvent's mass is 0.5%-2%; for example, it can be, but is not limited to, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or any range between any two of the above values. Reasonably controlling the percentage of the polymer monomer's mass relative to the mass of the solvent contained in the electrolyte can ensure a moderate polymer backbone network density, guaranteeing both the polymer backbone's liquid retention capacity and the normal conduction of lithium ions.

[0099] In some alternative embodiments, the electrolyte comprises a solvent, wherein the mass percentage of the polymer monomer relative to the mass of the solvent is 1%-2%.

[0100] One or more embodiments of this application provide an electrical device, including at least one of the above-described secondary battery and a secondary battery prepared by the above-described secondary battery preparation method.

[0101] The secondary battery and power-consuming device of this application will be described below with appropriate reference to the accompanying drawings.

[0102] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions move back and forth between the positive and negative electrodes, inserting and releasing. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing ions to pass through.

[0103] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer includes a positive active material.

[0104] The positive electrode active material accounts for 80-100% by weight in the positive electrode active material layer, based on the total weight of the positive electrode active material layer.

[0105] In some embodiments, the positive electrode active material layer may optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins. The binder accounts for 0-20% by weight of the positive electrode active material layer, based on the total weight of the positive electrode active material layer.

[0106] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The conductive agent accounts for 0-20% by weight of the positive electrode active material layer, based on the total weight of the positive electrode active material layer.

[0107] In some embodiments, the positive electrode sheet can be prepared by dispersing the components used to prepare the positive electrode sheet, such as the positive electrode active material, conductive agent, binder, and any other components, in a solvent to form a positive electrode slurry. The positive electrode slurry is then coated onto at least one surface of the positive electrode current collector. After drying, cold pressing, and other processes, the positive electrode sheet is obtained. Cold pressing can be performed using a cold rolling mill. The solvent can be selected from, but is not limited to, any of the solvents described in the foregoing embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode current collector coated with the positive electrode slurry can be a single surface or both surfaces of the positive electrode current collector. The solid content of the positive electrode slurry can be 40wt%~80wt%. The viscosity of the positive electrode slurry at room temperature can be adjusted to 5000-25000 mPa·s. When coating the positive electrode slurry, the coating areal density (dry weight, minus solvent) can be 15-35 mg / cm³. 2 The compaction density of the positive electrode sheet can be 3.0-3.6 g / cm³. 3 The selectable value is 3.3-3.5 g / cm³. 3 .

[0108] The formula for calculating the compaction density is:

[0109] Compacted density = Coated surface density / (Cold-pressed electrode thickness - Current collector thickness).

[0110] The negative electrode sheet includes a negative current collector and a negative active material layer disposed on at least one surface of the negative current collector, wherein the negative active material layer includes a negative active material.

[0111] As a non-limiting example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode active material layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0112] The weight ratio of the negative electrode active material in the negative electrode active material layer can be 70-100% by weight, based on the total weight of the negative electrode active material layer.

[0113] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on the polymer material substrate. The metal material may include, but is not limited to, copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys, etc., and the polymer material substrate may include, but is not limited to, one or more of the following substrates: polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0114] In some embodiments, the negative electrode active material layer may optionally include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). The binder may constitute 0-30% by weight of the negative electrode active material layer, based on the total weight of the negative electrode active material layer.

[0115] In some embodiments, the negative electrode active material layer may optionally include a conductive agent. The conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight percentage of the conductive agent in the negative electrode active material layer may be 0-20% by weight, based on the total weight of the negative electrode active material layer.

[0116] In some embodiments, the negative electrode active material layer may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)). The weight percentage of the other additives in the negative electrode active material layer may be 0-15% by weight, based on the total weight of the negative electrode active material layer.

[0117] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder, and any other components, in a solvent (a non-limiting example of a solvent is deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto at least one surface of a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing, and other processes. The surface of the negative electrode current collector coated with the negative electrode slurry can be a single surface of the negative electrode current collector or both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt%-60wt%. The compaction density of the negative electrode sheet can be 1.0 g / cm3-1.8 g / cm3. The solid content of the negative electrode slurry can be 30-70wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000-10000 mPa·s. When coating the negative electrode slurry, the coating unit areal density (excluding solvent) on a dry weight basis can be 75-220 g / m3. 2 The compacted density of the negative electrode sheet can be 1.2-2.0 g / cm³. 3 .

[0118] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.

[0119] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.

[0120] In some embodiments, the thickness of the isolation membrane is 6-40 μm, optionally 12-20 μm.

[0121] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.

[0122] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the electrode assembly and electrolyte described above.

[0123] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch-type soft pack. The material of the soft pack can be plastic; further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0124] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.

[0125] In this application, unless otherwise specified, "cell battery" refers to the basic unit capable of converting chemical energy into electrical energy, and generally includes at least a positive electrode, a negative electrode, and an electrolyte. During the charging and discharging process of the battery, active ions move back and forth between the positive and negative electrode plates, inserting and extracting. The electrolyte acts as a conductor for the active ions between the positive and negative electrode plates.

[0126] This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 1 The example shown is a square-structured battery cell 5.

[0127] In some implementations, refer to Figure 2 The outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 can be placed over the opening to close the receiving cavity. The positive electrode sheet, negative electrode sheet, and separator can be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, which can be selected by those skilled in the art according to actual needs.

[0128] The secondary battery can be either battery module 4 or battery pack 1.

[0129] A battery module includes at least one battery cell. The number of battery cells in a battery module can be one or more, and those skilled in the art can select an appropriate number based on the application and capacity of the battery module.

[0130] Figure 3 This is battery module 4, used as an example. (See reference...) Figure 3 In battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.

[0131] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0132] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the battery pack may contain one or more battery modules. Those skilled in the art can select an appropriate number based on the application and capacity of the battery pack.

[0133] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0134] In addition, this application also provides an electrical device, which includes the secondary battery provided in this application. The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0135] As the electrical device, a secondary battery can be selected according to its usage requirements.

[0136] Figure 6 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.

[0137] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.

[0138] The following describes some embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where the technology or conditions are not specified in the embodiments, they are performed according to the description above, or according to the technology or conditions described in the literature in this field, or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially, or can be synthesized from commercially available products using conventional methods.

[0139] Preparation of primary and secondary batteries

[0140] Example 1

[0141] Step S1: Mix ethylene carbonate (EC), diethyl carbonate (DEC), and dimethyl carbonate (DMC) in a volume ratio of 1:1:1, and then add 0.5% of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) by mass of the total solvent to dissolve LiPF6 in the solution to obtain a 1 mol / L LiPF6 electrolyte.

[0142] Step S2, LiNi 0.9 Co 0.05 Mn 0.05 O2 (NCM) 9 / 0.5 / 0.5 Conductive carbon black and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 9:0.5:0.5, and then N-methylpyrrolidone solvent was added. The mixture was stirred until homogeneous to obtain a positive electrode slurry with a solid content of 60%. The positive electrode slurry was then uniformly coated on both sides of an aluminum foil, with a coating surface density of 3.5 g / cm³. 2 After cold pressing and cutting, the positive electrode sheet is obtained.

[0143] Step S3: Mix artificial graphite, conductive carbon black, sodium carboxymethyl cellulose, and styrene-butadiene rubber in a mass ratio of 9.5:0.2:0.15:0.15, then add deionized water and stir until homogeneous to obtain a negative electrode slurry with a solid content of 65%. Coat both sides of the copper foil with the negative electrode slurry evenly, achieving a coating density of 1.65 g / cm³. 2 After cold pressing and cutting, the negative electrode sheet is obtained.

[0144] Step S4: Arrange the electrodes in the order of "separator-negative electrode-separator-positive electrode". Fix one end of the positive electrode, negative electrode, and two separators to the discharge roller. Stack the other ends together and fix them to the winding shaft. Use a motor to rotate the winding shaft to wind the positive electrode, negative electrode, and two separators, obtaining a wound electrode assembly. Inject the electrolyte prepared in step S1 into the wound electrode assembly at an injection rate of 2.2 g / Ah. After injection, allow the battery to stand at room temperature for 24 hours to complete the battery preparation. The battery capacity is 4Ah. The separator used is a PE separator.

[0145] Example 2

[0146] The preparation methods of Example 2 and Example 1 are similar, except that the amount of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) in step S1 of Example 2 is 1%, while the others are the same.

[0147] Example 3

[0148] The preparation methods of Example 3 and Example 1 are similar, except that the amount of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) in step S1 of Example 3 is 2%, and all other steps are the same.

[0149] Example 4

[0150] The preparation methods of Example 4 and Example 3 are similar, except that in step S1 of Example 4, the same mass of trimethylolpropane tris(3-acrididinylpropionate) is used instead of trimethylolpropane-tris[3-(2-methylacrididinyl)propionate](TTMAP), and all other steps are the same.

[0151] Example 5

[0152] The preparation methods of Example 5 and Example 3 are similar, except that in step S1 of Example 5, 2-methylaziridine and trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) are used together, and the amounts of 2-methylaziridine and trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) are 1% each.

[0153] Example 6

[0154] The preparation methods of Example 6 and Example 3 are similar, except that in step S1 of Example 6, trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are 1.6% and 0.4%, respectively.

[0155] Example 7

[0156] The preparation methods of Example 7 and Example 3 are similar, except that in step S1 of Example 7, trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are 1.4% and 0.6%, respectively.

[0157] Example 8

[0158] The preparation methods of Example 8 and Example 3 are similar, except that in step S1 of Example 8, trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are 1.36% and 0.64%, respectively.

[0159] Example 9

[0160] The preparation methods of Example 9 and Example 3 are similar, except that in step S1 of Example 9, trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) and 1-hydroxyethylaziridine are 1.64% and 0.36%, respectively.

[0161] Example 10

[0162] The preparation methods of Example 10 and Example 3 are similar, except that in step S1 of Example 10, trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are 1.6% and 0.4%, respectively.

[0163] Example 11

[0164] The preparation methods of Example 11 and Example 3 are similar, except that in step S1 of Example 11, trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are 1.4% and 0.6%, respectively.

[0165] Example 12

[0166] The preparation methods of Example 12 and Example 3 are similar, except that in step S1 of Example 12, trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are 1.36% and 0.64%, respectively.

[0167] Example 13

[0168] The preparation methods of Example 13 and Example 3 are similar, except that in step S1 of Example 13, trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are used together, and the amounts of trimethylolpropane tris(3-acrididinylpropionate) and 1-hydroxyethylaziridine are 1.64% and 0.36%, respectively.

[0169] Example 14

[0170] The preparation methods of Example 14 and Example 1 are similar, except that the amount of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) in step S1 of Example 14 is 2.1%, and all other steps are the same.

[0171] Example 15

[0172] The preparation methods of Example 15 and Example 1 are similar, except that the amount of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) in step S1 of Example 15 is 0.4%, and all other steps are the same.

[0173] Comparative Example 1

[0174] The preparation methods of Comparative Example 1 and Example 1 are similar, except that Trimethylolpropane-tris[3-(2-methylacridinyl)propionate] (TTMAP) was not added in Comparative Example 1, while all other methods are the same.

[0175] Comparative Example 2

[0176] The preparation methods of Comparative Example 2 and Comparative Example 1 are similar, except that 0.5% of fluoroethylene carbonate (FEC) is added to Comparative Example 2, while all other aspects are the same.

[0177] Comparative Example 3

[0178] The preparation methods of Comparative Example 3 and Comparative Example 1 are similar, except that 1% of fluoroethylene carbonate (FEC) is added to Comparative Example 3, while all other aspects are the same.

[0179] Comparative Example 4

[0180] The preparation methods of Comparative Example 4 and Comparative Example 1 are similar, except that 2% of fluoroethylene carbonate (FEC) is added to Comparative Example 4, while all other aspects are the same.

[0181] The differences between the above embodiments and comparative examples are shown in Table 1.

[0182] Table 1

[0183]

[0184] The total amount of polymer monomers refers to the percentage of the total mass of polymer monomers relative to the total mass of solvent in the electrolyte.

[0185] The method for testing the degree of crosslinking of the polymer backbone is as follows: The secondary battery is disassembled to obtain a membrane with a polymer backbone attached. The membrane with the polymer backbone is centrifuged in 97% ethanol (by mass percentage) to allow the electrolyte solution contained in the polymer backbone to dissolve in the ethanol, thus obtaining the polymer backbone and the membrane. Based on the different shapes of the polymer backbone and the membrane, the polymer backbone is separated from the membrane to obtain the polymer backbone. Nuclear magnetic resonance (NMR) testing is performed on the polymer backbone at a frequency of 21 MHz. The entire polymer signal is acquired, and the proportion of the crosslinked portion signal is calculated using fitting software to obtain the degree of crosslinking of the polymer backbone. The crosslinking network diagram of the polymer backbone measured in Example 1 is shown below. Figure 7 As shown, Figure 7 In this diagram, 'a' represents a cross-linked chain, 'b' a dangling chain, and 'c' a free chain (i.e., a solvated segment). Figure 7 It can be seen that the polymer backbone contains cross-linked chains and a cross-linked network.

[0186] II. Performance Testing

[0187] 1. The electrolytes obtained in step S1 of the above embodiments and comparative examples were subjected to acidity testing. The testing method was as follows: the electrolytes were allowed to stand at room temperature for 10 hours, and then the acidity value was tested using a pH meter at a testing temperature of 25°C. The test results of the above embodiments and comparative examples are shown in Table 2.

[0188] 2. Cyclic performance test

[0189] A 4 Ah secondary battery was charged to 4.25 V at a rate of 0.5C at 25℃, and then discharged to 2.5 V at a rate of 0.5C. This cycle test was repeated 200 times, and the capacity retention rate was calculated. The test results are shown in Table 2.

[0190] 3. The secondary battery, after undergoing 200 charge-discharge cycles as described in "2. Cyclic Performance Testing," was disassembled and subjected to inductively coupled plasma mass spectrometry (ICP) to monitor the Ni content of the transition metal element on the graphite surface. The test method is as follows:

[0191] a. Sample preparation: Take an appropriate amount of sample from the negative electrode plate, place the sample in a porcelain crucible, add a mixture of hydrochloric acid and nitric acid with a mass ratio of 4:1 to dissolve the sample; heat until the sample is completely dissolved, cool and bring the volume to 50 mL, then filter using a filter membrane to obtain the sample to be tested.

[0192] b. Preparation of standard solutions: Prepare Ni standard solutions of different concentrations, namely 10 μg / mL, 20 μg / mL, 50 μg / mL and 100 μg / mL, and make up to 50 mL with a mixture of hydrochloric acid and nitric acid in a mass ratio of 4:1.

[0193] c. ICP Analysis: Turn on the ICP instrument and set the operating parameters (RF power 27.12MHz, nebulizer gas flow 0.92L / min) to ensure the instrument is stable. Inject Ni standard solutions sequentially and measure their spectral intensity (selecting the characteristic spectral line of Ni at 318.35 nm), then plot a concentration-intensity standard curve. Inject the prepared sample solution into the ICP instrument and measure its spectral intensity. Calculate the Ni content in the sample using the standard curve. Calculate the mass fraction of Ni in the sample using the following formula:

[0194] The mass fraction of Ni (nickel) = the mass of Ni (g) / the total mass of the sample (g).

[0195] The test results are shown in Table 2.

[0196] Table 2

[0197]

[0198] As shown in Table 2, the introduction of polymer monomers in this application can effectively reduce the acidity of the electrolyte. This is mainly because the binding energy between the polymer monomer and water is higher than that between the fluorinated lithium salt and water, thereby effectively inhibiting the reaction between the fluorinated lithium salt and water and reducing the generation of HF. A comparison of the results from Examples 1-3 shows that when the mass percentage of the polymer monomer relative to the mass of the solvent in the electrolyte is 0.5%-2%, the acidity of the electrolyte decreases with increasing polymer monomer content.

[0199] As shown in Table 2 regarding the Ni content, the introduction of polymer monomers in this application effectively suppresses crosstalk. Furthermore, compared to the addition of fluoroethylene carbonate (FEC), the addition of polymer monomers in this application demonstrates a superior effect in mitigating crosstalk. This is primarily because the polymer monomers in this application can undergo cationic polymerization in the electrolyte system to form a polymer backbone. The liquid-binding function of the polymer backbone effectively suppresses crosstalk. A comparison of the results from Examples 1-3 shows that the content of transition metal elements decreases with increasing polymer monomer dosage, indicating that the improvement in crosstalk becomes more significant with increasing polymer monomer dosage.

[0200] As shown in Table 2, the introduction of polymer monomers in this application can effectively improve the cycle performance of the battery. Furthermore, compared with the addition of fluoroethylene carbonate (FEC), the addition of polymer monomers in this application has a better effect on improving cycle performance. This is mainly due to the suppression of HF and the improvement of crosstalk issues by the polymer monomers in this application. A comparison of the results from Examples 1-3 shows that the cycle capacity retention rate increases with the increase of polymer monomer dosage; indicating that the suppression of HF and the improvement of crosstalk issues become more significant with the increase of polymer monomer dosage.

[0201] The descriptions of the various implementation methods and embodiments above tend to emphasize the differences between them. Similarities or resemblances can be referenced interchangeably, and for the sake of brevity, they will not be repeated here. The technical features of the implementation methods and embodiments described above can be combined arbitrarily. For the sake of brevity, not all possible combinations of the technical features in the above embodiments have been described. However, as long as the combinations of these technical features do not contradict each other, they should be considered within the scope of this specification.

[0202] It should be noted that this application is not limited to the above-described embodiments and examples. The above-described embodiments and examples are merely examples, and any embodiments and examples that have the same structure and achieve the same effect as the technical concept within the scope of this application are included in the technical scope of this application. The embodiments and examples described above only illustrate several embodiments and examples of this application, and although the descriptions are relatively detailed, they should not be construed as limiting the scope of the patent. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments or examples, and other ways of constructing embodiments or examples by combining some of the constituent elements of the embodiments or examples, are also included in the scope of this application without departing from the spirit of this application.

Claims

1. A secondary battery, characterized in that, The secondary battery includes a gel electrolyte comprising a polymer backbone and an electrolyte located within the polymer backbone. The electrolyte contains a fluorinated lithium salt. The raw material of the polymer backbone includes polymer monomers, which include one or more of ternary nitrogen heterocyclic compounds and quaternary nitrogen heterocyclic compounds.

2. The secondary battery as described in claim 1, characterized in that, The polymer monomers include one or more of aziridine, 2-methylaziridine, trimethylolpropane-tris[3-(2-methylaziridine)propionate], trimethylolpropane-tris(3-aziridine)propionate, 1-hydroxyethylaziridine, and aziridine and its derivatives.

3. The secondary battery as described in claim 1 or 2, characterized in that, The polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.5:1.5-4:

1.

4. The secondary battery as described in claim 1 or 2, characterized in that, The polymer monomers include trimethylolpropane tris(3-acridinylpropionate) and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine is 3.5:1.5-4:

1.

5. The secondary battery according to any one of claims 1 to 4, characterized in that, The polymer backbone includes a cross-linked polymer with a degree of cross-linking of 0.4-0.

8.

6. The secondary battery according to any one of claims 1 to 5, characterized in that, The fluorinated lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, and lithium difluorophosphate.

7. The secondary battery according to any one of claims 1 to 6, characterized in that, The secondary battery is a lithium-ion secondary battery.

8. The secondary battery according to any one of claims 1 to 7, characterized in that, The secondary battery further includes a positive electrode and a negative electrode. The positive electrode includes a positive active material layer containing lithium nickel cobalt manganese oxide. The negative electrode includes a negative active material layer containing graphite.

9. The secondary battery as described in claim 8, characterized in that, The chemical formula of the lithium nickel cobalt manganese oxide is Li 1+d [Ni x Co y Mn z M w ]O 2+f Wherein, -0.2≤d≤0.2, x+y+z+w=1, 0.5≤x<1, 0≤y<0.3, 0.5≤z<1, 0≤w<0.3, -0.5≤f≤0.5, and M includes one or more of Zr, Al, Ti, Sb, Nb, Te, Mg, B, Ca, V, Ta or Sr.

10. A method for preparing a secondary battery, characterized in that, Includes the following steps: An electrolyte comprising a polymer monomer is prepared, the electrolyte comprising a fluorinated lithium salt; the polymer monomer comprising one or more of ternary nitrogen heterocyclic compounds and quaternary nitrogen heterocyclic compounds; The electrolyte is injected into the electrode assembly and left to stand so that the polymer monomers form a polymer skeleton with a three-dimensional network structure, thereby preparing the secondary battery.

11. The preparation method according to claim 10, characterized in that, The settling time is 24-36 hours.

12. The preparation method according to any one of claims 10 to 11, characterized in that, The electrolyte includes a solvent, and the mass percentage of the polymer monomer relative to the mass of the solvent is 0.5%-2%.

13. The preparation method according to claim 12, characterized in that, The electrolyte includes a solvent, and the mass percentage of the polymer monomer relative to the mass of the solvent is 1%-2%.

14. The preparation method according to any one of claims 10 to 13, characterized in that, The preparation method includes one or more of the following conditions: (1) The polymer monomers include one or more of aziridine, 2-methylaziridine, trimethylolpropane-tris[3-(2-methylaziridine)propionate], trimethylolpropane-tris(3-aziridine)propionate, 1-hydroxyethylaziridine, and aziridine and its derivatives; (2) The polymer monomers include trimethylolpropane-tris[3-(2-methylacridinyl)propionate] and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane-tris[3-(2-methylacridinyl)propionate] to 1-hydroxyethylaziridine is 3.5:1.5-4:1; (3) The polymer monomers include trimethylolpropane tris(3-acridinylpropionate) and 1-hydroxyethylaziridine, wherein the mass ratio of trimethylolpropane tris(3-acridinylpropionate) to 1-hydroxyethylaziridine is 3.5:1.5-4:1; (4) The fluorinated lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate and lithium difluorophosphate.

15. An electrical appliance, characterized in that, It includes at least one of the secondary batteries according to any one of claims 1 to 9 and the secondary batteries prepared by the preparation methods of any one of claims 10 to 14.