A class of weakly solvated electrolytes for achieving high performance in lithium-ion batteries and their applications

By constructing a combined system of lithium salt, solvent, and flame retardant, the shortcomings of weakly solvated electrolytes in long-term cycle stability and needle penetration safety performance are solved, achieving high capacity, long life and wide temperature range battery safety under high voltage, and significantly reducing the overall safety risk of the battery.

CN123073166APending Publication Date: 2026-11-10SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611087128.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-21
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing weakly solvated electrolytes are difficult to balance in terms of long-term cycle stability and needle penetration safety when matched with electrode materials. Furthermore, traditional carbonate electrolytes are flammable and hot under extreme conditions, resulting in insufficient battery safety.

Method used

An electrolyte system with both high electrochemical performance and high safety was constructed by using a combination of lithium salt, solvent, and flame retardant, including aliphatic fluorinated ether-ester compounds and aromatic fluorinated ether-ester compounds as solvents, carbonate compounds and sulfate compounds as co-solvents, and cyclic phosphazene flame retardants and phosphate ester flame retardants as flame retardants.

Benefits of technology

It maintains high capacity and long lifespan under high voltage, while effectively suppressing thermal runaway and combustion under extreme operating conditions, achieving dual safety protection and improving the overall safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073166A_ABST
    Figure CN123073166A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of lithium battery electrolyte technology, specifically relating to a type of weakly solvated electrolyte for achieving high performance in lithium-ion batteries and its applications. The weakly solvated electrolyte of this invention comprises lithium salt, solvent, and co-solvent, and may also include a flame retardant, providing a battery-grade, highly safe lithium salt-solvent-co-solvent-flame retardant combination system. This electrolyte not only significantly improves the overall safety performance of lithium batteries, but also enables high-energy-density lithium-ion batteries to maintain high capacity, long lifespan, fast charging rate, and a wide operating temperature range under high-voltage (greater than 4.2 V) charging cutoff voltage, thus having broad application value in flame-retardant lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium battery electrolyte technology. More specifically, it relates to a class of weakly solvated electrolytes for achieving high performance in lithium-ion batteries and their applications. Background Technology

[0002] Traditional commercial carbonate electrolytes for lithium-ion batteries typically use lithium hexafluorophosphate as the conductive salt and ethylene carbonate (EC), ethyl methyl carbonate, and dimethyl carbonate as the main carbonate solvents. This system has significant performance limitations: EC has strong coordination capabilities, resulting in a high desolvation energy barrier for lithium ions, limiting the battery's charge rate performance; simultaneously, lithium hexafluorophosphate has poor high-temperature stability, and the high melting point of EC further narrows the electrolyte's operating temperature range. In terms of safety, the large amount of organic solvent imparts high flammability to the electrolyte, and under extreme conditions such as puncture, overheating, and overcharging, the electrolyte is prone to strong exothermic side reactions with the positive and negative electrode materials, inducing battery thermal runaway. Therefore, the flammability of the electrolyte and its high reactivity with electrode materials are core factors restricting battery safety performance.

[0003] To improve safety, researchers have attempted to add phosphorus-containing flame retardants to the electrolyte to suppress combustion. However, flame retardants typically interfere with the stable formation of the solid electrolyte interphase (SEI) film on the graphite anode surface, leading to a significant decrease in reversible capacity and cycle life. Furthermore, even ignoring flame retardancy issues, the intrinsic safety of the battery (such as needle penetration safety) depends on the exothermic reaction characteristics of the electrolyte and electrode materials under abnormal operating conditions. Traditional carbonate systems, even without the addition of flame retardants, still exhibit significant exothermic behavior from both the electrolyte and the electrode.

[0004] In recent years, weakly solvated electrolytes have attracted attention as an emerging field. These systems utilize solvents with weak coordination capabilities, allowing the lithium-ion solvation sheath to be dominated by anions, which is beneficial for forming an inorganic-rich SEI and provides a potential pathway to improve interfacial stability. However, existing weakly solvated electrolyte systems still have significant shortcomings in achieving battery safety: on the one hand, even though this system helps form a more stable SEI, its compatibility with high-voltage cathode materials is still insufficient, and there is still considerable room for improvement in the capacity retention rate of the full battery during long-term cycling; on the other hand, existing research focuses mainly on performance under normal cycling conditions, lacking a systematic investigation of the thermal reaction behavior of the electrolyte and electrode materials under extreme conditions (such as nail penetration), resulting in the intrinsic safety advantages of this type of electrolyte not being fully explored and verified.

[0005] In summary, under current technological conditions, no weakly solvated electrolyte system has been reported that can simultaneously possess excellent electrochemical performance (especially good cycle stability) and good intrinsic safety characteristics (i.e., mild exothermic reaction with electrode materials under abnormal operating conditions). This leaves high-energy-density lithium-ion batteries lacking an effective electrolyte solution when simultaneously pursuing high specific capacity, long cycle life, and reliable electrochemical abuse safety (such as needle penetration safety). Summary of the Invention

[0006] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing weak solvation electrolyte in terms of long-term cycle stability and needle penetration safety performance that are difficult to achieve when matched with electrode materials, and to provide a weak solvation electrolyte for lithium batteries.

[0007] The purpose of this invention is to provide the application of the weakly solvated electrolyte for lithium batteries in the preparation of lithium-ion batteries.

[0008] Another object of the present invention is to provide a lithium-ion battery.

[0009] The above-mentioned objective of this invention is achieved through the following technical solution: This invention protects a weakly solvated electrolyte for lithium batteries, the weakly solvated electrolyte for lithium batteries comprising lithium salt, solvent, co-solvent, and flame retardant; The solvent is an aliphatic fluorinated ether-ester compound and / or an aromatic fluorinated ether-ester compound; The co-solvent is a carbonate compound and / or a sulfate compound; The flame retardant is at least one of cyclic phosphazene flame retardants, phosphate ester flame retardants, and phosphite ester flame retardants; The lithium salt accounts for 10% to 25% of the mass of the weakly solvated electrolyte in the lithium battery. The solvent accounts for 40% to 85% of the mass of the weakly solvated electrolyte in lithium batteries. The co-solvent accounts for 5% to 40% of the mass of the weakly solvated electrolyte for lithium batteries. The flame retardant accounts for 0% to 35% of the mass of the weakly solvated electrolyte in the lithium battery.

[0010] The lithium-ion battery weakly solvated electrolyte of this invention comprises lithium salt, solvent, and co-solvent, and flame retardant can be added as needed to construct a synergistic system of lithium salt-solvent-flame retardant-co-solvent that combines high electrochemical performance and high safety. It is worth emphasizing that even without the addition of flame retardant, this electrolyte system can pass the nail penetration safety test, demonstrating that it can effectively suppress thermal runaway under external mechanical abuse (such as internal short circuits caused by nail penetration), significantly reducing the overall safety risk of the battery. Furthermore, if a flame retardant is introduced, the electrolyte not only still meets the nail penetration safety requirements but also effectively resists external combustion caused by open flames, achieving dual safety protection from "internal short circuit protection" to "external fire source resistance." Simultaneously, this electrolyte maintains high capacity, long lifespan, fast charging rate, and a wide operating temperature range even under high-voltage (>4.2 V) charging cutoff conditions, making it highly valuable for applications in lithium-ion batteries.

[0011] Preferably, the lithium salt accounts for 12% to 20% of the mass of the weakly solvated electrolyte in the lithium battery; The solvent accounts for 50% to 66% of the mass of the weakly solvated electrolyte in lithium batteries. The co-solvent accounts for 5% to 20% of the mass of the weakly solvated electrolyte for lithium batteries. The flame retardant accounts for 15% to 25% of the mass of the weakly solvated electrolyte in the lithium battery.

[0012] Specifically, the lithium salt may constitute 10%, 15%, 20%, 25% of the mass of the weakly solvated electrolyte in a lithium battery, or any specific percentage value between these percentages, or any range of these specific percentage values. For the sake of simplicity, not all possible specific percentage values ​​or ranges are listed here.

[0013] Specifically, the solvent's mass percentage in the weakly solvated electrolyte of the lithium battery can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, etc., or any specific percentage value between the above percentages, or any range of these specific percentage values. For the sake of simplicity, not all possible specific percentage values ​​or ranges are listed here.

[0014] Specifically, the mass percentage of the co-solvent in the lithium battery weakly solvated electrolyte can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, etc., or any specific percentage value between the above percentages, or any range of these specific percentage values. For the sake of simplicity, not all possible specific percentage values ​​or ranges are listed here.

[0015] Specifically, the flame retardant may constitute 0%, 5%, 10%, 15%, 20%, 25%, 30%, 35% of the mass of the weakly solvated electrolyte in a lithium battery, or any specific percentage value between these percentages, or any range of these specific percentage values. For the sake of simplicity, not all possible specific percentage values ​​or ranges are listed here.

[0016] Further, the aliphatic fluorinated ether-ester compound is selected from methyl 2,2,3,3-tetrafluoro-3-methoxypropionate, ethyl 2,2,3,3-tetrafluoro-3-methoxypropionate, methyl 3,3,3-trifluoro-2-(2,2,2-trifluoroethoxy)propionate, methyl 2,2-difluoro-3-methoxypropionate, methyl 2,2-difluoro-2-methoxyacetate, and methyl 2,3-difluoro-3-methoxypropionate. At least one of the following: methyl 2-fluoro-3,3-dimethoxypropionate, methyl 2,3,3-trifluoro-3-methoxypropionate, methyl 3,3,3-trifluoro-2-methoxypropionate, methyl 2-methoxytetrafluoropropionate, methyl 2,2,3,3-tetrafluoro-4-methoxybutyrate, methyl 2,2,3,3,4,4-hexafluoro-4-methoxybutyrate, and methyl 3,3,4,4-tetrafluoro-4-methoxybutyrate.

[0017] Further, the aromatic fluorinated ether-ester compound is selected from at least one of methyl 4-trifluoromethoxybenzoate, methyl o-trifluoromethoxybenzoate, methyl m-trifluoromethoxybenzoate, methyl 4-(difluoromethoxy)benzoate, methyl 3-fluoro-4-methoxybenzoate, methyl 4-fluoro-2-methoxybenzoate, methyl 4-fluoro-3-methoxybenzoate, methyl 2-fluoro-6-methoxybenzoate, methyl 3-fluoro-2-methoxybenzoate, methyl 5-fluoro-2-methoxybenzoate, methyl 2-fluoro-3-methoxybenzoate, and methyl 2-fluoro-4-methoxybenzoate.

[0018] Preferably, the solvent is an aliphatic fluorinated ether-ester compound.

[0019] Preferably, the lithium salt is a lithium bissulfonylimide salt, more preferably a lithium fluorinated bissulfonylimide salt.

[0020] Further, the lithium salt is selected from at least one of lithium difluorosulfonylimide, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethylsulfonylimide), lithium difluorododecanoate, lithium tetra(trifluoromethyl)borate, lithium tetra(pentafluorophenyl)borate, lithium tetracyanoborate, lithium dioxalateborate, lithium difluorooxalateborate, lithium trifluoromethanesulfonate, lithium methanedisulfonate difluoroborate, lithium (2-fluoromalonate) difluoroborate, lithium dimalonate borate, lithium difluorophosphoroxytrifluoroborate, lithium di(difluorophosphoroxy)difluoroborate, lithium tetra(difluorophosphoroxy)borate, lithium tetrafluorooxalate phosphate, and lithium tetrafluorodioxalate phosphate.

[0021] Specifically, the lithium bissulfonylimide salt is selected from at least one of lithium bisfluorosulfonylimide and lithium bistrifluoromethylsulfonylimide.

[0022] Specifically, the fluorinated bis(sulfonyl)imide lithium salt is selected from at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

[0023] Preferably, the flame retardant is at least one of cyclic phosphazene flame retardants and phosphate ester flame retardants.

[0024] More preferably, the phosphate ester flame retardant is a fluorophosphate ester flame retardant.

[0025] More preferably, the cyclic phosphazene flame retardant is a fluorinated cyclic phosphazene flame retardant, and more preferably a fluorinated ether cyclic phosphazene flame retardant.

[0026] Furthermore, the flame retardant satisfies at least one of the following: (1) The cyclic phosphazene flame retardant is selected from at least one of hexafluorocyclotriphosphazene, (ethoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, phenoxycyclotriphosphazene, and (phenoxy)pentafluorocyclotriphosphazene; (2) The phosphate ester flame retardant is selected from at least one of tris(2,2,2-trifluoroethyl) phosphate, bis(2,2,2-trifluoroethyl) methyl phosphate, and triphenyl phosphate; (3) The phosphite flame retardant is selected from at least one of tris(2,2,2-trifluoroethyl) phosphite and bis(2,2,2-trifluoroethyl) phosphite.

[0027] Specifically, the phosphate ester flame retardant is selected from at least one of tris(2,2,2-trifluoroethyl) phosphate and bis(2,2,2-trifluoroethyl) methyl phosphate.

[0028] Specifically, the fluorophosphate flame retardant is selected from at least one of tris(2,2,2-trifluoroethyl) phosphate and bis(2,2,2-trifluoroethyl) methyl phosphate.

[0029] Specifically, the fluorinated cyclic phosphazene flame retardant is selected from at least one of hexafluorocyclotriphosphazene, (ethoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, and (phenoxy)pentafluorocyclotriphosphazene.

[0030] Specifically, the fluoroether-based cyclic phosphazene flame retardant is selected from at least one of (ethoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, and (phenoxy)pentafluorocyclotriphosphazene.

[0031] Furthermore, the co-solvent is a fluorocarbonate compound.

[0032] Furthermore, the co-solvent satisfies at least one of the following: (1) The carbonate compound is selected from at least one of fluoroethylene carbonate, difluoroethylene carbonate, methyl ethyl carbonate, dimethyl carbonate, diethyl carbonate, ethylene ethylene carbonate, and propylene carbonate; (2) The sulfate ester compound is selected from at least one of vinyl sulfate and vinyl sulfite.

[0033] Furthermore, the concentration of lithium ions in the lithium salt in the weakly solvated electrolyte of the lithium battery is 1~3 mol / L.

[0034] Specifically, the fluorocarbonate compound is selected from at least one of fluoroethylene carbonate and difluoroethylene carbonate.

[0035] Preferably, the concentration of lithium ions in the lithium salt in the weakly solvated electrolyte of the lithium battery is 1~2 mol / L, more preferably 1.2~1.6 mol / L.

[0036] Specifically, the concentration of lithium ions in the lithium salt in the weakly solvated electrolyte of the lithium battery can be 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L, 2.0 mol / L, 2.1 mol / L, 2.2 mol / L, 2.3 mol / L, 2.4 mol / L, 2.5 mol / L, 2.6 mol / L, 2.7 mol / L, 2.8 mol / L, 2.9 mol / L, 3.0 mol / L, or any specific concentration value between the above concentrations, or any range of these specific concentration values. For the sake of simplicity, not all possible specific concentration values ​​or ranges are listed here.

[0037] Further, the solvent and co-solvent are (3~20):1, preferably (3.5~15):1, and more preferably (4~10):1.

[0038] Specifically, the volume ratio of the solvent to the co-solvent can be 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, etc., or any specific volume ratio between the above-mentioned volume ratios, or any range of these specific volume ratios. For the sake of simplicity, not all possible specific volume ratios or ranges are listed here.

[0039] Further, the volume ratio of the solvent, co-solvent and flame retardant is (3~20):1:(1~5), preferably (3.5~15):1:(1~4), and more preferably (4~10):1:(1.5~3).

[0040] Specifically, the volume ratio of the solvent, co-solvent, and flame retardant can be 3:1:1, 4:1:1, 5:1:1, 6:1:1, 7:1:1, 8:1:1, 9:1:1, 10:1:1, 11:1:1, 12:1:1, 13:1:1, 14:1:1, 15:1:1, 16:1:1, 17:1:1, 18:1:1, 19:1:1, 20:1:1, etc. Or 3:1:2, 4:1:2, 5:1:2, 6:1:2, 7:1:2, 8:1:2, 9:1:2, 10:1:2, 11:1:2, 12:1:2, 13:1:2, 14:1:2, 15:1:2, 16:1:2, 17:1:2, 18:1:2, 19:1:2, 20:1:2, etc.; Or 3:1:3, 4:1:3, 5:1:3, 6:1:3, 7:1:3, 8:1:3, 9:1:3, 10:1:3, 11:1:3, 12:1:3, 13:1:3, 14:1:3, 15:1:3, 16:1:3, 17:1:3, 18:1:3, 19:1:3, 20:1:3, etc.; Or 3:1:4, 4:1:4, 5:1:4, 6:1:4, 7:1:4, 8:1:4, 9:1:4, 10:1:4, 11:1:4, 12:1:4, 13:1:4, 14:1:4, 15:1:4, 16:1:4, 17:1:4, 18:1:4, 19:1:4, 20:1:4, etc.; Or 3:1:5, 4:1:5, 5:1:5, 6:1:5, 7:1:5, 8:1:5, 9:1:5, 10:1:5, 11:1:5, 12:1:5, 13:1:5, 14:1:5, 15:1:5, 16:1:5, 17:1:5, 18:1:5, 19:1:5, 20:1:5, etc.; The specific volume ratios between any of the above volume ratios may also include any range of these specific volume ratios. For the sake of simplicity, not all possible specific volume ratios or ranges are listed here.

[0041] This invention protects the application of the lithium battery weak solvation electrolyte in the preparation of lithium-ion batteries.

[0042] This invention protects a lithium-ion battery, comprising a positive electrode, a negative electrode, a separator, and a weakly solvated electrolyte for the lithium battery.

[0043] Compared with existing technologies, the present invention has the following beneficial effects: The lithium battery weakly solvated electrolyte of the present invention includes lithium salt, solvent, and co-solvent, and may also include a flame retardant, providing a battery-grade highly safe lithium salt-solvent-flame retardant-co-solvent combination system. This electrolyte not only significantly improves the overall safety performance of lithium batteries, but also enables high-energy-density lithium-ion batteries to maintain high capacity, long lifespan, fast charging rate, and wide temperature operating range even under high-voltage (greater than 4.2 V) charging cutoff voltage, thus having broad application value in lithium batteries. Attached Figure Description

[0044] Figure 1 The specific capacity performance curves of the batteries prepared using the electrolytes of Examples 1 to 4 and Comparative Examples 1 to 4 as electrolytes for graphite||NMC lithium-ion batteries are obtained by performing a long charge-discharge cycle test of 500 cycles at room temperature (25 °C), 1 C charging rate and 1 C discharging rate.

[0045] Figure 2 The specific capacity performance curves of the batteries prepared using the electrolytes of Examples 1 to 4 and Comparative Examples 1 to 2 as electrolytes for graphite||NMC lithium-ion batteries are obtained by charging rate testing at charging rates of 0.2C, 0.33C, 0.5C, 1C, 2C, 3C, and 5C (discharge rate of 0.2C).

[0046] Figure 3 The specific capacity performance curves of the batteries prepared using the electrolytes of Examples 1 to 4, Comparative Examples 1 and 4 as electrolytes for graphite||NMC lithium-ion batteries are obtained by performing 500 charge-discharge long-cycle tests at 60 °C, 1 C charge rate and 1 C discharge rate.

[0047] Figure 4 The specific capacity performance curves of the batteries prepared using the electrolytes of Example 1 and Comparative Example 1 of the present invention as electrolytes for graphite||NMC lithium-ion batteries were obtained by charging and discharging at low temperatures.

[0048] Figure 5 The diagram shows the microscopic solvent sheath structure of Examples 1 (E-MF85, Figure (a), 3 (E-MFP, Figure (b), and 4 (E-TF, Figure (c)) under molecular dynamics simulations of the present invention. Different atoms are distinguished by different colors: sky blue represents C; red represents O; cyan represents Li; pink represents F; yellow represents S; light gray represents H; dark gray represents P; and blue represents N.

[0049] Figure 6 The figures show a comparison of the flammability of the conventional commercial electrolyte prepared in Comparative Example 1 (Figure (a)), the electrolyte prepared in Example 1 (Figure (b)), the electrolyte prepared in Example 3 (Figure (c)), the electrolyte prepared in Comparative Example 3 (Figure (d)), and the electrolyte prepared in Comparative Example 4 (Figure (e)), as well as a comparison of the combustion phenomena of the conventional commercial electrolyte prepared in Comparative Example 1 (Figure (f)), the electrolyte prepared in Example 1 (Figure (g)), the electrolyte prepared in Example 3 (Figure (h)), the electrolyte prepared in Comparative Example 2 (Figure (i)), and the electrolyte prepared in Comparative Example 4 (Figure (j)) after the fire source was removed.

[0050] Figure 7 This is a statistical graph showing the needle penetration test phenomenon of the electrolyte prepared in Example 1 in the application of battery-grade graphite||NMC soft-pack batteries.

[0051] Figure 8 The figure shows the statistical results of the needle penetration test on the conventional commercial electrolyte prepared in Comparative Example 1 (E-Baseline, Figure (a)), the electrolyte prepared in Example 3 (E-MFP, Figure (b)), the electrolyte prepared in Comparative Example 3 (E-FMF, Figure (c)), and the electrolyte prepared in Comparative Example 4 (E-FMFP, Figure (d)) in the application of battery-grade graphite||NMC pouch batteries. Detailed Implementation

[0052] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.

[0053] Unless otherwise specified, all reagents and materials used in the following examples are commercially available.

[0054] Figure 5 (a) indicates Figure 5 Figure (a) in the middle, Figure 6 (a) indicates Figure 6 Figure (a) is in the diagram, and the other figures are named in the same way.

[0055] Example 1: Preparation of a weakly solvated electrolyte for lithium batteries Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl 2,2,3,3-tetrafluoro-3-methoxypropionate and fluoroethylene carbonate (volume ratio of 8.5:1.5), with the lithium salt concentration in the system being 1.5 M. The mixture was stirred overnight to obtain a weakly solvated electrolyte, which was named E-MF85.

[0056] Of these, the mass percentage of lithium bis(fluorosulfonyl)imide is 17.2%, the mass percentage of methyl 2,2,3,3-tetrafluoro-3-methoxypropionate is 69.4%, and the mass percentage of fluoroethylene carbonate is 13.4%.

[0057] Example 2 Preparation of a weakly solvated electrolyte for lithium batteries The difference from Example 1 is that the proportion of the co-solvent is reduced, and the specific preparation includes the following steps: Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl 2,2,3,3-tetrafluoro-3-methoxypropionate and fluoroethylene carbonate (volume ratio of 9:1), with the lithium salt concentration in the system being 1.5 M. The mixture was stirred overnight to obtain a weakly solvated electrolyte, which was named E-MF90.

[0058] Of these, the mass percentage of lithium bis(fluorosulfonyl)imide is 17.2%, the mass percentage of methyl 2,2,3,3-tetrafluoro-3-methoxypropionate is 73.8%, and the mass percentage of fluoroethylene carbonate is 9.0%.

[0059] Example 3 Preparation of a weakly solvated electrolyte for flame-retardant lithium batteries The difference from Example 1 is that a flame retardant is introduced while maintaining the same lithium salt concentration. Since the flame retardant is a non-coordinating diluent, the proportion of the co-solvent is also appropriately increased. The specific preparation includes the following steps: Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl 2,2,3,3-tetrafluoro-3-methoxypropionate, fluoroethylene carbonate, and (ethoxy)pentafluorocyclotriphosphazene (volume ratio of the three is 4.6:1:1.8). The concentration of lithium salt in the system was 1.5 M. The mixture was stirred overnight to obtain a flame-retardant weakly solvated electrolyte, which was named E-MFP.

[0060] Of these, the mass percentages of lithium bis(fluorosulfonyl)imide, methyl 2,2,3,3-tetrafluoro-3-methoxypropionate, fluoroethylene carbonate, and (ethoxy)pentafluorocyclotriphosphazene are 16.7%, 52.1%, 10.0%, and 21.2%, respectively, based on their respective mass percentages in the electrolyte.

[0061] Example 4 Preparation of a weakly solvated electrolyte for lithium batteries The difference from Example 1 is that, while maintaining the same lithium salt concentration, a different solvent was used, and the volume ratio of solvent to co-solvent was adjusted according to optimal conditions. The specific preparation includes the following steps: Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl 4-trifluoromethoxybenzoate and fluoroethylene carbonate (volume ratio 8:2), with the lithium salt concentration in the system being 1.5 M. The mixture was stirred overnight to obtain a weakly solvated electrolyte, which was named E-TF.

[0062] Of these, the mass percentage of lithium bis(fluorosulfonyl)imide is 16.4%, the mass percentage of methyl 4-trifluoromethoxybenzoate is 66.6%, and the mass percentage of fluoroethylene carbonate is 17.0%.

[0063] Comparative Example 1: Preparation of Conventional Lithium-ion Battery Electrolyte Battery electrolyte preparation: Ethylene carbonate and ethyl methyl carbonate were mixed uniformly at a mass ratio of 3:7. The mixed solvent was added to a certain amount of lithium hexafluorophosphate and fully dissolved to form a conventional commercial electrolyte with a lithium salt concentration of 1 mol / L, which was named E-Baseline.

[0064] Comparative Example 2: Preparation of Weakly Solventized Electrolyte for Lithium Batteries The difference from Example 1 is that, while maintaining the same lithium salt concentration, a non-fluorinated control molecule using the solvent molecule from Example 1 was used. The specific preparation includes the following steps: Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl 3-methoxypropionate and fluoroethylene carbonate (volume ratio of 8.5:1.5), with the lithium salt concentration in the system being 1.5 M. The mixture was stirred overnight to obtain a weakly solvated electrolyte, which was named E-MMPF.

[0065] Of these, lithium bis(fluorosulfonyl)imide accounts for 20.7% of the total mass of the electrolyte, methyl 3-methoxypropionate accounts for 76.4%, and fluoroethylene carbonate accounts for 6.4%.

[0066] Comparative Example 3: Preparation of Weakly Solventized Electrolyte for Lithium Batteries The difference from Example 1 is that, while maintaining the same lithium salt concentration, a different solvent system was used, and the volume ratio of solvent to co-solvent was adjusted according to optimal conditions. The specific preparation includes the following steps: Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl trifluoropropionate and ethylene fluorocarbonate (volume ratio 9.3:0.7), with the lithium salt concentration in the system being 1.5 M. The mixture was stirred overnight to obtain a weakly solvated electrolyte, which was named E-FMF.

[0067] Of these, lithium bis(fluorosulfonyl)imide accounts for 17.2% of the total mass of the electrolyte, methyl trifluoropropionate accounts for 76.4%, and fluoroethylene carbonate accounts for 6.4%.

[0068] Comparative Example 4: Preparation of Weak Solvent Electrolyte for Flame-Retardant Lithium Batteries The difference from Comparative Example 3 is that a flame retardant was added, and the lithium salt concentration was reduced to decrease the heat of reaction. The specific preparation includes the following steps: Battery electrolyte preparation: Lithium difluorosulfonylimide was dissolved in a mixed solvent of methyl trifluoropropionate, fluoroethylene carbonate, and tris(2,2,2-trifluoroethyl) phosphate (volume ratio of the three is 7.7:0.6:1.7). The concentration of lithium salt in the system was 1.25 M. The mixture was stirred overnight to obtain a weakly solvated electrolyte, which was named E-FMFP.

[0069] Of these, the mass percentages of lithium difluorosulfonylimide, methyl trifluoropropionate, fluoroethylene carbonate, and tri(2,2,2-trifluoroethyl) phosphate are 17.5% by mass percentage, based on their respective mass percentages in the electrolyte.

[0070] Table 1. Components and percentage of each component in the electrolytes obtained in Examples 1-4 and Comparative Examples 1-4

[0071] Experimental example: Preparation and performance testing of lithium batteries The battery electrolytes obtained in Examples 1 to 4 and Comparative Examples 1 to 4 were further prepared into lithium batteries for battery performance testing.

[0072] Lithium-ion battery fabrication: 14 mm diameter graphite electrodes and 12 mm diameter NMC811 electrodes were vacuum-dried at 110 °C for 12 hours, then transferred to an argon-filled glove box. Each coin cell was assembled from an NMC811 electrode, a 19 mm diameter polypropylene separator, a graphite electrode, a gasket, a spring, and 50 μL of electrolyte (the electrolytes prepared in Examples 1-4 and Comparative Examples 1-4). To prevent anodic corrosion of the stainless steel under high voltage, all coin cells used an aluminum-plated positive electrode shell and an additional 19 mm diameter aluminum foil placed on top of the aluminum-plated positive electrode shell.

[0073] (1) Battery performance test (1.1) Long-term cyclic testing The button cells prepared above were placed in a temperature-controlled chamber (LONGYUE LBI-250) connected to a LAND battery testing system (CT2001A) and left to stand for 12 hours. After standing, the cells were subjected to one charge-discharge cycle at 0.05 C, followed by two charge-discharge cycles at 0.1 C to promote SEI formation. After SEI formation, the graphite||NMC811 cells were subjected to 500 cycles of long-term cycle performance evaluation at room temperature (25 °C), charging at 1 C, and discharging at 1 C. The battery charge-discharge cutoff voltage was controlled between 2.5 V and 4.4 V.

[0074] Battery cycle life such as Figure 1 As shown, in the long-term cycle test of the battery, after 500 cycles, the specific capacity and capacity retention of Example 1 and Example 2 were 177.5 mAh / g and 94.8%, and 174.4 mAh / g and 92.6%, respectively, confirming the cycle stability of the electrolyte system. In Example 3, even with the addition of a high content of flame retardant, the battery still maintained a considerably high specific capacity and capacity retention (174.6 mAh / g, 93.4%), comparable to Example 1, indicating that the electrolyte system can greatly avoid the impact of flame retardants on battery cycle stability. Example 4 used a solvent different from that of Example 1, and its specific capacity and capacity retention were 151.9 mAh / g and 90.9%, also showing good specific capacity and capacity retention. In other words, after multiple cycles, the capacity and capacity retention of Examples 1 to 4 were significantly better than Comparative Example 1 (124.6 mAh / g, 70.3%).

[0075] Comparative Example 2 used a solvent different from that of Example 1, and could not achieve stable cycling under the same conditions, thus failing prematurely. Comparative Examples 3 and 4 showed better room temperature cycling stability.

[0076] (1.2) Charging rate test In the charging rate test, the graphite||NMC811 battery was charged and discharged at charging rates of 0.2C, 0.33C, 0.5C, 1C, 2C, 3C, and 5C (discharge rate of 0.2C), with 5 cycles at each rate. The battery charge and discharge cutoff voltage was controlled between 2.5V and 4.4V.

[0077] Battery charging rate performance such as Figure 2 As shown, the capacities of Example 1 at the selected rate (0.2C~5C) were 207.4 mAh / g, 201.1 mAh / g, 199.4 mAh / g, 195.7 mAh / g, 191.0 mAh / g, 184.2 mAh / g, and 161.8 mAh / g, respectively; and the capacities of Example 2 at the selected rate were 205.5 mAh / g, 200.3 mAh / g, 198.4 mAh / g, 194.4 mAh / g, 189.1 mAh / g, 180.1 mAh / g, and 149.8 mAh / g, respectively. - ¹; The capacities of Example 3 at the selected rate were 202.3 mAh / g, 200.5 mAh / g, 198.8 mAh / g, 194.4 mAh / g, 187.6 mAh / g, 176.9 mAh / g, and 144.2 mAh / g, respectively; The capacities of Example 4 at the selected rate were 194.3 mAh / g, 190.8 mAh / g, 188.6 mAh / g, 182.2 mAh / g, 169.2 mAh / g, 154.7 mAh / g, and 123.4 mAh / g, respectively; The capacities of Comparative Example 1 at the selected rate were 187.8 mAh / g, 180.2 mAh / g, 176.8 mAh / g, 171.7 mAh / g, 165.0 mAh / g, 157.9 mAh / g, and 140.0 mAh / g, respectively. Due to poor battery stability, no valid data could be obtained for Comparative Example 2. The capacities of Comparative Example 2 at the selected rate were 197.1 mAh / g, 196.6 mAh / g, 194.5 mAh / g, 189.8 mAh / g, 183.4 mAh / g, 173.9 mAh / g, and 137.4 mAh / g, respectively.

[0078] The data above shows that, except for Comparative Example 2, Examples 1-4 and Comparative Example 1 all exhibit good rate performance. Specific analysis is as follows: Examples 1 and 2 show better performance than Comparative Example 1 at the selected rate. Example 3, due to the introduction of a non-coordinated flame retardant, has slightly worse rate performance than Example 1. Example 4 is slightly worse than Comparative Example 1 at rates above 2C. Comparative Example 2 is unstable during cycling and cannot demonstrate good rate performance.

[0079] (1.3) High and low temperature cycling test In high-temperature cycling tests, the graphite||NMC811 battery was placed in a 60 ℃ constant temperature chamber for 500 cycles of charging and discharging at a 1 C rate to evaluate its long-term cycling performance. The battery charge / discharge cutoff voltage was controlled between 2.5 V and 4.4 V. In low-temperature capacity tests, the graphite||NMC811 battery was cycled at different temperatures with a 0.1 C charge rate and a 0.1 C discharge rate. The selected temperature points were 25 ℃, 10 ℃, 0 ℃, -10 ℃, and -20 ℃, with 5 cycles at each temperature point. The battery charge / discharge cutoff voltage was controlled between 2.5 V and 4.4 V.

[0080] High temperature cycle life such as Figure 3 As shown, after 500 cycles at 60 °C, the specific capacity and capacity retention of Example 1 were 142.3 mAh / g, 71.8%; the specific capacity and capacity retention of Example 2 were 145.61 mAh / g, 75.0%; the specific capacity and capacity retention of Example 3 were 152.2 mAh / g, 74.0%; and the specific capacity and capacity retention of Example 4 were 102.6 mAh / g, 53.7%, all significantly better than Comparative Example 1 (which was close to complete failure). Comparative Example 4 showed significant performance degradation after 300 cycles, with its specific capacity dropping to only 117.7 mAh / g, corresponding to a capacity retention of 60.0%.

[0081] Furthermore, the lithium battery prepared in Example 1 was used as a representative battery for low-temperature stability testing, and the low-temperature discharge capacity was as follows: Figure 4 As shown, the capacities of Example 1 at the selected temperatures were 206.2 mAh / g, 197.4 mAh / g, 188.0 mAh / g, 177.9 mAh / g, and 161.3 mAh / g, respectively, while the capacities of Comparative Example 1 at the selected temperatures were 197.3 mAh / g, 189.2 mAh / g, 177.9 mAh / g, 161.9 mAh / g, and 135.9 mAh / g, respectively. It is evident that the low-temperature capacity of Example 1 is significantly better than that of Comparative Example 1.

[0082] (2) Molecular dynamics calculations Pre-optimized lithium salt, solvent, co-solvent, and flame retardant molecules were randomly inserted into a molecular dynamics simulation chamber according to experimental proportions and densities to construct the original structural model of the lithium salt / solvent / co-solvent / diluent mixture system. All systems were pre-equilibrated for 5 ps and simulated for 50 ps with a time step of 1 fs. Schematic diagrams of the results for Examples 1, 3, and 4 are shown below. Figure 5As shown in (a) to (c), the lithium salt and solvent molecules in the embodiments of the present invention have a tendency to form a solvation structure in the electrolyte, thereby forming a weakly solvated electrolyte with a solvent sheath structure.

[0083] (3) Flammability test Flammability tests were conducted using the battery electrolytes obtained in Examples 1 and 3, as well as the electrolyte obtained in Comparative Example 1.

[0084] The flammability of the electrolyte was determined by an ignition test. A 200 μL sample of electrolyte was dropped onto non-combustible glass fiber filter paper (Whatman, GF / D), and the sample was ignited with a butane flame for 1 second. The ignition and combustion phenomena of the electrolyte were continuously recorded using a digital camera.

[0085] Flammability test results as follows Figure 6 As shown, where Figure 6 (a) ~ Figure 6 (e) Flammability tests of Comparative Example 1 (E-Baseline), Example 1 (E-MF85), Example 3 (E-MFP), Comparative Example 3 (E-FMF), and Comparative Example 4 (E-FMFP), respectively. Figure 6 (f)~ Figure 6 (j) The phenomena observed after the heat source was removed from Comparative Example 1, Example 1, Example 3, Comparative Example 3, and Comparative Example 4 at the end of the test are shown. It can be seen that Comparative Example 1 was immediately ignited and continued to burn in the air; Examples 1 and 3, due to the absence of added flame retardant, were also ignited and did not show any flame-retardant effect; while Example 3, which added flame retardant to Example 1, could not be ignited by an external heat source and exhibited a significant flame-retardant effect. Comparative Example 4, which added flame retardant to Comparative Example 3, could not continue to burn after the heat source was removed, showing a certain flame-retardant effect.

[0086] (4) Needle penetration test of soft-pack battery Using the battery electrolytes obtained in Examples 1 and 3 as representative electrolytes, as well as the electrolytes obtained in Comparative Examples 1 and 3-4, a needle penetration test was conducted on a soft-pack battery.

[0087] Electrolyte was injected into a commercial graphite-based NMC811 pouch cell (1.8 Ah), charged to 4.25V using CCCV, and placed in a test chamber. A 3 mm diameter steel nail was driven into the geometric center of the cell and held for at least 1 minute. During this time, the cell temperature and voltage were monitored by an electrochemical workstation and a temperature sensor, respectively. Real-time changes were continuously recorded for 10–20 minutes after penetration.

[0088] The results of the needle penetration test of the soft-pack battery are as follows Figure 7 and Figure 8 As shown, Example 1 ( Figure 7) and Example 3 ( Figure 8 (b) The pouch battery passed the nail penetration test safely and without damage, demonstrating high safety; while the pouch battery prepared in Comparative Example 1 produced a large amount of dense smoke after being punctured, and could not safely pass the nail penetration test. Figure 8 (a) The battery in Comparative Example 3 immediately caught fire and could not safely pass the nail penetration test. Figure 8 (c)); Comparative Example 4, even with the addition of a flame retardant to Comparative Example 3 and further reduction of reaction heat by decreasing the lithium salt concentration, still produced a large amount of dense smoke in its prepared lithium battery, making it unsafe to pass the nail penetration test. Figure 8 (d) This indicates that the batteries in Comparative Examples 1 and 3-4 are prone to thermal runaway under internal short circuit conditions caused by needle penetration, posing a risk of explosion.

[0089] In summary, the lithium-ion battery weakly solvated electrolyte of this invention comprises lithium salt, solvent, and co-solvent, and flame retardant can be added as needed to construct a synergistic system of lithium salt-solvent-flame retardant-co-solvent that combines high electrochemical performance (high capacity, long lifespan) with high safety. It is worth emphasizing that even without the addition of flame retardant, this electrolyte system can pass the nail penetration safety test, demonstrating that it can effectively suppress thermal runaway under external mechanical abuse (such as internal short circuits caused by nail penetration), significantly reducing the overall safety risk of the battery. Furthermore, if a flame retardant is introduced, the electrolyte not only still meets the nail penetration safety requirements but also effectively resists external combustion caused by open flames, achieving dual safety protection from "internal short circuit protection" to "external fire source resistance." Simultaneously, this electrolyte can maintain fast charging rate and a wide operating temperature range, making it widely applicable in lithium-ion batteries.

[0090] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A weakly solvated electrolyte for lithium batteries, characterized in that, The lithium battery weakly solvated electrolyte includes lithium salt, solvent, co-solvent, and flame retardant; The solvent is an aliphatic fluorinated ether-ester compound and / or an aromatic fluorinated ether-ester compound; The co-solvent is a carbonate compound and / or a sulfate compound; Preferably, the carbonate compound is a fluorocarbonate compound; The flame retardant is at least one of cyclic phosphazene flame retardants, phosphate ester flame retardants, and phosphite ester flame retardants; Preferably, the cyclic phosphazene flame retardant is a fluorinated cyclic phosphazene flame retardant, more preferably a fluorinated ether cyclic phosphazene flame retardant; Preferably, the phosphate ester flame retardant is a fluorophosphate ester flame retardant; Preferably, the lithium salt is a lithium bissulfonylimide salt, more preferably a lithium fluorinated bissulfonylimide salt; The lithium salt accounts for 10% to 25% of the mass of the weakly solvated electrolyte in the lithium battery. The solvent accounts for 40% to 85% of the mass of the weakly solvated electrolyte in lithium batteries. The co-solvent accounts for 5% to 40% of the mass of the weakly solvated electrolyte for lithium batteries. The flame retardant accounts for 0% to 35% of the mass of the weakly solvated electrolyte in the lithium battery.

2. The lithium battery weak solvation electrolyte according to claim 1, characterized in that, The lithium salt accounts for 12% to 20% of the mass of the weakly solvated electrolyte in the lithium battery. The solvent accounts for 50% to 66% of the mass of the weakly solvated electrolyte in lithium batteries. The co-solvent accounts for 5% to 20% of the mass of the weakly solvated electrolyte for lithium batteries. The flame retardant accounts for 15% to 25% of the mass of the weakly solvated electrolyte in the lithium battery.

3. The lithium battery weak solvation electrolyte according to claim 1 or claim 2, characterized in that, The aliphatic fluorinated ether-ester compounds are selected from methyl 2,2,3,3-tetrafluoro-3-methoxypropionate, ethyl 2,2,3,3-tetrafluoro-3-methoxypropionate, methyl 3,3,3-trifluoro-2-(2,2,2-trifluoroethoxy)propionate, methyl 2,2-difluoro-3-methoxypropionate, methyl 2,2-difluoro-2-methoxyacetate, and methyl 2,3-difluoro-3-methoxypropionate. At least one of the following: methyl fluoro-3,3-dimethoxypropionate, methyl 2,3,3-trifluoro-3-methoxypropionate, methyl 3,3,3-trifluoro-2-methoxypropionate, methyl 2-methoxytetrafluoropropionate, methyl 2,2,3,3-tetrafluoro-4-methoxybutyrate, methyl 2,2,3,3,4,4-hexafluoro-4-methoxybutyrate, and methyl 3,3,4,4-tetrafluoro-4-methoxybutyrate.

4. The lithium battery weak solvation electrolyte according to claim 1 or claim 2, characterized in that, The aromatic fluorinated ether-ester compound is selected from at least one of methyl 4-trifluoromethoxybenzoate, methyl o-trifluoromethoxybenzoate, methyl m-trifluoromethoxybenzoate, methyl 4-(difluoromethoxy)benzoate, methyl 3-fluoro-4-methoxybenzoate, methyl 4-fluoro-2-methoxybenzoate, methyl 4-fluoro-3-methoxybenzoate, methyl 2-fluoro-6-methoxybenzoate, methyl 3-fluoro-2-methoxybenzoate, methyl 5-fluoro-2-methoxybenzoate, methyl 2-fluoro-3-methoxybenzoate, and methyl 2-fluoro-4-methoxybenzoate.

5. The lithium battery weak solvation electrolyte according to claim 1 or claim 2, characterized in that, The lithium salt is selected from at least one of lithium difluorosulfonylimide, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bis(trifluoromethylsulfonylimide), lithium difluorododecanoate, lithium tetra(trifluoromethyl)borate, lithium tetra(pentafluorophenyl)borate, lithium tetracyanoborate, lithium dioxalateborate, lithium difluorooxalateborate, lithium trifluoromethanesulfonate, lithium methanedisulfonate difluoroborate, lithium (2-fluoromalonate) difluoroborate, lithium dimalonate borate, lithium difluorophosphoroxytrifluoroborate, lithium di(difluorophosphoroxy)difluoroborate, lithium tetra(difluorophosphoroxy)borate, lithium tetrafluorooxalate phosphate, and lithium tetrafluorodioxalate phosphate.

6. The lithium battery weak solvation electrolyte according to claim 1 or claim 2, characterized in that, The flame retardant satisfies at least one of the following: (1) The cyclic phosphazene flame retardant is selected from at least one of hexafluorocyclotriphosphazene, (ethoxy)pentafluorocyclotriphosphazene, (trifluoroethoxy)pentafluorocyclotriphosphazene, phenoxycyclotriphosphazene, and (phenoxy)pentafluorocyclotriphosphazene; (2) The phosphate ester flame retardant is selected from at least one of tris(2,2,2-trifluoroethyl) phosphate, bis(2,2,2-trifluoroethyl) methyl phosphate, and triphenyl phosphate; (3) The phosphite flame retardant is selected from at least one of tris(2,2,2-trifluoroethyl) phosphite and bis(2,2,2-trifluoroethyl) phosphite.

7. The lithium battery weak solvation electrolyte according to claim 1 or claim 2, characterized in that, The cosolvent satisfies at least one of the following: (1) The carbonate compound is selected from at least one of fluoroethylene carbonate, difluoroethylene carbonate, methyl ethyl carbonate, dimethyl carbonate, diethyl carbonate, ethylene ethylene carbonate, and propylene carbonate; (2) The sulfate ester compound is selected from at least one of vinyl sulfate and vinyl sulfite.

8. The lithium battery weak solvation electrolyte according to claim 1 or claim 2, characterized in that, The concentration of lithium ions in the lithium salt in the weakly solvated electrolyte of the lithium battery is 1~3 mol / L.

9. The application of the lithium battery weak solvation electrolyte according to any one of claims 1 to 8 in the preparation of lithium-ion batteries.