Application of alkoxy-side fluorinated linear carboxylic esters in the preparation of silicon-based negative electrode lithium-ion battery electrolytes

By using alkoxy-side fluorinated linear carboxylic acid esters to form an inorganic-dominated SEI film on the surface of silicon-based anodes, the problem of short battery life caused by volume expansion of silicon-based anodes is solved, and long cycle life and high capacity retention of batteries are achieved.

CN123073174APending Publication Date: 2026-11-10TSINGHUA SHENZHEN INTERNATIONAL GRADUATE SCHOOL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611486617.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The SEI film formed on the surface of the silicon-based anode by the existing fluorinated electrolyte system is prone to rupture and cannot effectively resist the huge volume expansion of the silicon-based anode, resulting in a shortened battery cycle life.

Method used

Alkoxy-side fluorinated linear carboxylic esters are used to reduce and decompose on the surface of silicon-based anodes, forming a solid electrolyte interface film dominated by inorganic components, which suppresses the volume expansion of silicon-based anodes.

Benefits of technology

A robust SEI membrane dominated by inorganic components was constructed, which has good ion conductivity and mechanical strength, and significantly extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073174A_ABST
    Figure CN123073174A_ABST
Patent Text Reader

Abstract

This invention discloses the application of alkoxy-side fluorinated linear carboxylic acid esters in the preparation of electrolytes for silicon-based lithium-ion batteries and a method for suppressing volume expansion of silicon-based anodes, belonging to the field of lithium-ion battery technology. Addressing the problem that existing acyl-side fluorinated solvents easily cause runaway defluorination and generate organic byproducts at the silicon-based anode interface, leading to repeated interfacial film rupture and short cycle life, this invention uses alkoxy-side fluorinated linear carboxylic acid esters in silicon-based anode electrolytes. During reduction and decomposition on the silicon-based anode surface, the higher C-F bond breaking barrier on the alkoxy side suppresses the defluorination side reaction, forming a solid electrolyte interfacial film dominated by inorganic lithium fluoride and poor in organic components. This suppresses the volume expansion of the silicon-based anode and significantly extends the battery cycle life. The preferred alkoxy-side fluorinated linear carboxylic acid ester is 2,2-difluoroethyl acetate. After 600 cycles, the capacity retention rate of the pouch battery still reaches 80.4%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to lithium-ion battery technology, and in particular to the application of alkoxy-side fluorinated linear carboxylic esters in the preparation of silicon-based negative electrode lithium-ion battery electrolytes. Background Technology

[0002] The rapid development of portable electronic products and electric vehicles has created an urgent demand for high-energy-density lithium-ion batteries. Silicon-based anodes are considered one of the most ideal anode materials for next-generation high-energy-density lithium-ion batteries due to their extremely high theoretical capacity (approximately 4200 mAh / g, more than ten times that of graphite anodes), suitable discharge voltage platform, abundant reserves, and low cost. However, the practical application of silicon-based anodes is severely limited by their massive volume expansion (>300%) during charge and discharge. This drastic volume effect generates mechanical stress that causes severe pulverization of silicon particles, leading to continuous rupture and regeneration of the solid electrolyte interphase (SEI) film. This continuously consumes active lithium and electrolyte, significantly shortening battery cycle life, far from meeting the battery life requirements of applications such as electric vehicles.

[0003] To address the aforementioned issues, electrolyte regulation is considered an economical and effective technical approach. Introducing fluorinated solvents or additives into the electrolyte is a widely adopted method. The design concept involves preferentially reducing and decomposing the fluorinated components to form a rigid SEI film rich in lithium fluoride (LiF) and other inorganic components on the silicon-based anode surface, attempting to resist the volume expansion of the silicon-based anode. However, existing fluorinated electrolyte systems still face a key technical bottleneck: while fluorinated solvents successfully introduce rigid inorganic components, they inevitably generate a large amount of organic byproducts during the reduction and defluorination process. These fragile organic components cannot withstand the enormous mechanical stress generated by the over 300% volume expansion of the silicon-based anode, causing the SEI film to repeatedly rupture and regenerate during cycling. This continuously consumes active lithium and electrolyte, ultimately severely offsetting the gains from the fluorination strategy and leading to rapid performance degradation of the battery.

[0004] Fluorinated linear carboxylic esters widely used in existing technologies—including ethyl fluoroacetate, ethyl difluoroacetate, and ethyl trifluoroacetate—have their fluorine atoms located on the acyl side (i.e., on the alkyl group directly attached to the carbonyl carbon). Chemically, the CF bond in acyl-side fluorinated linear carboxylic esters is located on the alkyl group directly attached to the carbonyl carbon. Due to the electron-withdrawing inductive effect of the carbonyl group, the breaking energy barrier of this CF bond is typically relatively low. When these solvents come into contact with the highly active silicon-based anode surface, a runaway reductive defluorination reaction easily occurs, generating a large number of fragile organic oligomers. The resulting SEI film has an excessively high proportion of organic components and a loose structure, making it completely unable to resist the drastic volume expansion of silicon particles.

[0005] WO2024179363A1 discloses an electrolyte system containing fluorinated solvents (such as FEC, DFEA, FEMC, TTE, etc.), in which fluorinated linear carboxylic esters such as DFEA are used as low-viscosity fluorinated solvents to improve the rate performance of high-voltage systems, suppress lithium plating during charging, and improve high-voltage cycle life. CN113471535A also relates to an electrolyte containing fluorinated linear carboxylic esters, which, by compounding fluorinated linear carboxylic esters with cyclic carbonates, utilizes their low melting point and good interfacial compatibility with graphite anodes to achieve a balance of performance over a wide temperature window. The above literature focuses on improving rate performance, low-temperature conductivity, or high-voltage stability in graphite anode systems. Although both studies mention silicon-based materials as potential anodes in their general material lists, graphite anodes and silicon-based anodes differ fundamentally in terms of volume expansion, mechanical stress on the SEI film, and failure modes. Electrolyte strategies suitable for graphite cannot be simply extrapolated to silicon-based anodes. Neither study addressed the interfacial behavior of fluorinated linear carboxylic esters in the specific system of silicon-based anodes, nor their adaptability to silicon volume expansion. In particular, neither study recognized the potential impact of differences in the molecular structure of fluorinated solvents on their interfacial behavior on silicon-based anode surfaces, nor did they consider the potential selectivity differences that fluorinated linear carboxylic esters with different structures might exhibit in interfacial reactions or SEI film formation on silicon-based anodes.

[0006] How to effectively construct the SEI film on the surface of silicon-based anode in a fluorinated electrolyte system, so that it is dominated by rigid inorganic components (especially LiF), has sufficient mechanical strength to resist the high volume expansion rate of silicon particles, and maintains good ion conductivity, while avoiding interface degradation and capacity decay caused by excessive organic byproducts, is a key technical challenge to extend the cycle life of high-energy-density silicon-based anode lithium-ion batteries.

[0007] It should be noted that the information disclosed in the background section above is only for understanding the background of this application, and therefore may include information that does not constitute prior art known to those skilled in the art. Summary of the Invention

[0008] The main objective of this invention is to overcome the deficiencies in the aforementioned background technology and to provide the application of alkoxy-side fluorinated linear carboxylic acid esters in the preparation of silicon-based negative electrode lithium-ion battery electrolytes and a method for suppressing the volume expansion of silicon-based negative electrodes.

[0009] To achieve the above objectives, the present invention adopts the following technical solution: The application of alkoxy-side fluorinated linear carboxylic acid esters in the preparation of electrolytes for silicon-based negative electrodes in lithium-ion batteries involves the reduction and decomposition of the alkoxy-side fluorinated linear carboxylic acid esters on the surface of the silicon-based negative electrode to form a solid electrolyte interface film dominated by inorganic components, thereby suppressing the volume expansion of the silicon-based negative electrode.

[0010] Furthermore, the alkoxy-side fluorinated linear carboxylic ester has the general structural formula shown in formula (1): (1) Wherein, R is an alkyl group having 1 to 2 carbon atoms, R F It is a partially fluorinated or perfluorinated straight-chain or branched alkyl group having 1 to 3 carbon atoms.

[0011] Furthermore, the alkoxy-side fluorinated linear carboxylic ester is selected from at least one of 2,2-difluoroethyl acetate (DFEA), 2-fluoro-1-ethanol acetate (2-FEA), and 2,2,2-trifluoroethyl acetate (TFEA).

[0012] Furthermore, the electrolyte also includes lithium salt and fluorocyclic carbonate additives.

[0013] Further, the lithium salt is selected from at least one of lithium bis(fluorosulfonyl)imide, lithium (fluorosulfonyl)(trifluoromethane)sulfonylimide, lithium bis(trifluoromethane)sulfonylimide, lithium bis(pentafluoroethane)sulfonylimide, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium bis(oxalate borate), lithium difluorobis(oxalate) phosphate, lithium tetrafluorooxalate phosphate, and lithium difluorophosphate, and the concentration of the lithium salt in the electrolyte is 0.05~2.0 mol / L.

[0014] Further, the fluorocyclic carbonate additive is selected from at least one of fluoroethylene carbonate and difluoroethylene carbonate, and the volume ratio of the fluorocyclic carbonate additive to the alkoxy-side fluorinated linear carboxylic acid ester is (0.01~0.12):1.

[0015] Furthermore, the inorganic components include lithium fluoride and lithium oxide, and the solid electrolyte interface film is dominated by inorganic components and depleted of organic components.

[0016] Furthermore, the active material of the silicon-based anode is at least one of micron-sized silicon, nano-sized silicon, silicon-carbon composite material, or silicon-oxygen composite material.

[0017] A method for suppressing volume expansion of a silicon-based anode includes: during the charging and discharging process of a silicon-based lithium-ion battery, reducing and decomposing an alkoxy-side fluorinated linear carboxylic acid ester in the electrolyte on the surface of the silicon-based anode to form a solid electrolyte interface film dominated by inorganic components, thereby suppressing the volume expansion of the silicon-based anode.

[0018] Furthermore, the alkoxy-side fluorinated linear carboxylic ester has the general structural formula shown in formula (1): (1) Wherein, R is an alkyl group having 1 to 2 carbon atoms, R FIt is a partially fluorinated or perfluorinated straight-chain or branched alkyl group having 1 to 3 carbon atoms.

[0019] The present invention has the following beneficial effects: This invention overcomes the technical shortcomings of existing acyl-side fluorinated solvents, which are prone to runaway reduction and defluorination at the silicon-based anode interface, generating a large number of fragile organic byproducts. By studying the reductive decomposition behavior of linear carboxylic esters with different fluorination sites at the silicon-based anode interface, this invention clarifies for the first time the influence of fluorine substitution position on the interfacial defluorination pathway and SEI film composition. Based on this understanding, this invention abandons the conventional practice of indiscriminately using fluorinated linear carboxylic esters with different fluorination positions, and for the first time applies alkoxy-side fluorinated linear carboxylic esters to silicon-based anode electrolyte systems. Utilizing the higher CF bond breaking energy barrier of the alkoxy-side fluorinated structure, the violent reductive decomposition when the solvent contacts the highly active silicon-based anode surface can be suppressed at the molecular structure level, effectively cutting off the generation pathway of organic oligomer byproducts. This shifts the reductive decomposition behavior of the electrolyte at the silicon-based anode surface towards a film-forming pathway dominated by inorganic products.

[0020] Based on the above-described mechanism, the alkoxy-side fluorinated linear carboxylic acid ester can construct an extremely robust solid electrolyte interface film on the surface of a silicon-based anode undergoing massive volume expansion through reductive decomposition. This interface film is dominated by inorganic components (especially lithium fluoride) and lacks organic components. This interface film not only possesses excellent ion conductivity but, more importantly, has sufficient mechanical strength to withstand the enormous stress generated by the high volume expansion rate of silicon particles. It effectively inhibits the pulverization and cracking of the silicon-based anode, avoiding repeated damage and regeneration of the interface film during cycling, thereby significantly extending the battery's cycle life.

[0021] Experimental results show that, according to the present invention, the application of alkoxy-side fluorinated linear carboxylic acid esters to silicon-based anode electrolytes exhibits significantly better cycle stability than acyl-side fluorinated isomers (such as EDFA) in half-cell tests. In pouch full-cell tests, the Si@C||NCM811 battery based on the present invention maintained 80.4% capacity retention after 600 cycles at 0.5C / 0.5C charge / discharge rates, demonstrating excellent commercial application prospects. These results indicate that the present invention effectively solves the problem of interface degradation and capacity decay caused by excessive organic byproducts in fluorinated electrolyte systems in silicon-based anodes, providing a practical technical solution for long cycle life of high-energy-density silicon-based lithium-ion batteries.

[0022] Other beneficial effects of the embodiments of the present invention will be further described below. Attached Figure Description

[0023] Figure 1 The defluorination Gibbs free energy changes are shown in some embodiments and comparative examples of the present invention.

[0024] Figure 2 The values ​​represent the interfacial impedance and the fitted activation energy of Si||Si at different temperatures in Example 1 and Comparative Example 1.

[0025] Figure 3 The images show the surface morphology and cross-sectional view of the silicon-based anode after cycling in Example 1 and Comparative Example 1.

[0026] Figure 4 The image shows the ToF-SIMS diagrams of the silicon-based anode SEI after cycling in Example 1 and Comparative Example 1.

[0027] Figure 5 The charge-discharge cycle performance of the Li||Si batteries in Example 1 and Comparative Example 1 is shown.

[0028] Figure 6 The charge-discharge cycle performance of the Si||NCM811 full cells in Example 1 and Comparative Example 1 is shown.

[0029] Figure 7 The charge-discharge cycle performance of the Si||NCM811 pouch cell in Example 1 is shown. Detailed Implementation

[0030] The embodiments of the present invention will be described in detail below. It should be emphasized that the following description is merely exemplary and not intended to limit the scope and application of the present invention.

[0031] This invention aims to solve the problem of repeated SEI film rupture and short cycle life caused by the huge volume expansion of silicon-based anodes. Based on the understanding of the correlation between the molecular structure of fluorinated linear carboxylic esters and the interfacial film formation behavior of silicon anodes, it proposes to use alkoxy-side fluorinated linear carboxylic esters in silicon-based anode electrolytes, so that they can be reduced and decomposed on the silicon surface to form a solid electrolyte interfacial film dominated by inorganic components, thereby effectively suppressing the volume expansion of silicon-based anodes and significantly extending the battery cycle life.

[0032] This invention provides an application in which an alkoxy-side fluorinated linear carboxylic acid ester is used in the preparation of a silicon-based negative electrode lithium-ion battery electrolyte. The alkoxy-side fluorinated linear carboxylic acid ester is used to reduce and decompose on the surface of the silicon-based negative electrode to form a solid electrolyte interface film dominated by inorganic components, thereby suppressing the volume expansion of the silicon-based negative electrode.

[0033] In some embodiments, the alkoxy-side fluorinated linear carboxylic ester has the general structural formula shown in formula (1): (1) Wherein, R is an alkyl group having 1 to 2 carbon atoms, R F It is a partially fluorinated or perfluorinated straight-chain or branched alkyl group having 1 to 3 carbon atoms.

[0034] In some embodiments, the alkoxy-side fluorinated linear carboxylic acid ester is selected from at least one of 2,2-difluoroethyl acetate (DFEA), 2-fluoro-1-ethanol acetate (2-FEA), and ethyl 2,2,2-trifluoroacetate (TFEA).

[0035] In some embodiments, the electrolyte further includes a lithium salt and a fluorinated cyclic carbonate additive. In some embodiments, the amount of the fluorinated cyclic carbonate additive is 0.1 to 10 vol%.

[0036] In some embodiments, the lithium salt is selected from at least one of lithium bis(fluorosulfonyl)imide, lithium (fluorosulfonyl)(trifluoromethane)sulfonylimide, lithium bis(trifluoromethane)sulfonylimide, lithium bis(pentafluoroethane)sulfonylimide, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorobisoxalate phosphate, lithium tetrafluorooxalate phosphate, and lithium difluorophosphate, and the concentration of the lithium salt in the electrolyte is 0.05~2.0 mol / L.

[0037] In some embodiments, the fluorocyclic carbonate additive is selected from at least one of fluoroethylene carbonate and difluoroethylene carbonate, and the volume ratio of the fluorocyclic carbonate additive to the alkoxy-side fluorinated linear carboxylic acid ester is (0.01~0.12):1.

[0038] In some embodiments, the electrolyte is prepared by a method comprising the following steps: weighing solvent and lithium salt sequentially in an argon-filled glove box, dissolving the lithium salt by magnetic stirring at room temperature, slowly adding additives dropwise, and further magnetically stirring to obtain a homogeneous and clear solution, which is the fluorinated electrolyte. Alternatively, weighing solvent and additives sequentially in an argon-filled glove box, mixing them thoroughly, adding lithium salt, and magnetically stirring at room temperature to completely dissolve the lithium salt, obtaining a homogeneous and clear solution, which is the fluorinated electrolyte.

[0039] In some embodiments, the inorganic component includes lithium fluoride and lithium oxide, and the solid electrolyte interface film is dominated by the inorganic component and depleted of the organic component.

[0040] In some embodiments, the active material of the silicon-based anode is at least one of micron-sized silicon, nano-sized silicon, silicon-carbon composite material, or silicon-oxygen composite material.

[0041] In some embodiments, the silicon-based negative electrode lithium-ion battery includes a positive electrode, a silicon-based negative electrode, a separator, and the electrolyte. The separator is a polyolefin separator, and the positive electrode is a nickel-cobalt-manganese ternary, lithium cobalt oxide, lithium-rich manganese, or lithium manganese oxide positive electrode.

[0042] This invention also provides a method for suppressing the volume expansion of a silicon-based anode, comprising: during the charging and discharging process of a silicon-based anode lithium-ion battery, reducing and decomposing the alkoxy-side fluorinated linear carboxylic acid ester in the electrolyte on the surface of the silicon-based anode to form a solid electrolyte interface film dominated by inorganic components, thereby suppressing the volume expansion of the silicon-based anode.

[0043] In some embodiments, the alkoxy-side fluorinated linear carboxylic ester has the general structural formula shown in formula (1): (1) Wherein, R is an alkyl group having 1 to 2 carbon atoms, R F It is a partially fluorinated or perfluorinated straight-chain or branched alkyl group having 1 to 3 carbon atoms.

[0044] Existing technologies, when selecting fluorinated solvents, primarily focus on the improvement of electrolyte oxidation stability or interfacial compatibility with graphite anodes due to the introduction of fluorine atoms. However, they fail to recognize that the distribution position of fluorine atoms within the molecule also affects its reductive decomposition pathway at the silicon anode interface. This invention recognizes that the distribution position of fluorine atoms in fluorinated linear carboxylic esters is a key structural variable determining their defluorination behavior on the silicon anode surface and the composition of the SEI film. Based on this, this invention proposes using alkoxy-side fluorinated linear carboxylic esters (especially preferably 2,2-difluoroethyl acetate) as the solvent for silicon-based anode electrolytes. Utilizing their high CF bond breaking energy barrier, this method suppresses runaway reductive defluorination of the solvent on the silicon surface, reducing the generation of organic oligomer byproducts at the source. Because the derivation pathway of organic byproducts is effectively interrupted, the reductive decomposition of the electrolyte on the silicon-based anode surface shifts to a film-forming pathway dominated by inorganic products. This results in the construction of a solid electrolyte interfacial film dominated by lithium fluoride and poor in organic components on the silicon-based anode surface, which has undergone significant volume expansion. This interfacial film possesses both excellent ion conductivity and sufficient mechanical strength, enabling it to withstand the enormous stress generated by the high volume expansion rate of silicon particles, suppressing silicon particle pulverization and repeated damage to the interfacial film, thereby significantly extending the battery cycle life. Compared with systems using acyl-side fluorinated solvents (such as EDFA), the coin cell using the alkoxy-side fluorinated linear carboxylic acid ester of this invention exhibits superior capacity retention and cycle stability. Even in high-energy-density pouch cells, it achieved a capacity retention of 80.4% after 600 cycles, indicating that these effects stem from the interfacial film formation behavior determined by the selection of fluorination sites, rather than the general properties of fluorinated solvents.

[0045] The following further describes specific embodiments and experimental verifications of the present invention.

[0046] Example 1

[0047] This embodiment provides a fluorinated electrolyte composed of a lithium salt, a fluorinated solvent, and an additive. The lithium salt is lithium hexafluorophosphate (LiPF6) at a concentration of 1.0 mol / L, the fluorinated solvent is 2,2-difluoroethyl acetate (DFEA), and the additive is fluoroethylene carbonate (FEC) at a volume ratio of 9:1. The entire electrolyte preparation process is completed in an argon-filled glove box, including the following specific steps: 1. Measure 0.9 mL of DFEA and 0.1 mL of FEC into glass bottles and mix them thoroughly by magnetic stirring.

[0048] 2. Weigh 1.0 mmol of LiPF6 and add it to the mixed solution. Stir magnetically to dissolve it completely to obtain the final fluorinated electrolyte.

[0049] Example 2

[0050] The difference between Example 2 and Example 1 is that the fluorinated solvent 2,2-difluoroethyl acetate (DFEA) is replaced with the fluorinated solvent 2-fluoro-1-ethanol acetate (2-FEA), while the remaining steps are the same as in Example 1.

[0051] Example 3

[0052] The difference between Example 3 and Example 1 is that the fluorinated solvent of 2,2-difluoroethyl acetate (DFEA) is replaced with the fluorinated solvent of 2,2,2-trifluoroethyl acetate (TFEA), while the remaining steps are the same as in Example 1.

[0053] Comparative Example 1

[0054] This comparative example provides an electrolyte comprising a lithium salt, a fluorinated linear carboxylic acid ester solvent, and a fluorinated cyclic carbonate additive. The lithium salt is lithium hexafluorophosphate (LiPF6) with a concentration of 1.0 mol / L. The fluorinated linear carboxylic acid ester solvent is ethyl difluoroacetate (EDFA), and the fluorinated cyclic carbonate additive is fluoroethylene carbonate (FEC), with a volume ratio of EDFA to FEC of 9:1. The specific preparation steps are all performed in an argon-filled glove box and include the following steps: 1. Measure 0.9 mL of EDFA and 0.1 mL of FEC into glass bottles and mix them thoroughly by magnetic stirring.

[0055] 2. Weigh 1.0 mmol of LiPF6 and add it to the mixed solution. Stir magnetically to dissolve it completely to obtain the final electrolyte.

[0056] Comparative Example 2

[0057] The difference between Comparative Example 2 and Comparative Example 1 is that the fluorinated solvent of ethyl difluoroacetate (EDFA) is replaced with the fluorinated solvent of ethyl fluoroacetate (EFA), and the remaining steps are the same as those in Comparative Example 1.

[0058] Comparative Example 3

[0059] The difference between Comparative Example 3 and Comparative Example 1 is that the fluorinated solvent of ethyl difluoroacetate (EDFA) is replaced with the fluorinated solvent of ethyl trifluoroacetate (ETFA), and the remaining steps are the same as those in Comparative Example 1.

[0060] Test method: Li||Si batteries and Si||NCM811 batteries were assembled using the electrolytes of Examples 1-3 and Comparative Examples 1-3, and their charge-discharge cycle performance was tested.

[0061] Preparation of Si anode: The active material (micron Si), conductive carbon black (Super P), and binder (lithiated polyacrylic acid, PAALi) are mixed in a mass ratio of 6:2:2. After adding ultrapure water, the resulting uniform slurry is coated onto a copper foil current collector. After vacuum drying at 60 °C, it is cut into a circular piece with a diameter of 10 mm, which is the Si anode used for testing.

[0062] Preparation of NCM811 positive electrode: The active material (NCM811), conductive carbon black (Super P), and binder (PVDF) are mixed in a mass ratio of 8:1:1. After adding N-methylpyrrolidone, the resulting uniform slurry is coated onto an aluminum foil current collector. After vacuum drying at 80 °C, it is cut into a circular piece with a diameter of 12 mm, which is the NCM811 positive electrode used for testing.

[0063] Half-cell assembly: All battery assembly was completed in an argon-filled glove box, using 2032 battery cases to assemble coin cells. Li / Si cells were assembled separately using lithium metal as the negative electrode, Celgard 2500 porous polymer membrane as the separator, and Si as the working electrode, and tested after standing for 6 hours.

[0064] Lithium-ion battery assembly: All battery assembly processes were completed in an argon-filled glove box, using 2032 battery cases to assemble coin cells. Si||NCM811 lithium-ion batteries were assembled using Si as the negative electrode, Celgard 2500 porous polymer membrane as the separator, and NCM811 as the positive electrode, and tested after standing for 6 hours.

[0065] Half-cell testing: A battery testing system was used, and the test was conducted in a constant temperature chamber at 25°C. After activation at a charge / discharge rate of 0.05C / 0.05C for one cycle and at a charge / discharge rate of 0.1C / 0.1C for two cycles, constant current charge / discharge cycles were performed. The voltage range of the Li||Si battery was set to 0.01~1.0 V, and the charge / discharge rate was 0.25C / 0.25C.

[0066] Full cell testing: The battery was tested using a battery testing system placed in a constant temperature chamber at 25°C. After activation at 0.1C / 0.1C charge / discharge rates for 3 cycles, constant current charge / discharge cycles were performed. The voltage range of the Si||NCM811 lithium-ion battery was set to 2.5~4.3 V, and the charge / discharge rate was 0.5C / 0.5C.

[0067] Soft-pack battery testing: A battery testing system was used, and the batteries were tested in a 25°C constant temperature chamber. After activation at 0.1C / 0.1C charge / discharge rates for 3 cycles, constant current charge / discharge cycles were performed. The voltage range of the Si||NCM811 lithium-ion battery was set to 3.0~4.2 V, and the charge / discharge rate was 0.5C / 0.5C.

[0068] Capacity retention rate calculation formula: After a certain number of continuous cycles, record the discharge capacity of the first cycle and the discharge capacity of the Nth cycle, and calculate the capacity retention rate of N cycles according to the following formula.

[0069] Capacity retention rate (%) = C N / C 首圈 ×100%; where C N This represents the discharge capacity during the Nth cycle.

[0070] The change in free energy of C–F bond breaking in solvent molecules ( The calculation formula is:

[0071] The neutral parent, defluorinated organic radicals, and neutral F atoms were all calculated using the same functionals, basis sets, and PCM parameters. , and These represent the Gibbs free energies of an organic free radical, a neutral F atom, and a neutral molecule, respectively.

[0072] The calculated Gibbs free energy changes of the defluorinated solvent molecules in the examples and comparative examples are shown in Table 1.

[0073] Table 1. Gibbs free energy changes of defluorination for different fluorinated solvent molecules

[0074] From Table 1 and Figure 1As can be seen, the Gibbs free energy changes for defluorination of acyl-side fluorinated solvents EFA, EDFA, and ETFA are 3.964, 4.059, and 4.342 eV, respectively, while those of alkoxy-side fluorinated solvents 2-FEA, DFEA, and TFEA are 4.292, 4.451, and 4.702 eV, respectively. The alkoxy-side fluorinated structures generally possess a higher C–F bond breaking barrier. These results support the technical approach of selecting alkoxy-side fluorinated linear carboxylic esters as solvents for silicon-based negative electrode electrolytes in this invention: utilizing their higher C–F bond breaking barrier to suppress runaway reductive defluorination of the solvent on the highly active silicon surface, thereby reducing the generation of organic oligomer byproducts at the source.

[0075] Because the derivation pathway of organic byproducts is effectively interrupted, the reductive decomposition of the electrolyte on the silicon-based anode surface shifts to a film-forming pathway dominated by inorganic products. This results in the formation of a solid electrolyte interface film, primarily composed of lithium fluoride and low in organic components, on the silicon-based anode surface after undergoing significant volume expansion. For example... Figure 4 As shown, the ToF-SIMS characterization results of the silicon-based anode SEI after cycling indicate that inorganic components such as LiF dominate in the system using DFEA electrolyte, while the content of organic components is significantly lower than that in the system using EDFA electrolyte. Figure 3 As shown, the surface morphology and cross-sectional characterization results of the silicon-based anode after cycling indicate that the silicon particles in the DFEA system maintained a relatively intact structure, and the interface film did not show obvious rupture, while the silicon particles in the EDFA system underwent severe pulverization and interface film damage. Figure 2 As shown, the interfacial impedance test results of the Si||Si symmetric cell at different temperatures indicate that the ion conduction activation energy of the SEI film formed by the DFEA / FEC system is 12.07 kJ mol. -1 It is significantly lower than the 18.63 kJ / mol of the EDFA / FEC system. -1 This indicates that the interfacial film constructed using the DFEA system has a lower ion conduction barrier. These results demonstrate that the interfacial film possesses both good ion conductivity and sufficient mechanical strength, enabling it to withstand the enormous stress generated by the high volume expansion rate of silicon particles, suppressing silicon particle pulverization and repeated damage to the interfacial film, thereby significantly extending the battery cycle life.

[0076] like Figure 5 As shown, in Li||Si half-cells, the battery using DFEA electrolyte retained 70.0% capacity after 300 cycles at 0.25C / 0.25C, while the battery using EDFA electrolyte experienced a significant capacity decay under the same conditions (from approximately 2500 mAh / g to approximately 200 mAh / g). This comparison at the isomer level directly demonstrates the influence of fluorination sites on interfacial stability. Figure 6As shown, in Si||NCM811 coin cells, the cell using DFEA electrolyte maintained a specific capacity of approximately 150 mAh / g after 200 cycles at 0.5C / 0.5C, while the cell using EDFA electrolyte experienced capacity decay to approximately 50 mAh / g under the same conditions. The DFEA system exhibited significantly better cycle stability than the EDFA system. Figure 7 As shown in Table 2, in the 16 Ah Si@C||NCM811 pouch cell, the capacity retention rates of the cells using DFEA electrolyte after 100, 200, 300, 400, 500, and 600 cycles at 0.5C / 0.5C were 94.7%, 93.6%, 91.9%, 88.7%, 84.4%, and 80.4%, respectively. After 600 cycles, the capacity retention rate was still 80.4%, demonstrating excellent long-cycle performance.

[0077] Table 2 Cycle capacity retention of pouch cells

[0078] Based on the numerical calculation results and experimental verification, the beneficial effects of this invention are reflected in the following aspects. At the mechanistic level, based on the understanding of the correlation between the molecular structure of fluorinated linear carboxylic esters and the film-forming behavior at the silicon anode interface, this invention determines the influence of the fluorine substitution position on the interfacial defluorination pathway and the SEI film composition. Alkoxy-side fluorinated linear carboxylic esters (such as DFEA) are selected as the solvent for the silicon-based anode electrolyte. Their high C–F bond breaking energy barrier is utilized to suppress the runaway reduction and defluorination of the solvent on the silicon surface, reducing the generation of organic oligomer byproducts at the source. At the interfacial level, because the derivation pathway of organic byproducts is effectively interrupted, the reductive decomposition of the electrolyte on the silicon-based anode surface shifts to a film-forming pathway dominated by inorganic products. This results in the construction of a solid electrolyte interfacial film on the silicon-based anode surface, dominated by lithium fluoride and low in organic components. This interfacial film possesses both good ion conductivity and sufficient mechanical strength, capable of withstanding the enormous stress generated by the high volume expansion rate of silicon particles. In terms of battery performance, compared with systems using acyl-side fluorinated solvents (such as EDFA), the coin cell using the alkoxy-side fluorinated linear carboxylic acid ester of this invention exhibits superior capacity retention and cycle stability. It also achieves a capacity retention of 80.4% after 600 cycles in high-energy-density pouch cells, indicating that the above effects are due to the interfacial film formation behavior determined by the selection of fluorination sites, rather than the general properties of fluorinated solvents. This provides a practical and feasible technical solution for the long cycle life of high-energy-density silicon-based anode lithium-ion batteries.

[0079] The above description provides a further detailed explanation of the present invention in conjunction with specific / preferred embodiments, and it should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various substitutions or modifications can be made to these described embodiments without departing from the concept of the present invention, and all such substitutions or modifications should be considered within the scope of protection of the present invention. In the description of this specification, the reference to terms such as "an embodiment," "some embodiments," "preferred embodiment," "example," "specific example," or "some examples," etc., indicates that the specific features, structures, materials, or characteristics described in connection with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in any suitable manner in one or more embodiments or examples. Without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions, and modifications can be made herein without departing from the scope of protection of the patent application.

Claims

1. The application of alkoxy-side fluorinated linear carboxylic esters in the preparation of silicon-based negative electrode lithium-ion battery electrolytes, characterized in that, The linear carboxylic acid ester with fluorination on the alkoxy side is used to reduce and decompose on the surface of the silicon-based anode to form a solid electrolyte interface film dominated by inorganic components, thereby suppressing the volume expansion of the silicon-based anode.

2. The application according to claim 1, characterized in that, The alkoxy-side fluorinated linear carboxylic ester has the general structural formula shown in formula (1): (1) Wherein, R is an alkyl group having 1 to 2 carbon atoms, R F It is a partially fluorinated or perfluorinated straight-chain or branched alkyl group having 1 to 3 carbon atoms.

3. The application according to claim 2, characterized in that, The alkoxy-side fluorinated linear carboxylic acid ester is selected from at least one of 2,2-difluoroethyl acetate (DFEA), 2-fluoro-1-ethanol acetate (2-FEA), and 2,2,2-trifluoroethyl acetate (TFEA).

4. The application according to claim 1, characterized in that, The electrolyte also includes lithium salts and fluorocyclic carbonate additives.

5. The application according to claim 4, characterized in that, The lithium salt is selected from at least one of lithium bis(fluorosulfonyl)imide, lithium (fluorosulfonyl)(trifluoromethane)sulfonylimide, lithium bis(trifluoromethane)sulfonylimide, lithium bis(pentafluoroethane)sulfonylimide, lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorobisoxalate phosphate, lithium tetrafluorooxalate phosphate, and lithium difluorophosphate, and the concentration of the lithium salt in the electrolyte is 0.05~2.0 mol / L.

6. The application according to claim 4, characterized in that, The fluorocyclic carbonate additive is selected from at least one of fluoroethylene carbonate and difluoroethylene carbonate, and the volume ratio of the fluorocyclic carbonate additive to the alkoxy-side fluorinated linear carboxylic acid ester is (0.01~0.12):

1.

7. The application according to claim 1, characterized in that, The inorganic components include lithium fluoride and lithium oxide, and the inorganic components dominate the solid electrolyte interface film while being depleted of organic components.

8. The application according to claim 1, characterized in that, The active material of the silicon-based anode is at least one of micron-sized silicon, nano-sized silicon, silicon-carbon composite material, or silicon-oxygen composite material.

9. A method for suppressing volume expansion of a silicon-based anode, characterized in that, include: During the charging and discharging process of silicon-based negative electrode lithium-ion batteries, the linear carboxylic acid esters with fluorinated alkoxy groups in the electrolyte are reduced and decomposed on the surface of the silicon-based negative electrode to form a solid electrolyte interface film dominated by inorganic components, thereby suppressing the volume expansion of the silicon-based negative electrode.

10. The method according to claim 9, characterized in that, The alkoxy-side fluorinated linear carboxylic ester has the general structural formula shown in formula (1): (1) Wherein, R is an alkyl group having 1 to 2 carbon atoms, R F It is a partially fluorinated or perfluorinated straight-chain or branched alkyl group having 1 to 3 carbon atoms.

Citation Information

Patent Citations

  • Rate type lithium ion battery electrolytic solution with high and low temperature performance and lithium ion battery

    CN113471535A

  • Electrolyte and battery

    WO2024179363A1