An ether electrolyte for improving the cycle stability of sodium vanadium phosphate cathode

By designing an electrolyte containing specific electrolyte salts and solvents, a highly stable cathode electrolyte interface is formed, solving the problem of poor cycle performance of ether-based electrolytes in sodium-ion batteries with polyanionic compound cathodes. This achieves improved long-cycle stability and electrochemical performance, promoting the commercial application of sodium-ion batteries.

CN123073185APending Publication Date: 2026-11-10NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611079519.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing ether-based electrolytes exhibit significant variations in cycle performance in sodium-ion batteries using polyanionic compounds as the positive electrode, impacting battery stability and lifespan.

Method used

A mixed electrolyte containing electrolyte salts such as sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium trifluoromethanesulfonate (NaOTf), sodium bis(fluorosulfonyl)imide (NaFSI), and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI) and solvents such as dimethyl ethylene glycol (DME), diethylene glycol dimethyl ether (DEGDME), triethylene glycol dimethyl ether (TEGDME), and tetraethylene glycol dimethyl ether (TETRAEGDME) is used to form a cathode electrolyte interface (CEI) rich in fluorine-containing inorganic materials, thereby improving interface stability.

Benefits of technology

Maintaining long-term cycle stability at high rates improves the electrochemical performance and cycle life of sodium-ion batteries, providing the possibility for the commercial development of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073185A_ABST
    Figure CN123073185A_ABST
Patent Text Reader

Abstract

This invention discloses an ether-based electrolyte for improving the cycle stability of sodium vanadium phosphate cathodes, belonging to the field of sodium-ion battery technology. The electrolyte is composed of an electrolyte salt and an ether solvent. The electrolyte salt is one or more of sodium hexafluorophosphate, sodium perchlorate, sodium trifluoromethanesulfonate, sodium bis(fluorosulfonyl)imide, and sodium bis(trifluoromethanesulfonyl)imide; the ether solvent is one or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether. Preferably, the electrolyte salt is sodium hexafluorophosphate, and the solvent is tetraethylene glycol dimethyl ether. The electrolyte of this invention is used in sodium-ion batteries using polyanionic compounds as cathode materials. Experimental results show that the electrolyte containing sodium hexafluorophosphate forms a stable, low-resistance interfacial film on the cathode surface, effectively inhibiting the decomposition of the ether solvent, significantly improving the cycle stability of the battery, and exhibiting superior cycle performance compared to other sodium salt systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of sodium-ion battery technology, and more specifically to a sodium-ion battery electrolyte for improving the cycle stability of polyanionic compound cathode materials. Background Technology

[0002] Sodium-ion batteries are considered a strong candidate for next-generation large-scale energy storage systems due to their abundant resources, low cost, and high safety. The electrolyte, as a crucial component of sodium-ion batteries, directly affects the battery's cycle life, capacity utilization, rate performance, and safety.

[0003] Currently, sodium-ion battery electrolytes mainly consist of electrolyte salts, solvents, and additives. Electrolyte salts include inorganic and organic sodium salts. Inorganic sodium salts, such as sodium hexafluorophosphate (NaPF6), are widely used, but suffer from strong oxidizing properties and poor thermal stability. Organic sodium salts, such as sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), have better thermal stability, but are expensive and corrosive to current collectors. Regarding solvents, ether solvents such as tetraethylene glycol dimethyl ether (G4) have good compatibility with various negative electrodes and can form a stable solid electrolyte interphase (SEI) film at the negative electrode; however, their weak oxidation resistance limits their application in high-voltage systems.

[0004] In the field of cathode materials, polyanionic compounds such as sodium vanadium phosphate (Na3V2(PO4)3) have attracted attention due to their advantages such as structural stability and moderate operating voltage. However, the effects of different sodium salt anion types on the compatibility of electrolytes with polyanionic cathode materials, interfacial stability, and cycle performance remain unclear. Summary of the Invention

[0005] This invention provides an electrolyte for improving the cycle stability of sodium vanadium phosphate cathodes, thereby addressing the problem of significant performance differences in existing ether-based electrolytes in sodium-ion batteries using polyanionic compounds as cathodes. To solve the aforementioned problems, this invention adopts the following technical solution:

[0006] The electrolyte components include: electrolyte salt and solvent.

[0007] The electrolyte salt includes one or a mixture of sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium trifluoromethanesulfonate (NaOTf), sodium bis(fluorosulfonyl)imide (NaFSI), and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI).

[0008] The solvent includes one or a mixture of ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (DEGDME), triethylene glycol dimethyl ether (TEGDME), and tetraethylene glycol dimethyl ether (TETRAEGDME).

[0009] Preferably, the electrolyte salt mass fraction percentage in the electrolyte is 10% to 20%.

[0010] Preferably, the organic ether solvent has a mass fraction percentage of 80% to 90%.

[0011] The present invention also provides a method for preparing the electrolyte, comprising the following steps:

[0012] (1) Under an argon atmosphere, one or more solvents are thoroughly mixed in a volume ratio to obtain a pre-purified solution.

[0013] (2) According to the mass ratio between sodium salt and solvent, a certain amount of sodium salt is added to the pre-purified solution after mixing in step (1) and dissolved to obtain the ether-based electrolyte.

[0014] Compared with the prior art, the significant advantages of the present invention are as follows:

[0015] The ether-based electrolyte designed in this invention can form a cathode electrolyte interface (CEI) rich in fluorine-containing inorganic substances. This interface has good mechanical properties and high flexibility, and can effectively inhibit the continuous oxidative decomposition of ether solvents on the electrode surface. When applied to polyanionic compound cathode materials, the electrolyte system designed in this invention maintains long-term cycle stability at high rates, providing a feasible solution for the further commercialization of sodium-ion batteries. Attached Figure Description

[0016] Figure 1 These are cycle performance test diagrams of sodium-ion batteries assembled with the electrolytes described in Embodiment 1 and Comparative Examples 1, 2, 3, and 4 of the present invention.

[0017] Figure 2 This is a charge-discharge curve of the electrolyte described in Embodiment 1 of the present invention at room temperature.

[0018] Figure 3 This is a charge-discharge curve of the electrolyte described in Comparative Example 1 of the present invention at room temperature.

[0019] Figure 4 These are linear sweep voltammetry diagrams of the electrolytes described in Embodiment 1 and Comparative Example 1 of the present invention at room temperature.

[0020] Figure 5 These are impedance diagrams of the sodium-ion battery assembled with the electrolyte described in Embodiment 1 of the present invention after 3, 100, and 200 cycles.

[0021] Figure 6 The impedance diagrams are of the sodium-ion battery assembled with the electrolyte described in Comparative Example 1 of the present invention after 3, 100, and 200 cycles.

[0022] Figure 7These are conductivity graphs of sodium-ion batteries assembled with the electrolytes described in Embodiment 1 and Comparative Example 1 of the present invention at different temperatures. Detailed Implementation

[0023] The technical solutions in the embodiments and comparative examples of the present invention will be described in further detail below, but the present invention is not limited to the embodiments described below.

[0024] Example 1

[0025] In an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), NaPF6 was added to solvent G4, stirred for 10 minutes, and allowed to stand for 6 hours to obtain an electrolyte with a concentration of 1 mol / L.

[0026] Comparative Example 1

[0027] In an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), NaClO4 was added to solvent G4, stirred for 10 minutes, and allowed to stand for 6 hours to obtain an electrolyte with a concentration of 1 mol / L.

[0028] Comparative Example 2

[0029] In an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), NaOTf was added to G4 solvent, stirred for 10 minutes, and allowed to stand for 6 hours to obtain an electrolyte with a concentration of 1 mol / L.

[0030] Comparative Example 3

[0031] In an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), NaFSI was added to G4 solvent, stirred for 10 minutes, and allowed to stand for 6 hours to obtain an electrolyte with a concentration of 1 mol / L.

[0032] Comparative Example 4

[0033] In an argon glove box (H2O < 0.1 ppm, O2 < 0.1 ppm), NaTFSI was added to G4 solvent, stirred for 10 minutes, and allowed to stand for 6 hours to obtain an electrolyte with a concentration of 1 mol / L.

[0034] Sodium-ion batteries were assembled using the above-mentioned electrolyte. The positive electrode used was the polyanionic compound Na3V2(PO4)3, and the negative electrode used metallic sodium. The sodium-ion batteries were assembled under an argon atmosphere. The assembled batteries were then subjected to room temperature cycling tests at 25°C. The test conditions were: three cycles of activation at 0.2C, and constant current charge-discharge at 5.0C (1.0C = 100mAh / g). The voltage range was 2.3–3.8V.

[0035] Table 1 shows the cycle performance test results of sodium-ion batteries assembled with electrolytes from Examples 1-2 and Comparative Examples 1-3.

[0036]

[0037] The formula for calculating the capacity retention rate after 500 laps is:

[0038] Discharge capacity after 500 cycles / discharge capacity after activation in the first cycle × 100%.

[0039] Figure 1 The graph shows the cycle performance test results of sodium-ion batteries assembled using the electrolytes described in Example 1 and Comparative Examples 1, 2, 3, and 4. Figure 2 and Figure 3 These are the charge-discharge curves of the electrolyte described in Embodiment 1 and the comparative example of the present invention at room temperature. Figure 4 Linear sweep voltammetry plots are shown for the sodium-ion batteries assembled with the electrolytes described in Example 1 and the comparative example. Experimental results show that the electrolyte using NaPF6 as the electrolyte salt exhibits the best electrochemical performance in the electrolyte system, improving the battery's cycle stability. Figure 1 The test results show that, under the conditions of 2.3–3.8V, 0.2C activation, and 5.0C cycling, the sodium-ion battery using an electrolyte containing NaPF6 retains 96.13% of its capacity after 500 cycles.

[0040] Figure 5 and Figure 6 The impedance diagrams are shown for sodium-ion batteries assembled with the electrolytes described in Example 1 and Comparative Example 1, respectively, after 3, 100, and 200 cycles. Figure 5 and Figure 6 The experimental results show that the CEI formed by the electrolyte containing NaPF6 is more stable and has a lower impedance.

[0041] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. An ether-based electrolyte for improving the cycle stability of sodium vanadium phosphate cathodes, characterized in that, The electrolyte comprises: electrolyte salt components; solvent components.

2. The electrolyte for improving the cycle stability of sodium vanadium phosphate cathode according to claim 1, characterized in that, The electrolyte salt includes one or a mixture of sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium trifluoromethanesulfonate (NaOTf), sodium bis(fluorosulfonyl)imide (NaFSI), and sodium bis(trifluoromethanesulfonyl)imide (NaTFSI).

3. The electrolyte for improving the cycle stability of sodium vanadium phosphate cathode according to claim 1, characterized in that, The solvent component includes one or a mixture of DME (diethylene glycol dimethyl ether), DEGDME (diethylene glycol dimethyl ether), TEGDME (triethylene glycol dimethyl ether), and TETRAEGDME (tetraethylene glycol dimethyl ether).

4. The electrolyte for improving the cycle stability of sodium vanadium phosphate cathode according to claim 1, characterized in that, The electrolyte salt component has a mass fraction of 10%-20%; the solvent has a mass fraction of 80%-90%.

5. The electrolyte for improving the cycle stability of sodium vanadium phosphate cathode according to claim 1, characterized in that, The electrolyte is used in sodium-ion batteries with polyanionic compound materials as the positive electrode.

6. The polyanionic compound material according to claim 5 is sodium vanadium phosphate (Na3V2(PO4)3).

7. An electrolyte for improving the cycle stability of sodium-ion batteries according to claims 1-6, characterized in that, The method includes: The electrolyte salt is added to the designed volume of ether solvent according to the mass percentage, stirred for 5-10 minutes, and then allowed to stand for 4-6 hours to obtain the electrolyte solution.

8. A sodium-ion secondary battery with improved cycle stability according to claims 1-7, characterized in that, The battery includes: The positive electrode is a polyanionic compound positive electrode material; The negative electrode is a sodium metal sheet with a diameter of 13 mm; A diaphragm, located between the positive and negative electrodes, is used to isolate the positive and negative electrode plates and to transport sodium ions; The battery casing is used to assemble the positive electrode, negative electrode, separator, and electrolyte into a complete battery.