Mixed ether-based electrolyte for improving interface stability of layered oxide cathode and application thereof
By using a mixed ether-based electrolyte in a sodium-ion battery, the interface reaction between the cathode and electrolyte was regulated, solving the problem of interfacial instability of layered oxide cathode materials under high voltage and improving the cycle stability and electrochemical reversibility of the battery.
Patent Information
- Application Number
- CN202611524554.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-10
AI Technical Summary
In existing sodium-ion batteries, the interfacial instability of layered oxide cathode materials under high-capacity and high-voltage operating conditions leads to severe side reactions at the electrode-electrolyte interface, affecting the battery's cycle stability and capacity decay.
A mixed ether-based electrolyte, comprising two ether solvents with different molecular structures or coordination properties and a sodium salt, is used to optimize the solvation structure of the electrolyte, regulate the reaction process at the cathode-electrolyte interface, suppress side reactions such as transition metal dissolution, and improve interfacial compatibility.
Without altering the cathode material structure, the cycle stability of the cathode material under high voltage was improved, voltage polarization and energy loss were reduced, the oxidation stability of the electrolyte was enhanced, and the cycle life of the battery was extended.
Smart Images

Figure CN123073189A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery technology, specifically to a mixed ether-based electrolyte for improving the stability of the layered oxide cathode interface and its application. Background Technology
[0002] Sodium, with its abundant resources, wide distribution, and low cost, is considered a key candidate technology for large-scale energy storage and new energy systems, making sodium-ion batteries an important candidate technology. As sodium-ion batteries develop towards higher energy density and longer cycle life, developing cathode materials with high specific capacity and high operating voltage has become crucial for improving overall battery performance. Among these materials, layered transition metal oxide cathode materials (Na₂O₃) are particularly important. x TMO2 is widely used in high-energy-density sodium-ion battery systems due to its high theoretical capacity, high operating voltage, and tunable crystal structure.
[0003] However, interfacial instability of layered oxide cathode materials under high-capacity and high-voltage operating conditions is a common bottleneck restricting their application. In the deep sodium-free state of the battery, the transition metals on the surface of the layered oxide cathode are in a high valence state and possess strong oxidizing activity, easily inducing persistent electrode-electrolyte interfacial side reactions. These side reactions include high-level oxidative decomposition of the electrolyte, dissolution of transition metal elements, and surface phase transition reconstruction. These prevalent problems not only drastically consume active sodium ions but also damage the chemical stability of the cathode interface, inducing rapid capacity decay and intensified charge-discharge polarization. For example, P3-type layered transition metal oxides (such as P3-Na...) 0.67 Ni 1 / 3 Mn 2 / 3 O2 possesses unique sodium ion diffusion kinetics and high capacity utilization potential, but its interfacial instability under high voltage is particularly prominent. The lattice distortion accompanying the P3 to O3 phase transition further damages the integrity of the surface interfacial film and exacerbates interfacial side reactions.
[0004] Existing research largely focuses on bulk modification of the cathode material itself (such as elemental doping and surface coating) or optimization of electrolyte formulations, with cathode material design and electrolyte system optimization typically operating independently. However, bulk modification is insufficient to fundamentally suppress interfacial side reactions under high voltage. Furthermore, traditional carbonate electrolytes are prone to oxidative decomposition on the surface of high-voltage cathodes, while single ether solvents (such as ethylene glycol dimethyl ether) exhibit limited oxidative stability, both of which fail to meet the interfacial stability requirements of high-voltage layered oxide cathodes.
[0005] Chinese patent document CN119230934A discloses a cyclic / linear mixed ether electrolyte for sodium metal batteries, belonging to the field of sodium metal battery electrolyte technology. This prior art provides a cyclic / linear mixed ether electrolyte design to solve the technical problems of poor compatibility with sodium metal and low utilization efficiency of existing sodium metal battery electrolytes, while generating a more stable solid electrolyte interface phase and meeting the application requirements of sodium metal batteries. However, this prior art mainly improves electrolyte stability by suppressing sodium negative electrode side reactions and by generating an interface layer rich in inorganic matter at the electrolyte interface.
[0006] Therefore, it is necessary to develop a hybrid ether-based electrolyte that combines good oxidation stability and interfacial compatibility. By regulating the reaction process at the cathode-electrolyte interface, the structural stability and electrochemical reversibility of the layered oxide cathode can be improved, which is of great significance for realizing sodium-ion batteries with high energy density and long cycle life. Summary of the Invention
[0007] This invention provides a mixed ether-based electrolyte and its application for improving the interfacial stability of layered oxide cathodes, solving the problem of insufficient interfacial compatibility between traditional electrolyte systems and high-capacity layered oxide cathodes in existing sodium-ion batteries. The mixed ether system of this invention can effectively address the P3 cathode interfacial failure problem, regulate the electrolyte solvation structure and the cathode-electrolyte interfacial reaction process, optimize the chemical environment of the cathode surface interface, suppress side reactions such as transition metal dissolution, and improve interfacial compatibility, thereby enhancing interfacial stability.
[0008] To address the aforementioned technical problems, a first aspect of the present invention is to provide a mixed ether-based electrolyte for improving the interfacial stability of layered oxide cathodes, wherein the mixed ether-based electrolyte comprises: a mixed ether solvent and an electrolyte salt.
[0009] The mixed ether solvent includes at least two ether solvents with different molecular structures or coordination properties, and the electrolyte salt is a sodium salt.
[0010] Preferably, the mixed ether solvent includes a first ether solvent and a second ether solvent, and the volume ratio of the first ether solvent to the second ether solvent is 1:9 to 9:1.
[0011] Preferably, the volume ratio of the first ether solvent to the second ether solvent is 3:7 to 7:3. More preferably, it is 1:1.
[0012] By adopting the above technical solution, the reaction process at the cathode-electrolyte interface is controlled by optimizing the electrolyte solvent composition and solvation structure, thereby improving the interfacial compatibility between the layered oxide cathode and the electrolyte, and enhancing the cathode structural stability, electrochemical reaction reversibility, and cycle performance.
[0013] Preferably, both the first ether solvent and the second ether solvent are selected from one or more of ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (G2), triethylene glycol dimethyl ether (G3), and tetraethylene glycol dimethyl ether (G4).
[0014] Preferably, the concentration of the electrolyte salt in the mixed ether-based electrolyte is 0.2 mol / L to 2 mol / L.
[0015] Preferably, the concentration of the electrolyte salt in the mixed ether-based electrolyte is 0.5 mol / L.
[0016] Preferably, the electrolyte salt is selected from one or more of sodium hexafluorophosphate (NaPF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethylsulfonyl)imide, and sodium perchlorate (NaClO4).
[0017] Preferably, the electrolyte salt is sodium hexafluorophosphate (NaPF6).
[0018] A second aspect of the present invention is to provide the application of the mixed ether-based electrolyte as described in the first aspect of the present invention in the preparation of sodium-ion batteries.
[0019] Preferably, the positive electrode material used in the sodium-ion battery is a layered transition metal oxide with the chemical formula: Na. x TMO2, where 0 < x ≤ 1, and TM is one or more transition metals.
[0020] Preferably, the layered transition metal oxide is a metastable P3-type layered oxide.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The mixed ether-based electrolyte provided in this application does not require element doping, surface coating or crystal structure modification of the layered oxide cathode, and can still improve the cycle stability of the cathode material under high capacity operation conditions without changing the P3 to O3 phase transition of its structure, thus reducing the dependence on the complex modification process of the cathode material.
[0023] (2) This application constructs a mixed ether solvent system to regulate the solvation structure of the electrolyte and the reaction process at the cathode-electrolyte interface, optimizes the chemical environment of the cathode surface interface, suppresses side reactions such as the dissolution of transition metals, and improves the interface stability.
[0024] (3) The use of the mixed ether-based electrolyte of this application can improve the structural evolution behavior of the layered oxide cathode during the charging and discharging process, improve the reversibility of the sodium ion insertion / extraction process, and reduce voltage polarization and energy loss during the charging and discharging process.
[0025] (4) The mixed ether-based electrolyte provided in this application has good high-voltage oxidation stability, which can improve the oxidation resistance of the electrolyte system and reduce the electrolyte decomposition reaction during high-potential charging, making it suitable for high-voltage, high-capacity layered oxide cathode systems. Attached Figure Description
[0026] Figure 1 Fourier transform infrared spectra of different ether-based electrolytes of the present invention;
[0027] Figure 2 These are the NMR spectra of different ether-based electrolytes of the present invention; wherein (a) is 19 F spectrum, (b) is 23 Na spectrum;
[0028] Figure 3 The original infrared spectra of different ether-based electrolytes of the present invention and the P3-Na of electrolyte permeation. 0.67 Ni 1 / 3Mn 2 / 3 Comparison of FTIR spectra of O2 (P3-NNMO) cathode;
[0029] Figure 4 Linear sweep voltammetry curves of different ether-based electrolytes of the present invention in sodium metal batteries;
[0030] Figure 5 The cycling performance comparison curves of sodium-ion batteries with different electrolytes according to the present invention are shown.
[0031] Figure 6 The in-situ X-ray diffraction pattern of the layered oxide cathode of the mixed ether-based electrolyte in Specific Embodiment 1 of the present invention is shown; wherein (a) is the charge-discharge voltage-time curve; and (b) is the in-situ X-ray diffraction two-dimensional profile diagram of the evolution of the (003) crystal plane and the (006) crystal plane with charge-discharge time.
[0032] Figure 7 The images shown are optical images of the Na metal anode taken after 100 cycles and corresponding micro-area X-ray fluorescence (XRF) elemental distribution maps; where (a) is an optical contrast image of the Na metal anode, (b) is the corresponding micro-area XRF Ni elemental distribution map, and (c) is the corresponding micro-area XRF Mn elemental distribution map. Detailed Implementation
[0033] The specific embodiments of the present invention will be described in detail below, but the present invention is not limited thereto.
[0034] Unless otherwise specified, the preparation methods and usage conditions used in the following examples are conventional methods; the reagents and materials used in the following examples are commercially available unless otherwise specified. Furthermore, reagents not specifically mentioned in this invention are all commercially available reagents commonly used by those skilled in the art.
[0035] To avoid excessive and unnecessary detail, well-known structures or functions will not be described in detail in the following embodiments. The approximate language used in the following embodiments is for quantitative purposes, indicating that variations in quantity are permissible without altering the basic function. Unless otherwise defined, the technical and scientific terms used in the following embodiments have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0036] Example 1: A mixed ether-based electrolyte for improving the interfacial stability of layered oxide cathodes, comprising: a mixed ether solvent and an electrolyte salt, wherein the mixed ether solvent comprises at least two ether solvents with different molecular structures or coordination properties, and the electrolyte salt is a sodium salt. The mixed ether solvent comprises a first ether solvent and a second ether solvent, and the volume ratio of the first ether solvent to the second ether solvent is 1:9 to 9:1. Preferably, it is 3:7 to 7:3; more preferably, it is 1:1.
[0037] In this application, the sodium ion solvation structure is adjusted through the synergistic effect between different ether solvents, thereby optimizing the solvation environment at the cathode interface and reducing interfacial side reactions. Simultaneously, by optimizing the electronic structure and interfacial reaction behavior of the mixed ether system, the oxidative stability of the electrolyte under high-potential conditions is improved, reducing electrolyte oxidative decomposition during cathode charging. It should be noted that the volume ratio of the first ether solvent to the second ether solvent is 1:1, but 1:1 can also be 5:5, 4:4, or 3:3.
[0038] Both the first ether solvent and the second ether solvent are selected from one or more mixtures of ethylene glycol dimethyl ether (DME), diethylene glycol dimethyl ether (G2), triethylene glycol dimethyl ether (G3), and tetraethylene glycol dimethyl ether (G4). In this application, the first ether solvent and the second ether solvent are different ether solvents. For example, if the first ether solvent is ethylene glycol dimethyl ether (DME), then the second ether solvent is an ether solvent other than ethylene glycol dimethyl ether (DME).
[0039] The concentration of the electrolyte salt in the mixed ether-based electrolyte is 0.2 mol / L to 2 mol / L. Preferably, the concentration of the electrolyte salt in the mixed ether-based electrolyte is 0.5 mol / L.
[0040] The electrolyte salt is selected from one or more of sodium hexafluorophosphate (NaPF6), sodium bis(trifluoromethylsulfonyl)imide (NaFSI), sodium bis(trifluoromethylsulfonyl)imide, and sodium perchlorate (NaClO4). Preferably, the electrolyte salt is sodium hexafluorophosphate (NaPF6).
[0041] Example 2: Application of the mixed ether-based electrolyte of Example 1 in the preparation of a sodium-ion battery, wherein the sodium-ion battery comprises the mixed ether-based electrolyte of Example 1.
[0042] In some specific embodiments, the positive electrode material used in the sodium-ion battery is a layered transition metal oxide with the chemical formula: Na. x TMO2, where 0 < x ≤ 1, and TM is one or more transition metals.
[0043] In some specific embodiments, the layered transition oxide is a metastable P3-type layered oxide. This is to better observe the influence of the crystal structure on the electrolyte interface, for example, P3-Na. 0.67 Ni 1 / 3 Mn 2 / 3 O2.
[0044] The following detailed discussion will be conducted through several specific embodiments.
[0045] Specific Example 1: The mixed ether-based electrolyte comprises NaPF6 and a mixed ether solvent. The first ether solvent is diethylene glycol dimethyl ether (G2), and the second ether solvent is tetraethylene glycol dimethyl ether (G4). The ratio of the first ether solvent to the second ether solvent is 5:5. The sodium salt is sodium hexafluorophosphate (NaPF6), and the concentration of the sodium salt in the mixed ether electrolyte is 0.5 mol / L. The preparation method is as follows:
[0046] (1) In an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), G2 and G4 were mixed in a volume ratio of 5:5 to prepare 10 mL of mixed ether solvent;
[0047] (2) 0.84 g of NaPF6 was added to a pre-mixed ether solvent and the solution was stirred at room temperature until dissolved by magnetic stirring. A certain mass of 4 Å molecular sieve was added for dehydration treatment. After standing for 6 hours, a mixed ether electrolyte with a sodium salt concentration of 0.5 mol / L was obtained.
[0048] It should be noted that the amount of 4Å molecular sieve added here is the conventional amount used by those skilled in the art, and a few or a dozen sieves may be added depending on the amount of solution.
[0049] Specific Example 2: This mixed ether-based electrolyte comprises NaPF6 and a mixed ether solvent. The first ether solvent is diethylene glycol dimethyl ether (G2), and the second ether solvent is tetraethylene glycol dimethyl ether (G4). The ratio of the first ether solvent to the second ether solvent is 7:3. The sodium salt is sodium hexafluorophosphate (NaPF6), and the concentration of the sodium salt in the mixed ether electrolyte is 0.5 mol / L. The preparation method is as follows:
[0050] (1) In an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), G2 and G4 were mixed in a volume ratio of 7:3 to prepare 10 mL of mixed ether solvent;
[0051] (2) 0.84 g of NaPF6 was added to a pre-mixed ether solvent and the solution was stirred at room temperature until dissolved by magnetic stirring. A certain mass of 4 Å molecular sieve was added for dehydration treatment. After standing for 6 hours, a mixed ether electrolyte with a sodium salt concentration of 0.5 mol / L was obtained.
[0052] Specific Example 3: The mixed ether-based electrolyte comprises NaPF6 and a mixed ether solvent. The first ether solvent is diethylene glycol dimethyl ether (G2), and the second ether solvent is tetraethylene glycol dimethyl ether (G4). The ratio of the first ether solvent to the second ether solvent is 3:7. The sodium salt is sodium hexafluorophosphate (NaPF6), and the concentration of the sodium salt in the mixed ether electrolyte is 0.5 mol / L. The preparation method is as follows:
[0053] (1) In an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), G2 and G4 were mixed in a volume ratio of 3:7 to prepare 10 mL of mixed ether solvent;
[0054] (2) 0.84 g of NaPF6 was added to a pre-mixed ether solvent and the solution was stirred at room temperature until dissolved by magnetic stirring. A certain mass of 4 Å molecular sieve was added for dehydration treatment. After standing for 6 hours, a mixed ether electrolyte with a sodium salt concentration of 0.5 mol / L was obtained.
[0055] Comparative Example 1: Unlike Specific Example 1, only a single ether solvent was used. Specifically:
[0056] (1) Under an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), 0.84 g of NaPF6 was added to 10 mL of G2 solvent that had been pre-treated with 4 Å molecular sieves for dehydration. The mixture was magnetically stirred at 500 rpm for 2 h at room temperature until the solute was completely dissolved. Then, a certain mass of 4 Å molecular sieves was added for dehydration treatment. After standing for 6 hours, an electrolyte with a sodium salt concentration of 0.5 mol / L was obtained.
[0057] Comparative Example 2: The difference from Comparative Example 1 is the amount of sodium salt added. Specifically:
[0058] (1) Under an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), 1.68 g of NaPF6 was added to 10 mL of G2 solvent that had been pre-treated with 4 Å molecular sieves for dehydration. The mixture was magnetically stirred at 500 rpm for 2 h at room temperature until the solute was completely dissolved. Then, a certain mass of 4 Å molecular sieves was added for dehydration treatment. After standing for 6 hours, an electrolyte with a sodium salt concentration of 1 mol / L was obtained.
[0059] Comparative Example 3: Unlike Comparative Example 1, only a single ether solvent was used. Specifically:
[0060] (1) Under an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), 0.84 g of NaPF6 was added to 10 mL of G4 solvent that had been pre-treated with 4 Å molecular sieves for dehydration. The mixture was magnetically stirred at 500 rpm for 2 h at room temperature until the solute was completely dissolved. Then, a certain mass of 4 Å molecular sieves was added for dehydration treatment. After standing for 6 hours, an electrolyte with a sodium salt concentration of 0.5 mol / L was obtained.
[0061] Comparative Example 4: The difference from Comparative Example 3 is the amount of sodium salt added. Specifically:
[0062] (1) Under an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), 1.68 g of NaPF6 was added to 10 mL of G4 solvent that had been pre-treated with 4 Å molecular sieves for dehydration. The mixture was magnetically stirred at 500 rpm for 2 h at room temperature until the solute was completely dissolved. Then, a certain mass of 4 Å molecular sieves was added for dehydration treatment. After standing for 6 hours, an electrolyte with a sodium salt concentration of 1 mol / L was obtained.
[0063] Comparative Example 5: Unlike Specific Example 1, a non-ether organic solvent was used, specifically:
[0064] (1) In an inert atmosphere (H2O < 0.1 ppm, O2 < 0.1 ppm), ethylene carbonate (EC) was heated to 50 °C until dissolved and then mixed with propylene carbonate (PC) at a volume ratio of 1:1. 5% fluoroethylene carbonate (FEC) was added to prepare 10 mL of mixed solvent, and a certain mass of 4 Å molecular sieve was added for dehydration treatment.
[0065] (2) 1.68 g of NaPF6 was added to a pre-mixed ether solvent and magnetically stirred at 500 rpm for 2 h at room temperature until the solute was completely dissolved. Then, a certain mass of 4 Å molecular sieve was added for dehydration treatment. After standing for 6 hours, an electrolyte with a sodium salt concentration of 1 mol / L was obtained.
[0066] The electrolytes prepared in the above-mentioned specific embodiments 1-3 and comparative examples 1-5, with P3-Na 0.67 Ni 1 / 3 Mn 2 / 3 A CR2032 coin cell was assembled using O2 as the positive electrode, sodium metal as the negative electrode, and GF / D glass fiber as the separator for electrochemical performance testing. Charge-discharge cycle tests were conducted at a current density of 100 mA / g under conditions of 30±5℃.
[0067] (1) The steps for preparing the positive electrode are as follows:
[0068] In P3-Na 0.67 Ni 1 / 3 Mn 2 / 3 In the preparation of the O2 precursor powder, sodium acetate (CH3COONa, 8 mol% excess), nickel acetate (Ni(CH3COO)2), and manganese acetate (Mn(CH3COO)2) were dissolved in deionized water according to the stoichiometric ratio. Citric acid was dissolved in a small amount of deionized water in an equimolar amount and slowly added dropwise to the metal salt solution. The mixture was kept in an 80°C water bath until a gel was formed, and then dried overnight at 100°C under vacuum to obtain the precursor. Subsequently, the temperature was increased to 450°C at 10°C / min and held for 5 hours, and then increased to 700°C and held for 10 hours.
[0069] The positive electrode slurry is mainly composed of synthesized P3, O3, and P2 layered positive electrode active materials, prepared according to a mass ratio of active material:graphene:PVDF of 7:2:1. Using an 80-200μm (specifically 100μm) doctor blade, the slurry is evenly coated onto aluminum foil. The electrode is then transferred to a vacuum drying oven and dried at 110°C for 12 hours to remove residual solvent. The dried electrode is cut into 12mm diameter discs for battery assembly. The mass of the dried positive electrode active material is approximately 1-2mg.
[0070] (2) The assembly steps of sodium-ion batteries are as follows:
[0071] Sodium metal batteries (button cells, CR2032) were assembled in a glove box under an argon atmosphere (H2O < 0.01 ppm, O2 < 0.01 ppm), using sodium metal as the negative electrode and GF / D glass fiber (19 mm diameter) as the separator. The specific assembly sequence was: positive electrode shell, electrode sheet, separator, sodium sheet, gasket, spring sheet, and negative electrode shell, with 160 μL of electrolyte injected. The assembled battery needed to stand for at least 8 hours before testing.
[0072] The ether-based electrolyte and the resulting sodium-ion battery in the above embodiments were tested, including:
[0073] (1) Fourier transform infrared (FTIR) spectroscopy: from Figure 1 The test results show that, relative to the COC stretching vibration of the G2 solvent, Comparative Example 1 and Comparative Example 2 exhibit a similar effect in the FTIR spectra at ~1083 cm⁻¹. -1 The appearance of a shoulder peak indicates that the G2 molecule and Na + Strong coordination exists between the ions. This shoulder peak was significantly suppressed in Specific Example 1, indicating that Na in the mixed ether electrolyte... + -G2 interactions are weakened. Meanwhile, in specific embodiment 1, PF6... - Vibration characteristics (840.8cm) -1 Free PF6 - The displacement reflects the enhanced Na + -PF6 - Coordination.
[0074] (2) From Figure 2 The test results show that the NMR spectrum 19 F and 23 The Na spectrum further confirms that Na in specific embodiment 1... + -PF6 - The interaction is enhanced, and accompanied by a decrease in Na. + - Solvent coordination.
[0075] (3) Adsorption Fourier Transform Infrared (FTIR) Spectroscopy Test: Adsorption-based FTIR measurements were performed by comparing the pure electrolyte with the electrolyte permeated into the P3-NNMO electrode. Figure 3 In comparative example 2, after infiltration of P3-NNMO, the COC vibration was significantly enhanced, accompanied by PF6 -A slight shift in the relevant characteristics toward lower wavenumbers was observed. In contrast, this trend was less pronounced in Comparative Example 2 and almost negligible in Specific Example 1. Since no external potential was applied in this test, the observed spectral differences directly reflect the stronger interfacial hybridization between Comparative Example 1 and P3-NNMO. These results confirm a significant shift in solvation in the mixed ether electrolyte toward reduced cation-solvent and enhanced cation-anion interactions.
[0076] (4) The linear sweep voltammetry (LSV) method was used for testing. The scan rate was 1 mV / s. The current-potential curve was recorded to obtain the electrocatalytic performance of the electrode. Figure 4 The linear sweep voltammetry curve in a sodium metal battery; from Figure 4 The test results show that the mixed ether-based electrolyte of Specific Example 1 exhibits a significantly lower oxidation current in the high voltage region (>4.0V), indicating that the electrolyte system has better antioxidant stability and can effectively suppress the side reactions at the cathode-electrolyte interface under high voltage.
[0077] (5) Battery cycle charge and discharge test: Figure 5 The graph shows the comparison of cycle performance of sodium-ion batteries under different electrolyte systems. The experimental results show that the mixed ether-based electrolyte in Example 1 still maintains a discharge specific capacity of 160.5 mAh / g after 100 cycles, with a capacity retention rate of 72.7%, which is better than the comparative examples (specific performance test data are shown in Table 1). This indicates that the electrolyte system can effectively improve the interfacial stability of the layered oxide cathode and achieve excellent cycle reversibility.
[0078] Table 1. Comparison data of battery cycle performance between specific examples 1-3 and comparative examples 1-3.
[0079] experimental group <![CDATA[Initial discharge specific capacity (mA h g -1 )]]> Capacity retention rate (%) after 100 cycles Specific Implementation Example 1 160.5 72.7 Specific Implementation Example 2 150.7 67.0 Specific Implementation Example 3 137.8 64.8 Comparison Group 1 129.6 54.8 Comparison Group 2 139.1 45.1 Comparison Group 3 114.5 57.6 Comparison Group 4 122.1 66.3 Comparison Group 5 103.1 51.4
[0080] (6) XRD characterization: Figure 6 The image shows the in-situ X-ray diffraction pattern of the layered oxide cathode using the mixed ether-based electrolyte of Specific Example 1. Figure 6 Characterization results in (a) indicate that the P3 to O3 phase transition still occurs when using the mixed ether electrolyte of this application. During the initial charging process, Na... + The delamination resulted in a slight increase in interlayer spacing, as evidenced by the system shift of (003) to a lower angle. The subsequent splitting of the reflections of (003) and (006) at the low-voltage plateau (~2.0V) during discharge clearly indicates a phase transition from P3 to O3, accompanied by a significant contraction of the lattice parameter along the c-axis. In-situ two-dimensional X-ray diffraction profiles of (003) and (006) as a function of charge / discharge time are shown below. Figure 6(b) This structural transition is consistent with previous reports and is widely considered to be the primary cause of degradation of P3-type cathode structures in high-capacity operation. Despite still exhibiting a longer P3-to-O3 transition plateau, the electrochemical cycling stability observed in mixed ether electrolytes (see [reference]) Figure 5 The significant improvement means that the performance enhancement is not controlled by phase suppression, but by the regulation of interfacial reaction kinetics and chemomechanical coupling during the phase transition. Therefore, the P3 to O3 transformation is not the only determining factor for cyclic degradation.
[0081] (7) Characterization of elemental distribution by X-ray fluorescence (XRF): Figure 7 Optical images and corresponding micro-area X-ray fluorescence (XRF) elemental distribution maps of the Na metal anodes after 100 cycles of sodium-ion batteries using Comparative Example 1 and Specific Example 1, respectively. Figure 7 (a) Figure 7 (b) and Figure 7 As can be seen in (c), a significant amount of Ni can be detected on the surface of the circulating Na metal in the electrolyte system of Comparative Example 1 (see [reference]). Figure 7 (b) and Mn (see Figure 7 The signal in (c) is present, while in the electrolyte system of Specific Example 1, these transition metal signals are only weak trace amounts. This indicates that the mixed ether electrolyte exhibits a superior effect in suppressing the dissolution of transition metals such as Ni and Mn in the cathode material.
[0082] For those skilled in the art, the specific embodiments are merely illustrative descriptions of the present invention. Obviously, the specific implementation of the present invention is not limited to the above-described manner. Any non-substantial improvements made using the inventive concept and technical solution, such as changing the concentration of a substance or a reaction parameter, or directly applying the inventive concept and technical solution to other situations without modification, are all within the protection scope of the present invention.
Claims
1. A mixed ether-based electrolyte for improving the interfacial stability of layered oxide cathodes, characterized in that, The mixed ether-based electrolyte comprises: a mixed ether solvent and an electrolyte salt. The mixed ether solvent includes at least two ether solvents with different molecular structures or coordination properties, and the electrolyte salt is a sodium salt.
2. The mixed ether-based electrolyte according to claim 1, characterized in that, The mixed ether solvent includes a first ether solvent and a second ether solvent, and the volume ratio of the first ether solvent to the second ether solvent is 1:9 to 9:
1.
3. The mixed ether-based electrolyte according to claim 2, characterized in that, Both the first ether solvent and the second ether solvent are selected from one or more of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
4. The mixed ether-based electrolyte according to claim 2, characterized in that, The concentration of the electrolyte salt in the mixed ether-based electrolyte is 0.2 mol / L to 2 mol / L.
5. The mixed ether-based electrolyte according to claim 4, characterized in that, The concentration of the electrolyte salt in the mixed ether-based electrolyte is 0.5 mol / L.
6. The mixed ether-based electrolyte according to claim 4, characterized in that, The electrolyte salt is selected from one or more of sodium hexafluorophosphate, sodium difluorosulfonyl imide, sodium bis(trifluoromethylsulfonyl)imide, and sodium perchlorate.
7. The mixed ether-based electrolyte according to claim 6, characterized in that, The electrolyte salt is sodium hexafluorophosphate.
8. The use of the mixed ether-based electrolyte as described in any one of claims 1-7 in the preparation of sodium-ion batteries.
9. The application according to claim 8, characterized in that, The positive electrode material used in the sodium-ion battery is a layered transition metal oxide with the chemical formula: Na. x TMO2, where 0 < x ≤ 1, and TM is one or more transition metals.
10. The application according to claim 9, characterized in that, The layered transition metal oxide is a metastable P3-type layered oxide.
Citation Information
Patent Citations
Annular / linear mixed ether electrolyte for sodium metal battery
CN119230934A