A Low-Temperature Two-Stage Ultrafine Grinding Method for Vulcanizing Auxiliaries in Latex Gloves

By using a low-temperature two-stage ultrafine grinding method to grind sulfur and accelerators separately, and by using a compounding medium and dual closed-loop control, the problems of scorching and uneven dispersion of vulcanizing aids during high-temperature grinding were solved, thus improving the quality and storage stability of latex gloves.

CN123102451APending Publication Date: 2026-11-17SICHUAN GONGWU CHUANGZHI TECHNOLOGY CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611420542.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the current production of latex gloves, vulcanizing auxiliaries are prone to scorching during high-temperature grinding, resulting in defects such as rubber particles and pinholes in the finished gloves. Furthermore, the gloves are poorly dispersed and tend to agglomerate and settle during storage.

Method used

A low-temperature two-stage ultrafine grinding method is adopted to grind sulfur and accelerator separately. A compound medium of zirconia beads and alumina beads of different particle sizes is used. Combined with pH and zeta potential regulation, dual closed-loop control is achieved through online temperature and particle size detection to avoid high-temperature scorching and over-grinding.

Benefits of technology

It achieves ultrafine dispersion of vulcanizing aids, significantly reduces the rate of pinholes and rubber particles in finished gloves, and has good storage stability of the dispersion, making it suitable for the production modification of various latex gloves.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102451A_ABST
    Figure CN123102451A_ABST
Patent Text Reader

Abstract

This invention discloses a low-temperature two-stage ultrafine grinding method for vulcanizing accelerators used in latex gloves, relating to the field of latex glove manufacturing technology. The method involves separately preparing premixed slurries of sulfur, zinc oxide, and an accelerator; these slurries are then fed into a horizontal sand mill with a water-cooled jacket and milled using zirconia beads as the grinding medium for a first-stage grinding process, with the temperature controlled not to exceed 40°C; the two first-stage slurries are then combined and fed into a grinding jar with a water-cooled jacket for a second-stage circulating grinding process using a mixture of two different particle sizes of alumina beads as the grinding medium, with the temperature controlled not to exceed 35°C, until the particle size D... 50 Not greater than 1μm and D 90 A water-based dispersion of the vulcanizing aid is obtained with a particle size not exceeding 3 μm. This invention separates and finely grinds the sulfur and accelerator separately, then combines them at low temperature to eliminate the scorching condition at the source. The two heterogeneous media are compounded to achieve ultra-fine and uniform dispersion, reducing pinholes and adhesive particles in the finished gloves, and ensuring storage stability and versatility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of latex glove manufacturing technology, specifically to a low-temperature two-stage ultrafine grinding method for vulcanizing agents used in latex gloves. Background Technology

[0002] In the production of latex gloves, before dipping and molding, sulfur, zinc oxide, accelerators, and other vulcanizing agents must be ground into an aqueous dispersion. This dispersion is then mixed into concentrated latex in a specific ratio for formulation, pre-vulcanization, and dipping and molding. The particle size and dispersion uniformity of the vulcanizing agent dispersion, as well as the temperature control during the grinding process, directly affect the uniformity of the subsequent rubber film and the appearance quality of the finished gloves.

[0003] Existing technology CN104419042A discloses a latex glove and its preparation method, which involves grinding and dispersing sulfur, zinc oxide, accelerator, antioxidant, and dispersant together in deionized water, then mixing and impregnating them with latex. When the above-mentioned prior art is applied to the grinding of vulcanizing aids for latex gloves, the following main defects exist: Firstly, when sulfur, accelerator, and zinc oxide are mixed in the same slurry and subjected to high-energy grinding, the grinding media generates a large amount of heat during high-speed shearing and friction. The local temperature of the slurry can rise to above 45°C. Under the heating conditions, the newly formed high specific surface area particles cause sulfur and accelerator to undergo cross-linking reaction in advance, generating tiny scorched particles. When mixed into latex, these particles cause defects such as rubber particles and pinholes in the molded gloves. Secondly, most of the grinding is done on a single machine in a single stage, with a single grinding medium. The additives are coarse and poorly dispersed after grinding, which also causes defects in the adhesive film. Third, ultrafine dispersions are prone to particle reagglomeration and sedimentation during storage, resulting in uneven dispersion during formulation. Summary of the Invention

[0004] The purpose of this invention is to provide a low-temperature two-stage ultrafine grinding method for vulcanizing auxiliaries for latex gloves, so as to solve the problems of scorching of vulcanizing auxiliaries due to temperature runaway in existing grinding processes, as well as insufficient grinding fineness and uneven dispersion.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: A low-temperature two-stage ultrafine grinding method for vulcanizing agents used in latex gloves includes the following steps: S1. Ingredients: Vulcanization aids include sulfur, zinc oxide, and accelerators; sulfur, zinc oxide, dispersant, and water are mixed to prepare premixed slurry A; accelerator, dispersant, and water are mixed to prepare premixed slurry B; the solid content of premixed slurry A and premixed slurry B is 40%~55% respectively. S2, First Stage Grinding: Premixed slurry A and premixed slurry B are separately fed into a horizontal sand mill with a water-cooled jacket, and ground using zirconia beads as the grinding media. During the grinding process, the slurry temperature is controlled not to exceed 40℃, and the grinding continues until each slurry reaches D... 90 With a diameter not exceeding 10 μm, two slurries, A and B, were obtained respectively. S3. Two-stage grinding: First-stage slurry A and first-stage slurry B are combined and fed into a grinding jar with a water-cooled jacket. Grinding is performed using a grinding medium composed of two different alumina beads of varying particle sizes mixed in a specific mass ratio. During the grinding process, the slurry temperature is controlled to not exceed 35℃ until the particle size D is reached. 50 Not greater than 1μm and D 90 A water-based dispersion of the vulcanizing aid is obtained with a particle size not exceeding 3 μm.

[0006] Further, in S1, the dispersant is at least one of polycarboxylate dispersant and naphthalene sulfonate formaldehyde condensate, and the total amount of dispersant is 1% to 3% of the mass of the vulcanizing aid; the pH of premixed slurry A and premixed slurry B is adjusted to 8 to 10 so that the absolute value of the Zeta potential on the surface of the vulcanizing aid particles in premixed slurry A and premixed slurry is not less than 30mV.

[0007] Furthermore, in S1, the accelerator is at least one of zinc diethyldithiocarbamate and zinc dibutyldithiocarbamate.

[0008] Furthermore, when preparing premixed slurry B, S1 also adds an anti-scorching agent, which is N-cyclohexylthiophthalimide, and the dosage is 0.5%~2% of the mass of the accelerator.

[0009] Furthermore, in S1, the premixed slurry is pre-dispersed by a high-speed disperser for 5 to 15 minutes before being fed into the horizontal sand mill; in S2, the particle size of the zirconia beads is 1.2 mm to 1.5 mm, and the grinding linear speed of the horizontal sand mill is 8 m / s to 12 m / s.

[0010] Furthermore, in S3, there are two types of alumina beads with different particle sizes, including large beads and small beads. The large beads have a particle size of 0.8 mm to 1.0 mm, and the small beads have a particle size of 0.4 mm to 0.6 mm. The mass ratio of large beads to small beads is (1 to 2):1.

[0011] Furthermore, in S3, the number of cyclic grinding cycles is 3 to 6.

[0012] Furthermore, during the grinding processes of S2 and S3, the heating rate of the slurry is controlled to be no higher than 0.5℃ / min; when the heating rate exceeds 0.5℃ / min, the grinding spindle speed is reduced and the cooling water flow rate of the water-cooling jacket is increased simultaneously.

[0013] Furthermore, in S2 and S3, both the horizontal sand mill and the grinding tank are equipped with online temperature sensors, online particle size analyzers, and external circulation pumps. The online temperature sensor collects the slurry temperature in real time. When the slurry temperature reaches the set threshold, the grinding spindle speed is reduced, and the cooling water flow rate of the water-cooled jacket is increased simultaneously. The material circulation flow rate is also increased by adjusting the external circulation pump, so that the slurry temperature drops back to the set range. At the same time, the online particle size analyzer collects the slurry particle size in real time. When the particle size reaches the set target value, grinding is stopped.

[0014] The beneficial effects of this invention are as follows: 1. Sulfur and accelerator, which are prone to mutual reaction, are ground separately in the high-energy first-stage grinding stage, and only combined and finely ground in the low-temperature second-stage stage. This chemically cuts off the scorching premise of the coexistence of sulfur, accelerator and heat. Combined with low-temperature control throughout the process and the synergistic effect of anti-scorching agent, the water-based dispersion of vulcanizing aids basically does not produce scorched particles, and the defect rate of pinholes and rubber particles in the finished gloves is significantly reduced. 2. A two-stage grinding process, employing zirconia beads in one stage of coarse grinding and a blend of two types of alumina beads in two stages of fine grinding, achieves a dispersion particle size of up to D. 50 The particle size is no larger than 1 μm, and the particle size distribution is narrow and the dispersion is uniform. 3. Through pH and Zeta potential regulation and the synergistic effect of dispersants, the ultrafine dispersions are less prone to agglomeration and sedimentation during storage, resulting in good storage stability; 4. The system employs dual closed-loop control of temperature and online particle size, as well as a heating rate limit, to achieve ultrafine dispersion while avoiding over-grinding and scorching, thus balancing grinding efficiency and product quality. 5. The grinding process is an independent set of equipment, which does not rely on pre-vulcanization or molding equipment. It can be adapted to the transformation of various latex and nitrile glove mixing workshops and has strong versatility. Attached Figure Description

[0015] Figure 1 This is a flowchart of the grinding method in Example 1. Detailed Implementation

[0016] To make the objectives and technical solutions of this invention clearer, the invention will be further described below with reference to embodiments, but the scope of protection of this invention is not limited thereto. Unless otherwise specified, the vulcanizing auxiliaries, dispersants, and equipment used in the following embodiments are all commercially available products conventional in the art.

[0017] Example 1 like Figure 1 As shown, this embodiment provides a low-temperature two-stage ultrafine grinding method for vulcanizing auxiliaries for latex gloves, including the following steps: S1. Ingredients: By weight, take 10 parts sulfur and 8 parts zinc oxide, add polycarboxylate dispersant and deionized water, mix and pre-disperse in a high-speed disperser for 10 minutes to prepare a premixed slurry A with a solid content of 50%; separately take 2 parts zinc diethyldithiocarbamate and 0.03 parts N-cyclohexylthiophthalimide anti-scorching agent, add polycarboxylate dispersant and deionized water, mix and pre-disperse in a high-speed disperser for 10 minutes to prepare a premixed slurry B with a solid content of 50%; the total amount of dispersant in premixed slurry A and premixed slurry B is 2% of the total mass of vulcanizing aids, and adjust the pH of both slurries to 9; S2. First-stage grinding: Premixed slurry A and premixed slurry B are fed into a horizontal sand mill with a water-cooled jacket, using 1.3mm zirconia beads as the grinding medium to obtain first-stage slurry A and first-stage slurry B respectively. The grinding linear speed is 10m / s, and the slurry temperature is controlled not to exceed 40℃ throughout the process, with the heating rate controlled not to exceed 0.5℃ / min. When the temperature approaches 40℃, the spindle speed is automatically reduced and the cooling water flow and circulation flow are increased. Grinding is continued until the particle size D of each first-stage slurry is reached. 90 It is 8μm; S3. Two-stage grinding: First-stage slurry A and first-stage slurry B are combined and fed into a grinding jar with a water-cooled jacket. Alumina beads, a mixture of 0.9mm large beads and 0.5mm small beads at a mass ratio of 1.5:1, are used as the grinding medium. The mixture is circulated and ground four times, with the slurry temperature controlled to not exceed 35℃ throughout the process, until the particle size D is reached. 50 0.8μm, D 90 The particle size was 2.4 μm, resulting in an aqueous dispersion of the vulcanizing aid. During the grinding process, the slurry temperature was monitored in real time by an online temperature sensor, and the slurry particle size was monitored in real time by an online particle size analyzer. Grinding was stopped when the particle size reached the target value, and the spindle speed was automatically reduced and the cooling water flow rate and circulation flow rate were increased when the temperature approached 35℃.

[0018] The aqueous dispersion of the vulcanizing aid prepared in this embodiment is mixed with concentrated latex, and then pre-vulcanized and impregnated to form latex gloves.

[0019] Testing revealed that the zeta potential of the vulcanizing aid particles in premixed slurry A was -36mV, and in premixed slurry B it was -33mV, with absolute values ​​not lower than 30mV. The peak temperature of the first-stage grinding was 38℃, and the peak temperature of the second-stage grinding was 34℃. No charred particles were detected in the aqueous dispersion of the vulcanizing aid, and the particle size D of the dispersion was [not specified]. 50 0.8μm, D 90 The thickness is 2.4 μm; the aqueous dispersion of the vulcanizing aid, after standing at 25℃ for 30 days, has a D... 50 The particle size was 0.9 μm, with no obvious sedimentation; the defect rate of pinholes in the finished gloves was 0.3%, and the defect rate of rubber particles was 0.2%.

[0020] Example 2 This embodiment provides a low-temperature two-stage ultrafine grinding method for vulcanizing auxiliaries for latex gloves. The difference from Embodiment 1 is that the solid content of both premixed slurry A and premixed slurry B is 45%; the mass ratio of large beads to small beads in S3 is 2:1, and the grinding is repeated 5 times. The remaining steps are the same as in Embodiment 1.

[0021] Testing revealed that the zeta potential of the vulcanizing aid particles in premixed slurry A was -34 mV, and in premixed slurry B it was -32 mV, with absolute values ​​not lower than 30 mV. The peak temperature of the first-stage grinding was 39℃, and the peak temperature of the second-stage grinding was 34℃. No charred particles were detected in the aqueous dispersion of the vulcanizing aid, and the particle size D of the dispersion was [not specified]. 50 0.9μm, D 90 The thickness is 2.8 μm; the aqueous dispersion of the vulcanizing aid, after standing at 25℃ for 30 days, has a D... 50 The particle size was 1.0 μm, with no obvious sedimentation; the defect rate of pinholes in the finished gloves was 0.4%, and the defect rate of rubber particles was 0.3%.

[0022] Comparative Example 1 The difference between this comparative example and Example 1 is that a horizontal sand mill without a water-cooled jacket is used for single-stage grinding, and the temperature is not controlled during the grinding process. All other conditions are the same as in Example 1.

[0023] Testing revealed that the peak temperature during the grinding process reached 48℃, and obvious scorched particles were detected in the aqueous dispersion of the vulcanizing aid. The particle size of the dispersion was D. 50 2.6μm, D 90 The pinhole defect rate is 9.5μm, and the defect rate of finished gloves is 2.8%, while the defect rate of adhesive particles is 3.1%.

[0024] Comparative Example 2 The difference between this comparative example and Example 1 is that only a horizontal sand mill with a water-cooled jacket and zirconia beads of a single particle size are used for single-stage grinding, the temperature is controlled not to exceed 40°C throughout the process, and no second-stage grinding is performed. All other conditions are the same as in Example 1.

[0025] Testing revealed that the peak temperature during the grinding process was 39℃. No charred particles were detected in the aqueous dispersion of the vulcanizing aid, but the particle size D of the dispersion was [not specified]. 50 1.9μm, D 90 The pinhole defect rate is 6.2μm, and the defect rate of finished gloves is 1.2%, while the defect rate of rubber particles is 0.5%.

[0026] Comparative Example 3 The difference between this comparative example and Example 1 is that sulfur, zinc oxide and accelerator are mixed in the same slurry and ground together, and no anti-scorching agent is added. The other conditions (two-stage grinding, low temperature control, heterogeneous media compounding, temperature and particle size double closed loop) are the same as in Example 1.

[0027] Testing revealed that the peak temperature of the first-stage grinding was 39℃, and the peak temperature of the second-stage grinding was 34℃. A small amount of charred particles were detected in the aqueous dispersion of the vulcanizing aid. The particle size D of the dispersion was... 50 0.9μm, D 90 The pinhole defect rate is 0.9%, and the glue particle defect rate is 0.6%, with a thickness of 2.6μm.

[0028] The grinding effects of each embodiment and the comparative example are compared in Table 1 below: Table 1. Comparison of grinding effects between each embodiment and the comparative example. As can be seen from the above examples and comparative examples: Comparative Example 1 did not use water-cooled temperature control, and the grinding temperature rise caused the vulcanization aid to scorch. In addition, the single-stage grinding fineness was insufficient, and the defects of pinholes and rubber particles increased significantly. Although Comparative Example 2 avoided scorching through water-cooled temperature control, it only used single-stage grinding and a single medium, resulting in insufficient dispersion fineness and a still high pinhole defect rate. Although Comparative Example 3 also used low-temperature two-stage grinding, because sulfur and accelerator were mixed and ground without the addition of an anti-scorching agent, the newly formed high specific surface area particles still produced a small amount of scorching under the action of grinding heat, and the pinhole defect rate was still high. This invention achieves no scorching, ultra-fine uniform dispersion, and good storage stability by grinding sulfur and accelerator separately, combining low-temperature two-stage fine grinding, and using an anti-scorching agent and dual closed-loop control of temperature and particle size. The defects of pinholes and rubber particles in the finished gloves are significantly reduced.

[0029] The above embodiments are only used to illustrate the technical ideas and features of the present invention, and are not intended to be unique or to limit the present invention. Those skilled in the art should understand that various changes or equivalent substitutions made to the present invention without departing from its scope are all within the scope of protection of the present invention.

Claims

1. A low-temperature two-stage ultrafine grinding method for vulcanizing auxiliaries for latex gloves, characterized in that, Includes the following steps: S1. Ingredients: Vulcanization aids include sulfur, zinc oxide, and accelerators; sulfur, zinc oxide, dispersant, and water are mixed to prepare premixed slurry A; accelerator, dispersant, and water are mixed to prepare premixed slurry B; the solid content of premixed slurry A and premixed slurry B is 40%~55% respectively. S2, First Stage Grinding: Premixed slurry A and premixed slurry B are separately fed into a horizontal sand mill with a water-cooled jacket, and ground using zirconia beads as the grinding media. During the grinding process, the slurry temperature is controlled not to exceed 40℃, and the grinding continues until each slurry reaches D... 90 With a diameter not exceeding 10 μm, two slurries, A and B, were obtained respectively. S3. Two-stage grinding: First-stage slurry A and first-stage slurry B are combined and fed into a grinding jar with a water-cooled jacket. Grinding is performed using a grinding medium composed of two different alumina beads of varying particle sizes mixed in a specific mass ratio. During the grinding process, the slurry temperature is controlled to not exceed 35℃ until the particle size D is reached. 50 Not greater than 1μm and D 90 A water-based dispersion of the vulcanizing aid is obtained with a particle size not exceeding 3 μm.

2. The low-temperature two-stage ultrafine grinding method for vulcanizing auxiliaries for latex gloves according to claim 1, characterized in that, In S1, the dispersant is at least one of polycarboxylate dispersant and naphthalene sulfonate formaldehyde condensate, and the total amount of dispersant is 1% to 3% of the mass of the vulcanizing aid; the pH of premixed slurry A and premixed slurry B is adjusted to 8 to 10 so that the absolute value of the Zeta potential on the surface of the vulcanizing aid particles in premixed slurry A and premixed slurry is not less than 30mV.

3. The low-temperature two-stage ultrafine grinding method for vulcanizing auxiliaries for latex gloves according to claim 1, characterized in that, In S1, the accelerator is at least one of zinc diethyldithiocarbamate and zinc dibutyldithiocarbamate.

4. The low-temperature two-stage ultrafine grinding method for vulcanizing aids for latex gloves according to claim 1, characterized in that, In S1, when preparing premixed slurry B, an anti-scorching agent is also added. The anti-scorching agent is N-cyclohexylthiophthalimide, and the amount of anti-scorching agent is 0.5% to 2% of the mass of the accelerator.

5. The low-temperature two-stage ultrafine grinding method for vulcanizing aids for latex gloves according to claim 1, characterized in that, In S1, the premixed slurry is pre-dispersed by a high-speed disperser for 5 to 15 minutes before being fed into the horizontal sand mill; in S2, the particle size of the zirconia beads is 1.2 mm to 1.5 mm, and the grinding linear speed of the horizontal sand mill is 8 m / s to 12 m / s.

6. The low-temperature two-stage ultrafine grinding method for vulcanizing aids for latex gloves according to claim 1, characterized in that, In S3, there are two types of alumina beads with different particle sizes, including large beads and small beads. The particle size of the large beads is 0.8 mm to 1.0 mm, and the particle size of the small beads is 0.4 mm to 0.6 mm. The mass ratio of large beads to small beads is (1~2):

1.

7. The low-temperature two-stage ultrafine grinding method for vulcanizing aids for latex gloves according to claim 1, characterized in that, In S3, the number of cycles for cyclic grinding is 3 to 6.

8. The low-temperature two-stage ultrafine grinding method for vulcanizing aids for latex gloves according to claim 1, characterized in that, During the grinding processes of S2 and S3, the heating rate of the slurry should be controlled to be no higher than 0.5℃ / min; when the heating rate exceeds 0.5℃ / min, the grinding spindle speed should be reduced and the cooling water flow rate of the water-cooling jacket should be increased simultaneously.

9. The low-temperature two-stage ultrafine grinding method for vulcanizing aids for latex gloves according to claim 1, characterized in that, In S2 and S3, both the horizontal sand mill and the grinding tank are equipped with online temperature sensors, online particle size analyzers, and external circulation pumps. The online temperature sensor collects the slurry temperature in real time. When the slurry temperature reaches the set threshold, the grinding spindle speed is reduced, and the cooling water flow rate of the water-cooled jacket is increased simultaneously. The material circulation flow rate is also increased by adjusting the external circulation pump, so that the slurry temperature drops back to the set range. At the same time, the online particle size analyzer collects the slurry particle size in real time. When the particle size reaches the set target value, grinding is stopped.

Citation Information