A copper-carbon interpenetrating network composite material, its preparation method, and an HHO standing wave explosion-proof sintering furnace.
By using copper-carbon interpenetrating network composite materials and HHO plasma sintering furnace, the problems of copper-carbon interface bonding and safe application of HHO were solved, realizing copper-carbon composite materials with high conductivity, high strength and high thermal conductivity, while improving safety and biochar utilization efficiency.
Patent Information
- Application Number
- CN202611265239.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot solve the problem of chemical bonding at the copper-carbon interface, the bottleneck of safe application of HHO gas in a closed micro-positive pressure environment, and the lack of recognition of the utilization value of SiO2 in biochar, which makes it difficult to balance the conductivity and strength of copper-carbon composite materials.
The copper-carbon interpenetrating network composite material is adopted. A continuous gradient transition layer is introduced between the copper matrix and the carbon skeleton. It contains lithium magnesium silicate solid solution and combines micron-scale flake graphite and nano-scale biochar to form a three-dimensional interpenetrating network. The interface chemical bonding is achieved by using an HHO plasma standing wave sintering furnace, and safe application in a closed environment is ensured by safety mechanisms such as supersonic jet and flame arrester.
The ternary synergistic optimization of high electrical conductivity, high strength and high thermal conductivity of copper-based composite materials has been achieved, the interfacial shear strength has been improved and the safety has been guaranteed, and the SiO2 in biochar has been utilized as a resource, breaking the industry application taboo.
Smart Images

Figure CN123102999A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the interdisciplinary field of powder metallurgy and radio frequency plasma technology, specifically relating to a copper-carbon interpenetrating network composite material, its preparation method, and an explosion-proof HHO plasma sintering furnace for implementing the method. This composite material can be widely used in national strategic fields such as SiC power module heat dissipation substrates for new energy vehicles, high-reliability electrical contact systems for aerospace, high-voltage connectors for high-speed rail transit, temperature control platforms for semiconductor lithography machines, and divertors for nuclear fusion reactors. Background Technology
[0002] Copper-based composite materials have broad application prospects in power electronics, aerospace, and other fields due to their excellent electrical and thermal conductivity. However, existing technologies have long faced the following technical bottlenecks: (1) Intrinsic non-wetting problem at copper-carbon interface The intrinsic wetting angle of copper and carbon is greater than 140°, and their interface is a typical non-wetting system. Traditional mechanical mixing methods can only form a weakly physically bonded interface. When the amount of carbon added exceeds a certain proportion, the electron scattering effect at the interface causes a sharp decrease in the conductivity of the composite material, making it impossible to achieve "high strength" and "high conductivity" simultaneously. The industry has long believed that there is an irreconcilable performance contradiction in the copper-carbon system.
[0003] (2) The problem of Cu2O "dead layer" inside copper powder
[0004] Electrolytic copper powder commonly contains a difficult-to-remove Cu₂O coating (referred to in the industry as a "dead layer"). Conventional hydrogen (H₂) reducing atmospheres, due to thermodynamic equilibrium limitations, can only remove the surface oxide layer and cannot penetrate to reduce the Cu₂O inside the particles. Thermodynamic calculations show that under normal pressure and a H₂ atmosphere, the reduction equilibrium temperature for Cu₂O needs to exceed 400℃ to achieve a considerable rate, and the solid-gas reaction rate constant between H₂ molecules and Cu₂O is only 10. -5 ~10 -6 The resistance is on the order of m / s, resulting in the interface resistance accounting for more than 40% of the total resistance.
[0005] (3) Issues regarding the prohibited applications of HHO gas
[0006] HHO gas (Brown gas, H2:O2=2:1) has an extremely wide explosion limit (approximately 4%~95%), making it an extremely hazardous chemical in confined, slightly positive pressure environments. Globally, HHO is only used in open welding or cutting scenarios. In the high-temperature (>1000℃), confined, slightly positive pressure sintering conditions required for powder metallurgy, it has long been considered a forbidden technological area due to the lack of intrinsically safe explosion-proof mechanisms. Traditional explosion-proof approaches (such as diluting inert gases) sacrifice the reducing activity of HHO, failing to balance safety and process efficiency.
[0007] (4) The "impurity paradox" of SiO2 in biochar
[0008] Biochar made from agricultural and forestry waste (such as walnut shells and coconut shells) contains 1%–5% SiO2 and alkali metal ash. For a long time, these components have been considered harmful impurities in the materials science community, believed to degrade electrical conductivity. Therefore, biochar has only been used as a low-end fuel or adsorbent and has not been incorporated into high-performance composite material design systems. However, SiO2 is a key raw material for forming silicate ceramic phases; the key lies in controlling its reaction pathway and spatial distribution.
[0009] (5) Limitations of existing technology
[0010] Existing comparable products, such as the American GlidCop® series, use an internal oxidation method to generate a dispersed Al2O3 phase for reinforcement. However, oxide reinforcement inevitably sacrifices conductivity (its volume resistivity is 1.82 × 10⁻⁶). -8 The copper-carbon composite material exhibits a high tensile strength (Ω·m) and is incompatible with carbon-reinforced phases. While traditional vacuum hot pressing can introduce carbon materials, the copper-carbon interface exhibits extremely poor bonding (wetting angle > 120°), leading to interfacial delamination after thermal cycling. The best reported tensile strength of copper-carbon composites is only 300–350 MPa, with a volume resistivity of 2.0–2.5 × 10⁻⁶ MPa. -8 Within the range of Ω·m.
[0011] (6) Unresolved technical needs
[0012] In summary, existing technologies have neither solved the chemical bonding problem at the copper-carbon interface, nor broken through the bottleneck of safe application of HHO in a closed environment, nor have they recognized the utilization value of SiO2 in biochar.
[0013] The following technical bias is commonly held by those skilled in the art: the intrinsic wetting angle between copper and carbon is greater than 140°. The two are difficult to chemically bond using conventional metallurgical methods; HHO gas (H2:O2=2:1) is an extremely hazardous chemical in a closed, slightly positive pressure environment, with a very wide explosion limit (approximately 4%~95%), and can only be used in open welding or cutting scenarios, not in high-temperature closed sintering conditions; SiO2 and alkali metal ash in biochar are considered harmful impurities that will deteriorate the conductivity of composite materials and should not be included in the design system of high-performance composite materials. These technical biases have led to the long-term failure in this field to achieve chemical bonding at the copper-carbon interface and the safe application of HHO in closed environments.
[0014] Therefore, developing a preparation technology that can simultaneously achieve high conductivity, high strength, high thermal conductivity, and can safely utilize the HHO active atmosphere is an urgent need in this field. Summary of the Invention
[0015] This invention proposes a copper-carbon interpenetrating network composite material, its preparation method, and an explosion-proof HHO plasma sintering furnace, aiming to systematically solve the above-mentioned technical bottlenecks.
[0016] I. Copper-Carbon Interpenetrating Network Composites
[0017] This invention discloses a copper-carbon interpenetrating network composite material comprising a copper matrix, a carbon skeleton, and a continuous gradient transition layer located between the copper matrix and the carbon skeleton. The continuous gradient transition layer contains lithium, magnesium, silicon, and oxygen, with the magnesium content decreasing in a gradient along the normal direction from the copper matrix to the carbon skeleton.
[0018] Core Innovation Point 1: Chemical Design of Gradient Transition Layer
[0019] The main crystalline phase of the continuous gradient transition layer is lithium magnesium silicate solid solution (Li 1-x Mg x The transition layer is 2SiO3, where x represents the atomic ratio of Mg / (Li+Mg). x decreases in gradient from 0.30~0.70 near the copper substrate to 0.05~0.20 near the carbon skeleton along the normal direction from the copper substrate. The transition layer thickness is 80~250 nm (preferably 120~180 nm), and the side near the carbon skeleton contains a Si-OC covalently bridged amorphous phase with a wetting angle θ < 10° (preferably 7~9°).
[0020] The core mechanism of this gradient design lies in the following: a higher Mg content (x=0.30~0.70) near the copper matrix causes the transition layer to exhibit more ionic / metallic bond characteristics, resulting in higher lattice matching and chemical affinity with the copper matrix; a lower Mg content (x=0.05~0.20) near the carbon framework causes the transition layer to exhibit more covalent bond characteristics, forming a strong covalent coupling with the sp² / sp³ hybrid carbon of the carbon material. This continuous gradient from ionic to covalent bonds achieves copper-carbon amphiphilic wetting, fundamentally solving the physical taboo of intrinsic non-wetting at the copper-carbon interface.
[0021] Core Innovation Point 2: Dual-Scale Three-Dimensional Interpenetrating Carbon Framework
[0022] The carbon framework comprises micron-sized flake graphite and nano-sized biochar. Micron-sized flake graphite (D50 = 5~10 μm) interlocks to form a continuous conductive framework penetrating the copper matrix, undertaking the main functions of current carrying and thermal conductivity. Nano-sized biochar (D50 = 5~15 μm) is distributed at the grain boundaries of the copper matrix, pinning dislocations through the Orowan strengthening mechanism to enhance the material's strength. Together, they form a two-scale, three-dimensional interpenetrating network structure, achieving spatial division and synergy of electrical conductivity, thermal conductivity, and strengthening functions.
[0023] Core Innovation Point 3: Resource Utilization of "Impurities" in Biochar
[0024] Based on a total composite material mass of 100 wt%, the formulation is as follows: 74.5–76.5 wt% copper powder, 10–12 wt% flake graphite, 8–10 wt% lithium hydroxide, 3–5 wt% agricultural and forestry waste-based biochar, and 0.3–0.8 wt% magnesium chloride hexahydrate. The silicon content in the biochar is 1.5–3.0 wt%. The SiO2 in the biochar reacts with Li2O and Mg²⁺ under HHO plasma activation. + In-situ reaction generates a (Li,Mg)₂SiO₃ gradient transition layer, turning waste into treasure. The carbon matrix of biochar also participates in the construction of a three-dimensional interpenetrating carbon framework, and alkali metals such as K and Na in its residual ash play a catalytic activation role in the plasma environment, promoting the rearrangement and graphitization of C-C bonds.
[0025] Core Innovation Point 4: Gradient Regulation of Interfacial Binding Energy
[0026] In the continuous gradient transition layer, ionic / metallic bonds dominate near the copper matrix, while covalent bonds dominate near the carbon framework. The interfacial bonding energy gradients from 45–65 J / m² near the copper side to 25–40 J / m² near the carbon side, with an overall interfacial shear strength ≥85 MPa. This gradient bonding energy design avoids brittle fracture caused by stress concentration at the interface, endowing the material with excellent thermal cycling stability.
[0027] II. Preparation Method of Copper-Carbon Interpenetrating Network Composites
[0028] The preparation method provided by this invention includes three core steps: mechanical alloying pretreatment (S0), vacuum preactivation (S1), and HHO plasma standing wave sintering (S2).
[0029] Step S0: Mechanical alloying pretreatment
[0030] Copper powder and carbon material were mixed at a mass ratio of 74.5-76.5:10-12, with anhydrous ethanol added as a dispersion medium. The mixture was then mechanically alloyed and ground in a planetary ball mill at 200-400 rpm for 2-6 hours. This step achieves three functions: (a) mechanically adhering the copper powder uniformly to the surface of the carbon material, forming a core-shell composite powder; (b) introducing high dislocation density and lattice distortion onto the copper powder surface, increasing surface active sites; and (c) breaking the passivation layer on the copper powder surface, exposing the fresh metal surface. The ground slurry was then vacuum-dried at 50-80℃ for 8-16 hours and passed through a 100-200 mesh sieve for later use.
[0031] Step S1: Vacuum pre-activation
[0032] The composite powder obtained in step S0 is mixed evenly with a lithium source compound (lithium hydroxide), silicon-containing biochar, and a magnesium source compound (magnesium chloride hexahydrate). The mixture is then heated in a vacuum environment to 400-500°C (preferably 450°C) and held at that temperature for 1-2 hours (preferably 1-1.5 hours), with a vacuum degree not exceeding 10. - ²Pa. The chemical reaction in this step is as follows:
[0033] Volatile byproducts (H2O, HCl) are extracted from the furnace by a vacuum pump, preventing porosity caused by gas release during subsequent high-temperature sintering. Meanwhile, Li2O and MgO are uniformly coated on the surfaces of copper powder and carbon materials in a nanoscale dispersion, providing precursors for subsequent interfacial reactions.
[0034] Step S2: HHO Plasma Standing Wave Sintering (Core Innovative Step)
[0035] HHO gas with a volume ratio of H2 to O2 of 2:1 is introduced into the furnace to maintain a slight positive pressure of 0.03~0.07MPa. A longitudinal standing wave field is generated by exciting the wave using a radio frequency field (frequency 10~60MHz, power 500~900W). The physical essence of the longitudinal standing wave field is to confine electromagnetic energy to the antinodes, forming energy spatial modulation: the electric field strength at the antinodes can reach several thousand V / m, but the standing wave structure causes the electron energy distribution to oscillate in a pulsed manner in time and is spatially confined within the volume of the antinodes, thus avoiding the accumulation of energy on a macroscopic scale.
[0036] HHO dissociation mechanism: Under the influence of a standing wave field, HHO gas undergoes non-equilibrium plasma dissociation, and the reaction chain is as follows:
[0037] The surface reaction rate constant k of active hydrogen atom H· is ≥ 5 × 10⁻⁶ - ³m / s, compared to the reduction rate of traditional molecular hydrogen (H2) (≈10 -5 The speed (m / s) is increased by 2-3 orders of magnitude. The key is that H· is a free radical, which can undergo a low-activation-energy direct electron transfer reaction with Cu₂O.
[0038] This reaction can be carried out at room temperature, overcoming the limitation that the reduction of molecular H2 requires high-temperature thermodynamic driving.
[0039] The dual role of OH in HHO: ·OH, as an oxidizing free radical, forms a dynamic equilibrium with H· in a standing wave field environment. When H· is in excess (a stoichiometric ratio of H2:O2 = 2:1 ensures that H· is dominant), the presence of ·OH is actually beneficial to maintaining the chemical activity of the plasma and promotes interface cleaning through the following reactions:
[0040] Simultaneously, ·OH can react with dangling bonds on the surface of carbon materials to generate COH active sites, promoting the covalent bonding of subsequent silicate phases with the carbon framework. OES monitoring showed that the steady-state concentration ratio of H· to ·OH was approximately 5:1 to 10:1, ensuring an overall reducing atmosphere. The degree of dissociation can be quantitatively characterized by the intensity ratio of Hα (656.28 nm) and Hβ (486.13 nm) spectral lines, which satisfy the relationship: I(Hα) / I(Hβ)∝exp(-1.89 / T) e For specific values, please refer to Table 8 of Example 3.
[0041] In-situ interface reaction: During the heat preservation stage at 1100~1150℃ (preferably 1120℃), SiO2 in biochar reacts with Li2O and MgO in a solid state under HHO plasma activation:
[0042] Due to Mg² + Directional diffusion occurs under the drive of a temperature gradient (concentration decreases from the copper side to the carbon side), forming a continuous gradient distribution of Mg content. Simultaneously, an axial pressure of 25–35 MPa (preferably 30 MPa) is applied, and the temperature is maintained for 10–20 min (preferably 15 min) to achieve densification sintering. After sintering, the temperature is lowered to room temperature at a rate of 3–8 °C / min.
[0043] III. Explosion-proof HHO plasma sintering furnace
[0044] The explosion-proof HHO plasma sintering furnace provided by this invention comprises five subsystems, forming a three-dimensional intrinsically safe system.
[0045] Subsystem 1: Radio Frequency Standing Wave Forming Structure (Intrinsically Safe Core)
[0046] It includes a spiral radio frequency induction coil 2 and a λ / 4 resonant cavity 3. The spiral radio frequency induction coil is made of copper hollow tube wound with cooling water flowing inside; one end of the λ / 4 resonant cavity is electrically connected to the coil, and the other end is grounded. When fed by a radio frequency power supply (13.56MHz, 500~900W), the two work together to form a longitudinal standing wave field 7 inside the furnace.
[0047] The physical basis of the explosion-proof mechanism of standing wave fields: the electric field strength at the standing wave node is 0, forming a cold barrier; ≥2.5
[0048] The Mach-speed supersonic jet forms an aerodynamic firewall; the <10μm flame arrester provides physical quenching. These three elements constitute a three-dimensional...
[0049] Develop an inherently safe system.
[0050] Subsystem 2: Supersonic air supply structure
[0051] The system includes an H2 gas source, an O2 gas source, a mass flow controller, a static mixer, and a multi-stage Venturi supersonic nozzle (9). H2 and O2 are precisely mixed at a volume ratio of 2:1 and then accelerated to a speed of not less than Mach 2.5 (approximately 850 m / s) by the multi-stage Venturi nozzle before being injected into the furnace. The core safety mechanism of the supersonic jet is that the upper limit of the propagation speed of the deflagration wave is approximately tens of m / s (for HHO / air premixed gas), while the momentum of the supersonic jet is much greater than the propagation speed of the deflagration wave, forming an "aerodynamic firewall" effect. Even if ignition occurs accidentally, the flame cannot travel back to the gas source against the supersonic airflow. At the same time, the supersonic jet disrupts the laminar flow conditions required for deflagration, suppressing the flame propagation speed to within 0.1 m / s.
[0052] Subsystem 3: Fire-retardant structure
[0053] This is a sintered metal powder flame arrester with an aperture <10μm and a response time <1ms. Its working principle is based on the slit quenching effect: when a flame enters a slit with an aperture much smaller than the flame quenching diameter, the heat conduction of the device wall rapidly carries away the heat from the combustion reaction, reducing the flame temperature below the ignition point. For HHO gas, the theoretical quenching diameter is approximately 0.2~0.5mm; this invention uses an aperture <10μm, providing a safety margin of over 20 times.
[0054] Subsystem 4: Pressure Monitoring and Control
[0055] Including a high-precision back pressure valve, it controls furnace pressure fluctuations within ±0.005MPa, maintaining the furnace pressure within a slightly positive pressure range of 0.03~0.07MPa. The slightly positive pressure design ensures that external air cannot infiltrate the furnace (avoiding the formation of a combustible mixture) while preventing leakage due to excessive pressure. The back pressure valve is linked to a PID controller, with a response time of <100ms.
[0056] Subsystem 5: Hydrogen Concentration Monitoring Array
[0057] The system includes multiple electrochemical hydrogen sensors, installed inside the furnace, in the exhaust pipe, and in the operating area, with a monitoring accuracy of no less than 0.1% LEL (Lower Explosive Limit). When any sensor detects an H2 concentration exceeding the 25% LEL safety threshold, the system automatically cuts off the gas supply valve, activates emergency ventilation, and triggers an audible and visual alarm. A three-level redundancy design ensures that a single sensor failure will not cause the entire safety system to malfunction.
[0058] Compared with the prior art, the present invention has the following beneficial effects: 1. For the first time, a ternary synergistic optimization of high electrical conductivity, high strength, and high thermal conductivity in copper-based composite materials was achieved. Volume resistivity (close to oxygen-free copper) Tensile strength 428 MPa (11.2% higher than GlidCop® AL-60), thermal conductivity (7.0% improvement) solved a common problem in this field that has persisted for nearly 30 years.
[0059] 2. For the first time, safe sintering of HHO in a slightly positive pressure closed environment was achieved, breaking the industry's application restrictions. Through a quadruple intrinsic safety mechanism of "standing wave explosion protection + supersonic pneumatic firewall + sintering metal flame arrestor + multi-parameter monitoring", the safety qualification rate of 50 furnaces in continuous operation reached 100%.
[0060] 3. It overturned the industry's perception that impurities in biochar are harmful, and transformed the impurities in biochar... Transform into The enhanced phase, with carbon as the main component forming an interpenetrating conductive network, and alkali metal ash catalyzing graphitization, enables the high-value utilization of all components of agricultural and forestry waste.
[0061] 4. HHO plasma in-situ reduction technology will The reduction rate is increased by 2 to 3 orders of magnitude, fundamentally eliminating the interface "dead layer" problem and reducing the interface resistance by 62.7%.
[0062] 5. The gradient transition layer design allows for a continuous and gradual transition from ionic to covalent bonds at the interface, resulting in an interfacial shear strength of 92 MPa and excellent thermal cycling stability. It represents a 75.9% improvement over existing products. Attached Figure Description
[0063] Figure 1 This is a structural diagram of the sintering furnace;
[0064] Figure 2 For equipment system block diagram;
[0065] Figure 3 A flowchart of the preparation process;
[0066] Figure 4 This is a hierarchical diagram of the material's microstructure. Detailed Implementation
[0067] The embodiments of the present invention will now be described in detail with reference to the accompanying drawings.
[0068] like Figures 1 to 4 As shown, the explosion-proof HHO plasma sintering furnace provided in this embodiment of the invention includes a furnace body 1, a radio frequency standing wave forming structure, a gas supply structure 4, a flame arrestor structure 5, and a pressure and concentration monitoring structure.
[0069] The furnace body 1 is a sealed cavity structure with an internal support tray for placing the mixed powder to be sintered. The top of the furnace body 1 is equipped with a furnace door for loading and unloading materials; the inner wall of the furnace body 1 is equipped with an insulation layer for heat preservation and uniform heat distribution.
[0070] The radio frequency standing wave forming structure includes a spiral radio frequency induction coil 2 and a λ / 4 resonant cavity 3. The spiral radio frequency induction coil 2 is wound around the outer periphery of the furnace body 1, and the λ / 4 resonant cavity 3 is configured in conjunction with the spiral radio frequency induction coil 2. In this embodiment, specifically: the spiral radio frequency induction coil 2 is made of a hollow copper tube and has cooling water circulating inside to prevent overheating; the λ / 4 resonant cavity 3 is a quarter-wavelength resonant cavity, one end of which is electrically connected to the spiral radio frequency induction coil 2, and the other end is grounded. When the radio frequency power supply feeds power to the spiral radio frequency induction coil 2, the λ / 4 resonant cavity 3 and the spiral radio frequency induction coil 2 work together to form a longitudinal standing wave field 7 within the furnace body 1. This longitudinal standing wave field 7 forms a stable field strength distribution with alternating antinodes and nodes within the furnace, ensuring that the gas temperature under the standing wave field remains below the auto-ignition point of HHO, avoiding energy concentration that could ignite the gas, and eliminating the risk of deflagration at its source.
[0071] The gas supply structure 4 is connected to the furnace body 1 and is used to supply HHO gas into the furnace body 1. In this embodiment, specifically: the gas supply structure 4 includes an H2 gas source, an O2 gas source, a mixer, and a multi-stage Venturi supersonic nozzle 9. The H2 gas source and the O2 gas source are connected to the mixer through a pressure reducing valve and a flow controller, respectively. The mixer mixes H2 and O2 at a volume ratio of 2:1 to form HHO gas. The multi-stage Venturi supersonic nozzle 9 is installed on the pipeline between the gas supply structure 4 and the furnace body 1, and its gas injection velocity is not less than Mach 2.5. Through supersonic injection, the HHO gas enters the furnace body 1 in the form of a high-speed jet, destroying the laminar flow conditions required for deflagration. Even if accidental ignition occurs, the flame propagation velocity can be suppressed to within 0.1 m / s.
[0072] The flame arrestor structure 5 is connected in series in the gas supply pipeline that supplies HHO gas to the furnace body 1, and is used to block flame backpropagation. In this embodiment, specifically: the flame arrestor structure 5 is a sintered metal powder flame arrestor with an aperture of less than 10 μm and a response time of less than 1 ms. When flame backpropagation occurs in the gas supply pipeline, the sintered metal powder flame arrestor blocks flame propagation within 1 ms through the slit quenching effect, ensuring the safety of the upstream gas source.
[0073] The pressure and concentration monitoring structure includes a back pressure valve 6 and a hydrogen concentration sensor array 8. The back pressure valve 6 is located at the exhaust port of the furnace body 1 and is used to control the furnace pressure. In this embodiment, specifically, the back pressure valve 6 is a high-precision back pressure valve, controlling the furnace pressure fluctuation within ±0.005 MPa and maintaining the furnace pressure within a slightly positive pressure range of 0.03 MPa to 0.07 MPa. The hydrogen concentration sensor array 8 is located inside and / or outside the furnace body 1 and is used to monitor the hydrogen concentration. In this embodiment, specifically, the hydrogen concentration sensor array 8 includes multiple electrochemical hydrogen sensors, respectively installed inside the furnace body 1, in the exhaust pipe, and in the operating area around the furnace body 1. Its monitoring accuracy is not less than 0.1% LEL, enabling comprehensive, blind-spot-free hydrogen concentration monitoring. When any sensor detects that the hydrogen concentration exceeds the safety threshold, the system automatically cuts off the gas supply and starts the exhaust.
[0074] The copper-carbon interpenetrating network composite material provided in this invention comprises a copper matrix, a carbon skeleton, and a continuous gradient transition layer located between the copper matrix and the carbon skeleton. This continuous gradient transition layer contains lithium, magnesium, silicon, and oxygen, with the magnesium element exhibiting a gradient distribution along the normal direction of the continuous gradient transition layer. The main crystalline phase of the continuous gradient transition layer is lithium magnesium silicate solid solution (Li). 1-x Mg xThe composite material is 2SiO3, where x decreases gradually from 0.30~0.70 to 0.05~0.20 along the normal direction. The transition layer thickness is 80~250nm, and the side near the carbon skeleton contains a Si-OC covalently bridged amorphous phase. In this embodiment, specifically: the thickness of the continuous gradient transition layer is 120nm~180nm, and the wetting angle between the continuous gradient transition layer and the copper substrate is less than 10°; in the continuous gradient transition layer, the magnesium content on the side near the copper substrate is higher than the magnesium content on the side near the carbon skeleton. Based on a total mass of 100wt% of the composite material, the composite material contains: 74.5wt%~76.5wt% copper powder, 10wt%~12wt% flake graphite, 8wt%~10wt% lithium hydroxide, 3wt%~5wt% agricultural and forestry waste-based biochar, and 0.3wt%~0.8wt% magnesium chloride hexahydrate, wherein the silicon content in the biochar is 1.5wt%~3.0wt%. The carbon framework consists of micron-sized flake graphite and nano-sized biochar. The micron-sized flake graphite overlaps to form a continuous conductive framework that runs through the copper matrix, while the nano-sized biochar is distributed at the grain boundaries of the copper matrix. Together, they form a two-scale three-dimensional interpenetrating network structure. The chemical composition of the continuous gradient transition layer is (Li,Mg)2SiO3.
[0075] The preparation method of copper-carbon interpenetrating network composite material provided in this embodiment of the invention includes two steps: S1 vacuum pre-activation and S2HHO plasma standing wave sintering.
[0076] S1: A mixed powder containing copper powder, carbon materials, lithium source compound, silicon-containing biochar, and magnesium source compound is placed in a vacuum environment, heated to 400℃~500℃ and held at that temperature to decompose the lithium source compound and remove volatile byproducts from the magnesium source compound. In this embodiment, specifically: the vacuum degree of the vacuum environment is not higher than 10. - The furnace is heated to 450℃ at 2 Pa for 1-1.5 hours. During this process, lithium hydroxide decomposes into Li₂O and releases water vapor, while magnesium chloride hexahydrate removes its water of crystallization and completely releases HCl gas. These volatile byproducts are extracted from the furnace by a vacuum pump, preventing the formation of pores during subsequent sintering.
[0077] S2: HHO gas is introduced into a vacuum environment while maintaining a slight positive pressure inside the furnace. A longitudinal standing wave field 7 is generated by excitation using a radio frequency field, dissociating the HHO gas into active free radicals to in-situ reduce the oxide layer on the surface of the copper powder. Subsequently, the temperature is increased and sintering is carried out under pressure to generate a lithium- and magnesium-containing silicate gradient transition layer in situ at the copper-carbon interface. After cooling, a copper-carbon interpenetrating network composite material is obtained. In step S2, the radio frequency is 10~60MHz, the power is 500~900W, and the H flux is ≥1×10¹. 9 m - ²·s -¹, heating rate 8~12℃ / min, sintering temperature 1100~1150℃, axial pressure 25~35MPa, holding time 10~20min, cooling rate 3~8℃ / min. The degree of dissociation of HHO gas ≥8%, determined by optical emission spectroscopy (OES) through the intensity ratio of Hα to Hβ spectral lines; the surface reaction rate constant k of active hydrogen atoms H· ≥5×10⁻⁶. - ³m / s. In this embodiment, specifically: the volume ratio of H2 to O2 in the HHO gas is 2:1, the furnace pressure is 0.03MPa~0.07MPa, the frequency of the radio frequency field is 13.56MHz, the power is 500W~900W, the holding sintering temperature is 1120℃, the applied pressure is 30MPa, and the holding time is 15min. The longitudinal standing wave field 7 dissociates the HHO gas into active hydrogen atoms and hydroxyl radicals, whose reducing power is about three orders of magnitude higher than that of conventional H2, and can completely peel off the Cu2O oxide layer on the surface and inside of the copper powder within seconds. During the sintering process, SiO2 in the biochar reacts with Li2O and Mg²⁺. + An in-situ reaction was carried out under HHO plasma activation to generate a continuous (Li,Mg)2SiO3 gradient transition layer with a thickness of about 150 nm at the interface between the copper matrix and the carbon skeleton.
[0078] Example 1: Preparation of composite materials under optimal formulation and process conditions
[0079] Electrolytic copper powder with a purity ≥99.9% and a particle size ≤45μm (D50=18.7μm, oxygen content 0.012wt%), and flake graphite with a purity ≥99.5% and a particle size ≤30μm (D50=8.2μm, carbon content 99.7wt%, ash content 0.06wt%) were selected.
[0080] Step S0 – Mechanical alloying pretreatment: Copper powder and flake graphite were mixed in a molar ratio of Cu:C = 1:0.35, and anhydrous ethanol was added as a dispersion medium. The mixture was then ground in a planetary ball mill at 300 rpm for 4 hours to allow the copper powder to uniformly adhere to the surface of the graphite flakes, forming a core-shell structure. The ground slurry was then vacuum dried at 60℃ for 12 hours and passed through a 200-mesh sieve to obtain copper-graphite composite powder.
[0081] Step S1 – Vacuum Pre-activation: The above composite powder was mixed evenly with 8.5 wt% lithium hydroxide, 4 wt% walnut shell biochar (Si content 2.4 wt%), and 0.5 wt% magnesium chloride hexahydrate. The mixture was then placed in a vacuum sintering furnace and evacuated to a vacuum of 5 × 10⁻⁶. - The temperature was increased to 450℃ at 5℃ / min and held for 1.2h. During this process, LiOH decomposed into Li2O, MgCl2·6H2O lost its water of crystallization and released HCl, and the byproducts were extracted by a vacuum pump.
[0082] Step S2 – HHO Plasma Standing Wave Sintering: The S1-treated mixed powder was loaded into a graphite mold with an inner diameter of 30 mm and placed in a sintering furnace. H2:O2 gas (H2:O2 = 2:1) was introduced at a flow rate of 3 L / min, maintaining a furnace pressure of 0.05 MPa. The radio frequency power supply (13.56 MHz, 800 W) was activated to create a longitudinal standing wave field within the furnace. Online OES monitoring showed an Hα / Hβ spectral line intensity ratio of 4.1, corresponding to an H2 dissociation degree of 28.4% and an H· flux of 4.9 × 10¹. 5 cm - ²·s - ¹.
[0083] Under an HHO plasma atmosphere, the temperature was increased to 1120℃ at a rate of 10℃ / min, while an axial pressure of 30MPa was applied, and the temperature was held for 15 min. The temperature was then decreased to room temperature at a rate of 5℃ / min. HHO gas was continuously supplied throughout the sintering process to ensure a continuous reducing atmosphere.
[0084] The measured values of the process parameters are shown in Table 1.
[0085] Table 1 Process parameters of Example 1
[0086] The obtained composite material was characterized by its microstructure and its properties were tested. The results are shown in Tables 2 and 3.
[0087] Table 2 Interface characterization results of Example 1
[0088] As shown in Table 2, the present invention forms a transition layer with a thickness of about 148 nm at the copper-graphite interface through in-situ reaction. The transition layer includes an outer Cu2O amorphous layer (5~12 nm) and an inner Cu nanocrystalline transition region, realizing a continuous compositional gradient from the ceramic interface to the metallic interface (x=0.52→0.08), a wetting angle as low as 7.3°, an interfacial bonding energy of 58 J / m², and a shear strength of 92 MPa.
[0089] The macroscopic performance of Example 1 was compared with that of the commercial GlidCop® AL-60, and the results are shown in Table 3.
[0090] Table 3. Comparison of macroscopic performance between Example 1 and GlidCop® AL-60
[0091] As shown in Tables 2 and 3, this invention forms a (Li,Mg)₂SiO₃ gradient transition layer with a thickness of approximately 148 nm at the copper-graphite interface through in-situ reaction, with a wetting angle as low as 7.3° and an interfacial shear strength of 92 MPa. The macroscopic properties are comprehensively superior to commercially available benchmark materials, especially in terms of thermal cycling stability and interfacial contact resistance.
[0092] The key node data of the 20 sampling points of the interface EDS line scan are shown in Table 4.
[0093] Table 4. Key nodes (partial) of EDS line scan interface in Example 1.
[0094] Table 4 shows that Mg, Li, and Si exhibit an asymmetric gradient distribution on both sides of the interface: on the copper side (positive value region), the element concentration decreases exponentially with increasing distance from the interface; on the carbon side (negative value region), the element concentration increases with increasing distance from the interface and then tends to plateau. This asymmetric distribution reflects the Mg²⁺... + The directional diffusion trend from the copper side to the carbon side, and the enrichment characteristics of SiO2 on the carbon side.
[0095] A blind test was conducted on Example 1 by a third-party testing organization (Quality Inspection Center of China Nonferrous Metals Industry Association), and the results are shown in Table 5.
[0096] Table 5. Results of Third-Party Blind Test Re-test
[0097] As shown in Table 5, the relative deviations between the third-party blind test retest results and the data from our laboratory are all less than 3%, indicating that the data are authentic and reliable.
[0098] Example 2: Effects of different biomass carbon sources on Si content and performance
[0099] Copper-graphite composite materials were prepared according to the method in Example 1, except that walnut shell carbon powder (Si content 2.4 wt%), rice husk carbon powder (Si content 3.8 wt%), and corn stalk carbon powder (Si content 1.2 wt%) were used to replace part of the flake graphite, with the addition amount being 15% of the total carbon mass. The results are shown in Table 6.
[0100] Table 6. Si content and performance of different biomass carbon sources in Example 2
[0101] As shown in Table 6, when the Si content is in the range of 1.5~3.8 wt%, the interfacial wetting angle is less than 10°, the interfacial bonding energy is higher than 50 J / m², and the tensile strength is greater than 400 MPa. When the Si content decreases to 1.2 wt% (sample C), the wetting angle increases to 9.8°, the bonding energy decreases to 46 J / m², and the tensile strength decreases to 389 MPa. Therefore, the preferred Si content in this invention is controlled within the range of 1.5~3.8 wt%.
[0102] Example 3: The Influence of Radio Frequency Power on Plasma Characteristics and Performance
[0103] Copper-graphite composite materials were prepared according to the method of Example 1, except that radio frequency plasma assistance was applied during the sintering process, and the radio frequency power was set to 400W, 600W, 800W and 1000W respectively. The effect of power on plasma characteristics and final performance was investigated, and the results are shown in Table 7.
[0104] Table 7 shows the effect of radio frequency power on plasma characteristics and performance in Example 3.
[0105]
[0106] As shown in Table 7, with increasing RF power, the H2 dissociation degree and H· flux monotonically increase, the interfacial transition layer thickness increases, the wetting angle decreases, and the volume resistivity decreases. Considering the balance between energy consumption and performance, the preferred RF power range for this invention is 600~800W. Below 600W, the dissociation degree is insufficient (<22%), limiting the reduction effect; above 800W, marginal benefits decrease and energy consumption increases sharply.
[0107] The OES spectral diagnostic data are shown in Table 8.
[0108] Table 8. Calculation of OES spectral line intensity and H2 dissociation degree
[0109] According to the collisional radiation model, the intensity ratio of the Hα / Hβ spectral lines is related to the electron temperature T. e The relationship is: I(Hα) / I(Hβ)∝exp(-1.89 / T) e From the data in Table 8, T can be obtained. e The range is 0.95~1.38 eV, corresponding to a H2 dissociation degree of 12.3%~32.1%. OES can be used as an effective means to monitor the dissociation degree in real time and realize closed-loop control of the sintering process.
[0110] Security verification
[0111] The safety of the production process of this invention is verified, including continuous operation stability testing and flame arrester performance testing.
[0112] Continuous operation safety data are shown in Table 9.
[0113] Table 950 Boiler Continuous Operation Safety Data
[0114] The flame return test results of the flame arrester are shown in Table 10.
[0115] Table 10 Flame Return Test Results of Flame Arresters
[0116] As shown in Tables 9 and 10, all safety indicators were within the control limits during the continuous operation of 50 furnaces. The flame arrester successfully blocked flame propagation within <1ms in 5 simulated flame return tests, proving that the process of this invention has excellent inherent safety.
[0117] Comparative Example
[0118] Comparative Example 1: Lack of mechanical alloying pretreatment
[0119] Copper-graphite composite materials were prepared according to the method in Example 1, with the difference that step S0 was omitted, and the composite powder was not subjected to mechanical alloying pretreatment. The copper powder and graphite sheets were directly dry-mixed and then sintered in a mold. This comparative example demonstrates that mechanical alloying pretreatment is a prerequisite for achieving uniform copper-carbon dispersion and interfacial reaction. The results showed severe segregation of copper and graphite, no transition layer forming at the interface, a wetting angle >120°, and an interfacial bonding energy <5 J / m². The composite material cracked upon demolding, making subsequent performance testing impossible.
[0120] Comparative Example 2: Sintering temperature lower than the lower limit of this invention
[0121] Copper-graphite composite materials were prepared according to the method of Example 1, with the difference that the sintering temperature in step S2 was set to 850℃ (lower than the lower limit of sintering temperature of 1100℃ in this invention). This comparative example demonstrates that a sintering temperature of 1100~1150℃ is a necessary condition for achieving sufficient interfacial reaction—below 1100℃, the solid-state reaction kinetics of Li2O and SiO2 are limited, and a continuous gradient transition layer cannot be generated. As a result, the interfacial transition layer thickness was only 32nm (far less than the lower limit of 80nm in this invention), the wetting angle was 18.7° (exceeding the upper limit of 10° in this invention), the interfacial bonding energy was 21J / m², the tensile strength was 312MPa, and the volume resistivity was 2.41×10⁻⁶. -8 Ω·m, the performance is significantly worse than that of Example 1.
[0122] Comparative Example 3: Lack of lithium / magnesium / silicon additives
[0123] Copper-graphite composite materials were prepared according to the method in Example 1, except that lithium hydroxide, biochar, and magnesium chloride hexahydrate were not added to the raw materials (i.e., only pure copper powder and flake graphite were used). This comparative example demonstrates that the synergistic effect of Li, Mg, and Si is key to the formation of the gradient transition layer—the absence of any one of these elements prevents the establishment of a chemical bond bridge between copper and carbon. The results showed no silicate transition layer forming at the interface, a wetting angle of 112°, an interfacial bonding energy of <3 J / m², and the composite material peeling off entirely along the interface during bending tests, with a tensile strength of only 187 MPa.
[0124] Table 11 summarizes the missing elements and failure modes in the comparison.
[0125]
[0126] In the radio frequency plasma-assisted sintering process of Example 3, the plasma composition was monitored online using optical emission spectroscopy (OES), and the degree of H2 dissociation was calculated based on the intensity ratio of Hα (656.3 nm) and Hβ (486.1 nm) spectral lines. The data are shown in Table 11.
[0127] Quantitative verification of the explosion-proof mechanism of standing wave field
[0128] To verify the explosion-proof mechanism of the standing wave field, a one-dimensional standing wave field plasma model was established. The radio frequency was set to f = 13.56 MHz, and the standing wave wavelength was λ = c / f ≈ 6.5 m. Within the furnace cavity length L = 0.5 m, the number of standing wave modes was L / (λ / 2) ≈ 0.15, meaning the furnace could accommodate approximately 0.15 half-wavelengths of standing waves, forming a single-peak standing wave distribution.
[0129] Standing wave electric field distribution: E(z) = 2E0sin(πz / L), where E0 is the amplitude of the traveling wave electric field. Taking E0 = 2kV / m (corresponding to 800W power), the maximum electric field E at the antinode is... max =4kV / m. Electron motion equation: Where ν is the collision frequency (ν≈10 in air). 8 s - (¹Order of magnitude). Numerical solutions show that the average electron energy at the antinodes is <0.5 eV, corresponding to a gas temperature <300℃, which is far below the auto-ignition point of HHO, 570℃.
[0130] At the node positions (z=0 and z=L), E=0, and electrons cannot obtain enough energy to excite HHO molecules, forming a natural "cold zone barrier." Even if the gas is accidentally ignited at the antinode, the flame will be extinguished when it reaches the node due to the sudden drop in energy and quenching by the vessel wall. This mechanism was experimentally confirmed through safety verification of 50 furnaces operating continuously (Table 9).
[0131] Phase transformation pathway of biochar during sintering
[0132] Biochar undergoes complex phase transformations during the sintering process of this invention, and all its components are utilized at high value: (a) Carbon matrix: Nanoscale biochar particles are distributed at the grain boundaries of the copper matrix and undergo partial graphitization at a sintering temperature of 1120℃ and a pressure of 30MPa (confirmed by XRD). 002 The strength increases by approximately 80–100 MPa (from 3.45 Å to 3.37 Å) by pinning dislocation movements in the copper matrix through the Orowan strengthening mechanism. Simultaneously, alkali metals (K, Na) in the biochar catalyze graphitization.
[0133] (b) SiO2 component: Amorphous SiO2 in biochar undergoes a stepwise solid-phase reaction with Li2O and MgO under HHO plasma activation, ultimately forming a (Li,Mg)2SiO3 solid solution. The reaction pathway is as follows: Mg² + The doping causes a continuous change in the lattice parameters of lithium silicate, forming a gradient transition layer.
[0134] (c) Alkali metal ash: Alkali metal oxides such as K2O and Na2O partially volatilize during sintering (reducing the oxygen partial pressure of the system) and partially dissolve in the lithium silicate matrix, acting as flux and reducing the activation energy of interfacial reactions.
[0135] This invention comprises three inventive subjects: copper-carbon interpenetrating network composite material (product), its preparation method (method), and explosion-proof HHO plasma sintering furnace (equipment). These three subjects share specific technical connections and synergies. (1) The sintering furnace is a special equipment tailored to the preparation process of this specific material. The radio frequency standing wave parameters (frequency, power), the supersonic jet parameters of the gas supply structure, the specifications of the flame arrester, etc. in the furnace are all designed around the core process of HHO plasma standing wave sintering, which directly serves the in-situ generation of the gradient transition layer in the composite material.
[0136] (2) The preparation method is a link that connects the composite material to the sintering furnace. The HHO plasma standing wave sintering process in step S2 of the method must be carried out in the sintering furnace, and each process parameter of the method (radio frequency, power, HHO flow rate, pressure, etc.) corresponds one-to-one with each structural parameter of the sintering furnace.
[0137] (3) The three parties work together to solve a general technical problem: how to achieve chemical bonding at the copper-carbon interface under safe conditions, and prepare copper-based composite materials with high conductivity, high strength and high thermal conductivity. The product is obtained through the method, and the method is implemented through the equipment, forming a complete technology chain.
[0138] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A copper-carbon interpenetrating network composite material, characterized in that, It comprises a copper substrate, a carbon skeleton, and a continuous gradient transition layer located between the copper substrate and the carbon skeleton; The main crystalline phase of the continuous gradient transition layer is lithium magnesium silicate solid solution (Li 1-x Mg x )2SiO3, where x represents the atomic ratio of Mg / (Li+Mg), and x decreases from 0.30~0.70 near the copper matrix to 0.05~0.20 near the carbon skeleton along the normal direction from the copper matrix to the carbon skeleton. The thickness of the continuous gradient transition layer is 80~250nm, and the side near the carbon framework contains a Si-OC covalently bridged amorphous phase. The wetting angle θ at the interface between the continuous gradient transition layer and the copper substrate satisfies 0° < θ < 10°; Based on a total mass of 100 wt% of the composite material, the composite material comprises: 74.5-76.5 wt% copper powder, 10-12 wt% flake graphite, 8-10 wt% lithium hydroxide, 3-5 wt% agricultural and forestry waste-based biochar, and 0.3-0.8 wt% magnesium chloride hexahydrate, wherein the silicon content of the biochar is 1.5-3.0 wt%. The carbon framework comprises micron-sized flake graphite that overlaps to form a continuous conductive network and submicron-sized biochar distributed at the grain boundaries of the copper matrix.
2. The copper-carbon interpenetrating network composite material according to claim 1, characterized in that, The median particle size D50 of the micron-sized flake graphite is 5~10μm, and the median particle size D50 of the submicron-sized biochar is 0.5~15μm; the biochar is derived from one or more of walnut shells, coconut shells or rice husks, and is obtained by pyrolysis in an inert atmosphere at 500~700℃ followed by crushing and sieving.
3. The copper-carbon interpenetrating network composite material according to claim 1, characterized in that, In the continuous gradient transition layer, the side near the copper matrix is dominated by ionic / metallic bonds, while the side near the carbon framework is dominated by covalent bonds. The interfacial bonding energy changes from 45~65 J / m² near the copper side to 25~40 J / m² near the carbon side, and the overall interfacial shear strength is ≥85 MPa.
4. A method for preparing a copper-carbon interpenetrating network composite material as described in any one of claims 1 to 3, characterized in that, Includes the following steps: S0: Copper powder and flake graphite are mixed in the mass ratio described above, anhydrous ethanol is added as a dispersion medium, and mechanical alloying grinding is carried out in a planetary ball mill at 200~400rpm for 2~6h. Then, the mixture is vacuum dried at 50~80℃ for 8~16h and passed through a 100~200 mesh sieve to obtain composite powder. S1: Mix the composite powder obtained in step S0 with lithium hydroxide, silicon-containing biochar and magnesium chloride hexahydrate, and place it under a vacuum of ≤10°C. - In an environment of 2Pa, heat to 400~500℃ and keep warm for 1~2h to decompose lithium hydroxide into Li2O and remove volatile byproducts; S2: Introduce HHO gas with a volume ratio of H2 to O2 of 2:1 into the furnace and maintain a slight positive pressure of 0.03~0.07MPa inside the furnace; use a radio frequency field to excite and form a longitudinal standing wave field with a frequency of 10~60MHz and a power of 500~900W to dissociate HHO into active hydrogen atoms (H·) and hydroxyl radicals (·OH), wherein the H· flux is ≥1×10¹ 9 m - ²·s - ¹, H· Surface reaction rate constant k ≥ 5 × 10 - ³m / s; then, the temperature is increased to 1100~1150℃ at a rate of 8~12℃ / min, while an axial pressure of 25~35MPa is applied, and the temperature is held for 10~20min for densification sintering, in situ generating the (Li) at the copper-carbon interface. 1-x Mg x A continuous gradient transition layer of 2SiO3 was formed; after sintering, the temperature was lowered to room temperature at a rate of 3~8℃ / min.
5. The preparation method according to claim 4, characterized in that, In step S2, the average electron energy at the antinodes of the longitudinal standing wave field is ≤0.5eV, corresponding to a gas dynamic temperature <300℃; the degree of dissociation of the HHO gas is ≥8%, which is determined by optical emission spectroscopy (OES) through the intensity ratio of Hα (656.28nm) and Hβ (486.13nm) spectral lines.
6. An explosion-proof HHO plasma sintering furnace for implementing the preparation method as described in claim 4 or 5, characterized in that, include: The furnace body (1) is a closed cavity structure with a support tray and insulation layer inside; The radio frequency standing wave forming structure includes a spiral radio frequency induction coil (2) and a λ / 4 resonant cavity (3). The two work together to form a longitudinal standing wave field (7) in the furnace body (1). The average electron energy at the antinode of the standing wave is ≤0.5eV, corresponding to a gas dynamic temperature <300℃. The electric field strength at the standing wave node is 0, forming a flame quenching cold barrier. The gas supply structure (4) includes an H2 gas source, an O2 gas source and a multi-stage Venturi supersonic nozzle (9), with an HHO gas injection speed ≥ Mach 2.5, forming a pneumatic firewall; The flame arrestor structure (5) is a sintered metal powder flame arrestor connected in series with the gas supply pipeline, with an aperture of <10μm and a response time of <1ms. The pressure and concentration monitoring structure includes a back pressure valve (6) and a hydrogen concentration sensor array (8) to maintain a furnace pressure of 0.03~0.07MPa with a slight positive pressure and a hydrogen concentration monitoring accuracy of ≤0.1%LEL.
7. The explosion-proof HHO plasma sintering furnace according to claim 6, characterized in that, The spiral radio frequency induction coil (2) is made of copper hollow tube and is circulated with cooling water; one end of the λ / 4 resonant cavity (3) is electrically connected to the spiral radio frequency induction coil (2), and the other end is grounded.