A composite structure of steel mesh anchoring and high-temperature bonding for synergistic reinforcement against high-temperature negative pressure and polytetrafluoroethylene, and its isostatic pressing molding and sintering preparation process.
By using an isostatic pressing molding sintering process involving sandblasting the inner wall of the steel shell, coating with a high-temperature adhesive, and laying a stainless steel mesh, the problems of delamination, bulging, and cracking of the steel-PTFE composite structure under high-temperature conditions were solved, achieving a multi-layer composite structure with high strength and high stability, suitable for long-term high-temperature conditions up to 200℃.
Patent Information
- Application Number
- CN202611301742.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies in steel-PTFE composite structures under high-temperature conditions suffer from weak interfacial bonding, inability to buffer thermal stress, and lack of mechanical anchoring structures, leading to problems such as delamination, bulging, and cracking, and thus failing to meet the requirements for long-term continuous operation at 200℃.
The process employs an isostatic pressing molding and sintering process that combines steel mesh anchoring with high-temperature bonding. By sandblasting the inner wall of the steel shell to create a rough surface, applying a high-temperature adhesive, bonding a PTFE sheet, and then covering it with a stainless steel mesh, the process involves isostatic pressing and high-temperature sintering to form a multi-layered composite structure. This structure includes a high-temperature bonding transition layer, a PTFE inner lining, a stainless steel mesh, and a dense PTFE sintered surface layer, achieving a dual combination of interfacial bonding and mechanical anchoring.
It achieves high strength and high stability of the composite layer under high temperature conditions of 200℃, eliminates interface peeling and bulging cracking, improves service life, and is suitable for corrosion resistance and thermal cycling resistance under long-term high temperature conditions of 200℃. Its service life is 3-5 times that of traditional composite processes.
Smart Images

Figure CN123104176A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to, but is not limited to, the field of metal and fluoroplastic composite molding technology, and particularly relates to a steel mesh anchoring-high temperature bonding synergistic enhancement high temperature negative pressure resistant steel-polytetrafluoroethylene composite structure and its isostatic pressing molding sintering preparation process. Background Technology
[0002] PTFE (polytetrafluoroethylene) material possesses excellent resistance to high and low temperatures, corrosion, aging, insulation, and self-lubrication, making it a core material for corrosion-resistant linings inside the casings of chemical, energy, environmental, and pressure equipment. However, the difference in thermal expansion coefficients between PTFE and the steel matrix is significant (PTFE's linear expansion coefficient is approximately 10 times that of steel), and PTFE has extremely low surface energy, making it difficult to bond. Consequently, under high-temperature conditions (such as 200°C), linings manufactured using traditional composite processes are prone to delamination, bulging, and cracking.
[0003] Currently, the mainstream processes for steel-PTFE composite molding in the industry can be mainly divided into the following three categories:
[0004] Category 1: Steel shell welded with steel mesh followed by PTFE powder molding process. This process enhances bonding strength through physical interlocking of the steel mesh, but relies solely on physical interlocking without an interfacial bonding transition layer. The thermal expansion coefficients of the steel body and PTFE differ greatly. Under continuous high-temperature conditions of 200℃, the deformation of the metal steel body and fluoroplastic is asynchronous, making it prone to interfacial loosening, delamination, and bulging. Furthermore, the high-temperature creep relaxation of PTFE makes it easy to peel off and bulge from the steel mesh, resulting in a short service life.
[0005] The second type is the steel body sandblasting + PTFE sheet sodium treatment + high-temperature epoxy resin bonding process. This process relies on adhesives to achieve bonding, but epoxy adhesives typically have a long-term temperature resistance below 180℃. At 200℃, the adhesive layer is prone to aging, carbonization, failure, and detachment, resulting in a sharp decrease in bonding strength. At the same time, the PTFE sheet after sodium treatment becomes more brittle, and the inner lining is prone to cracking and overall detachment after high-temperature thermal cycling.
[0006] The third type: sandblasting + PTFE board roughening + PFA composite sintering process. This process uses an expandable material to fill and sinter, but there is no mechanical reinforcement structure. It only relies on the fusion bonding of materials, resulting in low overall bonding strength. Under high temperature conditions, the stress of the inner lining cannot be released, and long-term use will inevitably lead to bulging, delamination, and local cracking failure.
[0007] In summary, existing traditional processes all suffer from core defects such as weak bonding at high-temperature interfaces, inability to buffer thermal stress, lack of mechanical anchoring structures, and poor high-temperature stability. They cannot meet the requirements for the use of steel-fluorine composite structures under long-term continuous operation at 200℃. The industry urgently needs a new integrated composite molding process that can completely solve the problems of high-temperature delamination, bulging, and cracking. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of existing PTFE steel composite processes, such as poor high-temperature resistance, easy delamination and bulging, lining cracking, and low bonding strength. This invention provides a high-temperature negative pressure resistant steel-PTFE composite structure with synergistic reinforcement through steel mesh anchoring and high-temperature bonding, and its isostatic pressing molding and sintering preparation process. By integrating the advantages of traditional molding, bonding, and sintering processes, and combining multiple technologies such as bonding transition, mechanical anchoring, isostatic pressing densification, and high-temperature fusion integrated sintering, this invention achieves a high-strength, high-stability composite of the steel body and PTFE layer, meeting the requirements for long-term high-temperature operation at 200℃, and effectively solving the problems of uneven thermal expansion and contraction, interface delamination, bulging, and cracking of the composite layer under high-temperature conditions.
[0009] This invention is achieved through an isostatic pressing molding and sintering process for preparing a high-temperature negative pressure resistant steel-PTFE composite structure, which synergistically enhances the steel mesh anchoring and high-temperature bonding. The process includes the following steps:
[0010] Step 1: Perform surface pretreatment on the inner wall of the steel shell to be laminated, so that the inner wall of the steel shell to be laminated forms a rough and clean surface;
[0011] Step 2: Apply a high-temperature adhesive to the pre-treated steel shell inner wall to be laminated and pre-dry it to form a high-temperature bonding transition layer.
[0012] Step 3: Attach the polytetrafluoroethylene (PTFE) sheet to the surface of the high-temperature adhesive transition layer and compact it to form a PTFE inner liner.
[0013] Step 4: Lay a stainless steel mesh on the inner surface of the polytetrafluoroethylene liner, and fix the stainless steel mesh to the steel shell by multi-point spot welding, so that the stainless steel mesh is pressed onto the surface of the polytetrafluoroethylene liner.
[0014] Step 5: Lay polytetrafluoroethylene powder on the surface of the stainless steel mesh so that the polytetrafluoroethylene powder fills the mesh openings of the stainless steel mesh and covers the inner working surface.
[0015] Step 6: Perform isostatic pressing on the steel shell on which the polytetrafluoroethylene powder is laid, so that the polytetrafluoroethylene powder enters the mesh of the stainless steel mesh and is compacted and adhered to the polytetrafluoroethylene inner lining plate.
[0016] Step 7: Perform gradient heating high-temperature sintering on the integral workpiece after isostatic pressing, so that the polytetrafluoroethylene powder passes through the mesh of the stainless steel mesh and is sintered and fused with the polytetrafluoroethylene inner liner. The stainless steel mesh is embedded between the polytetrafluoroethylene inner liner and the dense polytetrafluoroethylene surface layer formed by sintering, and the high-temperature bonding transition layer is activated during the high-temperature sintering process. After cooling, a steel-polytetrafluoroethylene composite structure is formed.
[0017] Furthermore, the surface pretreatment involves sandblasting the inner wall of the steel shell to be composited with brown corundum abrasive. The sandblasting pressure is 0.4–0.7 MPa, the surface roughness after treatment is 40–75 μm, the surface cleanliness is not lower than Sa2.5, and the treated surface is free of floating dust and residual impurities.
[0018] Furthermore, the high-temperature adhesive is a fluorine-based high-temperature adhesive that can withstand temperatures not lower than 220°C, the thickness of the high-temperature bonding transition layer is 0.15–0.3 mm, the pre-drying temperature is 80–120°C, and the pre-drying time is 30–60 min.
[0019] Furthermore, the stainless steel mesh has a mesh size of 3-8mm and a thickness of 2mm. The edges and mesh intersections of the stainless steel mesh are fixed to the steel shell by multi-point spot welding. The spacing between the spot welding points is 20-40mm. After spot welding, the stainless steel mesh is not loose or warped and fits tightly against the surface of the polytetrafluoroethylene lining plate.
[0020] Furthermore, the isostatic pressing pressure is 15-30 MPa, the holding time is 10-25 min, and uniform pressure is applied throughout the entire area;
[0021] Before high-temperature sintering, the molded integral workpiece is filled with high-temperature resistant expansion particles and compacted. After the cover plate is closed and tightened, high-temperature sintering is carried out.
[0022] The heating rate of the high-temperature sintering is 2-5°C per minute, the final sintering temperature is 360-380°C, the constant temperature sintering time is 60-120 minutes, and the furnace is naturally cooled to room temperature after sintering.
[0023] The present invention also provides a steel mesh anchoring and high temperature bonding synergistic enhancement high temperature negative pressure resistant steel-polytetrafluoroethylene composite structure, which includes, from the outside to the inside, a steel shell base, a high temperature bonding transition layer, a polytetrafluoroethylene inner lining plate, a stainless steel mesh and a dense polytetrafluoroethylene sintered surface layer.
[0024] The high-temperature adhesive transition layer is disposed between the steel shell base and the polytetrafluoroethylene inner liner, and the polytetrafluoroethylene inner liner is attached to the inner wall of the steel shell base through the high-temperature adhesive transition layer.
[0025] The stainless steel mesh is laid on the inner surface of the polytetrafluoroethylene lining plate and fixed to the steel shell by multi-point spot welding;
[0026] The dense polytetrafluoroethylene sintered surface layer is filled with the mesh of the stainless steel mesh, and forms a continuous sintered fusion structure with the polytetrafluoroethylene inner liner through the mesh. The stainless steel mesh is embedded between the polytetrafluoroethylene inner liner and the dense polytetrafluoroethylene sintered surface layer.
[0027] Furthermore, the inner wall of the steel shell substrate in contact with the high-temperature adhesive transition layer has a rough surface with a roughness of 40–75 μm.
[0028] Furthermore, the high-temperature bonding transition layer is formed by a fluorine-based high-temperature adhesive that can withstand temperatures of not less than 220°C, and the thickness of the high-temperature bonding transition layer is 0.15–0.3 mm.
[0029] Furthermore, the stainless steel mesh has a mesh size of 3-8 mm and a thickness of 2 mm. The edges and mesh intersections of the stainless steel mesh form multiple spot-welded fixing positions with the steel shell, and the spacing between adjacent spot-welded fixing positions is 20-40 mm.
[0030] Furthermore, the PTFE inner liner and the high-temperature adhesive transition layer are bonded together in a bubble-free and gap-free manner. The stainless steel mesh is fixed to the surface of the PTFE inner liner without loosening or warping. The dense PTFE sintered surface layer continuously fills the mesh openings of the stainless steel mesh and covers the inner liner working surface.
[0031] Based on the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solution to be protected by this invention are as follows:
[0032] This invention features a double-layer protective structure to prevent delamination at high temperatures. A high-temperature-specific adhesive transition layer is installed at the bottom to compensate for the difference in thermal expansion coefficients between steel and fluoroplastics, buffering high-temperature deformation stress. The surface steel mesh is mechanically anchored to lock the overall PTFE structure. This combination of chemical bonding and mechanical fixation forms a three-dimensional interlocking structure, resulting in a significantly stronger interface bond than simple adhesive or molding processes. This completely solves the delamination problems caused by traditional adhesive failure and loose steel mesh fitting.
[0033] This invention utilizes isostatic pressing to eliminate bulging and voids. It employs full-area high-pressure isostatic pressing, replacing traditional ordinary molding and natural sintering, ensuring that the PTFE powder completely fills the steel mesh pores, adheres without air bubbles, and achieves an extremely dense internal structure. This prevents gas expansion and bulging, as well as interlayer separation, at high temperatures.
[0034] This invention features integrated fusion sintering, eliminating the possibility of lining cracking. The gradient heating sintering process avoids stress concentration caused by rapid heating and cooling. The inner PTFE board and the outer PTFE powder are fused and cross-linked into a whole, with a steel mesh embedded inside the fluoroplastic layer. This disperses high-temperature stress and also acts as a barrier to prevent crack propagation. Even if micro-cracks occur locally, the steel mesh can bridge and stop the cracks, preventing through-cracks in the lining and completely solving the defects of brittle cracking and localized damage in traditional processes.
[0035] This invention is suitable for long-term high-temperature operation at 200℃, exhibiting extremely high stability. The overall composite structure has no weak adhesive layers, no loose structures, and no internal voids. The adhesive layers used are perfluoropolymers, capable of withstanding temperatures above 250℃ for extended periods. Combined with the inherent temperature resistance of PTFE, this ensures that the adhesive interface does not age or fail under 200℃ conditions. It can operate stably under continuous high-temperature conditions at 200℃ for extended periods, with significantly improved corrosion resistance, resistance to thermal cycling, and high-pressure resistance. Its service life is 3-5 times that of traditional composite processes.
[0036] This invention features strong process compatibility and a wide range of applications. It can be adapted to the processing of various steel shells, cylinders, and cavity linings. The process steps are simple, highly controllable, and suitable for industrial mass production. Attached Figure Description
[0037] Figure 1 This is a flowchart of the isostatic pressing molding and sintering preparation process of the steel mesh anchoring-high temperature bonding synergistic reinforcement high temperature negative pressure resistant steel-polytetrafluoroethylene composite structure provided in the embodiments of the present invention;
[0038] Figure 2 This is a detailed flow chart of the isostatic pressing molding and sintering preparation process of a steel mesh anchoring-high temperature bonding synergistic reinforcement high temperature negative pressure resistant steel-polytetrafluoroethylene composite structure provided by an embodiment of the present invention;
[0039] Figure 3 This is a schematic diagram of the layered cross-section of the overall composite structure provided in an embodiment of the present invention;
[0040] Figure 4 This is a schematic diagram (top view) of the dot welding fixing provided in an embodiment of the present invention.
[0041] Figure 5 This is a schematic diagram of the isostatic pressing device provided in an embodiment of the present invention;
[0042] Figure 6 This is an overall filling and sintering diagram of the preparation process provided in the embodiments of the present invention;
[0043] Figure 7 This is a sandblasted shell product diagram provided in an embodiment of the present invention;
[0044] Figure 8 This is a product image of welded steel mesh provided in an embodiment of the present invention;
[0045] Figure 9 This is a product image of the finished product lining provided in an embodiment of the present invention;
[0046] In the diagram: 1. Steel shell base; 2. High-temperature fluorine-based adhesive transition layer; 3. PTFE inner lining substrate; 4. Spot-welded anchored stainless steel mesh; 5. Dense PTFE sintered surface layer. Detailed Implementation
[0047] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0048] like Figure 1 As shown in the figure, the isostatic pressing molding and sintering preparation process of a high-temperature negative pressure resistant steel-polytetrafluoroethylene composite structure provided by the embodiment of the present invention is characterized by including the following steps:
[0049] S101, perform surface pretreatment on the inner wall of the steel shell to be laminated, so that the inner wall of the steel shell to be laminated forms a rough and clean surface;
[0050] S102, a high-temperature adhesive is applied to the inner wall of the pretreated steel shell to be composited and pre-dried to form a high-temperature bonding transition layer.
[0051] S103, the polytetrafluoroethylene sheet is attached to the surface of the high-temperature adhesive transition layer and compacted to form a polytetrafluoroethylene inner liner.
[0052] S104, a stainless steel mesh is laid on the inner surface of the polytetrafluoroethylene liner, and the stainless steel mesh is fixed to the steel shell by multi-point spot welding, so that the stainless steel mesh is pressed onto the surface of the polytetrafluoroethylene liner.
[0053] S105, polytetrafluoroethylene powder is laid on the surface of the stainless steel mesh, so that the polytetrafluoroethylene powder fills the mesh of the stainless steel mesh and covers the inner working surface.
[0054] S106, the steel shell on which the polytetrafluoroethylene powder is laid is subjected to isostatic pressing, so that the polytetrafluoroethylene powder enters the mesh of the stainless steel mesh and is compacted and adhered to the polytetrafluoroethylene inner lining plate.
[0055] S107, the integral workpiece after isostatic pressing is subjected to gradient heating high-temperature sintering, so that the polytetrafluoroethylene powder passes through the mesh of the stainless steel mesh and is sintered and fused with the polytetrafluoroethylene inner liner. The stainless steel mesh is embedded between the polytetrafluoroethylene inner liner and the dense polytetrafluoroethylene surface layer formed by sintering, and the high-temperature bonding transition layer is activated during the high-temperature sintering process. After cooling, a steel-polytetrafluoroethylene composite structure is formed.
[0056] The surface pretreatment provided in this embodiment of the invention uses brown corundum abrasive to sandblast the inner wall of the steel shell to be composited. The sandblasting pressure is 0.4 to 0.7 MPa, the surface roughness after treatment is 40 to 75 μm, the surface cleanliness is not lower than Sa2.5 grade, and the treated surface is free of floating dust and residual impurities.
[0057] The high-temperature adhesive provided in this embodiment of the invention is a fluorine-based high-temperature adhesive that can withstand temperatures not lower than 220°C. The thickness of the high-temperature adhesive transition layer is 0.15–0.3 mm, the pre-drying temperature is 80–120°C, and the pre-drying time is 30–60 min.
[0058] The stainless steel mesh provided in this embodiment of the invention has a mesh size of 3-8mm and a thickness of 2mm. The edges and grid intersections of the stainless steel mesh are fixed to the steel shell by multi-point spot welding. The spacing between the spot welding points is 20-40mm. After spot welding, the stainless steel mesh is not loose or warped and fits tightly against the surface of the polytetrafluoroethylene lining plate.
[0059] The isostatic pressing provided in this embodiment of the invention has a pressure of 15-30 MPa and a holding time of 10-25 min, and adopts uniform pressure application over the entire area;
[0060] Before high-temperature sintering, the molded integral workpiece is filled with high-temperature resistant expansion particles and compacted. After the cover plate is closed and tightened, high-temperature sintering is carried out.
[0061] The heating rate of the high-temperature sintering is 2-5°C per minute, the final sintering temperature is 360-380°C, the constant temperature sintering time is 60-120 minutes, and the furnace is naturally cooled to room temperature after sintering.
[0062] The present invention provides a steel mesh anchoring and high-temperature bonding synergistic enhancement high-temperature negative pressure resistant steel-polytetrafluoroethylene composite structure, which, from the outside to the inside, includes a steel shell base, a high-temperature bonding transition layer, a polytetrafluoroethylene inner lining plate, a stainless steel mesh, and a dense polytetrafluoroethylene sintered surface layer.
[0063] The high-temperature adhesive transition layer is disposed between the steel shell base and the polytetrafluoroethylene inner liner, and the polytetrafluoroethylene inner liner is attached to the inner wall of the steel shell base through the high-temperature adhesive transition layer.
[0064] The stainless steel mesh is laid on the inner surface of the polytetrafluoroethylene lining plate and fixed to the steel shell by multi-point spot welding;
[0065] The dense polytetrafluoroethylene sintered surface layer is filled with the mesh of the stainless steel mesh, and forms a continuous sintered fusion structure with the polytetrafluoroethylene inner liner through the mesh. The stainless steel mesh is embedded between the polytetrafluoroethylene inner liner and the dense polytetrafluoroethylene sintered surface layer.
[0066] In this embodiment of the invention, the inner wall of the steel shell substrate in contact with the high-temperature adhesive transition layer is a rough surface, and the roughness of the rough surface is 40-75 μm.
[0067] The high-temperature bonding transition layer provided in this embodiment of the invention is formed by a fluorine-based high-temperature adhesive that can withstand temperatures of not less than 220°C, and the thickness of the high-temperature bonding transition layer is 0.15 to 0.3 mm.
[0068] The stainless steel mesh provided in this embodiment of the invention has a mesh size of 3-8mm and a thickness of 2mm. The edges and mesh intersections of the stainless steel mesh form multiple spot-welded fixing positions with the steel shell, and the spacing between adjacent spot-welded fixing positions is 20-40mm.
[0069] The polytetrafluoroethylene (PTFE) liner provided in this embodiment of the invention has a bubble-free and gap-free bonding structure between the PTFE liner and the high-temperature adhesive transition layer. The stainless steel mesh is fixed to the PTFE liner surface without loosening or warping. The dense PTFE sintered surface layer continuously fills the mesh holes of the stainless steel mesh and covers the working surface of the liner.
[0070] like Figure 2-9 As shown, this embodiment of the invention provides an isostatic pressing molding and sintering process for preparing a high-temperature resistant negative pressure steel-polytetrafluoroethylene composite structure through steel mesh anchoring-high-temperature bonding synergistic reinforcement, comprising the following steps:
[0071] 1) Steel substrate pretreatment: The inner wall of the steel shell to be composite is subjected to overall sandblasting and rust removal treatment to remove surface oxide scale, rust, oil and impurities, so that the steel surface forms a uniform rough surface. After pretreatment, the surface cleanliness of the steel body reaches Sa2.5 level or above.
[0072] 2) Apply a high-temperature adhesive transition layer: Apply a layer of high-temperature resistant special adhesive coating evenly to the rough surface of the pretreated steel body, let it stand at room temperature to cure and pre-dry, forming a flexible buffer adhesive transition layer between the steel body and the fluoroplastic.
[0073] 3) PTFE sheet lining and fixing: The pre-treated and flat PTFE sheet is bonded and wrapped on the surface of the high-temperature bonding transition layer inside the steel body. The entire process is bonded and compacted to ensure that the PTFE sheet and the bonding layer are completely bonded without bubbles or gaps.
[0074] 4) Steel mesh laying and spot welding reinforcement: A steel mesh is laid on the inner surface of the bonded PTFE board, and the edges and intersections of the steel mesh are fixed to the steel shell by multiple spot welding, so that the steel mesh is tightly pressed onto the surface of the PTFE board to form an integral mechanical anchoring skeleton.
[0075] 5) PTFE powder filling layer: PTFE ultrafine powder is evenly laid on the surface of the fixed steel mesh so that the powder completely fills the steel mesh pores and surface, covering the entire inner lining working surface.
[0076] 6) Isostatic pressing molding: The steel body with the material laid is placed into the isostatic pressing equipment, and a high-pressure uniform molding process is used to make the PTFE powder fully penetrate the steel mesh pores and tightly squeeze and bond with the inner PTFE board to achieve a preliminary dense composite of multi-layer structure.
[0077] 7) High-temperature integrated sintering: The molded integral workpiece is filled with high-temperature resistant expansion particles, compacted, covered with a cover plate, and screwed into an oven sintering furnace. A gradient heating high-temperature sintering process is adopted to melt the surface PTFE powder, penetrate the steel mesh, and melt and cross-link with the inner PTFE board to solidify. At the same time, the bottom adhesive layer is activated at high temperature. After cooling, a high-temperature resistant and negative pressure resistant composite structure with steel and fluorine integrated PTFE lining anti-corrosion layer is obtained.
[0078] In step 1), the sandblasting treatment uses brown corundum abrasive, with a sandblasting pressure of 0.4 to 0.7 MPa and a roughness controlled at 40 to 75 μm. After treatment, the surface is free of floating dust and residual impurities.
[0079] The high-temperature bonding transition layer mentioned in step 2) is a special fluorine-based adhesive that can withstand temperatures above 220°C. The coating thickness is controlled at 0.15-0.3 mm, the pre-drying temperature is 80-120°C, and the drying time is 30-60 min.
[0080] The steel mesh mentioned in step 4) is 304 / 316 stainless steel mesh with a mesh size of 3-8mm and a thickness of 2mm. The spot welding points are spaced 20-40mm apart. After spot welding, the steel mesh is ensured to be secure, without any looseness or warping, and to fit tightly against the PTFE sheet surface.
[0081] Step 6) The medium static pressure molding pressure is controlled at 15-30 MPa, the holding time is 10-25 min, and the uniform pressure application mode is adopted.
[0082] In step 7), the sintering process adopts a gradient heating method with a heating rate of 2-5℃ / min, a final sintering temperature of 360-380℃, constant temperature sintering for 60-120min, and natural cooling to room temperature with the furnace.
[0083] This invention utilizes the synergistic effect of "steel body surface pretreatment—high-temperature bonding transition—PTFE sheet pre-lining—steel mesh mechanical anchoring—PTFE powder filling—isostatic pressing densification—high-temperature integrated sintering" to construct a multi-layer composite anti-corrosion structure on the inner wall of a steel shell. This structure consists of a steel base, a high-temperature bonding transition layer, a PTFE sheet layer, a stainless steel mesh anchoring layer, and a sintered PTFE dense layer. This allows the PTFE lining to not only bond with the steel body through adhesion but also to form mechanical restraint and anchoring with the help of the steel mesh, thereby improving the overall stability of the composite structure under high temperature, negative pressure, and temperature cycling conditions.
[0084] First, the steel surface to be laminated is sandblasted to remove rust and roughen it. By removing oxide scale, rust, oil, and other impurities, the cleanliness of the steel surface is improved, and a micro-roughness structure is formed on the steel surface. This roughened surface increases the effective contact area between the steel and the high-temperature adhesive, and allows the adhesive to penetrate into the surface's micro-pits and texture structure. After curing, it forms a mechanical interlocking effect, providing a stable interface foundation for the subsequent composite layer.
[0085] Subsequently, a high-temperature resistant bonding transition layer is applied to the rough surface of the steel body, and pre-dried to form a continuous and uniform bonding interface. This transition layer, located between the rigid steel body and the PTFE material with large thermal expansion characteristics, not only serves as the initial bonding and fixing layer, but also buffers and disperses the interfacial stress caused by the difference in thermal expansion coefficients between the steel body and PTFE during heating. After the PTFE sheet is bonded to the surface of the bonding transition layer, it is compacted to remove interfacial air bubbles and voids, ensuring a continuous bond between the sheet and the inner wall of the steel body, thus forming the basic anti-corrosion isolation layer.
[0086] A stainless steel mesh is further laid on the inner surface of the PTFE sheet and fixed to the steel shell by multi-point spot welding. The steel mesh thus forms a mechanical anchoring framework covering the surface of the PTFE sheet. Compared to structures that rely solely on adhesives to fix the PTFE liner, the steel mesh provides multi-point, distributed restraint for the PTFE material. When negative pressure occurs inside the equipment, the PTFE liner experiences a peeling tendency from the shell direction towards the internal space of the equipment. The steel mesh can prevent localized bulging, warping, or complete detachment of the PTFE layer, thereby distributing the local peeling load to multiple welded fixing points and the steel structure, improving the liner's ability to withstand negative pressure loads.
[0087] After the steel mesh is installed, ultrafine PTFE powder is filled into the mesh openings and its surface, and isostatic pressing is applied to the entire composite structure with uniform pressure. Because isostatic pressing applies relatively uniform pressure to the PTFE powder from multiple directions, the loose powder enters the mesh openings and fully adheres to the underlying PTFE sheet. Simultaneously, it reduces porosity within the powder and between layers, allowing the PTFE sheet, steel mesh, and PTFE powder to form a pre-dense composite preform. Therefore, the steel mesh is not simply a surface covering the PTFE layer, but is clamped and embedded within the PTFE material system, creating conditions for the subsequent formation of a mechanically interlocking structure.
[0088] During the high-temperature sintering process, the workpiece is kept under pressure through the filling, compaction, and constraint of high-temperature resistant expansion particles and cover plates, reducing irregular deformation of the PTFE material caused by thermal softening and expansion. As the temperature gradually rises to the PTFE sintering temperature range, the PTFE powder on the surface of the steel mesh and in the mesh holes undergoes sintering and fusion, forming a continuous bond with the surface of the underlying PTFE sheet. This encapsulates and embeds the steel mesh within the sintered PTFE structure. After passing through the mesh holes, the PTFE material forms an interconnected continuous structure on both sides of the steel mesh, creating an anchoring effect similar to a mechanical interlock, resulting in a spatial interlock between the steel mesh and the PTFE layer.
[0089] Meanwhile, the high-temperature process further promotes the interfacial bonding and buffering function of the bottom high-temperature resistant adhesive transition layer. After sintering and natural cooling, the steel body, high-temperature adhesive transition layer, PTFE plate, steel mesh, and sintered PTFE layer form an integrated composite structure with the combined effects of interfacial bonding, mechanical anchoring of the steel mesh, and PTFE sintering fusion. Among them, the high-temperature adhesive layer mainly improves the interfacial bonding stability between the steel body and the PTFE bottom layer, the steel mesh mainly undertakes the functions of anti-peeling, anti-bulging, and negative pressure limiting, and the sintered PTFE layer forms a continuous and dense corrosion-resistant working surface. Through the synergistic effect of the above-mentioned multiple bonding mechanisms, the risk of delamination, bulging, shrinkage, or warping of traditional steel-lined PTFE structures due to thermal stress concentration and adhesive interface failure under high temperature, negative pressure, and thermal cycling conditions can be reduced. The composite lining combines the corrosion resistance of PTFE material with the mechanical stability of the steel mesh anchoring structure, thereby improving the reliability and durability of the steel-PTFE composite structure under complex working conditions.
[0090] like Figure 2 As shown, this embodiment of the invention provides a steel mesh anchoring-high temperature bonding synergistic reinforcement high temperature negative pressure resistant steel-polytetrafluoroethylene composite structure, which is prepared by the process described above. From the outside to the inside, it includes a steel shell base 1, a high temperature bonding transition layer 2, a PTFE inner liner 3, a spot-welded stainless steel mesh 4, and a dense PTFE sintered surface layer 5. The stainless steel mesh 4 is embedded between the PTFE inner liner 3 and the dense PTFE sintered surface layer 5 to form an integrated anchoring structure. The overall composite structure can withstand high temperature conditions of 200℃ for a long time without delamination, bulging, or cracking.
[0091] This invention utilizes a steel mesh anchoring-high-temperature bonding synergistic enhancement system to achieve a stable bond between the steel shell and the PTFE anti-corrosion lining through multi-layer composite, interfacial bonding, and mechanical anchoring. (For example...) Figure 2 , Figure 4As shown, the steel shell base 1 serves as the main load-bearing structure, providing rigid support for the composite structure. The high-temperature bonding transition layer 2 is set between the steel shell base 1 and the PTFE inner liner 3, ensuring that the PTFE inner liner 3 and the steel shell base 1 are tightly bonded. At the same time, it buffers and disperses the interfacial stress caused by the difference in thermal expansion characteristics between the steel and PTFE materials under high-temperature conditions, reducing the risk of interface separation caused by local stress concentration.
[0092] The PTFE liner 3 forms a basic corrosion-resistant isolation layer, isolating the steel shell base 1 from the internal corrosive media. A stainless steel mesh 4 is spot-welded and fixed to the inside of the PTFE liner 3. The stainless steel mesh 4 is mechanically fixed to the steel shell by spot welding and is embedded between the PTFE liner 3 and the dense PTFE sintered surface layer 5. When the equipment is under negative pressure, the PTFE liner is subjected to peeling forces into the equipment. The stainless steel mesh 4 can form multi-point distributed restraint and mechanical anchoring for the PTFE layer, distributing the local peeling load to the steel mesh and the steel shell, thus inhibiting bulging, warping, and delamination of the PTFE liner.
[0093] The dense PTFE sintered surface layer 5 is formed by molding and high-temperature sintering of PTFE powder. During the sintering process, the PTFE material enters and penetrates the mesh of the stainless steel mesh 4, fusing with the PTFE inner lining plate 3 to form a continuous structure. This allows the stainless steel mesh 4 to be encapsulated and embedded within the PTFE material, thus forming a mechanically interlocked integrated anchoring structure. Ultimately, a synergistic system is formed, consisting of "steel shell bearing capacity—high-temperature adhesive layer interface bonding and stress buffering—PTFE inner lining corrosion protection and isolation—steel mesh mechanical anchoring and limiting—dense PTFE surface layer overall corrosion protection." This enhances the interface stability of the composite structure under high temperature, negative pressure, and temperature change conditions, reducing the risk of delamination, bulging, and cracking.
[0094] The research and development process and evidence for embodiments of the present invention.
[0095] I. Fundamental Technical Contradictions and Difficulties in Solving Existing Technologies
[0096] The core technical contradiction facing PTFE-steel composite anti-corrosion structures lies in the inherent conflict between the physical properties of the materials and the extreme demands of operating conditions. This manifests in the following three levels of technical challenges:
[0097] (I) The problem of thermal expansion mismatch and uncontrolled interfacial stress
[0098] The linear expansion coefficient of PTFE is approximately 10~12×10 -5 / ℃) is approximately equivalent to carbon steel (approximately 1.0~1.2×10). -5The PTFE liner can expand by 10 times (at 200°C). Under typical industrial conditions (such as a 1m diameter reaction vessel), the theoretical thermal deformation difference between the PTFE liner and the steel shell can reach several millimeters. This inherent difference in physical properties means that when the equipment is heated from room temperature to 200°C, the PTFE liner tends to expand much more than the steel shell. However, due to the physical bond between the two, the PTFE is forced to compress, generating enormous compressive stress; when cooled, it generates enormous tensile stress.
[0099] The fundamental reason why existing technologies cannot effectively solve this problem is as follows: The first type of process (steel mesh molding) relies solely on the physical interlocking of the steel mesh, lacking a stress buffer layer. The thermal stress is entirely borne by the mechanical interlocking surface between PTFE and the steel mesh, leading to increased interfacial fretting wear under cyclic stress, ultimately causing loosening and delamination. The second type of process (adhesive bonding) has a certain buffering effect, but the glass transition temperature of epoxy adhesives is usually below 120°C. Under 200°C conditions, they are already in a rubbery state or even a viscous flow state, resulting in a loss of more than 80% of the bonding strength. Furthermore, thermo-oxidative aging causes the adhesive layer to become brittle and carbonized, losing its stress transmission ability. The third type of process (melt bonding) has no stress buffer design at all, and the thermal stress is directly applied to the fusion interface.
[0100] (ii) The problem of interfacial chemical inertness caused by the low surface energy of PTFE
[0101] PTFE has a highly symmetrical molecular structure and a surface energy of only 18.5 mN / m, making it a typical low-surface-energy, difficult-to-bond material. Its critical surface tension is much lower than that of commonly used adhesives, preventing effective wetting and spreading. While existing sodium treatments can improve adhesion in the short term, they disrupt the CF bonds on the PTFE surface, introducing polar groups such as carboxyl and hydroxyl groups. This also causes surface molecular chain breakage, forming a fragile layer (embrittlement layer) of approximately 10–50 μm. This embrittlement layer is highly susceptible to microcracks during high-temperature thermal cycling, becoming a weak point for lining cracking.
[0102] (III) The problem of structural instability induced by high temperature creep and stress relaxation
[0103] PTFE's creep modulus at 200℃ decreases by approximately two orders of magnitude compared to room temperature, and it exhibits significant creep relaxation characteristics under sustained stress. In traditional steel mesh molding processes, PTFE creeps and slips from the steel mesh over time, gradually losing the mesh's pre-tightening force and ultimately leading to interface separation. The challenge in solving this problem lies in the fact that increasing the fit exacerbates shear damage to PTFE during molding, while increasing the temperature accelerates the creep rate, creating a design dilemma.
[0104] The three technical challenges mentioned above are interdependent and mutually reinforcing. Improving only one aspect (such as simply increasing the temperature resistance of the adhesive or simply increasing the density of the steel mesh) cannot completely solve the systemic problem. This is the root cause of why existing technologies have failed to make breakthroughs for so long.
[0105] II. Unique Technical Path and Mechanism of Action for Solving the Technical Problem by This Invention
[0106] The innovation of this invention lies in its approach: instead of addressing a single defect, it constructs a multi-layered protection system characterized by "synergistic complementarity and hierarchical progression." The following details how each technical feature specifically addresses the aforementioned challenges:
[0107] (a) High-temperature fluorine-based adhesive transition layer: dual function of thermal stress buffering and interfacial chemical bridging
[0108] This invention selects a perfluoropolymer resin with a long-term temperature resistance of ≥360℃ as the adhesive transition layer (thickness 0.15~0.3mm), and its technical effects include three aspects:
[0109] 1. Gradient transition in thermal expansion coefficient: The linear expansion coefficient of perfluoropolymer is between that of steel and PTFE (approximately 6~8×10). -5 / ℃), this transition layer acts as an "elastic buffer layer", which uses its own elastic deformation ability to absorb part of the thermal expansion difference, so that the thermal stress that was originally concentrated on the steel-PTFE interface is "shaving the peak and filling the valley" and transformed into uniformly distributed stress inside the transition layer.
[0110] 2. Guaranteed High-Temperature Chemical Stability: The main chain of perfluoropolymer has a CF bond structure, sharing the same chemical framework as PTFE. Its temperature resistance far exceeds that of epoxy adhesives (epoxy long-term service temperature ≤120℃, perfluoropolymer ≥250℃). Under long-term service conditions at 200℃, the transition layer does not undergo thermo-oxidative aging, decomposition, or carbonization, and the bond strength retention rate is >90% (experimental data: after aging at 200℃ / 1000h, the shear strength retention rate is 92%~95% of the initial value).
[0111] 3. Enhanced interfacial chemical affinity: Both the perfluoropolymer adhesive and the PTFE inner liner substrate belong to the fluoroplastic system. During high-temperature sintering, molecular chain segments interpenetrate and physically entangle at the interface, forming a "self-adhesive" effect. This eliminates the need for sodium treatment of PTFE, thus avoiding the formation of an embrittled layer. This feature has never been revealed or adopted in existing technologies.
[0112] (II) Spot-welded anchored stainless steel mesh: Synergistic effect of rigid mechanical anchoring and crack arrest
[0113] In this invention, stainless steel mesh (1.5-3mm thick, 10-20mm aperture) is fixed to a steel shell by spot welding (20-30mm spacing), forming a sandwich structure with two layers of PTFE. The technical effect of this design far surpasses the traditional understanding of "physical anchoring."
[0114] 1. Three-dimensional constraint effect: The steel mesh is embedded inside the PTFE layer rather than just attached to the surface, forming a through-type composite structure of "PTFE-steel mesh-PTFE". PTFE powder permeates the steel mesh and coats the steel mesh wires under isostatic pressing conditions. After sintering, a "riveting" mechanical interlock is formed. The steel mesh provides three-dimensional omnidirectional constraint to the PTFE layer, significantly inhibiting the creep and slippage of PTFE at high temperatures (experimental comparison: creep rate at 200℃ / 100h is reduced by approximately 65% compared to the traditional steel mesh molding process).
[0115] 2. Stress Redistribution and Dispersion: The spot-welded steel mesh, serving as a high-modulus skeleton, is embedded within the low-modulus PTFE matrix. Based on the principles of composite material mixing, this structure transforms the overall thermal stress from being solely borne by PTFE into a composite load-bearing mode of "steel mesh skeleton bearing + PTFE matrix deformation coordination." The steel mesh divides the large-area PTFE layer into multiple smaller regions, dispersing thermal expansion stress within each mesh unit and preventing large-area stress concentration.
[0116] 3. Crack bridging and crack arrest function: This function is one of the most innovative technical effects of this invention. When microcracks are generated in the PTFE layer due to accidental overheating or impact, and the crack tip extends to the steel mesh wire, the interface of the steel mesh wire becomes an "energy dissipation barrier" for crack propagation—the crack needs to bypass the steel mesh wire or deflect along the steel mesh-PTFE interface, significantly extending the propagation path; at the same time, the steel mesh wire itself bears the bridging force generated by the crack opening displacement, effectively reducing the stress intensity factor at the crack tip. Experimental results show that the fracture toughness of the PTFE composite layer with embedded steel mesh is increased by about 120%~150% compared to the pure PTFE layer, and through-cracking only occurs when the critical crack length extends to more than 3 times that of the pure PTFE layer.
[0117] (III) Isostatic pressing full-domain molding + gradient sintering: process guarantee for dense integrated structure
[0118] This invention employs a combination of isostatic pressing (15-25 MPa) across the entire molding range and gradient temperature sintering (370-383℃), the technical effects of which are not readily apparent.
[0119] 1. Unique advantages of isostatic pressing: Traditional unidirectional molding exhibits a pressure gradient, with higher density near the indenter and lower density further away. This density unevenness leads to inconsistent sintering shrinkage, a source of internal stress. Isostatic pressing, through uniform pressure transmission in all directions via a liquid medium, ensures that the PTFE powder is simultaneously compressed in all directions within the steel mesh, achieving "360° dense coverage of the steel mesh wires by the powder," eliminating voids in the shaded area on the back of the steel mesh. This effect is theoretically impossible to achieve in unidirectional molding.
[0120] 2. Stress Management in Gradient Sintering: The PTFE sintering process involves crystallization melting (327℃) and molecular chain rearrangement, with a volume shrinkage rate of approximately 2.5%~3.0%. This invention employs a gradient heating method (typical curve: room temperature → 200℃ holding → 250℃ holding → 320℃ holding → 370~383℃ sintering → slow cooling) to synchronize the temperature fields of each layer. The fusion crosslinking process of the PTFE inner substrate and the surface powder occurs within the same thermal history, avoiding the interface problem caused by the traditional process of "forming the substrate first and then sintering the surface layer". Experimental data show that the interlayer peel strength of the gradient sintered sample is about 40% higher than that of the isothermal sintered sample, and the internal porosity is reduced from 3%~5% in the traditional process to below 0.5%.
[0121] III. Quantitative and Unpredictable Analysis of Creative Technological Effects
[0122] The technical effect produced by this invention is not a simple summation of the effects of each feature, but rather exhibits a significant synergistic gain effect, specifically manifested in:
[0123] Technical performance indicators: Traditional molding process, traditional bonding process, traditional fusion bonding process; Improvement of this invention.
[0124] Interfacial shear strength at 200℃ (MPa): 1.2~1.8 (physical bonding), 0.5~1.0 (after adhesive aging), 0.8~1.5, 4.2~5.8, 3~5 times.
[0125] After 200℃ / 500h thermal cycling, the interfacial peel force retention rate was <50% (loosening), <30% (adhesive layer failure), <40% (interfacial separation), and ≥92%, far exceeding expectations.
[0126] Critical bulging temperature of lining (°C): 120~140, 100~120, 130~150, ≥230. Breakthrough improvement.
[0127] Fracture toughness improvement rate - - - 120%~150% qualitative improvement
[0128] Under negative pressure of -0.1MPa, the lining is prone to bulging, delamination, and deformation, and there is no abnormality. This technology fills a gap in the field.
[0129] The creative significance of the above data is as follows: 1) The interfacial shear strength of 4.2~5.8MPa is close to 20%~30% of the tensile strength of PTFE body (20~30MPa), which means that the failure mode has changed from "interfacial debonding" to "PTFE body failure", realizing the ideal state of "interfacial strength is higher than body strength"; 2) The critical drum temperature is ≥230℃, which leaves a safety margin of 30℃ compared with the target working condition of 200℃, and is significantly higher than the ≤150℃ of the existing process. This leapfrog improvement cannot be derived from a single technology improvement, reflecting the unpredictability of multiple synergies; 3) In terms of negative pressure resistance, the present invention fills the gap that the existing technology cannot operate reliably under the dual harsh conditions of high temperature and negative pressure.
[0130] IV. The Non-Obviousness Argument When Combined with Existing Technologies
[0131] While some of the technical features of this invention have been disclosed in the prior art, they have never been taught to be combined in accordance with the manner of this invention to produce the aforementioned synergistic effects:
[0132] 1. The combination of an adhesive transition layer and steel mesh has been avoided in existing technologies: Traditionally, the physical integration of adhesive and steel mesh is considered an alternative rather than a complementary solution. Those skilled in the art generally believe that the adhesive layer softens at high temperatures, and the integration of steel mesh would disrupt the continuity of the adhesive layer. This invention, by using perfluoropolymer (rather than epoxy) as the adhesive and leveraging its compatibility with PTFE, combined with the rigid constraint of spot-welded steel mesh, achieves a complementary combination of "flexible buffering + rigid anchoring." This approach has not been explored in existing technical literature.
[0133] 2. The crack-arresting function of steel mesh embedded within PTFE layers was previously unrecognized: In existing processes, steel mesh is either fixed between the steel shell and PTFE (Type I process) or merely serves as a surface covering layer; it has never been designed as a "crack-arresting skeleton embedded within the PTFE layer." This invention places the steel mesh between two PTFE layers and allows it to melt-crosslink with the PTFE, making the crack-arresting function of the steel mesh possible. This represents a new technological discovery and utilization of the function of steel mesh.
[0134] 3. The synergy between isostatic pressing and steel mesh integration is not explicit: Those skilled in the art might consider using isostatic pressing to form PTFE products (this technology is known), but when the steel mesh is pre-spot-welded to the shell, achieving uniform isostatic pressing while ensuring the steel mesh is not crushed and the spot welds are not damaged presents significant technical challenges. This invention achieves the optimal process window of "sufficient densification without structural damage" by controlling the matching relationship between the steel mesh aperture (10~20mm), thickness (1.5~3mm), and spot weld spacing (20~30mm), combined with isostatic pressing parameters of 15~25MPa. Discovering this process window requires extensive experimental exploration and is not simply a matter of parameter selection.
[0135] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any modifications, equivalent substitutions, and improvements made by those skilled in the art within the scope of the technology disclosed in the present invention, and within the spirit and principles of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A process for isostatic pressing and sintering to prepare a high-temperature negative pressure resistant steel-PTFE composite structure, characterized in that: Includes the following steps: Step 1: Perform surface pretreatment on the inner wall of the steel shell to be laminated, so that the inner wall of the steel shell to be laminated forms a rough and clean surface; Step 2: Apply a high-temperature adhesive to the pre-treated steel shell inner wall to be laminated and pre-dry it to form a high-temperature bonding transition layer. Step 3: Attach the polytetrafluoroethylene (PTFE) sheet to the surface of the high-temperature adhesive transition layer and compact it to form a PTFE inner liner. Step 4: Lay a stainless steel mesh on the inner surface of the polytetrafluoroethylene liner, and fix the stainless steel mesh to the steel shell by multi-point spot welding, so that the stainless steel mesh is pressed onto the surface of the polytetrafluoroethylene liner. Step 5: Lay polytetrafluoroethylene powder on the surface of the stainless steel mesh so that the polytetrafluoroethylene powder fills the mesh openings of the stainless steel mesh and covers the inner working surface. Step 6: Perform isostatic pressing on the steel shell on which the polytetrafluoroethylene powder is laid, so that the polytetrafluoroethylene powder enters the mesh of the stainless steel mesh and is compacted and adhered to the polytetrafluoroethylene inner lining plate. Step 7: Perform gradient heating high-temperature sintering on the integral workpiece after isostatic pressing, so that the polytetrafluoroethylene powder passes through the mesh of the stainless steel mesh and is sintered and fused with the polytetrafluoroethylene inner liner. The stainless steel mesh is embedded between the polytetrafluoroethylene inner liner and the dense polytetrafluoroethylene surface layer formed by sintering, and the high-temperature bonding transition layer is activated during the high-temperature sintering process. After cooling, a steel-polytetrafluoroethylene composite structure is formed.
2. The isostatic pressing molding and sintering preparation process of the high-temperature negative pressure resistant steel-PTFE composite structure with synergistic reinforcement of steel mesh anchoring and high-temperature bonding as described in claim 1, is characterized in that... The surface pretreatment involves sandblasting the inner wall of the steel shell to be composited with brown corundum abrasive. The sandblasting pressure is 0.4 to 0.7 MPa, the surface roughness after treatment is 40 to 75 μm, the surface cleanliness is not lower than Sa2.5 grade, and the treated surface is free of floating dust and residual impurities.
3. The isostatic pressing molding and sintering preparation process of the high-temperature negative pressure resistant steel-PTFE composite structure with synergistic reinforcement of steel mesh anchoring and high-temperature bonding as described in claim 1, is characterized in that... The high-temperature adhesive is a fluorine-based high-temperature adhesive that can withstand temperatures not lower than 220°C. The thickness of the high-temperature bonding transition layer is 0.15–0.3 mm, the pre-drying temperature is 80–120°C, and the pre-drying time is 30–60 min.
4. The isostatic pressing molding and sintering preparation process of the high-temperature negative pressure resistant steel-PTFE composite structure with synergistic reinforcement of steel mesh anchoring and high-temperature bonding as described in claim 1, is characterized in that... The stainless steel mesh has a mesh size of 3-8mm and a thickness of 2mm. The edges and grid intersections of the stainless steel mesh are fixed to the steel shell by multi-point spot welding. The spacing between the spot welding points is 20-40mm. After spot welding, the stainless steel mesh is not loose or warped and fits tightly against the surface of the polytetrafluoroethylene lining plate.
5. The isostatic pressing molding and sintering preparation process of the high-temperature negative pressure resistant steel-PTFE composite structure with synergistic reinforcement of steel mesh anchoring and high-temperature bonding as described in claim 1, is characterized in that... The isostatic pressing pressure is 15-30 MPa, the holding time is 10-25 min, and uniform pressure is applied over the entire area. Before high-temperature sintering, the molded integral workpiece is filled with high-temperature resistant expansion particles and compacted. After the cover plate is closed and tightened, high-temperature sintering is carried out. The heating rate of the high-temperature sintering is 2-5°C per minute, the final sintering temperature is 360-380°C, the constant temperature sintering time is 60-120 minutes, and the furnace is naturally cooled to room temperature after sintering.
6. A steel-PTFE composite structure for high-temperature negative pressure resistance, characterized by synergistic reinforcement of steel mesh anchoring and high-temperature bonding, using an isostatic pressing molding and sintering process according to any one of claims 1-5, is as follows: From the outside to the inside, it consists of a steel shell base, a high-temperature adhesive transition layer, a polytetrafluoroethylene (PTFE) inner lining, a stainless steel mesh, and a dense PTFE sintered surface layer. The high-temperature adhesive transition layer is disposed between the steel shell base and the polytetrafluoroethylene inner liner, and the polytetrafluoroethylene inner liner is attached to the inner wall of the steel shell base through the high-temperature adhesive transition layer. The stainless steel mesh is laid on the inner surface of the polytetrafluoroethylene lining plate and fixed to the steel shell by multi-point spot welding; The dense polytetrafluoroethylene sintered surface layer is filled with the mesh of the stainless steel mesh, and forms a continuous sintered fusion structure with the polytetrafluoroethylene inner liner through the mesh. The stainless steel mesh is embedded between the polytetrafluoroethylene inner liner and the dense polytetrafluoroethylene sintered surface layer.
7. The steel mesh anchoring and high-temperature bonding synergistic reinforcement high-temperature negative pressure resistant steel-PTFE composite structure according to claim 6, characterized in that, The inner wall of the steel shell substrate in contact with the high-temperature adhesive transition layer has a rough surface with a roughness of 40–75 μm.
8. The steel mesh anchoring and high-temperature bonding synergistic reinforcement high-temperature negative pressure resistant steel-PTFE composite structure according to claim 6, characterized in that, The high-temperature bonding transition layer is formed by a fluorine-based high-temperature adhesive that can withstand temperatures of not less than 220°C, and the thickness of the high-temperature bonding transition layer is 0.15 to 0.3 mm.
9. The steel mesh anchoring and high-temperature bonding synergistic reinforcement high-temperature negative pressure resistant steel-PTFE composite structure according to claim 6, characterized in that, The stainless steel mesh has a mesh size of 3-8mm and a thickness of 2mm. The edges and mesh intersections of the stainless steel mesh form multiple spot-welded fixing positions with the steel shell, and the spacing between adjacent spot-welded fixing positions is 20-40mm.
10. The steel mesh anchoring and high-temperature bonding synergistic reinforcement high-temperature negative pressure resistant steel-PTFE composite structure according to claim 6, characterized in that, The PTFE inner liner and the high-temperature adhesive transition layer are bonded together without bubbles or gaps. The stainless steel mesh is attached to the surface of the PTFE inner liner without loosening or warping. The dense PTFE sintered surface layer continuously fills the mesh of the stainless steel mesh and covers the inner liner working surface.