A method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials via a short process
By combining external field-enhanced segmented roasting and multi-stage circulating water leaching with acidification pre-reduction and countercurrent extraction, the problem of directly preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials has been solved, realizing efficient and short-process vanadium leaching and electrolyte preparation, which is suitable for all-vanadium redox flow batteries.
Patent Information
- Application Number
- CN202611030594.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-12
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for preparing electrolytes for all-vanadium redox flow batteries suffer from problems such as long process flow, high energy consumption, large vanadium flow loss, and difficulty in controlling impurities. In particular, the vanadium leaching rate in vanadium-containing solid raw materials is low, and the concentration and valence state control are difficult to meet the requirements for electrolyte preparation.
A short-process method combining microwave-based external field-enhanced segmented roasting activation of vanadium-containing solid raw materials with multi-stage circulating water leaching, acidification pre-reduction, and countercurrent extraction back-extraction is used to directly prepare vanadium oxysulfate electrolyte.
It improves vanadium conversion efficiency, shortens the process chain, reduces activation intensity, and enables the preparation of high-concentration, high-purity tetravalent vanadium electrolyte, which is suitable for vanadium-containing solid raw materials from different sources.
Smart Images

Figure CN123105718A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of vanadium resource comprehensive utilization and vanadium redox flow battery electrolyte preparation. It relates to a short-process method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials, and more particularly to a method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials through external field enhanced activation, multi-stage circulating water leaching, valence state directional control, countercurrent extraction, and countercurrent back-extraction. Background Technology
[0002] Vanadium redox flow batteries (VRBs) are characterized by high safety, long cycle life, and scalable capacity, making them suitable for large-scale energy storage applications. The electrolyte is the energy carrier in a VRB, and its preparation cost and impurity level directly affect the initial investment, charge-discharge efficiency, and long-term operational stability of the battery system. Existing electrolyte preparation routes mostly use high-purity vanadium chemical products as precursors, obtained through acid dissolution, reduction, valence state adjustment, and compounding. While the product quality of this type of route is relatively easy to control, it usually requires the preparation of solid vanadium intermediates, followed by redissolution and conversion, resulting in a long process, high energy consumption, and significant vanadium loss.
[0003] Vanadium-containing solid raw materials are abundant, widely sourced, and contain complex associated components. A significant portion of these raw materials contain vanadium in a stable structural form, making direct water leaching insufficient to achieve high vanadium leaching rates. Traditional activation roasting-leaching processes typically employ external heat transfer, which suffers from long heat transfer paths, localized overheating, high activator consumption, and the co-conversion of impurities. For raw materials with high levels of associated components such as silicon, aluminum, magnesium, calcium, and titanium, the activator is easily consumed by competition from these components. Furthermore, the dense phase formed at high temperatures may encapsulate leached vanadium, making it difficult to simultaneously meet the requirements for subsequent electrolyte preparation in terms of vanadium conversion efficiency, leachate concentration, and impurity control.
[0004] On the other hand, the direct preparation of vanadium oxysulfate electrolyte from vanadium-containing leachate requires addressing three issues simultaneously: concentration, valence state, and impurities. If the vanadium concentration in the leachate is too low, additional evaporation concentration or crystallization steps are necessary; if the valence state is not uniformly controlled, extraction selectivity, valence state stability of the back-extraction solution, and electrolyte consistency will all decrease; if the impurity ion concentration is too high, it will affect the battery's cycle life. Therefore, it is necessary to develop a short-process method that can directly connect vanadium-containing solid raw materials to vanadium oxysulfate electrolyte, achieving efficient vanadium release, leachate enrichment, directional valence state conversion, and deep purification without vanadium precipitation and redissolution of solid vanadium oxide intermediates. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a short-process method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials. This method improves the activation efficiency of vanadium-containing structures through microwave-based external field-enhanced segmented roasting, gradually enriches low-concentration leachate into high-vanadium, low-impurity leachate through multi-stage circulating water leaching, converts pentavalent vanadium into tetravalent vanadium oxysulfate ions through acidification pre-reduction, and finally obtains vanadium oxysulfate electrolyte through countercurrent extraction and countercurrent back-extraction.
[0006] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short process, comprising the following steps: S1. Raw material pretreatment and activation mixing: After drying and grinding the vanadium-containing solid raw material, it is mixed with an alkaline activator. If necessary, a binder and water are added to obtain the activated mixture. S2. External field enhanced segmented roasting: The activated mixture obtained in step S1 is placed under external field enhanced heating conditions mainly based on microwave for segmented roasting, so that the difficult-to-leach vanadium is converted into leached vanadium, and the activated roasted material is obtained. S3. Multi-stage circulating water leaching enrichment: The activated roasted material obtained in step S2 is ground and then leached in water. The previous leaching solution or the previous batch of leaching solution is used as the subsequent leaching agent for recycling, so that vanadium is enriched in the aqueous phase step by step to obtain a high vanadium and low impurity leaching solution. S4. Acidification and pre-reduction: The high-vanadium, low-impurity leaching solution obtained in step S3 is adjusted to an acidic system, and a reducing medium is added to reduce pentavalent vanadium to tetravalent vanadium oxide ions, thereby obtaining a tetravalent vanadium reduction solution. S5. Countercurrent extraction purification: Adjust the tetravalent vanadium reducing solution obtained in step S4 to a suitable extraction acidity, and conduct multi-stage countercurrent contact with the extraction organic phase to allow tetravalent vanadium ions to enter the organic phase, thereby obtaining a vanadium-rich organic phase. S6. Countercurrent back-extraction solution preparation: The vanadium-rich organic phase obtained in step S5 is subjected to countercurrent back-extraction using an acidic back-extraction medium containing sulfate ions, so that vanadium enters the back-extraction aqueous phase to obtain vanadium oxysulfate electrolyte.
[0007] In a preferred embodiment, in step S1, the vanadium-containing solid raw material is one or a combination of at least two of the following: natural vanadium-containing raw materials, beneficiated concentrates, metallurgical intermediate materials, and vanadium-containing secondary resource materials; the vanadium-containing solid raw material contains 0.20% to 5.00% vanadium as oxide by mass, 20% to 65% iron as total iron by mass, and contains one or more associated components of titanium, silicon, aluminum, magnesium, and calcium.
[0008] In a preferred embodiment, in step S1, the alkaline activator is an activation system containing alkali metal compounds, and its addition amount is 1% to 20% of the dry basis mass of the vanadium-containing solid raw material, calculated based on the effective alkali equivalent. Before mixing, the vanadium-containing solid raw material is ground to a particle size of -0.074 mm with a particle size ratio of 50% to 98%, and a binder and water can be added to form granular, agglomerated, or loose activated mixtures. The alkali metal compound is one or more combinations of sodium carbonate, sodium bicarbonate, and sodium hydroxide.
[0009] In a preferred embodiment, in step S2, the external field enhanced heating includes one of microwave heating, microwave coupled with conventional heating, and microwave coupled with electromagnetic field assisted heating; the segmented calcination includes a preheating activation section and a high-temperature conversion section, wherein the temperature of the preheating activation section is 650~900℃ and the time is 10~60 min, and the temperature of the high-temperature conversion section is 900~1150℃ and the time is 10~60 min.
[0010] In the preferred embodiment, in step S3, the leaching agent for multi-stage circulating water leaching is water, the previous batch of leaching solution, the previous stage leaching solution, or a combination thereof. The leaching solution-to-solid ratio is 1.5~6.0 mL / g, the leaching temperature is 40~95℃, the single-stage leaching time is 30~180min, the stirring rate is 100~800 r / min, and the number of cyclic leaching stages is 5~30.
[0011] In a preferred embodiment, in step S3, the total vanadium concentration in the high-vanadium, low-impurity leachate is 10-35 g / L (V), and the concentration of any one of the impurities Fe, Al, Ti, Cr, Mn, and Si is not higher than 50 mg / L.
[0012] In the preferred embodiment, in step S4, the acidic system uses an acidic medium containing sulfate to adjust the pH of the high-vanadium, low-impurity leachate to 0-1.0; the reduction and conversion process uses an inorganic reducing agent, an organic reducing agent, an electrochemical reduction system, or a combination thereof. The inorganic reducing agent includes one or more of sodium sulfite, sodium bisulfite, sodium metabisulfite, or sulfur dioxide; the organic reducing agent includes one or more of oxalic acid, ascorbic acid, or glucose; the ratio of the effective reducing equivalent of the reducing medium to the total molar amount of vanadium is 0.35~1.20; the reduction temperature is 20~70℃; and the reduction time is 10~120 min.
[0013] In a preferred embodiment, in step S5, the pH of the tetravalent vanadium reducing solution is adjusted to 1.0~3.0 before entering the countercurrent extraction, and the proportion of tetravalent vanadium to the total vanadium is not less than 95%.
[0014] In a preferred embodiment, in step S5, the extracted organic phase includes one or more of the following: an acidic phosphorus-containing extractant, a co-extraction component, a modified component, and a diluent component. The acidic phosphorus-containing extractant includes P204, P507, Cyanex 272, or a combination thereof; the co-extraction component or modified component includes TBP, 2-octanol, isooctanol, or a combination thereof; the diluent includes sulfonated kerosene, No. 260 solvent oil, and n-alkane solvent oil; wherein the volume fraction of the acidic phosphorus-containing extractant is 15%~60%, the extraction ratio O / A is 0.3~2.5, the number of countercurrent extraction stages is 2~6, and the single-stage mixing time is 3~30 min.
[0015] In a preferred embodiment, in step S6, the acid concentration of the sulfate-containing acidic back-extraction medium is 1.0~6.0 mol / L, the back-extraction ratio O / A is 1~10, the number of countercurrent back-extraction stages is 1~4, and the single-stage back-extraction time is 3~30 min.
[0016] In the preferred embodiment, in step S6, the regenerated organic phase after back-extraction is returned to the countercurrent extraction step for recycling; the leaching residue obtained from multi-stage circulating water leaching is washed and returned to the comprehensive utilization process as iron-titanium solid material or as raw material for subsequent resource recovery.
[0017] In the preferred embodiment, in step S6, the total vanadium concentration in the obtained vanadium oxysulfate electrolyte is 60~120 g / L (based on V), and the vanadium valence state is mainly tetravalent, which can be used as an electrolyte for all vanadium redox flow batteries or its precursor.
[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: First, it has a wide range of applicable raw materials, covering vanadium-containing solid raw materials from different sources; Second, replacing single external heat transfer activation with external field-enhanced segmented roasting is beneficial to improving vanadium conversion efficiency and reducing activation intensity. Third, multi-stage circulating water leaching can increase the vanadium concentration of the leachate without additional evaporation and concentration. Fourth, acidification and pre-reduction unify the vanadium valence state to tetravalent, which is beneficial to the stable operation of subsequent extraction and back-extraction. Fifth, the entire process avoids the steps of ammonium salt precipitation of vanadium, preparation of solid vanadium oxide intermediates, and redissolution of solid vanadium oxide, thus shortening the process chain from raw materials to vanadium oxysulfate electrolyte. Attached Figure Description
[0019] Figure 1 This is a process flow diagram of a method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials according to the present invention. Detailed Implementation
[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0021] The following examples further illustrate the technical solution of the present invention. The raw materials used in the examples are designated as Raw Material A, Raw Material B, and Raw Material C, all of which are vanadium-containing solid raw materials from different sources. The activator, reducing agent, extraction organic phase, and back-extraction medium used can all be replaced with commonly used industrial substances that perform the same function. The specific parameters in the examples are used to illustrate that the present invention can be implemented and are not intended to limit the scope of protection of the present invention.
[0022] Unless otherwise specified, all percentages in the examples are mass percentages; percentages in the organic phase composition are volume percentages; total vanadium concentration is expressed as V; impurity concentrations are determined using conventional elemental analysis methods; and vanadium valence states are determined using chemical titration or spectroscopic methods that can distinguish between pentavalent and tetravalent vanadium.
[0023] The following description, through specific embodiments and accompanying drawings, provides further details. Example 1
[0024] In this embodiment, vanadium oxysulfate electrolyte is prepared using raw material A. Raw material A contains 0.62% V₂O₅, 55.14% TFe, 12.86% TiO₂, 0.83% CaO, 2.47% MgO, 2.90% SiO₂, and 3.47% Al₂O₃.
[0025] Step 1, raw material pretreatment. Dry raw material A and grind it finely so that the proportion of -0.074 mm particle size is 85%; add 6.0% sodium carbonate, 1.0% sodium humate and 8.5% water according to the dry weight of raw material A, mix for 15 min and make activated granules with a particle size of 10~14 mm.
[0026] Step 2, external field enhanced segmented calcination. The activated granules are placed in a microwave heating device, first heated to 750℃ with a power of 1000 W and held for 25 min, then heated to 1050℃ with a power of 2250 W and held for 22.5 min; after calcination, they are cooled in air to obtain activated calcined material.
[0027] Step 3: Multi-stage circulating water leaching. The activated roasted material was crushed and ground to a particle size of -0.074 mm, accounting for no less than 90%. Water was used as the first-stage leaching agent, and the first leaching was carried out under the conditions of a liquid-to-solid ratio of 3.0 mL / g, a leaching temperature of 80℃, a stirring rate of 400 r / min, and a leaching time of 120 min. After solid-liquid separation, a first-stage vanadium-containing leachate was obtained. Subsequently, the obtained vanadium-containing leachate was used as the leaching agent for the next batch of activated roasted material, and leaching was carried out under the same conditions, for a total of 21 cycles. After the cycle, the total vanadium concentration in the leachate was 19.8 g / L, the overall vanadium recovery rate was approximately 81%, and the concentration of any one of the impurity ions, Fe, Al, and Ti, was less than 2.5 mg / L.
[0028] Step 4, acidification pre-reduction. The high-vanadium, low-impurity leachate obtained in Step 3 is adjusted to pH 0 using an acidic medium containing sulfate. Sodium sulfite is added at a ratio of effective reduction equivalent to total vanadium molar amount of 0.60. The reaction is carried out at 35°C and a stirring rate of 200 r / min for 45 min to obtain a tetravalent vanadium reduced solution. After reduction, the proportion of tetravalent vanadium in the total vanadium is not less than 98%.
[0029] Step 5, countercurrent extraction. Adjust the pH of the tetravalent vanadium reducing solution to 2.0; prepare an extractable organic phase consisting of 40% organophosphonate extractant (P507) and 60% hydrocarbon dilution component (sulfonated kerosene); perform three-stage countercurrent extraction with a phase ratio of O / A of 1, mixing for 10 min per stage and allowing the phases to separate for 15 min to obtain a vanadium-rich organic phase.
[0030] Step 6, Countercurrent Back-Extraction. A 3.0 mol / L sulfuric acid solution was used to perform two-stage countercurrent back-extraction on the vanadium-rich organic phase with a phase ratio of 5 (O / A). Each stage of back-extraction lasted 8 minutes, followed by a 15-minute settling period to separate the phases, yielding a vanadium oxysulfate electrolyte. The total vanadium concentration in the resulting electrolyte was 85.87 g / L, with vanadium primarily existing as tetravalent vanadium oxyions. The overall vanadium yield was 95.41%, and the capacity retention after 50 charge-discharge cycles was 95.4%. Example 2
[0031] In this embodiment, vanadium oxysulfate electrolyte is prepared using raw material B. Raw material B contains 0.72% V₂O₅, 54.88% TFe, 9.87% TiO₂, 0.46% CaO, 3.98% MgO, 4.21% SiO₂, and 3.55% Al₂O₃.
[0032] Step 1, raw material pretreatment. Dry raw material B and grind it finely so that the proportion of -0.074 mm particle size is 88%; add 8.0% sodium carbonate, 1.2% sodium humate and 9.0% water according to the dry basis of raw material B, mix for 18 min and make activated granules with a particle size of 9~13 mm.
[0033] Step 2, external field enhanced segmented calcination. The activated granules are placed in a microwave heating device, first heated to 800℃ with a power of 1000 W and held for 25 min, then heated to 1025℃ with a power of 2250 W and held for 22 min; after calcination, they are cooled in air to obtain activated calcined material.
[0034] Step 3: Multi-stage circulating water leaching. The activated roasted material is crushed and ground to a particle size of -0.074 mm or less (at least 90%). Water is used as the primary leaching agent, and leaching is carried out under the following conditions: liquid-to-solid ratio of 3.0 mL / g, leaching temperature of 80℃, stirring rate of 400 r / min, and leaching time of 120 min. After solid-liquid separation, the leachate is reused for subsequent batches of activated roasted material, with a total of 20 cycles. After the cycle is completed, the total vanadium concentration in the leachate is 21.6 g / L, the overall vanadium recovery rate is approximately 83%, and the concentration of any one of the impurity ions (Fe, Al, Ti) is below 3.0 mg / L.
[0035] Step 4, acidification pre-reduction. The high-vanadium, low-impurity leachate obtained in Step 3 is adjusted to pH 0.2 using an acidic medium containing sulfate. Sodium sulfite is added at a ratio of effective reduction equivalent to total vanadium molar amount of 0.62. The reaction is carried out at 35°C and a stirring rate of 220 r / min for 50 min to obtain a tetravalent vanadium reduced solution. After reduction, the proportion of tetravalent vanadium in the total vanadium is not less than 98%.
[0036] Step 5, countercurrent extraction. Adjust the pH of the tetravalent vanadium reducing solution to 2.1; prepare an extractable organic phase consisting of 40% organophosphonate extractant (P507) and 60% hydrocarbon dilution component (sulfonated kerosene); perform three-stage countercurrent extraction with a phase O / A ratio of 1.1, mixing for 10 min per stage and allowing the phases to separate for 15 min to obtain a vanadium-rich organic phase.
[0037] Step 6, Countercurrent Back-Extraction. A 3.2 mol / L sulfuric acid solution was used to perform two-stage countercurrent back-extraction on the vanadium-rich organic phase with a phase ratio of 5 (O / A). Each stage of back-extraction lasted 8 minutes, followed by a 15-minute settling period to separate the phases, yielding a vanadium oxysulfate electrolyte. The total vanadium concentration in the resulting electrolyte was 88.4 g / L, with vanadium primarily existing as tetravalent vanadium oxyions. The overall vanadium yield was 94.8%, and the impurity content met the requirements for battery electrolyte precursor solutions. Example 3
[0038] In this embodiment, vanadium oxysulfate electrolyte is prepared using raw material C. Raw material C contains 0.65% V₂O₅, 55.84% TFe, 11.37% TiO₂, 0.76% CaO, 2.33% MgO, 3.68% SiO₂, and 3.60% Al₂O₃.
[0039] Step 1, raw material pretreatment. Dry raw material C and grind it finely so that the proportion of -0.074 mm particles is 86%; add 7.0% sodium carbonate, 1.0% sodium humate and 8.0% water according to the dry weight of raw material C, mix for 15 min and make activated granules with a particle size of 10~14 mm.
[0040] Step 2, external field enhanced segmented calcination. The activated granules are placed in a microwave heating device, first heated to 780℃ with a power of 1000 W and held for 25 min, then heated to 1050℃ with a power of 2250 W and held for 20 min; after calcination, they are cooled in air to obtain activated calcined material.
[0041] Step 3: Multi-stage circulating water leaching. The activated roasted material was crushed and ground to a particle size of -0.074 mm or less (at least 90%). Water was used as the primary leaching agent, and leaching was carried out under the following conditions: liquid-to-solid ratio of 3.0 mL / g, leaching temperature of 80℃, stirring rate of 400 r / min, and leaching time of 120 min. After solid-liquid separation, the resulting leachate was recycled for subsequent batches of activated roasted material, with a total of 18 cycles. After the cycle was completed, the total vanadium concentration in the leachate was 18.7 g / L, the overall vanadium recovery rate was approximately 80%, and the concentration of any one of the impurity ions (Fe, Al, Ti) was below 3.0 mg / L.
[0042] Step 4, acidification pre-reduction. The high-vanadium, low-impurity leachate obtained in Step 3 is adjusted to pH 0.1 using an acidic medium containing sulfate. Sodium sulfite is added at a ratio of effective reduction equivalent to total vanadium molar amount of 0.60. The reaction is carried out at 35°C and a stirring rate of 200 r / min for 45 min to obtain a tetravalent vanadium reduced solution. After reduction, the proportion of tetravalent vanadium in the total vanadium is not less than 98%.
[0043] Step 5, countercurrent extraction. Adjust the pH of the tetravalent vanadium reducing solution to 2.0; prepare an extractable organic phase consisting of 40% organophosphonate extractant (P507) and 60% hydrocarbon dilution component (sulfonated kerosene); perform three-stage countercurrent extraction with a phase ratio of O / A of 1, mixing for 10 min per stage and allowing the phases to separate for 15 min to obtain a vanadium-rich organic phase.
[0044] Step 6, Countercurrent Back-Extraction. A 3.0 mol / L sulfuric acid solution was used to perform two-stage countercurrent back-extraction on the vanadium-rich organic phase with a phase ratio of 5 (O / A). Each stage of back-extraction lasted 8 minutes, followed by a 15-minute settling period to separate the phases, yielding a vanadium oxysulfate electrolyte. The total vanadium concentration in the resulting electrolyte was 82.6 g / L, with vanadium primarily existing as tetravalent vanadium oxyions. The overall vanadium yield was 94.1%, and the impurity content met the requirements for battery electrolyte precursor solutions.
[0045] Comparative Example 1: Conventional external heat roasting-single-stage water immersion-ammonium salt precipitation route; Using the same raw material A as in Example 1, conventional resistance furnace external heating sodium roasting was performed. The roasting temperature, activator addition amount, clinker grinding particle size and water leaching liquid-solid ratio were the same as in Example 1. Only a single-stage water leaching was performed, and the resulting leachate was treated with ammonium salt vanadium precipitation.
[0046] The results showed that the total vanadium concentration in the single-stage water leaching solution was 0.76 g / L, the vanadium leaching rate was 64.8%, the V2O5 residue in the leaching residue was 0.22%, the ammonium salt precipitation rate was 72.1%, and the effective vanadium recovery rate was 43.8% based on the vanadium intermediates that can be used in the subsequent acid leaching solution.
[0047] Comparative Example 2: Acid leaching for vanadium extraction - neutralization and impurity removal route; Using the same raw material A as in Example 1, acid leaching was enhanced with sulfuric acid-fluoride salts at a liquid-to-solid ratio of 3.0 mL / g. The leaching solution was neutralized and purified before being used as the raw material for subsequent extraction.
[0048] The results showed that the vanadium leaching rate was 88.7%, and the total vanadium concentration in the acid leaching solution was 1.03 g / L; the Fe concentration was 7.20 g / L. After neutralization and impurity removal, the vanadium entrained in the impurity-removed residue accounted for 13.8% of the total vanadium in the acid leaching solution. The Ti and colloidal silicon concentrations in the purified solution were still 0.085 g / L and 0.26 g / L, respectively, which are far from meeting the requirements for vanadium battery electrolyte preparation.
[0049] Comparative Example 3: Low-concentration leachate concentration-vanadium precipitation-calcination-redissolution route; The low-concentration vanadium-containing solutions obtained by conventional water leaching were combined, concentrated, precipitated with ammonium salts, and calcined to prepare vanadium oxide intermediates. Then, vanadium oxysulfate precursor solution was prepared by dissolving in sulfuric acid and reducing and adjusting its valence.
[0050] The results showed that the total vanadium concentration increased from 0.72 g / L to 13.4 g / L after concentration, and the suspended solids content increased to 1.62 g / L; the ammonium salt precipitation rate of vanadium was 79.3%, and the total vanadium concentration of the vanadium precipitation mother liquor was 1.08 g / L. The total vanadium concentration of the vanadium-containing solution obtained after calcination and redissolution was 54.6 g / L, and the vanadium recovery rate into the usable vanadium oxysulfate precursor solution was 65.2%.
[0051] Comparative Example 4: Direct extraction route omitting acidification and pre-reduction; Using the high-vanadium, low-impurity leachate obtained in Example 1 as the subject, extraction was performed directly after adjusting only the acidity, without adding a reducing medium; the extraction, washing, and back-extraction conditions were the same as in Example 1.
[0052] The results showed that tetravalent vanadium accounted for 24.7% of the total vanadium in the feed liquid, the vanadium extraction rate after three-stage countercurrent extraction was 76.8%, and the total vanadium concentration in the raffinate was 4.22 g / L; the total vanadium concentration in the second-stage back-extraction liquid was 61.5 g / L, tetravalent vanadium accounted for 63.8% of the total vanadium, and the overall vanadium recovery rate was 72.6%.
[0053] As can be seen from the above comparative examples, the combination of external field enhanced segmented roasting, multi-stage circulating water leaching enrichment, acidification pre-reduction and countercurrent extraction-back-extraction of the present invention is beneficial to simultaneously improve vanadium release, liquid phase enrichment, impurity control and valence state stability.
[0054] In summary, the raw material pretreatment, enhanced roasting in an external field, water leaching, acidification reduction, countercurrent extraction, and countercurrent back-extraction employed in this invention can all be achieved using existing metallurgical and chemical equipment. Multi-stage circulating water leaching can be configured using intermittent, semi-continuous, or continuous countercurrent methods; extraction and back-extraction can be performed using mixing and clarification tanks, extraction towers, or other liquid-liquid contact equipment; and the regenerated organic phase can be recycled. Therefore, this invention has a good foundation for industrial scale-up and is suitable for the high-value utilization of vanadium-containing solid raw materials and the preparation of vanadium oxysulfate electrolyte.
[0055] The above content is only a specific implementation example of the present invention, and not all application examples of the present invention. All schemes that follow the technical concept of the present invention or make modifications based on the technical concept of the present invention are within the protection scope of the claims of the present invention.
Claims
1. A method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method, characterized in that, Includes the following steps: S1. Raw material pretreatment and activation mixing: After drying and grinding the vanadium-containing solid raw material, it is mixed with an alkaline activator. If necessary, a binder and water are added to obtain the activated mixture. S2. External field enhanced segmented roasting: The activated mixture obtained in step S1 is placed under external field enhanced heating conditions mainly based on microwave for segmented roasting, so that the difficult-to-leach vanadium is converted into leached vanadium, and the activated roasted material is obtained. S3. Multi-stage circulating water leaching enrichment: The activated roasted material obtained in step S2 is ground and then leached in water. The previous leaching solution or the previous batch of leaching solution is used as the subsequent leaching agent for recycling, so that vanadium is enriched in the aqueous phase step by step to obtain a high vanadium and low impurity leaching solution. S4. Acidification and pre-reduction: Adjust the high-vanadium, low-impurity leaching solution obtained in step S3 to an acidic system, add a reducing medium to reduce pentavalent vanadium to tetravalent vanadium oxide ions, and obtain a tetravalent vanadium reduction solution. S5. Countercurrent extraction purification: Adjust the tetravalent vanadium reducing solution obtained in step S4 to a suitable extraction acidity, and conduct multi-stage countercurrent contact with the extraction organic phase to allow tetravalent vanadium ions to enter the organic phase, thereby obtaining a vanadium-rich organic phase. S6. Countercurrent back-extraction solution preparation: The vanadium-rich organic phase obtained in step S5 is subjected to countercurrent back-extraction using an acidic back-extraction medium containing sulfate ions, so that vanadium enters the back-extraction aqueous phase to obtain vanadium oxysulfate electrolyte.
2. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S1, the vanadium-containing solid raw material is one or a combination of at least two of the following: natural vanadium-containing raw materials, beneficiated concentrates, metallurgical intermediate materials, and vanadium-containing secondary resource materials; the vanadium-containing solid raw material contains 0.20% to 5.00% vanadium as oxide by mass, 20% to 65% iron as total iron by mass, and contains one or more associated components of titanium, silicon, aluminum, magnesium, and calcium.
3. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S1, the alkaline activator is an activation system containing alkali metal compounds. Based on the effective alkali equivalent, its addition amount is 1% to 20% of the dry basis mass of the vanadium-containing solid raw material. Before mixing, the vanadium-containing solid raw material is ground to a particle size of -0.074 mm with a proportion of 50% to 98%, and a binder and water can be added to form granular, agglomerated, or loose activated mixtures. The alkali metal compound is one or more combinations of sodium carbonate, sodium bicarbonate, and sodium hydroxide.
4. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S2, the external field enhanced heating includes one of microwave heating, microwave coupled with conventional heating, and microwave coupled with electromagnetic field assisted heating; the segmented calcination includes a preheating activation section and a high-temperature conversion section. The temperature of the preheating activation section is 650~900℃ and the time is 10~60 min. The temperature of the high-temperature conversion section is 900~1150℃ and the time is 10~60 min.
5. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S3, the leaching agent for multi-stage circulating water leaching is water, the previous batch of leaching solution, the previous stage leaching solution, or a combination thereof. The leaching solution-to-solid ratio is 1.5~6.0 mL / g, the leaching temperature is 40~95℃, the single-stage leaching time is 30~180 min, the stirring rate is 100~800 r / min, and the number of circulating leaching stages is 5~30. The total vanadium concentration in the high-vanadium, low-impurity leachate is 10-35 g / L (V), and the concentration of any one of the impurities Fe, Al, Ti, Cr, Mn, and Si is not higher than 50 mg / L.
6. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S4, the acidic system uses an acidic medium containing sulfate to adjust the pH of the high-vanadium, low-impurity leachate to 0-1.0; the reduction and conversion process uses an inorganic reducing agent, an organic reducing agent, an electrochemical reduction system, or a combination thereof. The inorganic reducing agent includes one or more of sodium sulfite, sodium bisulfite, sodium metabisulfite, or sulfur dioxide; the organic reducing agent includes one or more of oxalic acid, ascorbic acid, or glucose; the ratio of the effective reducing equivalent of the reducing medium to the total molar amount of vanadium is 0.35~1.20; the reduction temperature is 20~70℃; and the reduction time is 10~120 min.
7. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S5, the pH of the tetravalent vanadium reducing solution is adjusted to 1.0~3.0 before entering the countercurrent extraction, and the proportion of tetravalent vanadium in the total vanadium is not less than 95%. The extracted organic phase includes one or more of the following: acidic phosphorus-containing extractant, co-extraction component, modified component, and diluent component; wherein the volume fraction of the acidic phosphorus-containing extractant is 15% to 60%, the extraction ratio O / A is 0.3 to 2.5, the number of countercurrent extraction stages is 2 to 6, and the single-stage mixing time is 3 to 30 min.
8. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S6, the acid concentration of the sulfate-containing acidic back-extraction medium is 1.0~6.0 mol / L, the back-extraction ratio O / A is 1~10, the number of countercurrent back-extraction stages is 1~4, and the single-stage back-extraction time is 3~30 min.
9. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S6, the regenerated organic phase after back-extraction is returned to the countercurrent extraction step for recycling; the leaching residue obtained from multi-stage circulating water leaching is washed and returned to the comprehensive utilization process as iron-titanium solid material or as raw material for subsequent resource recovery.
10. The method for preparing vanadium oxysulfate electrolyte from vanadium-containing solid raw materials using a short-process method according to claim 1, characterized in that, In step S6, the total vanadium concentration in the obtained vanadium oxysulfate electrolyte is 60~120 g / L (based on V), and the vanadium valence state is mainly tetravalent, which can be used as an electrolyte for all vanadium redox flow batteries or its precursor.