Low-volatile PMMA substrate adapted for 450nm blue laser and its preparation method

By introducing laser-absorbing media and chain transfer agents into PMMA sheets and combining them with a stepped heating polymerization process, low-volatile PMMA sheets adapted to 450nm blue lasers were prepared, solving the problems of low efficiency and poor safety of blue laser cutting, and achieving high-efficiency cutting and low release of volatile organic compounds.

CN123106963APending Publication Date: 2026-11-17ANHUI XINTAO OPTOELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611278982.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PMMA sheets have low absorption rates for 450nm blue laser light, resulting in low cutting efficiency and the generation of a large number of harmful volatile organic compounds during the cutting process, which cannot meet the requirements of home DIY users for surface finish and safety.

Method used

By introducing organic dyes or nano-metal oxides with absorption peaks at 450 nm wavelength into PMMA sheets as laser absorption media, and combining them with chain transfer agents and a step-by-step heating polymerization process, low-volatility PMMA sheets are prepared, achieving efficient capture and thermal conversion of blue light energy while reducing the release of organic compounds.

Benefits of technology

It improves the absorption efficiency of blue laser light, reduces the release of organic compounds during the cutting process, improves the quality and safety of the cut surface, and solves the problems of low cutting efficiency and safety hazards of traditional PMMA sheets under blue laser light.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a low-volatile PMMA sheet adapted for 450nm blue laser and its preparation method, comprising: S1, mixing and prepolymerizing methyl methacrylate monomer, initiator, chain transfer agent, laser absorbing medium and heat stabilizing agent, controlling the conversion rate to 15%~25%; S2, casting followed by step-heating bulk polymerization to a conversion rate of over 95%; S3, demolding followed by annealing to obtain the final product. The laser absorbing medium is an organic dye or nano-metal oxide with an absorption peak at 450nm. By introducing a laser absorbing medium, efficient capture and thermal conversion of 450nm blue light is achieved. The residual monomer content is reduced to less than 0.5% through chain transfer agent and step-polymerization, solving the problem of ineffective cutting and processing of general PMMA due to the blue light absorption blind zone, and addressing the issue of high volatile content. This method is suitable for desktop laser DIY applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of PMMA preparation technology, specifically to a low-volatile PMMA substrate adapted to 450nm blue laser and a method for preparing such a substrate. Background Technology

[0002] In recent years, desktop laser processing equipment using 450nm blue diode lasers as its core light source has developed rapidly, and is becoming increasingly popular, transitioning from industrial geek tools to home creative appliances. These devices, with their advantages of miniaturization, long lifespan, and high beam quality, have become a technological pillar in the personal DIY market. However, the leapfrog development of hardware performance has lagged far behind the matching level of downstream consumables.

[0003] Currently, most general-purpose PMMA sheets on the market are designed for traditional 10.6-micron wavelength carbon dioxide lasers. Due to the intrinsic absorption of infrared light in this wavelength band by the ordinary PMMA molecular chain, the processing efficiency is acceptable. However, for 450nm blue light, ordinary transparent or light-colored PMMA sheets are almost in a physical "absorption blind zone"—the light energy transmittance is too high, and most of the laser energy passes directly through the sheet without being effectively converted into heat energy, resulting in extremely low cutting efficiency, and sometimes even failing to cut through at rated power. Even if processing is attempted, severe yellowing, melting and flowing, or edge slag are easily caused by localized overheating, completely failing to meet the requirements of DIY users for surface finish and processing precision.

[0004] Furthermore, desktop laser equipment is primarily used in relatively enclosed indoor environments such as homes, classrooms, or studios, making users extremely sensitive to odors and safety concerns generated during processing. General-purpose PMMA sheets typically have a high residual monomer content, which releases large amounts of methyl methacrylate monomers and other volatile organic compounds during the high-temperature laser ablation process, producing a pungent odor and posing a potential health risk to users. Summary of the Invention

[0005] This invention addresses the problems in the prior art by providing a low-volatility PMMA substrate adapted to 450nm blue laser light and its preparation method. The specific technical solution is as follows: On one hand, the present invention provides a method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser light, comprising the following steps: S1: Methyl methacrylate monomer, initiator, chain transfer agent, laser absorbing medium and heat stabilizer are mixed and prepolymerized under stirring conditions. The reaction temperature is controlled at 50~80℃ and the conversion rate is 15%~25% to obtain prepolymer slurry. The laser absorption medium is an organic dye or nanoscale metal oxide with an absorption peak at a wavelength of 450 nm, which is soluble or stably dispersed in methyl methacrylate monomer, and the amount added is 0.001% to 0.5% of the mass of methyl methacrylate monomer; S2: The prepolymer slurry obtained in step S1 is poured into a mold, and a step-by-step heating program is used to carry out the bulk polymerization reaction. The step-by-step heating program includes: first, holding at 50~65℃ for 3~8 hours, then heating to 70~90℃ and holding for 6~14 hours, and finally heating to 100~120℃ and holding for 1~4 hours, so that the monomer conversion rate reaches more than 95%. S3: After the polymerization reaction is completed, the material is demolded, annealed, and cut to obtain a low-volatile PMMA sheet material that is compatible with 450nm blue laser light. The annealing conditions are as follows: heat treatment at 80~110℃ for 2~6 hours, followed by slow cooling to room temperature.

[0006] As a further technical solution of the present invention, the laser absorption medium in step S1 is selected from at least one organic dye selected from Solvent Yellow 93, Solvent Orange 60, Solvent Red 52, Solvent Green 3, and Solvent Blue 97, and its addition amount is 0.005% to 0.1% of the mass of methyl methacrylate monomer.

[0007] As a further technical solution of the present invention, the laser absorption medium in step S1 is nano-indium tin oxide or nano-tungsten oxide, with an average particle size of 10~100 nanometers, and the amount added is 0.01%~0.3% of the mass of methyl methacrylate monomer.

[0008] As a further technical solution of the present invention, the initiator in step S1 is a compound system of azobisisobutyronitrile and benzoyl peroxide, with a mass ratio of 1:3 to 3:1, and the total amount added is 0.01% to 0.5% of the mass of methyl methacrylate monomer.

[0009] As a further technical solution of the present invention, the chain transfer agent in step S1 is an iodoalkane compound selected from at least one of ethyl iodoacetate, iodopropane, and iodobutane, and the amount added is 0.01% to 0.5% of the mass of methyl methacrylate monomer.

[0010] As a further technical solution of the present invention, the heat stabilizing agent in step S1 includes a primary antioxidant, a secondary antioxidant, and a heat stabilizer. The primary antioxidant is antioxidant 1076, the secondary antioxidant is dilauryl thiodipropionate, and the total amount of the two added is 0.05% to 0.5% of the mass of methyl methacrylate monomer. The heat stabilizer is calcium stearate or zinc stearate, and the amount added is 0.01% to 0.2% of the mass of methyl methacrylate monomer.

[0011] As a further technical solution of the present invention, organic or inorganic pigments are added in step S1 to obtain a plate with a specific color, wherein the amount of pigment added is 0.01% to 1% of the mass of methyl methacrylate monomer.

[0012] As a further technical solution of the present invention, the mold mentioned in step S2 is a circulating water bath jacket mold, and the temperature fluctuation of the mold cavity is controlled within ±1℃; before casting, the prepolymer slurry is subjected to vacuum degassing treatment, with a vacuum degree of -0.08~-0.1MPa and a degassing time of 10~60 minutes.

[0013] As a further technical solution of the present invention, the annealing conditions in step S3 are: holding at 90~100℃ for 3~4 hours, and then slowly cooling to room temperature at a rate of no more than 5℃ / hour.

[0014] On the other hand, the present invention also provides a low-volatile PMMA sheet material adapted to 450nm blue laser, which is prepared by the above method. The PMMA sheet material has an absorbance of 0.5~3.0 at a wavelength of 450nm, a residual monomer content of less than 0.5%, and a heat-affected zone width of no more than 0.3 mm when cut by 450nm blue laser. The amount of volatile organic compounds released during the cutting process is reduced by more than 50% compared with PMMA sheet material of the same specification without laser absorption medium.

[0015] The beneficial effects of this invention are as follows: (1) In this invention, organic dyes with strong absorption peaks at 450nm wavelength or nano-metal oxides with plasma resonance effect are introduced at the molecular level as laser absorption media to achieve efficient capture and thermal conversion of blue light energy without destroying the basic color of the board. This solves the problems of general PMMA boards being almost "optically transparent" to 450nm blue light, having low energy utilization, and being unable to be effectively cut.

[0016] (2) In this invention, by precisely controlling the molecular weight distribution of the chain transfer agent and coordinating with the step-heating bulk polymerization process, an ultra-low residual level of less than 0.5% of the residual monomer content is achieved, thereby reducing the release of volatile organic compounds during laser ablation from the source and solving the problem of pungent odor and health risks in desktop laser processing in indoor environments.

[0017] (3) In this invention, by combining stepped heating polymerization with annealing treatment, a polymerization conversion rate of over 95% and full elimination of internal stress in the plate are achieved, thus solving the problem of edge microcracks and edge chipping caused by thermal stress concentration under the action of high-energy laser beam.

[0018] (4) In this invention, by combining the laser absorption medium with pigments, a unified adaptation of black, yellow, orange, green and other colored plates to the 450nm blue light cutting process is achieved, which solves the problem that the cutting effect of traditional colored plates is inconsistent due to different pigment formulas and that a unified process parameter library cannot be established. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments.

[0020] The detection method of the present invention is as follows: Absorbance: The absorbance of a 3 mm thick plate was measured at a wavelength of 450 nm using a UV-Vis spectrophotometer.

[0021] Residual monomer content: determined by gas chromatography.

[0022] Cutting performance: Cutting tests were conducted on a desktop device equipped with a 450nm blue diode laser, and the width of the heat-affected zone on the cut surface was measured using an optical microscope.

[0023] Volatile organic compound (VOC) emission: Laser cutting was performed in a sealed test chamber, and the peak concentration of total volatile organic compounds (VOCs) in the chamber was measured using a VOC detector to compare the percentage reduction with that of PMMA sheets of the same specifications without laser absorption media.

[0024] Transmittance and haze: determined according to GB / T 7134-2008 standard.

[0025] Impact strength: According to GB / T 7134-2008 standard, unnotched specimens of simply supported beams.

[0026] The following are specific embodiments; Example 1

[0027] Step S1: Take 10 kg of methyl methacrylate monomer, after removing the polymerization inhibitor by vacuum distillation, and add it to the reactor. Add sequentially 10 g of a 1:1 mixture of azobisisobutyronitrile (AIBN) and benzoyl peroxide (CPO), 5 g of ethyl iodoacetate (EIA) chain transfer agent, 0.5 g of solvent yellow 93 (laser absorption medium), 3 g of primary antioxidant 1076, 3 g of dilauryl thiodipropionate (ADT) auxiliary antioxidant, and 5 g of calcium stearate (heat stabilizer). Stir at 100 rpm under nitrogen protection and react at 65°C until the conversion rate reaches approximately 20%. Cool to terminate the reaction, obtaining the prepolymer slurry.

[0028] Step S2: Degas the slurry under vacuum at -0.095MPa for 30 minutes, then inject it into a circulating water bath jacketed mold. Step heating: 55℃ for 5 hours → 80℃ for 8 hours → 110℃ for 2 hours, with mold cavity temperature fluctuation controlled within ±0.8℃.

[0029] Step S3: Cooling and demolding. Anneal the sheet at 95°C for 3 hours, then slowly cool it to room temperature at 5°C / hour, and cut it to obtain the finished product.

[0030] Finished product performance: Absorbance at 450nm 1.8, residual monomer 0.28%, heat-affected zone width 0.12 mm, volatile organic compound reduction rate 72%, light transmittance 89.5%, impact strength 18.1.8 kJ / m² 2 The cut surface has a mirror-like smoothness, with no yellowing or slag residue.

[0031] Example 2

[0032] Step S1: 10 kg of monomer, the laser absorption medium is changed to nano-indium tin oxide with an average particle size of 50 nm and an addition amount of 20 g, the rest is the same as in Example 1.

[0033] Step S2: Step heating: 60℃ for 4 hours → 85℃ for 7 hours → 115℃ for 2 hours.

[0034] Step S3: Anneal the sheet at 100℃ for 4 hours, then slowly cool it at 5℃ / hour.

[0035] Finished product performance: Absorbance at 450nm 1.5, residual monomer 0.31%, heat-affected zone width 0.18 mm, volatile organic compound reduction rate 65%, light transmittance 91.2%, impact strength 17.8 kJ / m² 2 .

[0036] Example 3

[0037] Step S1: Based on the formulation of Example 1, add an additional 30 grams of black organic pigment carbon black dispersion and increase the laser absorption medium solvent yellow 93 to 0.8 grams.

[0038] Steps S2 and S3 are the same as in Example 1.

[0039] Finished product performance: 450nm absorbance 2.8, residual monomer 0.25%, heat-affected zone width 0.08 mm, volatile organic compound reduction rate 78%, the sheet is uniformly black, and the cut surface is flat and smooth.

[0040] Example 4

[0041] Step S1: Based on the formulation of Example 1, add 20 grams of orange organic pigment and replace the laser absorption medium with 0.6 grams of Solvent Orange 60.

[0042] Steps S2 and S3 are the same as in Example 1.

[0043] Finished product performance: 450nm absorbance 2.1, residual monomer 0.29%, heat-affected zone width 0.10 mm, volatile organic compound reduction rate 70%, the board is bright orange, and the cut surface has no discoloration.

[0044] Comparative Example 1 Without adding any laser-absorbing medium, the rest is the same as in Example 1.

[0045] Results: The absorbance at 450 nm was only 0.08, making it impossible to cut through a 3 mm thick sheet at rated power. Even after increasing the power to its limit, it was barely cut through, but the heat-affected zone width reached 0.65 mm, with severe yellowing and slagging at the edges, and the release of volatile organic compounds was approximately three times higher than in Example 1.

[0046] VII. Comparative Example 2 No chain transfer agent was added, and a one-stage 85°C isothermal polymerization process was used. The rest of the formulation was the same as in Example 1.

[0047] Results: The residual monomer content was as high as 1.5%, the odor during laser cutting was pungent, and the reduction rate of volatile organic compounds was only 18%. The width of the heat-affected zone on the cut surface was 0.35 mm, and microcracks were generated.

[0048] Performance tests were conducted on Examples 1-4 and Comparative Examples 1 and 2, and the test results are shown in Table 1.

[0049]

[0050] Table 1 Examples 1-4 all showed an absorbance greater than 1.5 at 450nm, and the width of the heat-affected zone on the cut surface did not exceed 0.2 mm, which was far better than the 0.65 mm of Comparative Example 1. This proves that the introduction of the laser absorption medium fundamentally solves the problem of low blue light absorption efficiency.

[0051] The residual monomer content in all examples was less than 0.5%, and the volatile organic compound reduction rate was more than 65%, which was significantly better than the 1.5% and 18% of Comparative Example 2, demonstrating that the synergy between the chain transfer agent and the step polymerization process achieved ultra-low residue and low volatility.

[0052] Examples 3 and 4 show that by introducing pigments for coloring and adjusting the type and amount of laser absorption medium, it is possible to ensure that different colored boards have excellent blue light cutting performance and strong process adaptability.

[0053] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it.

Claims

1. A method for preparing low-volatile PMMA substrates adapted to 450nm blue laser light, characterized in that, Includes the following steps: S1: Methyl methacrylate monomer, initiator, chain transfer agent, laser absorbing medium and heat stabilizer are mixed and prepolymerized under stirring conditions. The reaction temperature is controlled at 50~80℃ and the conversion rate is 15%~25% to obtain prepolymer slurry. The laser absorption medium is an organic dye or nanoscale metal oxide with an absorption peak at a wavelength of 450 nm, which is soluble or stably dispersed in methyl methacrylate monomer, and the amount added is 0.001% to 0.5% of the mass of methyl methacrylate monomer; S2: The prepolymer slurry obtained in step S1 is poured into a mold, and a step-by-step heating program is used to carry out the bulk polymerization reaction. The step-by-step heating program includes: first, holding at 50~65℃ for 3~8 hours, then heating to 70~90℃ and holding for 6~14 hours, and finally heating to 100~120℃ and holding for 1~4 hours, so that the monomer conversion rate reaches more than 95%. S3: After the polymerization reaction is completed, the material is demolded, annealed, and cut to obtain a low-volatile PMMA sheet material that is compatible with 450nm blue laser light. The annealing conditions are as follows: heat treatment at 80~110℃ for 2~6 hours, followed by slow cooling to room temperature.

2. The method for preparing low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The laser absorption medium in step S1 is selected from at least one organic dye selected from Solvent Yellow 93, Solvent Orange 60, Solvent Red 52, Solvent Green 3, and Solvent Blue 97, and its addition amount is 0.005% to 0.1% of the mass of methyl methacrylate monomer.

3. The method for preparing low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The laser absorption medium mentioned in step S1 is nano-indium tin oxide or nano-tungsten oxide, with an average particle size of 10~100 nanometers, and the amount added is 0.01%~0.3% of the mass of methyl methacrylate monomer.

4. The method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The initiator mentioned in step S1 is a compound system of azobisisobutyronitrile and benzoyl peroxide, with a mass ratio of 1:3 to 3:1, and the total amount added is 0.01% to 0.5% of the mass of methyl methacrylate monomer.

5. The method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The chain transfer agent mentioned in step S1 is an iodoalkane compound selected from at least one of ethyl iodoacetate, iodopropane, and iodobutane, and the amount added is 0.01% to 0.5% of the mass of methyl methacrylate monomer.

6. The method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The heat stabilizing agent mentioned in step S1 includes a primary antioxidant, a secondary antioxidant, and a heat stabilizer. The primary antioxidant is antioxidant 1076, the secondary antioxidant is dilauryl thiodipropionate, and the total amount of the two added is 0.05% to 0.5% of the mass of methyl methacrylate monomer. The heat stabilizer is calcium stearate or zinc stearate, and the amount added is 0.01% to 0.2% of the mass of methyl methacrylate monomer.

7. The method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: In step S1, organic or inorganic pigments are added to obtain a board with a specific color. The amount of pigment added is 0.01% to 1% of the mass of methyl methacrylate monomer.

8. The method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The mold mentioned in step S2 is a circulating water bath jacketed mold, and the temperature fluctuation of the mold cavity is controlled within ±1℃; before casting, the prepolymer slurry is subjected to vacuum degassing treatment, with a vacuum degree of -0.08~-0.1MPa and a degassing time of 10~60 minutes.

9. The method for preparing a low-volatile PMMA substrate adapted to 450nm blue laser according to claim 1, characterized in that: The annealing conditions described in step S3 are as follows: hold at 90~100℃ for 3~4 hours, and then slowly cool to room temperature at a rate not exceeding 5℃ / hour.

10. A low-volatile PMMA substrate adapted for 450nm blue laser light, characterized in that, The PMMA sheet prepared by the method according to any one of claims 1 to 9 has an absorbance of 0.5 to 3.0 at a wavelength of 450 nm, a residual monomer content of less than 0.5%, and a heat-affected zone width of no more than 0.3 mm on the cut surface when cut with a 450 nm blue laser. The amount of volatile organic compounds released during the cutting process is reduced by more than 50% compared with PMMA sheets of the same specifications without laser absorption medium.