A method for preparing hydrogels by surfactant vesicle-assisted free radical polymerization
By regulating the hydrogel network structure through the self-assembly of vesicles by anionic and cationic surfactants, the problem of insufficient mechanical properties of traditional hydrogels is solved, achieving high toughness and excellent energy dissipation capacity, and improving the durability of hydrogels under extreme mechanical stress.
Patent Information
- Application Number
- CN202611191171.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional hydrogel sensors suffer from insufficient mechanical properties, limited toughness, and weak energy dissipation, which restricts their durability under extreme mechanical stress.
Vesicles formed by the self-assembly of cationic and anionic surfactants serve as nanoreactors and physical cross-linking nodes. The polymer network structure is regulated through hydrophobic association and electrostatic interactions, increasing the number of physical cross-linking points and providing multiple energy dissipation pathways.
This improves the mechanical stability, elastic recovery, and deformation resistance of the hydrogel, enhancing its durability under extreme mechanical stress.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of hydrogel preparation technology, and more particularly to a hydrogel and a method for preparing the hydrogel. Background Technology
[0002] Hydrogels have significant applications in biomedicine, flexible electronics, and smart sensing due to their excellent biocompatibility and tunable mechanical properties. However, the mechanical properties of traditional hydrogel sensors still need further improvement. For example, the limited toughness and weak energy dissipation of traditional hydrogel sensors restrict their durability under extreme mechanical stress. Summary of the Invention
[0003] In a first aspect, the present invention provides a method for preparing a hydrogel, comprising: mixing a cationic surfactant and anionic surfactant to form a precursor solution containing vesicles; mixing a hydrophobic monomer, a hydrophilic monomer, a crosslinking agent and the precursor solution to form a prepolymerization solution; and using a photoinitiator to initiate crosslinking copolymerization of the prepolymerization solution to form a hydrogel.
[0004] In any embodiment of the first aspect of the present invention, the cationic surfactant includes a quaternary ammonium salt cationic surfactant.
[0005] In any embodiment of the first aspect of the present invention, the anionic surfactant mixture includes sulfate ester salt anionic surfactants.
[0006] In any embodiment of the first aspect of the present invention, the quaternary ammonium salt cationic surfactant includes at least one of hexadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, and hexadecyltrimethylammonium chloride.
[0007] In any embodiment of the first aspect of the present invention, the sulfate ester salt anionic surfactant includes at least one of sodium dodecyl sulfate, ammonium dodecyl sulfate, and monoethanolamine dodecyl sulfate.
[0008] In any embodiment of the first aspect of the present invention, the molar ratio of cationic surfactant to anionic surfactant is 1:0.5-1:1.1.
[0009] In any embodiment of the first aspect of the present invention, the total mass fraction of cationic surfactant and anionic surfactant is 0.58% to 2.02% based on the total mass of the precursor fluid.
[0010] In any embodiment of the first aspect of the present invention, the bilayer thickness of the vesicles in the precursor solution is 4 nm to 10 nm. This structure facilitates further control of the polymer network structure and imparts superior overall performance to the hydrogel.
[0011] In any embodiment of the first aspect of the present invention, the average diameter of the vesicles in the precursor solution is 50 nm to 800 nm. This structure facilitates further control of the polymer network structure and imparts superior overall performance to the hydrogel.
[0012] In any embodiment of the first aspect of the present invention, the bilayer thickness of the vesicles in the hydrogel is 4 nm to 10 nm. This structure facilitates further control of the polymer network structure and imparts superior overall performance to the hydrogel.
[0013] In any embodiment of the first aspect of the present invention, the average diameter of the vesicles in the hydrogel is 50 nm to 800 nm. This structure facilitates further control of the polymer network structure and imparts superior overall performance to the hydrogel.
[0014] In any embodiment of the first aspect of the present invention, the hydrophobic monomer includes alkyl methacrylate hydrophobic monomers, wherein the carbon number of the carbon backbone in the alkyl methacrylate hydrophobic monomer is 12 to 18, for example 12, 14, 16 or 18. Optionally, the alkyl methacrylate hydrophobic monomer includes one of dodecyl methacrylate and octadecyl methacrylate.
[0015] In any embodiment of the first aspect of the present invention, the hydrophilic monomer includes an acrylamide-type hydrophilic monomer, wherein the number of carbon atoms in the acrylamide-type hydrophilic monomer is 3 to 10, for example 3, 4, 5, 6, 7, 8, 9 or 10. Optionally, the acrylamide-type hydrophilic monomer includes one of acrylamide, dimethylacrylamide, diethylacrylamide, and N-isopropylacrylamide.
[0016] In any embodiment of the first aspect of the present invention, the mass ratio of the hydrophilic monomer to the hydrophobic monomer is 8:2 to 9.5:0.5, preferably 9:1.
[0017] In any embodiment of the first aspect of the present invention, the sum of the mass fractions of the hydrophilic monomer and the hydrophobic monomer is 15% to 30% of the total mass of the prepolymer solution.
[0018] In any embodiment of the first aspect of the present invention, the photoinitiator includes at least one of 2,2-diethoxyacetophenone, 1-hydroxycyclohexylphenyl ketone, and α-ketoglutaric acid.
[0019] In any embodiment of the first aspect of the present invention, the mass fraction of the photoinitiator is 0.4% to 0.6% based on the total mass of the prepolymer solution.
[0020] In any embodiment of the first aspect of the present invention, the step of mixing a cationic surfactant and anionic surfactant to form a precursor solution comprising self-assembled vesicles includes: The cationic surfactant, anionic surfactant and water were mixed and stirred evenly at 20 °C to 40 °C, and then sonicated for 10 min to 20 min to prepare a precursor solution containing vesicles.
[0021] In any embodiment of the first aspect of the present invention, the step of mixing the hydrophobic monomer, the hydrophilic monomer, the crosslinking agent and the precursor liquid to form a prepolymerization solution includes: adding the hydrophobic monomer and the hydrophilic monomer to the precursor liquid at 20 °C to 40 °C and stirring for 10 min to 20 min to dissolve them, and then adding the crosslinking agent to prepare a prepolymerization solution.
[0022] In any embodiment of the first aspect of the present invention, the step of using a photoinitiator to initiate cross-linking copolymerization of a prepolymer solution to form a hydrogel includes: adding a photoinitiator and a cross-linking agent to a prepolymer solution and stirring for 10 min-20 min to dissolve them, and then initiating free radical polymerization by ultraviolet light irradiation to form a hydrogel.
[0023] The core of this invention lies in utilizing vesicles formed by the self-assembly of anionic and cationic surfactants as "nanoreactors" and "physical cross-linking nodes." Compared to traditional spherical micelles, vesicles possess a unique bilayer structure, providing a larger hydrophobic interface, more stable hydrophobic microregions, and a reaction microenvironment separated by internal and external phases. Therefore, vesicles not only serve as a space for the containment and enrichment of hydrophobic monomers but also participate in regulating monomer distribution, chain growth behavior, and polymer network formation during polymerization. Specifically, hydrophobic monomers can be anchored in the vesicle bilayer structure through hydrophobic interactions, making the vesicles local sites for polymer chain growth and network connection during polymerization. This structure is beneficial for increasing the number of physical cross-linking points in the polymer network, improving network cross-linking density, and reducing network defects. Simultaneously, when the hydrogel deforms under external forces, the vesicle bilayer provides multiple energy dissipation pathways through reversible destruction and recombination of hydrophobic associations, interface deformation, and local chain segment slippage, thereby improving the mechanical stability, elastic recovery ability, and deformation resistance of the hydrogel. Therefore, vesicles can more effectively regulate the polymer network structure and endow hydrogels with superior overall properties compared to spherical micelles.
[0024] In a second aspect, the present invention provides a hydrogel obtained by the preparation method of any embodiment of the first aspect.
[0025] In any embodiment of the second aspect of the present invention, the fracture stress of the hydrogel is 30 kPa to 100 kPa.
[0026] In any embodiment of the second aspect of the present invention, the fracture strain of the hydrogel is 130% to 360%.
[0027] In any embodiment of the second aspect of the present invention, the elastic modulus of the hydrogel is 70 kPa to 140 kPa.
[0028] In any embodiment of the second aspect of the present invention, the hydrogel has a toughness of 10 kJ / m. 3 ~220 kJ / m 3 .
[0029] In any embodiment of the second aspect of the present invention, the conductivity of the hydrogel is 0.04 S / m to 0.12 S / m.
[0030] The vesicle-assisted free radical polymerization hydrogel provided by this invention overcomes the shortcomings of traditional hydrogels, such as poor mechanical properties under extreme external force conditions. Furthermore, the preparation method is mild, the process is simple, and the structure is controllable. At the same time, it broadens the research direction of surfactants in assisting free radical polymerization.
[0031] Hydrogels consist of polyacrylamide molecular chains and alkyl methacrylate hydrophobic segments. The molecular chains are mainly linked by hydrophobic association and hydrogen bonding to form dynamic physical cross-linking points, thus forming a uniform and dense three-dimensional porous network structure.
[0032] Hydrogels also include cations and anions generated by the dissociation of cationic and anionic surfactants. These ions are uniformly distributed in the polymer network, providing stable electrical conductivity to the hydrogel.
[0033] The preparation method of this invention is simple, easy to implement, and highly applicable. Attached Figure Description
[0034] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the embodiments of the present invention will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0035] Figure 1 The infrared spectrum of the vesicle-assisted free radical polymerized hydrogel provided in Embodiment 1 of the present invention is shown. Figure 2 Scanning electron microscope image and energy dispersive spectroscopy (EDS) image of the vesicle-assisted free radical polymerized hydrogel prepared in Example 1; Figure 3 The single tensile stress-strain curves of hydrogels prepared under three free radical polymerization conditions are shown. Figure 4 SAXS diagrams of the vesicle structures before and after polymerization in Example 1; Figure 5The images show the molecular dynamics simulation of the hydrophobic monomer entering the vesicle bilayer in Example 1 and the changes in the diameter of the vesicle bilayer. Figure 6 The cyclic progressive stretching curve and energy dissipation rate of the vesicle-assisted free radical polymerized hydrogel prepared in Example 1 are shown. Detailed Implementation
[0036] To make the objectives, technical solutions, and beneficial effects of this invention clearer, the invention will be described in detail below with reference to specific embodiments. It should be understood that the embodiments described in this specification are merely illustrative and not intended to limit the scope of the invention.
[0037] For simplicity, this paper only explicitly discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, just as any upper limit can be combined with any other upper limit to form an undefined range. Furthermore, although not explicitly stated, every point or individual value between the endpoints of a range is included within that range. Therefore, each point or individual value can serve as its own lower or upper limit and be combined with any other point or individual value, or with other lower or upper limits, to form an undefined range.
[0038] The above description of the invention is not intended to describe every disclosed embodiment or implementation of the invention. Instead, the following description provides more specific examples of exemplary embodiments. Throughout the invention, guidance is provided through a series of embodiments that can be used in various combinations. In each example, the examples are listed only as representative groups and should not be construed as exhaustive.
[0039] In related technologies, surfactants are considered to prepare micelles to solubilize hydrophobic monomers and improve toughness. However, micelles are usually a single hydrophobic core structure, and the hydrophobic interface they can provide is limited. Their main function is still concentrated on solubilizing hydrophobic monomers and a certain degree of physical cross-linking. It is difficult to further regulate the monomer distribution, chain growth behavior and hydrogel network topology during the free radical polymerization process.
[0040] In contrast, this invention considers that cationic and anionic surfactants can self-assemble into vesicles with a bilayer structure through electrostatic interactions and hydrophobic association, which have a larger hydrophobic interface and greater separation between the inner and outer phases. However, in free radical polymerization systems, hydrophobic monomers, initiators, and growing polymer chains may disrupt the vesicle structure. Therefore, how to maintain vesicle stability during polymerization and utilize vesicles to regulate the formation of hydrogel networks remains a problem that urgently needs to be solved.
[0041] To further address the above technical problems, the present invention aims to provide a method for preparing hydrogels by surfactant vesicle-assisted free radical polymerization. The preparation method is safe and simple, the raw materials are readily available, and the obtained hydrogels have excellent mechanical properties.
[0042] In this invention, the hydrophobic monomer backbone is relatively long, and the long alkyl chain can be embedded in the vesicle bilayer through hydrophobic association. The photoinitiator can also be enriched in the hydrophobic microregions of the vesicles. The hydrophilic monomer has a relatively short molecular chain, mainly distributed in the aqueous phase, and copolymerizes with the hydrophobic monomer in the vesicle bilayer after free radical initiation. Thus, the vesicles serve as local reaction microregions and dynamic physical cross-linking nodes, forming a dense and low-defect hydrogel network. The hydrophilic monomer acts as a "bridge" between different vesicles, connecting the hydrophobic monomers on different vesicles to copolymerize, thereby constructing a polymer network with a high cross-linking density. At the same time, the hydrophilic monomer can bind water molecules, thus maintaining the elasticity of the hydrogel and preventing water loss and loss of elasticity. As nanoscale microregions, the vesicles can enhance the local monomer concentration at the nanoscale, thereby promoting the free radical polymerization reaction. Meanwhile, the hydrophobic association between the vesicles and the hydrophobic monomers can effectively dissipate energy and prevent damage to the hydrogel during application.
[0043] The inventors have conducted extensive research on the polymerization mechanism and mechanical properties of anionic and cationic surfactant vesicle-assisted polymerization hydrogels. They have studied how the copolymerization of acrylamide hydrophilic monomers and alkyl methacrylate hydrophobic monomers in a vesicle system can prepare hydrogels with excellent mechanical properties.
[0044] Therefore, the first aspect of the present invention provides a method for preparing a vesicle composite hydrogel, the method comprising: step S100 of preparing a precursor solution containing vesicles with anionic and cationic surfactants; step S200 of mixing a hydrophilic monomer and a hydrophobic monomer with the precursor solution containing vesicles to form a prepolymerization solution; and step S300 of using a photoinitiator to initiate crosslinking copolymerization of the prepolymerization solution to form an antifreeze vesicle hydrogel.
[0045] Step S100: Prepare a precursor solution containing vesicles.
[0046] In step S100, the cationic surfactant, anionic surfactant and water are stirred evenly at 20~40 ℃ and sonicated for 10 min-20 min.
[0047] Surfactants can rapidly self-assemble into stable vesicles at 20~40 ℃ to obtain a homogeneous nanostructure dispersion system without the need for additional heating, which is convenient for industrial production.
[0048] In some embodiments, the cationic surfactant includes at least one of hexadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, and hexadecyltrimethylammonium chloride.
[0049] In some embodiments, the anionic surfactant includes at least one of sodium dodecyl sulfate, ammonium dodecyl sulfate, and monoethanolamine dodecyl sulfate.
[0050] Cationic and anionic surfactants spontaneously form a stable bilayer vesicle structure through electrostatic attraction and hydrophobic association, providing a solubilizing interface for hydrophobic monomers and dynamic physical cross-linking points for hydrogels, thus significantly improving mechanical properties.
[0051] In some embodiments, the total mass fraction of cationic and anionic surfactants is 0.58% to 2.02% based on the total mass of the precursor fluid containing vesicles, optionally 1.15%–1.73%, and more preferably 1.44%–1.73%.
[0052] For example, the total mass fraction of cationic surfactants and anionic surfactants is 0.58%, 0.86%, 1.15%, 1.44%, 1.73%, 2.02%, or any range of two of the above values.
[0053] When the total mass fraction of cationic and anionic surfactants is within the above range, it is beneficial to the integrity and stability of the vesicle structure, giving the hydrogel excellent mechanical properties.
[0054] Step S200: Prepare the prepolymerization solution In step S200, at least the acrylamide hydrophilic monomer, the alkyl methacrylate hydrophobic monomer, and the precursor liquid containing vesicles are mixed to form a prepolymerization solution.
[0055] In some embodiments, the mass fraction of acrylamide hydrophilic monomers, based on the total mass of the prepolymerized solution, is 15% to 29%, exemplarily a range of 15%, 20%, 21%, 22%, 23%, 24%, 25%, 29%, or any two of these values. Optionally, the mass fraction of acrylamide hydrophilic monomers is 24% to 29%.
[0056] In some embodiments, the mass fraction of alkyl methacrylate hydrophobic monomers is greater than 0% and less than or equal to 6% based on the total mass of the prepolymerized solution. Optionally, the mass fraction of alkyl methacrylate hydrophobic monomers is from 1% to 6%, exemplarily a range of 1.0%, 2%, 3%, 4%, 5%, 6%, or any two of these values.
[0057] In some embodiments, the mass ratio of hydrophilic monomer to hydrophobic monomer is 8:2 to 9.5:0.5, and can be selected as 9.5:0.5, 9:1, 8.5:1.5, or 8:2, and is more preferably 9:1.
[0058] When the ratio of hydrophilic monomers to hydrophobic monomers is within the above range, the resulting hydrogel network is dense and uniform with a moderate cross-linking density, which is more conducive to improving mechanical toughness and ion transport stability.
[0059] As the content of hydrophobic monomers increases, the hydrophobic association of polymer chains is enhanced, the dissipation capacity of the hydrogel is significantly improved, and the elasticity is more excellent. The hydrophobic long-chain alkyl group forms a strong hydrophobic effect with the vesicle bilayer, which can further enhance the dissipation channel and achieve excellent mechanical effects.
[0060] In some embodiments, the sum of the mass fractions of hydrophilic and hydrophobic monomers is 15% to 30% based on the total mass of the prepolymer solution, and optionally 20% to 30%.
[0061] When the total monomer concentration is within the above range, the polymerization rate is moderate, the network structure is uniform, and the mechanical properties are optimal.
[0062] When the total concentration of monomers is too high, it will lead to excessive local cross-linking and uneven structure; when the concentration is too low, the network will be sparse and the strength and stability will be insufficient.
[0063] The inventors discovered that, while keeping the total monomer concentration essentially constant, appropriately increasing the proportion of hydrophobic monomers can significantly enhance the mechanical properties of the hydrogel. The mechanical properties of the hydrogel are significantly enhanced with increasing content of hydrophobic monomers and vesicles, because: The polymer chains form strong hydrophobic associations with the hydrophobic bilayer of vesicles, resulting in a significant increase in physical cross-linking. At the same time, the hydrophobic monomers are anchored in the vesicle bilayer, and free radical polymerization takes place in the vesicles as the polymerization site. The increased local monomer concentration and photoinitiator concentration lead to a faster free radical polymerization rate and a significant enhancement in mechanical properties.
[0064] In some embodiments, the acrylamide hydrophilic monomer includes at least one of acrylamide, dimethylacrylamide, diethylacrylamide, and N-isopropylacrylamide.
[0065] The monomers mentioned above contain amide groups, which can form intermolecular hydrogen bonds and enhance the hydrogel properties.
[0066] In some embodiments, alkyl methacrylate hydrophobic monomers include at least one of dodecyl methacrylate and hexadecyl methacrylate.
[0067] The aforementioned monomers contain long-chain alkyl groups that can be inserted into the hydrophobic bilayer of vesicles to form strong physical cross-links, thereby enhancing toughness and dissipation capacity.
[0068] For example, the hydrophilic monomer is acrylamide and the hydrophobic monomer is dodecyl methacrylate. The two are copolymerized in an anionic and cationic vesicle system to form a three-dimensional network framework, achieving excellent mechanical properties.
[0069] Step S300: Photoinitiated polymerization to form vesicle hydrogel In step S300, a photoinitiator is used to initiate the cross-linking copolymerization of the prepolymer solution to form a vesicle composite hydrogel.
[0070] In some embodiments, the photoinitiator mass fraction is 0.4%–0.6% based on the total mass of the prepolymer solution, exemplarily a range of 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, or any two of these values.
[0071] The system prior to copolymerization can be understood as a prepolymerization solution. For example, the total mass of each raw material (organic solvent, monomer, etc.) in the system is taken as the total mass of the prepolymerization solution.
[0072] In some embodiments, the photoinitiator includes at least one of 2,2-diethoxyacetophenone, 1-hydroxycyclohexylphenyl methyl ketone, and α-ketoglutaric acid, used to generate free radicals under ultraviolet light to initiate efficient copolymerization of hydrophilic and hydrophobic monomers.
[0073] In some embodiments, the prepolymer solution is irradiated under ultraviolet light for 10-20 minutes at 20°C to 40°C to complete the crosslinking polymerization.
[0074] According to embodiments of the present invention, a hydrogel is obtained by photoinitiated free radical polymerization of acrylamide hydrophilic monomers and alkyl methacrylate hydrophobic monomers in the presence of anionic and cationic vesicles.
[0075] In the system of this invention, water is used as the solvent to prepare hydrogels. By preparing a precursor solution containing vesicles in an aqueous system and further using vesicles as local reaction areas, hydrogels are prepared, resulting in hydrogels with excellent mechanical properties.
[0076] In some embodiments, the hydrogel of the present invention exhibits excellent mechanical resilience and cyclic stability at room temperature. Mechanical testing was performed using an electronic universal testing machine; the compressed specimen was cylindrical with a diameter of 20–22 mm and a height of 9–11 mm.
[0077] The compression rate for compression tests, cyclic progressive compression tests, and cyclic compression tests is 20–30 mm / min. The compression response and recovery time of the hydrogel is 0.15–0.20 s, and it can completely recover its original shape under 40–80% compressive strain without cracking or plastic deformation.
[0078] Meanwhile, the hydrogel has excellent fatigue resistance, can stably achieve 50 to 1000 compression cycle tests, can complete about 500 continuous compression cycles under 50% constant strain without significant performance degradation, and can achieve continuous progressive compression within the strain range of 10 to 80% while maintaining structural integrity and signal stability.
[0079] This invention utilizes a vesicle bilayer formed by the self-assembly of anionic and cationic surfactants as enriched microregions for hydrophobic monomers and photoinitiators. This maintains the stability of the vesicle structure during free radical polymerization and serves as a dynamic physical crosslinking node in the construction of the hydrogel network. Compared to micellar-assisted polymerization hydrogels, the resulting hydrogel exhibits higher network density, lower network defects, and superior mechanical properties.
[0080] The above results demonstrate that the vesicle-assisted composite hydrogel of the present invention exhibits high elasticity, rapid response, low residual deformation, and long-cycle fatigue resistance at room temperature, providing reliable material support for the practical application of flexible sensors, wearable devices, and smart insole systems.
[0081] The above test parameters can be determined using conventional testing equipment and standard methods in this field, or characterized in accordance with relevant national standards.
[0082] The following examples describe the disclosure of this invention in more detail. These examples are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of this disclosure. Unless otherwise stated, all fractions, percentages, and ratios reported in the following examples are based on weight, and all reagents used in the examples are commercially available or synthesized using conventional methods and are ready for use without further processing. The instruments used in the examples are also commercially available. Example
[0083] In this embodiment, a precursor solution containing vesicles is prepared using hexadecyltrimethylammonium bromide, sodium dodecyl sulfate, and water. Acrylamide and dodecyl methacrylate are used as monomers and mixed and dissolved with the vesicle-containing precursor solution. High-performance hydrogels are prepared by polymerization initiated by a photoinitiator, specifically including the following steps: (1) Preparation of vesicle-containing precursor solution: Accurately weigh hexadecyltrimethylammonium bromide and sodium dodecyl sulfate in a 1:1 molar ratio, i.e., 0.0335 g of hexadecyltrimethylammonium bromide (CTAB) and 0.0265 g of sodium dodecyl sulfate (SDS). Add 3.41 g of deionized water and mix. Stir at 32 °C for 10 min at a stirring speed of 500 rpm, and then sonicate for 10 min to allow the surfactants to fully self-assemble into vesicles. The surfactant mass fraction was 1.73% based on the total mass of the vesicle-containing precursor solution.
[0084] (2) Preparation of the prepolymerization solution: Accurately weigh acrylamide:dodecyl methacrylate in a mass ratio of 9:1, i.e., 1.35 g of acrylamide and 0.15 g of dodecyl methacrylate. Add 0.005 g of crosslinking agent N,N′-methylenebisacrylamide. Add the monomer to the vesicle-containing precursor solution in (1) above and stir to dissolve at 32 °C. Finally, add 0.025 g of photoinitiator 2,2-diethoxyacetophenone to obtain the prepolymerization solution. The mass fraction of acrylamide in the prepolymerization solution is 27%, and the mass fraction of dodecyl methacrylate is 3%.
[0085] (3) Preparation of hydrogel: The prepolymer solution was injected into a polytetrafluoroethylene mold and irradiated under ultraviolet light for 10 min to obtain a vesicle-assisted composite hydrogel.
[0086] Figure 1 The infrared spectra of the hydrogel prepared in Example 1 with acrylamide and dodecyl methacrylate monomers are shown. A comparison of the spectra of the monomers and the hydrogel reveals that the hydrogel polymerization mechanism is UV-initiated free radical polymerization. The figure shows that the amide carbonyl peak at 1663 cm⁻¹ and the N–H doublet at 3337 cm⁻¹ and 3162 cm⁻¹ of the acrylamide monomer, as well as the long alkyl chain characteristic peaks at 2922 cm⁻¹ and 2853 cm⁻¹ of the dodecyl methacrylate monomer, shift to 1651 cm⁻¹, 3339 cm⁻¹ and 3191 cm⁻¹, and 2921 cm⁻¹ and 2851 cm⁻¹, respectively, in the hydrogel, indicating successful copolymerization of the monomers. Simultaneously, Figure 2 The characteristic signals of surfactants in the hydrogel are shown, and the Br and Na elements are evenly distributed, indicating that the vesicle structure is uniformly dispersed in the hydrogel network.
[0087] Figure 3 The figures show the continuous loading-unloading curves of the hydrogel prepared in Example 1 under different strain levels during the tensile process. Under tension, the hysteresis energy is extremely low, and the dissipation ratio remains around 5%, exhibiting near-ideal elastomer properties. In vesicle-assisted polymerization hydrogel materials, compared to the polymer network without assisted polymerization hydrogels, the introduction of vesicle structures provides an additional internal energy dissipation pathway. During deformation, reversible micromorphological changes and interfacial frictional slip occur at the vesicle interfaces, absorbing mechanical energy and thus causing the hysteresis phenomenon during the loading-unloading cycle.
[0088] This invention verifies the existence of various structures in the hydrogel using small-angle X-ray diffraction (SAXS).
[0089] Figure 4 The images show SAXS diagrams of the vesicle structures before and after polymerization. Figure 5Molecular dynamics simulation images of the hydrophobic monomer entering the vesicle bilayer and the changes in the diameter of the vesicle bilayer.
[0090] like Figure 4 and Figure 5 As shown, both the prepolymerized solution and the vesicle-assisted composite hydrogel exhibit scattering characteristic peaks related to vesicle aggregates, indicating that the vesicle structure formed by anionic and cationic surfactants can exist stably before and after free radical polymerization. Furthermore, a "three-shell spherical model" was used to fit the SAXS curves, where the three shells correspond to the outer hydrophilic layer, hydrophobic layer, and inner hydrophilic layer in the vesicle bilayer, respectively. The fitting results show that the thickness of the vesicle bilayer in the prepolymerized solution is approximately 5.8 nm, and the thickness after polymerization to form the hydrogel is approximately 5.5 nm. The difference between the two is small, indicating that the vesicle bilayer structure was not significantly damaged during polymerization. Simultaneously, a kinetic simulation of the process of hydrophobic monomers entering the vesicle bilayer was performed, and the simulated bilayer thickness was approximately 5 nm, which is very close to the model fitting data, further verifying the accuracy of the model fitting. Example
[0091] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that the total mass fraction of cationic and anionic surfactants was adjusted to 0.58% in Example 2. The specific steps are as follows: (1) Preparation of precursor solution containing vesicles: accurately weigh hexadecyltrimethylammonium bromide and sodium dodecyl sulfate in a molar ratio of 1:1, i.e., 0.0112 g of hexadecyltrimethylammonium bromide and 0.0088 g of sodium dodecyl sulfate, add 3.45 g of deionized water and mix. Stir at 32 °C for 10 min at 500 rpm and then sonicate for 10 min. Example
[0092] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that the total mass fraction of cationic and anionic surfactants was adjusted to 0.86% in Example 3. The specific steps are as follows: (1) Preparation of precursor solution containing vesicles: accurately weigh hexadecyltrimethylammonium bromide and sodium dodecyl sulfate in a molar ratio of 1:1, i.e., 0.0167 g of hexadecyltrimethylammonium bromide and 0.0133 g of sodium dodecyl sulfate, add 3.44 g of deionized water and mix. Stir at 32 °C for 10 min at 500 rpm and then sonicate for 10 min. Example
[0093] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that the total mass fraction of anionic and cationic surfactants was adjusted to 1.15% in Example 4. The specific steps are as follows: (1) Preparation of precursor solution containing vesicles: accurately weigh hexadecyltrimethylammonium bromide and sodium dodecyl sulfate in a molar ratio of approximately 1:1, i.e., 0.0223 g of hexadecyltrimethylammonium bromide and 0.0177 g of sodium dodecyl sulfate, add 3.43 g of deionized water and mix. Stir at 32 °C for 10 min at 500 rpm and then sonicate for 10 min. Example
[0094] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that the total mass fraction of anionic and cationic surfactants was adjusted to 1.44% in Example 5. The specific steps are as follows: (1) Preparation of precursor solution containing vesicles: accurately weigh hexadecyltrimethylammonium bromide and sodium dodecyl sulfate in a molar ratio of approximately 1:1, i.e., 0.0279 g of hexadecyltrimethylammonium bromide and 0.0221 g of sodium dodecyl sulfate, add 3.42 g of deionized water and mix. Stir at 32 °C for 10 min at 500 rpm and then sonicate for 10 min. Example
[0095] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that in Example 7, the monomer ratio was adjusted to acrylamide:dodecyl methacrylate at 9.5:0.5. The specific steps are as follows: (2) Preparation of prepolymer solution: 1.425 g of acrylamide, 0.075 g of dodecyl methacrylate, 0.005 g of N,N′-methylenebisacrylamide, and 0.025 g of 2,2-diethoxyacetophenone were added after the dispersion was dissolved. Example
[0096] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that the monomer ratio in Example 8 was adjusted to acrylamide:dodecyl methacrylate of 8.5:1.5. The specific steps are as follows: (2) Preparation of prepolymer solution: 1.275 g of acrylamide, 0.225 g of dodecyl methacrylate, 0.005 g of N,N′-methylenebisacrylamide, and 0.025 g of 2,2-diethoxyacetophenone were added after the dispersion was dissolved. Example
[0097] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 is that the monomer ratio in Example 9 was adjusted to acrylamide:dodecyl methacrylate of 8:2. The specific steps are as follows: (2) Preparation of prepolymer solution: 1.2 g of acrylamide, 0.3 g of dodecyl methacrylate, 0.005 g of N,N′-methylenebisacrylamide, and 0.025 g of 2,2-diethoxyacetophenone were added after the dispersion was dissolved.
[0098] Comparative Example 1 Hydrogels were prepared using a method similar to that of Example 1, except that no surfactants were added in Comparative Example 1 to obtain a blank hydrogel. The specific steps are as follows: (1) Preparation of precursor solution: 3.47 g of deionized water.
[0099] (2) Preparation of prepolymer solution: Acrylamide:dodecyl methacrylate = 9:1, 1.35 g of acrylamide, 0.15 g of dodecyl methacrylate, 0.005 g of N,N′-methylenebisacrylamide, and 0.025 g of 2,2-diethoxyacetophenone were added after dissolution.
[0100] (3) Preparation of hydrogel: 10 min of ultraviolet light irradiation to form.
[0101] Comparative Example 2 Hydrogels were prepared using a method similar to that of Example 1. However, unlike Example 1, Comparative Example 2 used only hexadecyltrimethylammonium bromide to prepare the micelle system, without adding sodium dodecyl sulfate, to obtain micelle-assisted hydrogels. The specific steps are as follows: (1) Preparation of micelle precursor solution: 0.06 g of hexadecyltrimethylammonium bromide and 3.41 g of deionized water were stirred at 32 °C for 10 min at 500 rpm and then sonicated for 10 min.
[0102] (2) Preparation of prepolymer solution: Acrylamide:dodecyl methacrylate is 9:1, acrylamide 1.35 g, dodecyl methacrylate 0.15 g, N,N′-methylenebisacrylamide 0.005 g, and 2,2-diethoxyacetophenone 0.025 g is added after the dispersion is dissolved.
[0103] (3) Preparation of hydrogel: 10 min of ultraviolet light irradiation to form.
[0104] Hydrogels were prepared using a method similar to that of Example 1. The difference from Example 1 was that the monomer ratio in Comparative Example 3 was adjusted to acrylamide:dodecyl methacrylate at 10:0 (dodecyl methacrylate was not added). The specific steps are as follows: (2) Preparation of prepolymerization solution: 1.5 g of acrylamide, 0.005 g of N,N′-methylenebisacrylamide, and 0.025 g of 2,2-diethoxyacetophenone were added after the dispersion was dissolved.
[0105] Based on Example 1, the amount of raw materials added was adjusted, and the specific adjustment parameters are shown in Table 1 and Table 2.
[0106] Table 1
[0107] Table 2
[0108] The test results are shown in Table 3.
[0109] Table 3
[0110] Figure 6 The figures show the single-strand tensile stress-strain curves of unassisted polymerization hydrogel (Comparative Example 1), micelle-assisted polymerization hydrogel (Comparative Example 2), and vesicle-assisted polymerization hydrogel (Example 1). To investigate the effects of micelle and vesicle-assisted polymerization on the mechanical properties of hydrogels, single-strand tensile tests were conducted on hydrogels under different polymerization conditions. As can be seen from the figures, compared to unassisted polymerization, the vesicle-assisted polymerization hydrogel exhibits the best mechanical properties, with both fracture stress and fracture strain being improved. This is because the addition of vesicles increases the physical cross-linking in the hydrogel, thereby increasing the fracture stress, while the hydrophobic interactions introduced by the vesicles better disperse stress concentration, thus increasing the fracture strain. Micellar-assisted polymerization has a similar effect, but the improvement is not as significant as that of vesicle-assisted polymerization.
[0111] In this embodiment of the invention, as the surfactant concentration increases, the tensile fracture strain, fracture stress, elastic modulus, and toughness of the hydrogel all increase significantly. Even a small gradient difference in surfactant concentration can cause significant changes in performance, indicating that the hydrogel performance has a significant concentration dependence. This is because higher concentrations of surfactant can provide more physical cross-linking sites, simultaneously improving the material's flexibility and mechanical strength; when the surfactant concentration reaches 1.73%, the overall performance (elastic modulus and toughness) reaches its peak. If the concentration is further increased, for example, to greater than 1.73%, the stability of the pregel solution decreases, phase separation easily occurs, and subsequently, the performance deteriorates.
[0112] Introducing LMA (acrylamide macromolecular atom) can create additional hydrophobic interactions and anchor monomers to the hydrophobic regions of vesicles through hydrophobic association, stabilizing the hydrophobic aggregates. Hydrophobic domains possess dynamic reversibility, dissipating stress and achieving rapid recovery during deformation, thereby optimizing mechanical properties. When the acrylamide (AM) to LMA ratio is 9:1, the hydrogel's fracture stress, fracture strain, toughness, and elastic modulus reach optimal values. Further increasing the LMA content exacerbates phase separation, increases structural heterogeneity, disrupts stress transfer, and causes a simultaneous decrease in fracture stress and fracture strain. Comparing the mechanical properties of three types of hydrogels (blank hydrogel, micelle hydrogel, and vesicle composite hydrogel): Compared to the blank hydrogel, both micelle hydrogel and vesicle composite hydrogel show improved mechanical properties. Compared to micelles, vesicle structures can further improve the material's fracture strain, fracture stress, elastic modulus, and volumetric toughness. This is because vesicles provide more crosslinking sites than micelles, and the unique bilayer structure of vesicles can restrict polymer chain movement during polymerization, reducing network defects and improving material toughness. In vesicle-based hydrogels, the Br⁻ and Na⁺ generated by the dissociation of surfactants endow the material with excellent electrical conductivity. The conductivity of the hydrogel is 0.04 S / m to 0.12 S / m, giving it good application potential in the field of sensing.
Claims
1. A method for the preparation of a hydrogel by surfactant vesicle assisted radical polymerization, characterized in that, include: A precursor solution containing self-assembled vesicles is formed by mixing cationic and anionic surfactants. The hydrophobic monomer, hydrophilic monomer, crosslinking agent and the precursor solution are mixed to form a prepolymerization solution; A photoinitiator is used to initiate the crosslinking and copolymerization of the prepolymer solution to form a hydrogel.
2. The production method according to claim 1, characterized by, The cationic surfactant includes quaternary ammonium salt cationic surfactants; and / or the anionic surfactant mixture includes sulfate ester salt anionic surfactants; Optionally, the quaternary ammonium salt cationic surfactant includes at least one of hexadecyltrimethylammonium bromide, tetradecyltrimethylammonium bromide, and hexadecyltrimethylammonium chloride. Optionally, the sulfate ester anionic surfactant includes at least one of sodium dodecyl sulfate, ammonium dodecyl sulfate, and monoethanolamine dodecyl sulfate.
3. The preparation method according to claim 1, characterized in that, The molar ratio of the cationic surfactant to the anionic surfactant is 1:0.5-1:1.1; and / or The total mass fraction of the cationic surfactant and the anionic surfactant is 0.58% to 2.02% based on the total mass of the precursor solution.
4. The method of claim 1, wherein, The bilayer thickness of the vesicles in the precursor solution is 4 nm to 10 nm; and / or the average diameter of the vesicles in the precursor solution is 50 nm to 800 nm. and / or The thickness of the bilayer of vesicles in the hydrogel is 4 nm to 10 nm; and / or the average diameter of the vesicles in the hydrogel is 50 nm to 800 nm.
5. The preparation method according to claim 1, characterized in that, The hydrophobic monomer includes alkyl methacrylate hydrophobic monomers, wherein the carbon backbone of the alkyl methacrylate hydrophobic monomer has 12 to 18 carbon atoms. Optionally, the alkyl methacrylate hydrophobic monomer includes one of dodecyl methacrylate and octadecyl methacrylate; and / or The hydrophilic monomer includes acrylamide-based hydrophilic monomers, wherein the number of carbon atoms in the acrylamide-based hydrophilic monomers is 3 to 10. Optionally, the acrylamide-based hydrophilic monomers include one of acrylamide, dimethylacrylamide, diethylacrylamide, and N-isopropylacrylamide.
6. The method of claim 1, wherein, The mass ratio of the hydrophilic monomer to the hydrophobic monomer is from 8:2 to 9.5:0.5; and / or The sum of the mass fractions of the hydrophilic monomer and the hydrophobic monomer is 15% to 30% of the total mass of the prepolymer solution.
7. The method of claim 1, wherein the hydrogel is prepared by a process comprising: The step of mixing cationic and anionic surfactants to form a precursor solution containing self-assembled vesicles includes: Cationic and anionic surfactants were added to water and stirred for 10-20 minutes at 20 °C to 40 °C, and then sonicated for 10-20 minutes at 20 °C to 40 °C to prepare a precursor solution containing self-assembled vesicles.
8. The method for preparing hydrogels according to claim 1, characterized in that, The step of mixing the hydrophobic monomer, hydrophilic monomer, crosslinking agent and the precursor solution to form a prepolymerization solution includes: Hydrophobic and hydrophilic monomers were added to the precursor solution at 20 °C to 40 °C and stirred for 10 to 20 minutes to dissolve. Then, a crosslinking agent was added to prepare a prepolymer solution.
9. A hydrogel, characterized in that, The hydrogel is obtained by the preparation method of any one of claims 1 to 8.
10. The hydrogel according to claim 9, characterized in that, The fracture stress of the hydrogel is 30 kPa to 100 kPa; and / or The fracture strain of the hydrogel is 130%~400%; and / or The elastic modulus of the hydrogel is 70 kPa to 140 kPa; and / or The hydrogel has a toughness of 10 kJ / m 3 220 kJ / m 3 .