A silicone-modified waterborne polyurethane

By employing a synergistic preparation process involving polyol soft segments, modified alicyclic isocyanates, and phase-separated organosilicon monomers, the compatibility and water resistance issues of organosilicon-modified waterborne polyurethane were resolved, resulting in a highly stable organosilicon-modified waterborne polyurethane that improves the flexibility and water resistance of the film products.

CN123107031APending Publication Date: 2026-11-17FUJIAN DONGTAI HIGH POLYMER MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611348955.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-02
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicone-modified waterborne polyurethanes suffer from poor compatibility, easy delamination, and difficulty in achieving synergistic effects between water resistance and mechanical properties, resulting in limited hydrophobic and weather-resistant modification effects.

Method used

A stepwise preparation process using polyol soft segments, modified alicyclic isocyanates, phase-separated organosilicon monomers, and hydrophilic monomers is employed. By in-situ coating of hydrophilic monomers and controlling the polymerization reaction, a uniform cross-linked structure is formed, thereby improving the compatibility and mechanical properties of the components.

Benefits of technology

It achieves uniform emulsion particles, stable system, extended room temperature storage period, significantly improved flexibility, tensile strength and substrate adhesion of film products, and has excellent water resistance and hydrophobic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application discloses an organosilicon-modified waterborne polyurethane, relating to the field of waterborne polyurethane technology. It comprises, by weight, 80-100 parts of polyol soft segments, 35-45 parts of modified alicyclic isocyanate, 6-10 parts of phase-separated organosilicon monomer, 4-6 parts of hydrophilic monomer, 1.5-2.5 parts of chain extender, 0.2-0.4 parts of organobismuth catalyst, 3.5-5.5 parts of neutralizing agent, and 180-220 parts of deionized water. The phase-separated organosilicon monomer is composed of a low molecular weight flexible siloxane with a molecular weight of 500-800 and a high molecular weight weather-resistant siloxane with a molecular weight of 3000-5000. The hydrophilic monomer is dimethylolpropionic acid, used to obtain a coated hydrophilic monomer through an in-situ coating reaction with a portion of the polyol soft segments. This application has the effect of improving component compatibility and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of waterborne polyurethane technology, and particularly to an organosilicon-modified waterborne polyurethane. Background Technology

[0002] Waterborne polyurethane (WPU) uses deionized water as the dispersion medium, resulting in minimal organic solvent evaporation, low VOCs, and flame retardancy. It is widely used in coatings, industrial adhesives, leather finishing, waterproofing of textiles, plastic coatings, and wood protection. Conventional waterborne polyurethanes incorporate hydrophilic groups such as DMPA into their molecular chains to achieve water dispersion, leading to inherent limitations in water and weather resistance. Organosilicon (polysiloxane), with its high Si-O bond energy, low surface energy, resistance to high and low temperatures, hydrophobic slip properties, and UV resistance, is the most mainstream solution for modifying waterborne polyurethanes. Currently, organosilicon-modified waterborne polyurethanes generally employ physical blending and chemical copolymerization modifications, with chemical modification showing better stability than physical blending, making it the mainstream route for large-scale industrial production.

[0003] In existing technologies, the raw materials for preparing silicone-modified waterborne polyurethane mainly consist of polyol soft segment monomers, isocyanate hard segment monomers, hydrophilic monomers, silicone modifiers, and various functional additives. Among them, polyols are mostly polyether diols and polyester diols, isocyanates are commonly IPDI, HDI and other yellowing-resistant monomers, hydrophilic monomers are generally dimethylolpropionic acid and dimethylolbutyric acid, silicone modifiers are generally hydroxyl-terminated polydimethylsiloxanes and conventional silane coupling agents, and supporting additives include chain extenders, organotin catalysts, neutralizers and deionized water.

[0004] However, the compatibility between organosilicon segments and polyurethane molecular chains is poor, and the interfacial bonding between the two phases is weak. In the existing technology, the amount of organosilicon added is extremely low. If the amount added is too high, it will easily cause problems such as prepolymer aggregation, emulsion stratification and precipitation, and poor storage stability. As a result, the hydrophobic and weather-resistant modification effects of the product are limited, and it is difficult to achieve the effects of high water resistance and high slip. Improvement is needed. Summary of the Invention

[0005] In view of this, the purpose of this application is to provide an organosilicon-modified waterborne polyurethane to improve component compatibility and mechanical properties. The specific solution is as follows: An organosilicon-modified waterborne polyurethane comprises, by weight, 80-100 parts of polyol soft segments, 35-45 parts of modified alicyclic isocyanate, 6-10 parts of phase-separated organosilicon monomer, 4-6 parts of hydrophilic monomer, 1.5-2.5 parts of chain extender, 0.2-0.4 parts of organobismuth catalyst, 3.5-5.5 parts of neutralizing agent, and 180-220 parts of deionized water; wherein: The phase-separated organosilicon monomer is composed of a low molecular weight flexible siloxane with a molecular weight of 500-800 and a high molecular weight weather-resistant siloxane with a molecular weight of 3000-5000. The hydrophilic monomer is dimethylolpropionic acid, and it is used to obtain a coated hydrophilic monomer by in-situ coating reaction with a portion of polyol soft segments.

[0006] Preferably, the polyol soft segment comprises a polycarbonate diol and a polyether diol in a mass ratio of (2.5-3.5):1.

[0007] Preferably, the preparation method of the coated hydrophilic monomer includes pre-dehydrating 40-50 parts by weight of polyol soft segments under closed conditions of 90-100℃ and vacuum degree of -0.08 to -0.09MPa for 30-40 min, then cooling to 70-80℃ under inert gas atmosphere protection, and adding 4-6 parts of dry powdered hydrophilic monomer, controlling the stirring speed to 400-600 r / min and stirring continuously for 40-60 min to obtain a coated hydrophilic monomer with hydrophilic groups encapsulated in situ.

[0008] Preferably, the preparation method of the phase-separated organosilicon monomer includes taking low molecular weight flexible siloxane and high molecular weight weather-resistant siloxane in a mass ratio of (1-2):(3-4), heating to 60-80℃ under an inert gas atmosphere, controlling the stirring speed to 300-500r / min and stirring at a constant temperature for 30-50min, and then keeping it at a constant temperature for 1-1.5h to obtain the finished phase-separated organosilicon monomer.

[0009] Preferably, the low molecular weight flexible siloxane and the high molecular weight weather-resistant siloxane are obtained from dimethylcyclosiloxane (DMC) via a controlled ring-opening equilibrium polymerization reaction; and the controlled ring-opening equilibrium polymerization reaction includes step ① taking dimethylcyclosiloxane DMC with a water content ≤0.03%, a capping agent, and a catalyst for later use; step ② adding 2-5% of the catalyst (by mass of dimethylcyclosiloxane DMC) to the dimethylcyclosiloxane DMC under an inert gas atmosphere, and stirring at a temperature of 70-85℃ and a stirring speed of [missing value]. The process involves adding a capping agent at a rate of 200-400 r / min, with 1-1.8% of the mass of dimethylcyclosiloxane (DMC) as the end-capping agent, to prepare a low molecular weight flexible siloxane with a molecular weight of 500-800. Conversely, adding a capping agent at a rate of 0.15-0.35% of the mass of DMC as the end-capping agent, to prepare a high molecular weight weather-resistant siloxane with a molecular weight of 3000-5000. The dropping time is controlled at 30-60 min, and the reaction is carried out at a constant temperature for 3-4.5 h after the dropping is completed.

[0010] Preferably, the process further includes step ③ cooling to 40-50℃, filtering to remove the solid catalyst and obtaining a filtrate, then heating the filtrate to 120-150℃ and subjecting it to vacuum de-boiling treatment at a controlled vacuum degree of -0.09 to -0.098 MPa for 2-3 hours to obtain low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes with a terminal hydroxyl end-capping rate ≥98%.

[0011] Preferably, the capping agent is pure water.

[0012] Preferably, the catalyst is a macroporous, strongly acidic styrene-based cation exchange resin.

[0013] Preferably, the chain extender is 1,4-butanediol.

[0014] Preferably, the neutralizing agent is triethylamine.

[0015] Preferably, the method for preparing the modified alicyclic isocyanate includes preparing isophorone diisocyanate and isopropanol at a molar ratio of 1:(0.3-0.5), heating the isophorone diisocyanate to 50-60℃ and then adding isopropanol dropwise, controlling the dropwise addition time of isopropanol to 40-60 min, and reacting at a constant temperature for 1-2 h after the dropwise addition is completed to obtain the modified alicyclic isocyanate.

[0016] Preferably, the preparation includes the following steps: Step 1: Take 30-60 parts by weight of polyol soft segments and coated hydrophilic monomers and put them into a sealed anhydrous reactor. Control the temperature of the reactor to 105-115℃ and the vacuum degree to -0.08 to -0.095MPa. Dehydrate under vacuum for 1-2 hours, and then cool down to 75-85℃ under sealed pressure to obtain dehydrated raw materials for later use. Step 2: Add phase-separated organosilicon monomer and organobismuth catalyst to the reactor. Control the stirring speed at 300-500 r / min and react at a constant temperature for 15-25 min. Slowly and uniformly add modified alicyclic isocyanate, controlling the addition time to 0.8-1.2 h. After the addition is completed, keep the temperature at 75-85℃ for 3.5-4.5 h to obtain polyurethane prepolymer.

[0017] Step 3: Allow the polyurethane prepolymer to cool naturally to 40-50℃, add the neutralizing agent at a uniform rate and stir for 25-35 minutes to obtain the neutralized prepolymer; Step 4: Add the neutralized prepolymer into a high-speed shear dispersion vessel, control the shear speed at 1200-1600 r / min and room temperature, add deionized water and continue shearing emulsification for 35-45 min to obtain the prepolymer aqueous emulsion. Step 5: Control the temperature of the prepolymer aqueous emulsion to 25-35℃, add chain extender dropwise and keep warm while stirring for 1-2 hours to obtain emulsion-like organosilicon-modified waterborne polyurethane.

[0018] As can be seen from the above solutions, this application provides a silicone-modified waterborne polyurethane, which has the following beneficial effects: 1. By employing a synergistic and stepwise preparation process using polyol soft segments, modified alicyclic isocyanates, phase-separated organosilicon monomers, and hydrophilic monomers, this method effectively solves the technical problems of poor compatibility, easy delamination, and difficulty in synergistic water resistance and mechanical properties in existing organosilicon-modified waterborne polyurethanes based on multi-component structure regulation and process optimization. Furthermore, it produces organosilicon-modified waterborne polyurethanes with uniform emulsion particles, stable system, and significantly extended room temperature storage period. In application, it significantly improves the flexibility, tensile strength, and substrate adhesion of the film products. 2. By using polyol soft segments to in-situ coat and modify hydrophilic monomers, the hydrophilic groups in the hydrophilic monomers are distributed in a fixed and discrete manner under the molecular chain entanglement of the polyol soft segments. This avoids the formation of water-permeable channels by the hydrophilic groups in the continuous arrangement of the molecular backbone. Thus, while retaining the ionization and dispersion ability of the hydrophilic groups and ensuring the stable dispersion of the emulsion, the water penetration path is effectively blocked, achieving the effect of being hydrophilic but not water-conducting. This significantly reduces the water absorption rate of the film product during application and significantly improves the water wash resistance and moisture aging resistance of the film product during application. 3. By employing low-molecular-weight flexible siloxanes and high-molecular-weight weather-resistant siloxanes, the hydrophobic and weather-resistant properties of organosilicon are synergistically achieved with interfacial compatibility. Furthermore, by modifying alicyclic isocyanates to regulate the polymerization rate and crosslinking uniformity, the problems of localized excessive crosslinking and excessive internal stress are avoided. This not only improves the mechanical strength and structural stability of the crosslinked structure of the organosilicon-modified waterborne polyurethane, but also enhances the weather resistance, hydrophobicity, and mechanical properties of the film products used in the application. Detailed Implementation

[0019] The technical solutions described below in conjunction with the embodiments of this application will be clearly and completely described. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.

[0020] It should be noted that the molecular weights of the polycarbonate diol and polyether diol in the embodiments of this application are 1000-2000. The chain extender, organobismuth catalyst, and neutralizing agent are all commercially available and will not be described in detail here. In the embodiments of this application, the end-capping agent is pure water, the catalyst is a macroporous strong acid styrene-based cation exchange resin, the chain extender is 1,4-butanediol, and the neutralizing agent is triethylamine. Furthermore, nitrogen is used to create an inert gas atmosphere in all embodiments of this application. The polyol soft segment comprises a polycarbonate diol and a polyether diol in a mass ratio of (2.5-3.5):1.

[0021] The following is a detailed description of an organosilicon-modified waterborne polyurethane according to this application.

[0022] An organosilicon-modified waterborne polyurethane comprises 80-100 parts by weight of polyol soft segments, 35-45 parts by weight of modified alicyclic isocyanate, 6-10 parts by weight of phase-separated organosilicon monomer, 4-6 parts by weight of hydrophilic monomer, 1.5-2.5 parts by weight of chain extender, 0.2-0.4 parts by weight of organobismuth catalyst, 3.5-5.5 parts by weight of neutralizer, and 180-220 parts by weight of deionized water.

[0023] The polyol soft segment comprises polycarbonate diol and polyether diol in a mass ratio of (2.5-3.5):1. The preparation method of the modified alicyclic isocyanate includes preparing isophorone diisocyanate and isopropanol in a molar ratio of 1:(0.3-0.5), heating the isophorone diisocyanate to 50-60℃, and then adding isopropanol dropwise, controlling the dropwise addition time of isopropanol to 40-60 min. After the addition is complete, the reaction is carried out at a constant temperature for 1-2 h to obtain the modified alicyclic isocyanate.

[0024] Phase-separated organosilicon monomers are composed of low-molecular-weight flexible siloxanes with a molecular weight of 500-800 and high-molecular-weight weather-resistant siloxanes with a molecular weight of 3000-5000. The preparation method of phase-separated organosilicon monomers includes taking low-molecular-weight flexible siloxanes and high-molecular-weight weather-resistant siloxanes at a mass ratio of (1-2):(3-4), heating to 60-80℃ under an inert gas atmosphere, stirring at a constant temperature of 300-500 r / min for 30-50 min, and then allowing to stand at this temperature for 1-1.5 h to obtain the finished phase-separated organosilicon monomer.

[0025] In this embodiment, low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes are obtained from dimethylcyclosiloxane (DMC) via a controlled ring-opening equilibrium polymerization reaction. The controlled ring-opening equilibrium polymerization reaction includes: Step ① preparing dimethylcyclosiloxane DMC with a water content ≤0.03%, a capping agent, and a catalyst; Step ② adding 2-5% (by mass) of catalyst to the dimethylcyclosiloxane DMC under an inert gas atmosphere, treating it at 70-85°C and a stirring speed of 200-400 r / min, and then adding 1-1.8% (by mass) of capping agent to prepare a low molecular weight flexible siloxane with a molecular weight of 500-800. High molecular weight weather-resistant siloxanes with a molecular weight of 3000-5000 are prepared by adding 0.15-0.35% of the mass of DMC as a capping agent. The dropping time is controlled at 30-60 min, and the catalytic reaction is carried out at a constant temperature for 3-4.5 h after the dropping is completed. In step ③, the temperature is lowered to 40-50℃, the solid catalyst is removed by filtration and the filtrate is obtained. The filtrate is then heated to 120-150℃ and subjected to vacuum de-boiling treatment at a vacuum degree controlled at -0.09 to -0.098 MPa for 2-3 h to obtain low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes with a terminal hydroxyl capping rate ≥98%.

[0026] It should be mentioned that the hydrophilic monomer is dimethylolpropionic acid, and it is used to obtain coated hydrophilic monomers by in-situ coating reaction with some polyol soft segments. The preparation method of coated hydrophilic monomers includes pre-dehydrating 40-50 parts by weight of polyol soft segments under closed conditions of 90-100℃ and vacuum degree of -0.08 to -0.09MPa for 30-40 min, then cooling to 70-80℃ under inert gas atmosphere protection, and adding 4-6 parts of dry powdered hydrophilic monomer, controlling the stirring speed at 400-600 r / min and stirring continuously for 40-60 min to obtain coated hydrophilic monomers with hydrophilic groups encapsulated in situ.

[0027] The preparation method of this organosilicon-modified waterborne polyurethane includes: Step 1: Take 30-60 parts by weight of polyol soft segments and coated hydrophilic monomers and put them into a sealed anhydrous reactor. Control the temperature of the reactor to 105-115℃ and the vacuum degree to -0.08 to -0.095MPa. Dehydrate under vacuum for 1-2 hours, and then cool down to 75-85℃ under sealed pressure to obtain dehydrated raw materials for later use. Step 2: Add phase-separated organosilicon monomer and organobismuth catalyst to the reactor. Control the stirring speed at 300-500 r / min and react at a constant temperature for 15-25 min. Slowly and uniformly add modified alicyclic isocyanate, controlling the addition time to 0.8-1.2 h. After the addition is completed, keep the temperature at 75-85℃ for 3.5-4.5 h to obtain polyurethane prepolymer.

[0028] Step 3: Allow the polyurethane prepolymer to cool naturally to 40-50℃, add the neutralizing agent at a uniform rate and stir for 25-35 minutes to obtain the neutralized prepolymer; Step 4: Add the neutralized prepolymer into a high-speed shear dispersion vessel, control the shear speed at 1200-1600 r / min and room temperature, add deionized water and continue shearing emulsification for 35-45 min to obtain the prepolymer aqueous emulsion. Step 5: Control the temperature of the prepolymer aqueous emulsion to 25-35℃, add chain extender dropwise and keep warm while stirring for 1-2 hours to obtain emulsion-like organosilicon-modified waterborne polyurethane.

[0029] Example 1 An organosilicon-modified waterborne polyurethane comprises 80 parts by weight of polyol soft segments, 35 parts by weight of modified alicyclic isocyanate, 6 parts by weight of phase-separated organosilicon monomer, 4 parts by weight of hydrophilic monomer, 1.5 parts by weight of chain extender, 0.2 parts by weight of organobismuth catalyst, 3.5 parts by weight of neutralizer, and 180 parts by weight of deionized water.

[0030] The polyol soft segment comprises polycarbonate diol and polyether diol in a mass ratio of 2.5:1. The preparation method of the modified alicyclic isocyanate includes preparing isophorone diisocyanate and isopropanol in a molar ratio of 1:0.3, heating the isophorone diisocyanate to 50°C, and then adding isopropanol dropwise, controlling the dropwise addition time of isopropanol to 40 min. After the addition is complete, the reaction is carried out at a constant temperature for 1 h to obtain the modified alicyclic isocyanate.

[0031] The phase-separated organosilicon monomer is composed of a low molecular weight flexible siloxane with a molecular weight of 500 and a high molecular weight weather-resistant siloxane with a molecular weight of 3000. The preparation method of the phase-separated organosilicon monomer includes taking the low molecular weight flexible siloxane and the high molecular weight weather-resistant siloxane at a mass ratio of 1:3, heating to 60°C under an inert gas atmosphere, stirring at a constant temperature of 300 r / min for 30 min, and then allowing it to stand at that temperature for 1 h to obtain the finished phase-separated organosilicon monomer.

[0032] In this embodiment, low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes are obtained from dimethylcyclosiloxane (DMC) via a controlled ring-opening equilibrium polymerization reaction. The controlled ring-opening equilibrium polymerization reaction includes: Step ① preparing dimethylcyclosiloxane DMC with a water content ≤0.03%, a capping agent, and a catalyst; Step ② adding 2% (by mass) of catalyst to the dimethylcyclosiloxane DMC under an inert gas atmosphere, treating it at 70°C and a stirring speed of 200 r / min, and then adding 1% (by mass) of capping agent to the dimethylcyclosiloxane DMC to prepare a low molecular weight flexible siloxane with a molecular weight of 500. A high molecular weight weather-resistant siloxane with a molecular weight of 3000 was prepared by adding a capping agent accounting for 0.15% of the mass of dimethylcyclosiloxane (DMC). The addition time was controlled at 30 min, and the catalytic reaction was carried out at a constant temperature for 3 h after the addition was completed. In step ③, the temperature was lowered to 40 °C, the solid catalyst was removed by filtration and the filtrate was obtained. The filtrate was then heated to 120 °C and subjected to vacuum de-boiling treatment at a controlled vacuum degree of -0.09 MPa for 2 h to obtain a low molecular weight flexible siloxane with a terminal hydroxyl capping rate of ≥98% and a high molecular weight weather-resistant siloxane.

[0033] It should be mentioned that the hydrophilic monomer is dimethylolpropionic acid, and it is used to obtain coated hydrophilic monomers by in-situ coating reaction with some polyol soft segments. The preparation method of the coated hydrophilic monomer includes pre-dehydrating 40 parts by weight of polyol soft segments under closed conditions of 90°C and -0.08MPa for 30 min, then cooling to 70°C under inert gas atmosphere protection, and adding 4 parts of dry powdered hydrophilic monomer, and stirring continuously at 400 r / min for 40 min to obtain coated hydrophilic monomers with hydrophilic groups encapsulated in situ.

[0034] The preparation method of the organosilicon-modified waterborne polyurethane includes: Step 1, taking 30 parts by weight of polyol soft segments and coated hydrophilic monomers and putting them into a closed anhydrous reactor, controlling the temperature of the reactor to rise to 105℃, the vacuum degree to -0.08MPa, vacuum dehydration for 1h, and then sealing and maintaining pressure to cool down to 75℃ to obtain dehydrated raw materials for later use; Step 2, adding phase-separated organosilicon monomers and organobismuth catalysts to the reactor, controlling the stirring speed to 300r / min and constant temperature reaction for 15min, slowly and uniformly adding modified alicyclic isocyanate, controlling the adding time to 0.8h, and after the adding is completed, maintaining the temperature at 75℃ for 3.5h to obtain polyurethane prepolymer. Step 3: Cool the polyurethane prepolymer naturally to 40℃, add the neutralizing agent at a uniform rate and stir for 25 min to obtain the neutralized prepolymer; Step 4: Put the neutralized prepolymer into a high-speed shear dispersion vessel, control the shear speed at 1200 r / min and room temperature, add deionized water and continue shearing emulsification for 35 min to obtain the prepolymer aqueous emulsion; Step 5: Control the temperature of the prepolymer aqueous emulsion at 25℃, add the chain extender dropwise and keep it warm and stir for 1 h to obtain the emulsion-like organosilicon-modified waterborne polyurethane.

[0035] Example 2 An organosilicon-modified waterborne polyurethane comprises 90 parts by weight of polyol soft segments, 40 parts by weight of modified alicyclic isocyanate, 8 parts by weight of phase-separated organosilicon monomer, 5 parts by weight of hydrophilic monomer, 2 parts by weight of chain extender, 0.3 parts by weight of organobismuth catalyst, 4.5 parts by weight of neutralizer, and 200 parts by weight of deionized water.

[0036] The polyol soft segment comprises polycarbonate diol and polyether diol in a mass ratio of 3:1. The modified alicyclic isocyanate is prepared by mixing isophorone diisocyanate and isopropanol in a molar ratio of 1:0.4, heating the isophorone diisocyanate to 55°C, and then adding isopropanol dropwise over a time of 50 min. After the addition is complete, the mixture is kept at a constant temperature for 1.5 h to obtain the modified alicyclic isocyanate.

[0037] The phase-separated organosilicon monomer is composed of a low molecular weight flexible siloxane with a molecular weight of 650 and a high molecular weight weather-resistant siloxane with a molecular weight of 4000. The preparation method of the phase-separated organosilicon monomer includes taking the low molecular weight flexible siloxane and the high molecular weight weather-resistant siloxane at a mass ratio of 1.5:3.5, heating to 70°C under an inert gas atmosphere, stirring at a constant temperature of 400 r / min for 40 min, and then allowing it to stand at that temperature for 1.2 h to obtain the finished phase-separated organosilicon monomer.

[0038] In this embodiment, low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes are obtained from dimethylcyclosiloxane (DMC) via a controlled ring-opening equilibrium polymerization reaction. The controlled ring-opening equilibrium polymerization reaction includes step ① preparing dimethylcyclosiloxane DMC with a water content ≤0.03%, a capping agent, and a catalyst; step ② adding 3.5% (by mass) of catalyst to the dimethylcyclosiloxane DMC under an inert gas atmosphere, treating it at 78°C and a stirring speed of 300 r / min, and then adding 1.4% (by mass) of capping agent to the dimethylcyclosiloxane DMC to prepare a low molecular weight flexible siloxane with a molecular weight of 650. A high molecular weight weather-resistant siloxane with a molecular weight of 4000 was prepared by adding a capping agent accounting for 0.25% of the mass of dimethylcyclosiloxane (DMC). The addition time was controlled at 45 min, and the reaction was carried out at a constant temperature for 4 h after the addition was completed. In step ③, the temperature was lowered to 45 °C, the solid catalyst was removed by filtration and the filtrate was obtained. The filtrate was then heated to 135 °C and subjected to vacuum de-boiling treatment at a vacuum degree of -0.094 MPa for 2.5 h to obtain a low molecular weight flexible siloxane with a terminal hydroxyl capping rate of ≥98% and a high molecular weight weather-resistant siloxane.

[0039] It should be mentioned that the hydrophilic monomer is dimethylolpropionic acid, and it is used to obtain coated hydrophilic monomers by in-situ coating reaction with some polyol soft segments. The preparation method of coated hydrophilic monomers includes pre-dehydrating 45 parts by weight of polyol soft segments under closed conditions of 95°C and -0.085 MPa for 35 min, then cooling to 75°C under inert gas atmosphere protection, and adding 5 parts of dry powdered hydrophilic monomer, and stirring continuously at 500 r / min for 50 min to obtain coated hydrophilic monomers with hydrophilic groups encapsulated in situ.

[0040] The preparation method of the organosilicon-modified waterborne polyurethane includes: Step 1, taking 45 parts by weight of polyol soft segments and coated hydrophilic monomers and putting them into a closed anhydrous reactor, controlling the temperature of the reactor to rise to 110℃, the vacuum degree to -0.09MPa, vacuum dehydration for 1.5h, and then sealing and maintaining pressure to cool down to 80℃ to obtain dehydrated raw materials for later use; Step 2, adding phase-separated organosilicon monomers and organobismuth catalysts to the reactor, controlling the stirring speed to 400r / min and constant temperature reaction for 20min, slowly and uniformly adding modified alicyclic isocyanate, controlling the adding time to 1h, and after the adding is completed, maintaining the temperature at 80℃ for 4h to obtain polyurethane prepolymer. Step 3: Cool the polyurethane prepolymer naturally to 45℃, add the neutralizing agent at a uniform rate and stir for 30 min to obtain the neutralized prepolymer; Step 4: Put the neutralized prepolymer into a high-speed shear dispersion vessel, control the shear speed at 1400 r / min and room temperature, add deionized water and continue shearing emulsification for 40 min to obtain the prepolymer aqueous emulsion; Step 5: Control the temperature of the prepolymer aqueous emulsion at 30℃, add the chain extender dropwise and keep it warm and stir for 1.5 h to obtain the emulsion-like organosilicon-modified waterborne polyurethane.

[0041] Example 3 An organosilicon-modified waterborne polyurethane comprises 100 parts by weight of polyol soft segments, 45 parts by weight of modified alicyclic isocyanate, 10 parts by weight of phase-separated organosilicon monomer, 6 parts by weight of hydrophilic monomer, 2.5 parts by weight of chain extender, 0.4 parts by weight of organobismuth catalyst, 5.5 parts by weight of neutralizer, and 220 parts by weight of deionized water.

[0042] The polyol soft segment comprises polycarbonate diol and polyether diol in a mass ratio of 3.5:1. The preparation method of the modified alicyclic isocyanate includes preparing isophorone diisocyanate and isopropanol in a molar ratio of 1:0.5, heating the isophorone diisocyanate to 60°C, and then adding isopropanol dropwise, controlling the dropwise addition time of isopropanol to 60 min. After the addition is complete, the reaction is carried out at a constant temperature for 2 h to obtain the modified alicyclic isocyanate.

[0043] The phase-separated organosilicon monomer is composed of a low molecular weight flexible siloxane with a molecular weight of 800 and a high molecular weight weather-resistant siloxane with a molecular weight of 5000. The preparation method of the phase-separated organosilicon monomer includes taking the low molecular weight flexible siloxane and the high molecular weight weather-resistant siloxane at a mass ratio of 2:4, heating to 80°C under an inert gas atmosphere, stirring at a constant temperature of 500 r / min for 50 min, and then allowing it to stand at that temperature for 1.5 h to obtain the finished phase-separated organosilicon monomer.

[0044] In this embodiment, low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes are obtained from dimethylcyclosiloxane (DMC) via a controlled ring-opening equilibrium polymerization reaction. The controlled ring-opening equilibrium polymerization reaction includes: Step ① preparing dimethylcyclosiloxane (DMC) with a water content ≤0.03%, a capping agent, and a catalyst; Step ② adding 5% (by mass) of catalyst to the dimethylcyclosiloxane (DMC) under an inert gas atmosphere, treating the DMC at 85°C and a stirring speed of 400 r / min, and then adding 1.8% (by mass) of capping agent to the DMC to prepare a low molecular weight flexible siloxane with a molecular weight of 800, which is then added dropwise. A high molecular weight weather-resistant siloxane with a molecular weight of 5000 was prepared by adding a capping agent accounting for 0.35% of the mass of dimethylcyclosiloxane (DMC). The dropping time was controlled at 60 min, and the catalytic reaction was carried out at a constant temperature for 4.5 h after the dropping was completed. In step ③, the temperature was lowered to 50 °C, the solid catalyst was removed by filtration and the filtrate was obtained. The filtrate was then heated to 150 °C and subjected to vacuum de-boiling treatment at a controlled vacuum degree of -0.098 MPa for 3 h to obtain a low molecular weight flexible siloxane with a terminal hydroxyl capping rate of ≥98% and a high molecular weight weather-resistant siloxane.

[0045] It should be mentioned that the hydrophilic monomer is dimethylolpropionic acid, and it is used to obtain coated hydrophilic monomers by in-situ coating reaction with some polyol soft segments. The preparation method of the coated hydrophilic monomer includes pre-dehydrating 50 parts by weight of polyol soft segments under closed conditions of 100°C and -0.09 MPa for 40 min, then cooling to 80°C under inert gas atmosphere, and adding 6 parts of dry powdered hydrophilic monomer, while stirring continuously at 600 r / min for 60 min to obtain coated hydrophilic monomers with hydrophilic groups encapsulated in situ.

[0046] The preparation method of the organosilicon-modified waterborne polyurethane includes: Step 1, taking 60 parts by weight of polyol soft segments and coated hydrophilic monomers and putting them into a closed anhydrous reactor, controlling the temperature of the reactor to rise to 115℃, the vacuum degree to -0.095MPa, vacuum dehydration for 2h, and then sealing and maintaining pressure to cool down to 85℃ to obtain dehydrated raw materials for later use; Step 2, adding phase-separated organosilicon monomers and organobismuth catalysts to the reactor, controlling the stirring speed to 500r / min and constant temperature reaction for 25min, slowly and uniformly adding modified alicyclic isocyanate, controlling the adding time to 1.2h, and after the adding is completed, maintaining the temperature at 85℃ for 4.5h to obtain polyurethane prepolymer. Step 3: Cool the polyurethane prepolymer naturally to 50°C, add the neutralizing agent at a uniform rate and stir for 35 minutes to obtain the neutralized prepolymer; Step 4: Put the neutralized prepolymer into a high-speed shear dispersion vessel, control the shear speed at 1600 r / min and room temperature, add deionized water and continue shearing emulsification for 45 minutes to obtain the prepolymer aqueous emulsion; Step 5: Control the temperature of the prepolymer aqueous emulsion at 35°C, add the chain extender dropwise and keep it warm and stirred for 2 hours to obtain the emulsion-like organosilicon-modified waterborne polyurethane.

[0047] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the phase-separated organosilicon monomer in Comparative Example 1 is a low molecular weight flexible siloxane with a molecular weight of 500.

[0048] Comparative Example 2 The difference between Comparative Example 2 and Example 2 is that the hydrophilic monomer in Comparative Example 2 was added directly without in-situ coating reaction.

[0049] Comparative Example 3 The difference between Comparative Example 3 and Example 3 is that in Comparative Example 3, isophorone diisocyanate was used instead of modified alicyclic isocyanate.

[0050] Performance testing: The coating had a dry film thickness of 40 μm, was surface-dried at room temperature for 30 min, then dried at 60℃ for 2 h, and finally cured at room temperature for 7 days before testing. The substrate for the sample was a cold-rolled steel sheet.

[0051] 1. Appearance characterization: Refer to HG / T4761-2014 "Waterborne Polyurethane Coatings", store at room temperature and observe the emulsion state, whether it separates, precipitates, or flocculates; 2. Pencil hardness: Refer to GB / T6739-2006 "Determination of paint film hardness by pencil method", use Mitsubishi standard pencil, and test the hardness level of paint film by uniform scratching; 3. Adhesion: Refer to GB / T5210-2006 "Paints and Varnishes - Pull-off Test" to test the adhesion level between the paint film and the substrate; 4. Bending resistance: Refer to GB / T6742-2007 "Paints and Varnishes Bending Test (Cylindrical Shaft)", use a 2mm shaft diameter to test the flexibility of the paint film and observe whether it cracks or peels off; 5. Water resistance: Refer to GB / T1733-1993 "Test Method for Water Resistance of Paints and Varnishes", immerse in deionized water at room temperature for 72 hours, and observe the blistering, whitening and peeling of the paint film; 6. Dispersibility: The average particle size of the emulsion was measured using a laser particle size analyzer to characterize the uniformity of emulsion dispersion.

[0052] The performance test results are shown in Table 1 below.

[0053] Table 1 Performance Test Results

[0054] As shown in Table 1 above, the silicone-modified waterborne polyurethane in Example 1 of this application uses a composite of low-molecular-weight flexible siloxane and high-molecular-weight weather-resistant siloxane to form a phase-separated silicone monomer. This allows the low-molecular-weight flexible siloxane to migrate rapidly to the surface of the coating film, thereby improving the flexibility and smoothness of the film product during application. Furthermore, the high-molecular-weight weather-resistant siloxane is interwoven within the silicone-modified waterborne polyurethane, forming a dense cross-linked structure, and significantly improving the uniformity of emulsion dispersion, thus enhancing storage stability. In contrast, Comparative Example 1 suffers from insufficient structural density and a large free volume due to the low-molecular-weight flexible siloxane during application, resulting in a significant decrease in weather resistance and water resistance compared to Example 1. In Example 2 of this application, the silicone-modified waterborne polyurethane uses coated hydrophilic monomers to effectively prevent the aggregation of hydrophilic monomers. The resulting polyurethane prepolymer exhibits small emulsion particle size and high stability. This effectively binds the hydrophilic groups of the coated hydrophilic monomers within the crosslinking network in the applied film product, preventing the formation of continuous hydrophilic channels and significantly improving the film density and water resistance. In Comparative Example 2, the hydrophilic monomers are highly polar and exhibit severe aggregation, leading to emulsion particle aggregation and increased particle size. This results in increased hydrophilic channels in the film after formation, significantly reducing water resistance. In Example 3 of this application, the silicone-modified waterborne polyurethane uses isopropanol to modify alicyclic isocyanates, causing isopropanol to cap some -NCO groups, thereby reducing the reactivity of the isocyanate. This achieves a mild and controllable polymerization reaction, resulting in a regular molecular chain arrangement and uniform crosslinking density.

[0055] In summary, this application provides a silicone-modified waterborne polyurethane. This silicone-modified waterborne polyurethane employs a stepwise preparation process using polyol soft segments, modified alicyclic isocyanates, phase-separated silicone monomers, and hydrophilic monomers. Based on multi-component structural regulation and process optimization, it effectively solves the technical problems of poor compatibility, easy delamination, and difficulty in synergistic effects between water resistance and mechanical properties in existing silicone-modified waterborne polyurethanes. Furthermore, it produces silicone-modified waterborne polyurethane with uniform emulsion particles, stable system, and significantly extended room temperature storage period. In application, it significantly improves the flexibility, tensile strength, and substrate adhesion of the film product. Meanwhile, by in-situ encapsulating and modifying hydrophilic monomers with polyol soft segments, the hydrophilic groups in the hydrophilic monomers are spatially dispersed under the molecular chain entanglement of the polyol soft segments. This avoids the formation of water-permeable channels by the hydrophilic groups in the continuous arrangement of the molecular backbone. Thus, while retaining the ionization and dispersion ability of the hydrophilic groups and ensuring stable emulsion dispersion, it effectively blocks the water penetration path, achieving a hydrophilic yet non-conductive effect. This significantly reduces the water absorption rate of the film product during application and significantly improves its resistance to washing and moisture aging. Therefore, this silicone-modified waterborne polyurethane achieves synergistic effects of silicone hydrophobicity and weather resistance with interfacial compatibility through the synergistic use of low-molecular-weight flexible siloxanes and high-molecular-weight weather-resistant siloxanes. Furthermore, by modifying alicyclic isocyanates to regulate the polymerization rate and crosslinking uniformity, it avoids problems such as excessive local crosslinking and excessive internal stress. This improves the mechanical strength and structural stability of the crosslinked structure of the silicone-modified waterborne polyurethane while simultaneously enhancing the weather resistance, hydrophobicity, and mechanical properties of the film product during application.

[0056] The terms “first,” “second,” “third,” “fourth,” etc., used in this application (if applicable) are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments described herein can be implemented in orders other than those described herein. Furthermore, the terms “comprising” and “having,” and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, or apparatus that includes a series of steps or units is not necessarily limited to those explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, or apparatus.

[0057] It should be noted that the use of terms such as "first" and "second" in this application is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of those features. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. If the combination of technical solutions is contradictory or impossible to implement, such a combination of technical solutions should be considered non-existent and not within the scope of protection claimed in this application.

[0058] This document uses specific examples to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the methods and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A silicone-modified waterborne polyurethane, characterized in that: It includes 80-100 parts by weight of polyol soft segments, 35-45 parts of modified alicyclic isocyanate, 6-10 parts of phase-separated organosilicon monomer, 4-6 parts of hydrophilic monomer, 1.5-2.5 parts of chain extender, 0.2-0.4 parts of organobismuth catalyst, 3.5-5.5 parts of neutralizing agent, and 180-220 parts of deionized water; wherein: The phase-separated organosilicon monomer is composed of a low molecular weight flexible siloxane with a molecular weight of 500-800 and a high molecular weight weather-resistant siloxane with a molecular weight of 3000-5000. The hydrophilic monomer is dimethylolpropionic acid, and it is used to obtain a coated hydrophilic monomer by in-situ coating reaction with a portion of polyol soft segments.

2. The organosilicon-modified waterborne polyurethane according to claim 1, characterized in that: The polyol soft segment comprises polycarbonate diol and polyether diol in a mass ratio of (2.5-3.5):

1.

3. The organosilicon-modified waterborne polyurethane according to claim 1 or 2, characterized in that: The preparation method of the coated hydrophilic monomer includes pre-dehydrating 40-50 parts by weight of polyol soft segments under closed conditions of 90-100℃ and vacuum degree of -0.08 to -0.09MPa for 30-40 min, then cooling to 70-80℃ under inert gas atmosphere protection, and adding 4-6 parts of dry powdered hydrophilic monomer, controlling the stirring speed to 400-600 r / min and stirring continuously for 40-60 min to obtain a coated hydrophilic monomer with hydrophilic groups encapsulated in situ.

4. The organosilicon-modified waterborne polyurethane according to claim 1, characterized in that: The preparation method of the phase-separated organosilicon monomer includes taking low molecular weight flexible siloxane and high molecular weight weather-resistant siloxane in a mass ratio of (1-2):(3-4), heating to 60-80℃ under an inert gas atmosphere, stirring at a constant temperature of 300-500r / min for 30-50min, and then keeping it at the temperature for 1-1.5h to obtain the finished phase-separated organosilicon monomer.

5. The organosilicon-modified waterborne polyurethane according to claim 4, characterized in that: The low molecular weight flexible siloxane and high molecular weight weather-resistant siloxane are obtained from dimethylcyclosiloxane (DMC) via a controlled ring-opening equilibrium polymerization reaction; and the controlled ring-opening equilibrium polymerization reaction includes step ① taking dimethylcyclosiloxane DMC with a water content ≤0.03%, a capping agent, and a catalyst for later use; step ② adding 2-5% of the catalyst (by mass of dimethylcyclosiloxane DMC) to the dimethylcyclosiloxane DMC under an inert gas atmosphere, and stirring at a temperature of 70-85℃ and a stirring speed of 2. The process involves treating the sample at 00-400 r / min, adding 1-1.8% of a capping agent (based on the mass of dimethylcyclosiloxane DMC) to prepare a low molecular weight flexible siloxane with a molecular weight of 500-800, and adding 0.15-0.35% of a capping agent (based on the mass of dimethylcyclosiloxane DMC) to prepare a high molecular weight weather-resistant siloxane with a molecular weight of 3000-5000. The dropping time is controlled at 30-60 min, and the reaction is carried out at a constant temperature for 3-4.5 h after the dropping is completed.

6. The organosilicon-modified waterborne polyurethane according to claim 5, characterized in that: The process also includes step ③ cooling to 40-50℃, filtering to remove the solid catalyst and obtaining filtrate, then heating the filtrate to 120-150℃, and subjecting it to vacuum de-boiling treatment at a controlled vacuum degree of -0.09 to -0.098MPa for 2-3 hours to obtain low molecular weight flexible siloxanes and high molecular weight weather-resistant siloxanes with a terminal hydroxyl end-capping rate of ≥98%.

7. The organosilicon-modified waterborne polyurethane according to claim 5, characterized in that: The end-capping agent is pure water; the catalyst is a macroporous, strongly acidic styrene-based cation exchange resin.

8. The organosilicon-modified waterborne polyurethane according to claim 1, characterized in that: The chain extender is 1,4-butanediol; the neutralizing agent is triethylamine.

9. The organosilicon-modified waterborne polyurethane according to claim 1, characterized in that: The method for preparing the modified alicyclic isocyanate includes preparing isophorone diisocyanate and isopropanol at a molar ratio of 1:(0.3-0.5), heating the isophorone diisocyanate to 50-60℃ and then adding isopropanol dropwise, controlling the dropwise addition time of isopropanol to 40-60 min, and reacting at a constant temperature for 1-2 h after the dropwise addition is completed to obtain the modified alicyclic isocyanate.

10. A silicone-modified waterborne polyurethane according to any one of claims 1-9, characterized in that, The preparation steps include the following: Step 1: Take 30-60 parts by weight of polyol soft segments and coated hydrophilic monomers and put them into a sealed anhydrous reactor. Control the temperature of the reactor to 105-115℃ and the vacuum degree to -0.08 to -0.095MPa. Dehydrate under vacuum for 1-2 hours, and then cool down to 75-85℃ under sealed pressure to obtain dehydrated raw materials for later use. Step 2: Add phase-separated organosilicon monomer and organobismuth catalyst to the reactor. Control the stirring speed at 300-500 r / min and react at a constant temperature for 15-25 min. Slowly and uniformly add modified alicyclic isocyanate, controlling the addition time to be 0.8-1.2 h. After the addition is completed, keep the temperature at 75-85℃ for 3.5-4.5 h to obtain polyurethane prepolymer. Step 3: Allow the polyurethane prepolymer to cool naturally to 40-50℃, add the neutralizing agent at a uniform rate and stir for 25-35 minutes to obtain the neutralized prepolymer; Step 4: Add the neutralized prepolymer into a high-speed shear dispersion vessel, control the shear speed at 1200-1600 r / min and room temperature, add deionized water and continue shearing emulsification for 35-45 min to obtain the prepolymer aqueous emulsion. Step 5: Control the temperature of the prepolymer aqueous emulsion to 25-35℃, add chain extender dropwise and keep warm while stirring for 1-2 hours to obtain emulsion-like organosilicon-modified waterborne polyurethane.