Alkali-soluble peelable bio-based termination tape for lithium-ion batteries, its preparation method and application

By using poly(α,β-asparagine/aspartic acid ester) copolymer in lithium-ion battery termination tape, rapid de-adhesion separation in alkaline recycling solution was achieved, solving the problem of tape separation during lithium-ion battery recycling and ensuring the stability and environmental friendliness of the material.

CN123107568APending Publication Date: 2026-11-17SHANGHAI RUIDING NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611536880.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion battery termination tapes are difficult to separate efficiently during recycling, leading to breakage of positive and negative electrode materials and tape debris pollution, which affects recycling efficiency and the environment. Furthermore, existing chemical response systems cannot achieve differentiated responses in electrolyte and recycling liquid environments.

Method used

Poly(α,β-asparagine/aspartic acid ester) copolymer is used as pressure-sensitive adhesive. By rapidly hydrolyzing and breaking ester bonds in alkaline recycling solution, the tape maintains adhesion during battery service and automatically loses adhesion and separates during recycling. Bio-based materials are used to ensure degradability.

Benefits of technology

It achieves stable adhesion of lithium-ion battery termination tape during battery service, automatically detaches during recycling without interfering with subsequent recycling processes, reduces recycling costs, and the material is biodegradable and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107568A_ABST
    Figure CN123107568A_ABST
Patent Text Reader

Abstract

This invention discloses an alkali-soluble peelable bio-based termination tape for lithium-ion batteries, its preparation method, and its application. The alkali-soluble peelable bio-based termination tape includes a substrate and a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer contains a poly(α,β-asparagine / aspartic acid ester) copolymer formed by a ring-opening reaction of polysuccinimide, a first alkyl alcohol and its derivatives, and a second alkyl alcohol derivative. The short-chain ester bonds introduced by the second alkyl alcohol are highly stable in conventional battery electrolytes. When the battery is broken up and enters a hot alkali recovery solution, the short-chain ester bonds rapidly hydrolyze within minutes to tens of minutes, generating carboxylate anions. The adhesive layer changes from hydrophobic to hydrophilic, rapidly absorbing water, swelling, and disintegrating. This results in the simultaneous loss of interfacial adhesion between the termination tape and the metal foil, as well as the cohesive force of the adhesive layer itself. The tape automatically detaches in sheets, floats, or disperses, achieving efficient separation from the current collector metal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of pressure-sensitive adhesive technology, specifically relating to an alkali-soluble peelable bio-based termination tape for lithium-ion batteries, its preparation method, and its application. Background Technology

[0002] During the winding or stacking process of lithium-ion battery cells, terminating tape is required to fix and insulate the electrode ends, tab welds, and separator edges. Currently, widely used terminating tapes are primarily based on polyimide (PI) film or polyethylene terephthalate (PET) film coated with acrylic pressure-sensitive adhesive. While these tapes exhibit excellent electrolyte resistance and electrical insulation throughout the battery's lifespan, they pose a significant obstacle during the dismantling and recycling process after battery retirement, as the tape adheres firmly to the electrodes and separator and cannot detach spontaneously.

[0003] The mainstream dismantling process for lithium battery recycling in existing technologies includes: discharging retired cells, pyrolysis, leaching with organic solvents, and soaking in alkaline / acidic recycling solutions to separate the electrode sheets; because the adhesive tape is firmly bonded to the metal current collectors (aluminum foil, copper foil) and cannot be efficiently separated by simple physical methods, the terminating adhesive tape on the cell is removed by mechanical tearing. However, mechanical peeling easily tears the separator and scratches the copper and aluminum current collectors, causing breakage of the positive and negative electrode active materials and reducing the yield of direct repair and regeneration of the electrode sheets; mechanical peeling generates a large amount of adhesive tape debris mixed into the recycled material, increasing the impurity separation process, while manual or automated mechanical dismantling of adhesive tape recycling is inefficient, increasing the cost of power battery recycling; in particular, the large amount of adhesive tape residue after breakage interferes with the leaching of positive electrode materials and metal ion extraction during hydrometallurgy, and generates toxic gases such as fluorine and nitrogen in subsequent heat treatment, significantly increasing recycling costs and environmental impact. Even with mechanical sorting, the small difference in density and magnetic properties between the adhesive tape and foil limits the separation accuracy.

[0004] Existing technologies have reported on non-destructive battery disassembly using stretchable removable tapes or heat-resistant adhesive tapes. However, stretchable tapes rely on the high elongation and cohesive strength of the adhesive layer to be stretched parallel to the adhered object, causing plastic deformation and interfacial debonding. The adhesive layer lacks chemical responsiveness and is not affected by loss of adhesion induced by recycled liquid; it can only be peeled off by mechanical force. It cannot achieve automatic debonding triggered by recycled liquid. Therefore, in practical applications, stretching ends need to be reserved for the tape during the battery structure design stage, or an additional heating process needs to be introduced, which is incompatible with existing efficient crushing and sorting processes. Similarly, heat-resistant adhesive tapes rely on internal thermally foamed microspheres. After reaching the foaming temperature, the microspheres expand, causing a sharp decrease in the interfacial contact area of ​​the adhesive layer, resulting in loss of adhesion. The debonding trigger condition is temperature, not the chemical environment of the recycled liquid. Clearly, easy-pull tape relies on mechanical force, and heat-resistant tape relies on temperature. Neither of them belongs to a chemical response system. They cannot distinguish between electrolyte environment and recycled liquid environment, and cannot achieve differentiated responses such as stability when immersed in electrolyte and rapid loss of adhesion when chemically stimulated by recycled liquid. Both pose a risk of residual adhesive and adhesive debris pollution during battery recycling and dismantling, which directly affects the resource recycling and reuse of electrode sheets and separators.

[0005] Furthermore, existing technologies have also reported the use of ammonolysis to ring-open polysuccinimide with amino-containing hydrophilic compounds (such as amino acids, polyamines, etc.) to obtain polyasparagine materials. However, due to the extremely strong chemical inertness of the amide bonds, these materials exhibit high stability over a wide pH range, which cannot meet the requirement of rapid hydrolysis and bond breaking under specific mild alkaline conditions, thus losing adhesive strength. At the same time, the introduction of a large number of hydrophilic amino groups can lead to uncontrolled swelling and side reactions in the organic electrolyte of lithium batteries, severely degrading insulation and adhesive properties, making them unsuitable for use as electrolyte-resistant pressure-sensitive adhesives.

[0006] To address the aforementioned problems in existing technologies, this invention provides a termination tape that exhibits the same performance as conventional tapes during battery service. However, upon entering a specific recycling liquid medium, the adhesive undergoes chemical bond breakage, rapidly losing its adhesive strength. This causes the tape to automatically detach from the electrode, float out, or be screened out, thus not interfering with subsequent valuable metal recovery. Furthermore, it meets the green requirements of the entire lifecycle of new energy vehicles and energy storage industries. This termination tape uses renewable raw materials and is biodegradable in normal environments or after disposal. Summary of the Invention

[0007] The main objective of this invention is to provide an alkaline-soluble peelable bio-based termination tape for lithium-ion batteries, its preparation method, and its application, in order to overcome the shortcomings of the prior art.

[0008] To achieve the above-mentioned objectives, the present invention employs the technical solution described below.

[0009] As the first objective of the invention, the present invention provides an alkali-soluble peelable bio-based termination tape for lithium-ion batteries, comprising a substrate and a pressure-sensitive adhesive layer: wherein the pressure-sensitive adhesive layer comprises a poly(α,β-asparagine / aspartic acid ester) copolymer, the poly(α,β-asparagine / aspartic acid ester) copolymer being formed by a ring-opening reaction of polysuccinimide with at least one first alkyl alcohol and its derivative and at least one second alkyl alcohol derivative; the first alkyl alcohol is a C8-C18 alkyl alcohol; the second alkyl alcohol is a C1-C4 alkyl alcohol.

[0010] The first alkyl alcohol is a straight-chain or branched alkyl alcohol of C8 to C18, which provides pressure-sensitive adhesion; the second alkyl alcohol is a lower alkyl alcohol of C1 to C4, whose ester bond formed by the reaction with polysuccinimide can be rapidly hydrolyzed and broken in an aqueous medium with pH > 10.

[0011] In some preferred embodiments, the ring-opening reaction results in the copolymer containing a first structural unit (C8-C18 carbon chain) derived from the first alkyl alcohol and a second structural unit (C1-C4 carbon chain) derived from the second alkyl alcohol, wherein the second structural unit accounts for 5 mol% to 30 mol% of the total ring-opening units of all alkyl alcohols (including the first and second alkyl alcohols).

[0012] In some preferred embodiments, the polysuccinimide is prepared by polycondensation of bio-derived L-aspartic acid, with a weight-average molecular weight of 20,000 to 150,000.

[0013] In some specific embodiments, the first alkyl alcohol includes, but is not limited to, at least one of n-octanol, 2-ethylhexanol, n-dodecanol, isotridecyl alcohol, and n-hexadecyl alcohol.

[0014] In some preferred embodiments, the second alkyl alcohol includes, but is not limited to, at least one of methanol, ethanol, n-propanol, isopropanol, etc.

[0015] In some preferred embodiments, the substrate is any one of cellulose membrane, polyhydroxyalkanoate membrane, and polylactic acid membrane.

[0016] In some preferred embodiments, the ring-opening reaction further includes the addition of a multifunctional crosslinking agent.

[0017] Preferably, the amount of the multifunctional crosslinking agent added does not exceed 5% of the total molar number of the first alkyl alcohol and the second alkyl alcohol.

[0018] Preferably, the multifunctional crosslinking agent is selected from any one or a combination of several of lysine, ornithine, or 1,6-hexanediol.

[0019] As a second objective of the invention, the present invention provides a method for preparing the alkali-soluble peelable bio-based termination tape as described above, comprising dissolving polysuccinimide in a polar aprotic solvent, reacting it with a first alkyl alcohol in the presence of an alkaline catalyst, then adding a second alkyl alcohol to continue the reaction, precipitating and purifying the reaction product, dissolving or melting it onto a substrate, and drying or cooling it to form a pressure-sensitive adhesive layer, thereby obtaining the alkali-soluble peelable bio-based termination tape.

[0020] Preferably, the temperature of the first reaction and the second reaction is 40~80℃.

[0021] Preferably, the reaction time for the first reaction is 1 to 8 hours.

[0022] Preferably, the second reaction takes 0.5 to 4 hours.

[0023] Preferably, the alkaline catalyst is an aliphatic tertiary amine compound.

[0024] More preferably, the alkaline catalyst includes, but is not limited to, at least one of triethylamine, N,N-diisopropylethylamine, and tri-n-butylamine.

[0025] Preferably, the polar aprotic solvent includes, but is not limited to, at least one of N,N-dimethylformamide, dimethyl sulfoxide, etc.

[0026] As a third objective of the invention, the present invention provides a power battery comprising at least the alkali-soluble peelable bio-based termination tape described above.

[0027] As a fourth objective of the invention, the present invention provides a method for recycling power batteries. After dismantling the waste power battery as described above, the electrode containing the alkaline-soluble peelable bio-based termination tape is immersed in a recycling solution containing NaOH aqueous solution at a temperature of 40~80°C, so that the alkaline-soluble peelable bio-based termination tape loses its adhesion and automatically peels off from the current collector. Subsequently, the tape and the current collector are separated by flotation or sieving.

[0028] Preferably, the concentration of the NaOH aqueous solution is 0.5~2 mol / L.

[0029] Preferably, the soaking time is 5 to 60 minutes.

[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. In the alkali-soluble peelable bio-based termination tape provided by the technical solution of this invention, short-chain ester bonds (such as acetate or propionate esters) introduced by the second alkyl alcohol are highly stable in conventional battery electrolytes (nearly neutral or weakly acidic), but can trigger a de-adhesion mechanism in alkaline solutions. That is, when the battery is broken and enters the hot alkaline recovery solution (e.g., containing 0.5~2 mol / L NaOH, temperature 40~80℃), the short-chain ester bonds rapidly hydrolyze within a few minutes to tens of minutes, generating carboxylate anions. The adhesive layer changes from hydrophobic to hydrophilic, rapidly absorbs water, swells, and disintegrates. As a result, the interfacial adhesion between the termination tape and the metal foil and the cohesive force of the adhesive layer itself are lost simultaneously. The tape automatically falls off in sheets, floats, or disperses, achieving efficient separation from the current collector metal.

[0031] 2. The technical solution of this invention utilizes the polyaspartic acid ester main chain and its long-chain alkyl side chains to impart excellent hydrophobicity and resistance to organic carbonate electrolytes to the terminating adhesive layer. Even when immersed in an electrolyte containing 1M LiPF6, ethylene carbonate / dimethyl carbonate (EC / DMC) for more than 7 days at 85°C, the swelling rate of the adhesive layer is less than 10%, and the peel strength retention rate is higher than 85%, which is comparable to that of conventional acrylic ester terminating tapes, demonstrating excellent service stability.

[0032] 3. The polysuccinimide used in this invention is derived from bio-fermented aspartic acid, the first alkyl alcohol is a bio-based fatty alcohol, the substrate is a natural or biosynthetic biodegradable material, the entire tape can be degraded under industrial composting or specific enzymatic hydrolysis conditions, the degradation products are environmentally friendly and have no persistent toxic residues.

[0033] 4. Using the technical solution of the present invention, the polyamino acid degradation products released after the tape loses its adhesion are aspartic acid and fatty alcohol, which have no adverse effect on the subsequent wet recovery of valuable metals such as cobalt, nickel, and lithium, and can even be used as a carbon source by microorganisms, simplifying wastewater treatment. Attached Figure Description

[0034] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0035] Figure 1 This is a schematic diagram of the structure of the alkali-soluble peelable bio-based termination tape of the present invention; in the figure, 1-release paper, 2-pressure-sensitive adhesive layer, 3-substrate.

[0036] Figure 2This is a schematic diagram simulating the process of tape losing adhesion and peeling off in hot alkaline solution according to Embodiment 1 of the present invention; in the figure, 4-current collector, 5-tape, 6-alkaline solution, 7-tape fragment. Detailed Implementation

[0037] Together with Figure 1 Reading the detailed embodiments will provide a more complete understanding of the present invention.

[0038] Detailed embodiments of the invention are disclosed herein; however, it should be understood that the disclosed embodiments are merely exemplary of the invention, which may be embodied in various forms. Therefore, the specific functional details disclosed herein should not be construed as limiting, but rather as the basis for the claims and as intended to teach those skilled in the art to adopt the representative basis of the invention in different ways in any suitable detailed embodiment.

[0039] This invention provides an alkali-soluble, peelable, bio-based termination tape that maintains the same performance as conventional tapes during battery service. However, upon entering a specific recycling liquid medium, the adhesive undergoes chemical bond breakage, rapidly losing its adhesive strength, allowing the tape to automatically detach from the electrode, float out, or be screened away. Simultaneously, it meets the green requirements of the entire lifecycle of the new energy vehicle and energy storage industries. This termination tape uses renewable raw materials and is biodegradable in normal environments or after disposal. Furthermore, it solves the technical problem of existing lithium-ion battery termination tapes being extremely difficult to efficiently and thoroughly separate from metal foils during battery recycling, severely impacting the purity and economic efficiency of positive and negative electrode material recycling. The termination tape of this invention can automatically detach from the electrode without interfering with subsequent valuable metal recycling. Moreover, the fully bio-based and biodegradable raw materials used in this invention solve the problem of the lack of renewability and biodegradability in existing bio-based products.

[0040] Specifically, the present invention provides an alkali-soluble, peelable, bio-based termination tape, comprising a substrate and a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer is formed of a polyamino acid derivative composition; the polyamino acid derivative composition comprises a poly(α,β-asparagine / aspartic acid ester) copolymer, wherein the copolymer is obtained by a ring-opening reaction of polysuccinimide with at least two alkyl alcohols; wherein... The first alkyl alcohol is a C8-C18 straight-chain or branched alkyl alcohol, which provides pressure-sensitive adhesion; The second alkyl alcohol is a C1-C4 alkyl alcohol, and the ester bond formed by its reaction with polysuccinimide can be rapidly hydrolyzed and broken in an aqueous medium with pH > 10.

[0041] The ring-opening reaction results in the copolymer containing a first structural unit (C8-C18 straight or branched chain) derived from the first alkyl alcohol and a second structural unit derived from the second alkyl alcohol, wherein the second structural unit (C1-C4 carbon chain) accounts for 5 mol% to 30 mol% of the total ring-opening units of the alcohol.

[0042] In some specific embodiments, the polysuccinimide is prepared by thermal polycondensation of biologically derived L-aspartic acid, and its weight-average molecular weight is 10,000 to 200,000 g / mol.

[0043] In some specific embodiments, the first alkyl alcohol includes, but is not limited to, at least one of n-octanol, 2-ethylhexanol, n-dodecanol, isotridecyl alcohol, and n-hexadecyl alcohol.

[0044] In some specific embodiments, the second alkyl alcohol includes, but is not limited to, at least one of methanol, ethanol, n-propanol, isopropanol, etc.

[0045] Furthermore, a multifunctional crosslinking agent (such as lysine, ornithine, or 1,6-hexanediol) not exceeding 5% of the total alcohol molars can be added to the ring-opening reaction to adjust the cohesive strength.

[0046] The preparation method of the above-mentioned pressure-sensitive adhesive layer includes: dissolving polysuccinimide in a polar aprotic solvent (such as N,N-dimethylformamide, dimethyl sulfoxide), adding a first alcohol in the presence of a catalyst and reacting at 40~80℃ for 1~8 hours, then adding a second alcohol and continuing the reaction for 0.5~4 hours, and obtaining a polyamino acid derivative by precipitation, washing and drying after the reaction is completed; dissolving the derivative in a suitable solvent or directly heating and melting it, coating it on a substrate, and drying or cooling to form a pressure-sensitive adhesive layer.

[0047] See Figure 1 This is a schematic diagram of the structure of the alkali-soluble peelable bio-based termination tape sample provided by the present invention. The pressure-sensitive adhesive layer 2 is obtained by coating a polyamino acid derivative onto the surface of the substrate 3. The other side of the pressure-sensitive adhesive layer 2 can be formed into a termination tape product using release paper 1.

[0048] Preferably, the catalyst is an aliphatic tertiary amine compound.

[0049] More preferably, the alkaline catalyst includes, but is not limited to, at least one of triethylamine, N,N-diisopropylethylamine, and tri-n-butylamine.

[0050] In some specific embodiments, the substrate may be made of biodegradable materials such as cellulose film, polyhydroxyalkanoate (PHA) film, polylactic acid (PLA) film or paper to ensure the biodegradability of the entire tape at the end of its life cycle.

[0051] The present invention utilizes an alkaline-soluble, peelable, bio-based termination tape that exhibits a triggered loss-of-adhesion mechanism in alkaline solutions. This is because the short-chain ester bonds (such as acetate and propionate esters) introduced by the second alkyl alcohol are highly stable in conventional battery electrolytes (nearly neutral or weakly acidic). However, when the battery is broken up and enters a hot alkaline recovery solution (e.g., containing 0.5-2 mol / L NaOH at a temperature of 40-80°C), these short-chain ester bonds rapidly hydrolyze within minutes to tens of minutes, generating carboxylate anions. The adhesive layer changes from hydrophobic to hydrophilic, rapidly absorbing water, swelling, and disintegrating. This results in the simultaneous loss of interfacial adhesion between the tape and the metal foil, as well as the cohesive force of the adhesive layer itself. The tape automatically detaches, floats, or disperses in sheets, achieving efficient separation from the current collector metal.

[0052] The thickness and area of ​​the termination tape provided by this invention can be adjusted according to actual needs, and this invention does not impose specific limitations.

[0053] The technical solution of the present invention will be further illustrated below through specific embodiments.

[0054] Example 1 This embodiment provides a method for preparing an alkali-soluble, peelable, bio-based termination tape, the specific steps of which include: Step 1: Preparation of polysuccinimide (PSI) 100g of bio-based L-aspartic acid was mixed with 15g of 85% phosphoric acid and stirred at 180°C under reduced pressure for 4 hours to condense the mixture. The temperature was then raised to 210°C and the reaction was continued for another 4 hours. After cooling, the mixture was dissolved in N,N-dimethylformamide, poured into a large amount of methanol to precipitate the precipitate, filtered and dried to obtain polysuccinimide with a weight average molecular weight of approximately 65,000 g / mol.

[0055] Step 2: Preparation of Termination Tape 10 g of polysuccinimide and 60 mL of anhydrous DMF were added to a reaction flask and stirred until dissolved. Then, 8.5 g of n-dodecyl alcohol (primary alcohol, 0.046 mol) and 0.2 g of triethylamine were added, and the mixture was reacted at 60 °C for 4 hours. Subsequently, 1.2 g of anhydrous ethanol (secondary alcohol, 0.026 mol) was added, and the reaction was continued at 60 °C for 2 hours to obtain a reaction solution. The reaction solution was then poured into an ethanol / water mixture (ethanol / water volume ratio of 1:1) to precipitate the precipitate. After washing and drying, a poly(dodecyl aspartic acid ester-co-ethyl aspartic acid ester) copolymer was obtained. NMR calculations showed that the dodecyl structural units were approximately 85 mol% and the ethyl ester structural units were approximately 15 mol%.

[0056] The copolymer was prepared into a 30% solids solution with ethyl acetate, coated onto a 30μm thick regenerated cellulose membrane substrate, dried at 100℃ for 3 minutes, and then bonded with release paper to obtain tape sample A with an adhesive layer thickness of about 20μm.

[0057] Performance testing: Electrolyte composition: 1M LiPF6 EC / DMC (volume ratio 1:1) solution (the electrolyte composition used in other examples and comparative examples is the same).

[0058] (1) Electrolyte resistance test Initial adhesive properties: According to GB / T 2792, the initial peel strength of tape A against aluminum plate at 180° is 12.5 N / 25mm.

[0059] Remove the release paper and attach tape sample A to the surface of the aluminum sheet.

[0060] The aluminum sheet with tape was placed in the above electrolyte and stored at 85°C for 7 days. After that, the surface electrolyte was wiped off and the peel strength after immersion was tested, which was 11.2 N / 25mm.

[0061] Based on the initial peel strength and the peel strength after soaking, it can be calculated that the peel strength retention rate of the tape soaked in the electrolyte is 89.6%, and the adhesive layer does not dissolve or transfer.

[0062] (2) Alkali-triggered de-adhesion and peeling separation test: Prepare a 1.5 mol / L NaOH aqueous solution and heat it to 70°C in a water bath. Place the aluminum sheet soaked in the above electrolyte into the alkaline solution, immerse it statically, and observe the peeling of the tape.

[0063] The results showed that after soaking for 10 minutes, tape A automatically curled and floated from the aluminum foil surface, leaving no adhesive residue on the aluminum foil surface. Upon removal, the aluminum foil was observed to be bright and clean. (See also...) Figure 2 The figure shows a schematic diagram simulating the process of tape sample A losing its adhesion and peeling off after being immersed in hot alkaline solution in this embodiment. The figure shows the process of the tape breaking into pieces after swelling, curling up, and then breaking into pieces.

[0064] Example 2 The difference between this embodiment and Example 1 is that in step 2, the first alkyl alcohol is an equimolar mixture of n-octanol and 2-ethylhexanol (total 0.046 mol), the second alkyl alcohol is methanol (0.026 mol, accounting for 10 mol% of all alcohol ring-opening units), and L-lysine, accounting for 3% of the total alkyl alcohol moles, is added as a crosslinking agent. The remaining operations are the same as in Example 1.

[0065] The resulting copolymer was coated onto a PHA film substrate, tape sample B, with an adhesive layer thickness of approximately 20 μm.

[0066] The testing method is the same as in Example 1.

[0067] Test results: (1) The results of the electrolyte resistance test showed that after the tape B was immersed in the electrolyte for 7 days, its peel strength retention rate was 91%, and the adhesive layer did not dissolve or transfer.

[0068] (2) The results of the alkaline solution triggered deadhesion and peeling separation test showed that when it was soaked in 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 10 minutes and was in the form of small fragments, which were easier to sieve and separate.

[0069] Example 3 The only difference between this embodiment and Example 2 is that L-lysine is not added; all other steps are the same.

[0070] The resulting copolymer was coated onto a PHA film substrate, tape sample C, with an adhesive layer thickness of approximately 20 μm.

[0071] The testing method is the same as in Example 1.

[0072] Test results: (1) The results of the electrolyte resistance test show that the peel strength retention rate of tape C is 88%, and the adhesive layer does not dissolve or transfer.

[0073] (2) The results of the alkaline solution triggered deadhesion and peeling separation test showed that when it was soaked in 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 10 minutes and was in the form of small fragments, which were easier to sieve and separate.

[0074] Example 4 The only difference between this embodiment and Example 1 is that the first alcohol is n-hexadecyl alcohol (0.046 mol), and all other steps are the same. The product obtained is tape sample D.

[0075] The testing method is the same as in Example 1.

[0076] Test results: (1) The results of the electrolyte resistance test show that the peel strength retention rate of tape D is 92%, and the adhesive layer does not dissolve or transfer.

[0077] (2) The results of the alkaline solution triggered loss of adhesion and peeling separation test showed that when it was soaked in 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 12 minutes and was in sheet form.

[0078] Example 5 The only difference between this embodiment and Example 1 is that the first alcohol is n-octanol; all other steps are the same, and the product obtained is tape sample E.

[0079] The testing method is the same as in Example 1.

[0080] Test results: (1) The results of the electrolyte resistance test show that the peel strength retention rate of tape E is 87%, and the adhesive layer does not dissolve or transfer.

[0081] (2) The results of the alkaline solution-triggered loss of adhesion and peeling separation test showed that when it was soaked in 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 10 minutes and was in the form of small fragments.

[0082] Example 6 The only difference between this embodiment and Example 1 is that the first alcohol is an equimolar mixture of n-octanol and 2-ethylhexanol (total 0.046 mol). All other steps are the same, and the product obtained is tape sample F.

[0083] The testing method is the same as in Example 1.

[0084] Test results: (1) The results of the electrolyte resistance test show that the peel strength retention rate of tape F is 86%, and the adhesive layer does not dissolve or transfer.

[0085] (2) Alkali-triggered loss of adhesion and peeling separation test: In 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 9 minutes and was in the form of small fragments.

[0086] Example 7 The only difference between this embodiment and Example 1 is that the second alcohol is isopropanol (0.026 mol), while all other steps are the same, and the product obtained is tape sample G.

[0087] The testing method is the same as in Example 1.

[0088] Test results: (1) The results of the electrolyte resistance test show that the peel strength of tape G is maintained at 90%, and the adhesive layer does not dissolve or transfer.

[0089] (2) Alkali-triggered loss of adhesion and peeling separation test: In 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 15 minutes and was in sheet form.

[0090] Example 8 The only difference between this embodiment and Example 1 is that the obtained tape sample A was subjected to an alkaline-triggered loss of adhesion and peeling separation test in a 0.5 mol / L NaOH solution at 70°C. The results showed that the tape completely detached within 10 minutes and was in the form of small fragments.

[0091] Example 9 The only difference between this embodiment and Example 1 is the addition of 1,6-hexanediol, which accounts for 3% of the total alkyl alcohol molars, as a crosslinking agent. The rest of the operation is the same as in Example 1. The product obtained is tape sample H.

[0092] The testing method is the same as in Example 1.

[0093] Test results: (1) The results of the electrolyte resistance test show that the peel strength retention rate of tape G is 89%, and the adhesive layer does not dissolve or transfer.

[0094] (2) Alkali-triggered loss of adhesion and peeling separation test: In 70℃, 1.5mol / L NaOH solution, the tape completely fell off within 10 minutes and was in the form of small fragments.

[0095] Comparative Example 1 Commercially available standard lithium-ion battery termination tape (PI substrate, acrylic pressure-sensitive adhesive, Shenzhen Yizhong Technology Co., Ltd., model YZ-5146).

[0096] After being immersed in electrolyte for 7 days, the peel strength of the tape remained at 87%. This may be because the C4 alkyl chain was too short, causing severe swelling of the adhesive layer and collapse of cohesion.

[0097] In a 1.5 mol / L NaOH solution at 70℃, the tape showed no signs of detachment within 60 minutes, and manual peeling was difficult with residual adhesive.

[0098] Comparative Example 2 The only difference between this comparative example and Example 1 is that the first alcohol is n-hexanol (0.046 mol), and all other steps are the same.

[0099] After immersion in the electrolyte for 7 days, the peel strength of the tape remained at 72%. This may be because the C6 alkyl chain of the first alkyl alcohol is too short and its hydrophobicity is insufficient, causing it to swell significantly during immersion in the electrolyte.

[0100] In a 70℃, 1.5mol / L NaOH solution, the tape completely dissolved and dispersed within 3 minutes and could not be peeled off in sheets. The possible reason is that the C6 ester bond hydrolyzed too quickly, resulting in insufficient service stability.

[0101] Comparative Example 3 The only difference between this comparative example and Example 1 is that the first alcohol is n-butanol (0.046 mol), and all other steps are the same.

[0102] After being immersed in electrolyte for 7 days, the peel strength of the tape remained at 58%. This may be because the C4 alkyl chain was too short, causing severe swelling of the adhesive layer and collapse of cohesion.

[0103] In a 1.5 mol / L NaOH solution at 70℃, the tape completely dissolves and disperses within 2 minutes, making it impossible to peel off in sheets.

[0104] Comparative Example 4 The only difference between this comparative example and Example 1 is that the second alcohol is n-hexanol (0.026 mol, C6), and all other steps are the same.

[0105] Its peel strength retention rate is 85% after immersion in electrolyte.

[0106] In a 1.5 mol / L NaOH solution at 70℃, the tape did not completely detach within 60 minutes, leaving obvious residue. This may be because the carbon chain length of the C6 ester bond results in significant steric hindrance, leading to a slow hydrolysis rate that cannot meet the requirements for rapid de-adhesion.

[0107] In summary, the alkali-soluble peelable bio-based termination tape provided by this invention, through the introduction of short-chain ester bonds (such as acetate and propionate esters) via a second alkyl alcohol, exhibits high stability in conventional battery electrolytes (nearly neutral or weakly acidic). However, it can trigger a de-adhesion mechanism in alkaline solutions. Specifically, when the battery is broken up and enters a hot alkaline recovery solution, for example containing 0.5~2 mol / L NaOH at a temperature of 40~80℃, the short-chain ester bonds rapidly hydrolyze within minutes to tens of minutes, generating carboxylate anions. The adhesive layer changes from hydrophobic to hydrophilic, rapidly absorbing water, swelling, and disintegrating. This results in the simultaneous loss of interfacial adhesion between the termination tape and the metal foil, as well as the cohesive force of the adhesive layer itself. The tape automatically detaches, floats, or disperses in sheets, achieving efficient separation from the current collector metal. In particular, this invention utilizes the polyaspartic acid ester backbone and its long-chain alkyl side chains to endow the termination adhesive layer with excellent hydrophobicity and resistance to organic carbonate electrolytes, even in solutions containing 1M... When LiPF6 is immersed in ethylene carbonate / dimethyl carbonate (EC / DMC) electrolyte at 85°C for more than 7 days, the swelling rate of the adhesive layer is less than 10%, and the peel strength retention rate is higher than 85%, which is comparable to that of conventional acrylic termination tapes, demonstrating excellent service stability.

[0108] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the described embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims.

Claims

1. An alkali-soluble, peelable, bio-based termination tape for lithium-ion batteries, characterized in that, Including the substrate and pressure-sensitive adhesive layer: The pressure-sensitive adhesive layer comprises a poly(α,β-asparagine / aspartic acid ester) copolymer, which is formed by a ring-opening reaction of polysuccinimide with at least one first alkyl alcohol and its derivative and at least one second alkyl alcohol derivative. The first alkyl alcohol is a C8~C18 alkyl alcohol; The second alkyl alcohol is a C1~C4 alkyl alcohol.

2. The alkali-soluble peelable bio-based termination tape according to claim 1, characterized in that, The ring-opening reaction results in the copolymer containing a first structural unit derived from the first alkyl alcohol and a second structural unit derived from the second alkyl alcohol, wherein the second structural unit accounts for 5 mol% to 30 mol% of the total number of ring-opening units of the first alkyl alcohol and the second alkyl alcohol.

3. The alkali-soluble peelable bio-based termination tape according to claim 1, characterized in that, The polysuccinimide is prepared by polycondensation of bio-derived L-aspartic acid and has a weight-average molecular weight of 20,000 to 150,000.

4. The alkali-soluble peelable bio-based termination tape according to claim 1, characterized in that, The first alkyl alcohol is selected from at least one of n-octanol, 2-ethylhexanol, n-dodecanol, isotridecyl alcohol, and n-hexadecyl alcohol; And / or, the second alkyl alcohol is selected from at least one of methanol, ethanol, n-propanol, and isopropanol.

5. The alkali-soluble peelable bio-based termination tape according to claim 1, characterized in that, The substrate is any one of cellulose membrane, polyhydroxyalkanoate membrane, and polylactic acid membrane.

6. The alkali-soluble peelable bio-based termination tape according to any one of claims 1-5, characterized in that, The ring-opening reaction also includes the addition of a multifunctional crosslinking agent; And / or, the amount of the multifunctional crosslinking agent added does not exceed 5% of the total molar number of the first alkyl alcohol and the second alkyl alcohol; And / or, the multifunctional crosslinking agent is selected from any one or a combination of several of lysine, ornithine, or 1,6-hexanediol.

7. A method for preparing an alkali-soluble peelable bio-based termination tape as described in any one of claims 1-6, characterized in that, Polysuccinimide is dissolved in a polar aprotic solvent and reacted with a first alkyl alcohol in the presence of an alkaline catalyst. Then, a second alkyl alcohol is added to continue the reaction. After the reaction product is purified by precipitation, it is dissolved or melt-coated onto a substrate and dried or cooled to form a pressure-sensitive adhesive layer, thus obtaining the alkaline-soluble peelable bio-based termination tape.

8. The preparation method according to claim 7, characterized in that, The temperatures for the first and second reactions are 40~80℃; The first reaction takes 1 to 8 hours; The second reaction takes 0.5 to 4 hours; The alkaline catalyst is an aliphatic tertiary amine compound; preferably, the alkaline catalyst is at least one selected from triethylamine, N,N-diisopropylethylamine, and tri-n-butylamine. The polar aprotic solvent is at least one of N,N-dimethylformamide and dimethyl sulfoxide.

9. A power battery, characterized in that, It includes at least the alkali-soluble peelable bio-based termination tape as described in any one of claims 1-6.

10. A method for recycling a power battery, characterized in that, After the discarded power battery as described in claim 9 is disassembled, the electrode where the alkaline-soluble peelable bio-based termination tape is located is immersed in a recovery solution containing NaOH aqueous solution at 40~80°C, so that the alkaline-soluble peelable bio-based termination tape loses its adhesion and automatically peels off from the current collector. Then, the tape and the current collector are separated by flotation or sieving. Preferably, the concentration of the NaOH aqueous solution is 0.5~2 mol / L; Preferably, the soaking time is 5 to 60 minutes.