A high electrolyte-resistant modified acrylic pressure-sensitive adhesive and lithium battery tape

By using a unique design and crosslinking system for modified acrylic pressure-sensitive adhesive, the durability problem of lithium battery tape in high-temperature and electrolyte environments has been solved, achieving improved peel strength and electrolyte resistance, thus ensuring the safety and lifespan of lithium batteries.

CN123107584APending Publication Date: 2026-11-17GUANGDONG CHUANGYANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611490574.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional acrylic pressure-sensitive adhesives have insufficient resistance to electrolytes in lithium batteries, exhibiting problems such as swelling, peeling, discoloration, and insufficient high-temperature retention, making it difficult to simultaneously meet the requirements of high peel strength and resistance to electrolyte corrosion.

Method used

High electrolyte-resistant modified acrylic pressure-sensitive adhesive is used. Through the unique design of acrylic macromolecular structure, selection of anti-dissolution tackifying resin and covalent-coordination dual crosslinking system, combined with fluorinated monomers and high-temperature crosslinking agents, multiple crosslinking networks and chemical anchoring effects are formed, which enhance the electrolyte resistance and high-temperature stability of the adhesive layer.

Benefits of technology

It achieves long-term stability in high-temperature environments of 150℃ and electrolyte environments of 85℃, without peeling or discoloration, and has a high peel strength of 800-1100 gf/25mm and good initial adhesion, ensuring stable adhesion of lithium battery tape in polar environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a highly electrolyte-resistant modified acrylic pressure-sensitive adhesive, comprising the following raw materials by weight: 100 parts acrylic copolymer resin; 0.2-0.8 parts polyisocyanate crosslinking agent; 0.05-0.2 parts metal chelate crosslinking agent; 0.1-1.0 parts silane coupling agent; 5-15 parts fully hydrogenated tackifying resin; and 0.1-0.5 parts antioxidant; wherein the mass ratio of the polyisocyanate crosslinking agent to the metal chelate crosslinking agent is 3:1-6:1. This invention also discloses a method for preparing the highly electrolyte-resistant modified acrylic pressure-sensitive adhesive. The highly electrolyte-resistant modified acrylic pressure-sensitive adhesive provided by this invention has good high-temperature resistance and electrolyte corrosion resistance, and can be used to prepare lithium battery tapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of functional polymer adhesive materials technology, and in particular to a high electrolyte-resistant modified acrylic pressure-sensitive adhesive and lithium battery tape. Background Technology

[0002] In the manufacturing process of lithium-ion batteries, special adhesive tapes are widely used for cell termination and fixation, tab protection and wrapping, and internal insulation. As a permanent or semi-permanent auxiliary material inside the battery, the performance of the tape directly affects the battery's safety and cycle life. The interior of a lithium battery is filled with an electrolyte composed of highly polar organic solvents (such as ethylene carbonate EC, dimethyl carbonate DMC, diethyl carbonate DEC, and methyl ethyl carbonate EMC) and lithium hexafluorophosphate (LiPF6). During battery filling, formation, and high-rate charging and discharging, the internal temperature often rises to a high level.

[0003] Traditional acrylic pressure-sensitive adhesives have fatal defects in terms of resistance to electrolyte immersion: (1) swelling and shedding: small molecules of electrolyte can easily penetrate into the gaps between acrylic resin molecular chains, causing the adhesive layer to swell violently and the coagulation force to break, resulting in the tape falling off; (2) dissolution and discoloration of small molecules: ordinary tackifying resins added to improve peel strength are easily extracted and dissolved by electrolyte, contaminating the electrolyte and causing discoloration; (3) contradiction between high peel strength and temperature / electrolyte resistance: if the crosslinking density is low, the peel strength is high but the temperature resistance at 150℃ is extremely poor; if the crosslinking density is too high, the adhesive becomes hard, and the initial tack and peel strength cannot meet the requirements (800-1100 gf / 25mm).

[0004] Therefore, developing a lithium battery-specific tape that possesses both high peel strength and the ability to remain stable and undiscolored for extended periods in high-temperature environments of 150°C and electrolyte environments of 85°C is an urgent need in this field. Summary of the Invention

[0005] The purpose of this invention is to provide a high electrolyte-resistant modified acrylic pressure-sensitive adhesive and lithium battery tape. Through a unique acrylic macromolecular structure design, selection of anti-leaching tackifying resin, and covalent-coordination dual crosslinking system, it solves the technical problem of mutual constraints between high adhesive strength (peel force 800-1100 gf / 25mm), 150℃ temperature resistance, and 85℃ electrolyte corrosion resistance.

[0006] The first aspect of this invention provides a highly electrolyte-resistant modified acrylic pressure-sensitive adhesive, comprising the following raw materials by weight: 100 parts of acrylic copolymer resin; 0.2–0.8 parts of polyisocyanate crosslinking agent; 0.05–0.2 parts of metal chelating crosslinking agent; 0.1 to 1.0 parts of silane coupling agent; 5-15 parts of fully hydrogenated tackifying resin; Antioxidant 0.1–0.5 parts; The mass ratio of the polyisocyanate crosslinking agent to the metal chelate crosslinking agent is 3:1 to 6:1.

[0007] Furthermore, the acrylic copolymer resin is prepared by free radical solution polymerization of the following parts by weight of comonomers in the presence of an organic solvent and an initiator: 55-70 parts of soft acrylic monomer, 15-25 parts of hard acrylic monomer, 3-8 parts of polar functional monomer, 5-15 parts of electrolyte-resistant special monomer, and 0.5-2.0 parts of silane coupling monomer containing polymerizable double bonds.

[0008] Further, the soft acrylic monomer is selected from at least one of isooctyl acrylate, n-butyl acrylate, and isostearate acrylate; the hard acrylic monomer is selected from at least one of methyl methacrylate, isopropyl acrylate, isobornyl acrylate, and cyclohexyl methacrylate.

[0009] Furthermore, the polar functional monomer includes a carboxyl monomer and a hydroxyl monomer; wherein the carboxyl monomer is selected from at least one of acrylic acid and methacrylic acid, and the hydroxyl monomer is selected from at least one of 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; and the mass ratio of the carboxyl monomer to the hydroxyl monomer is 1.5:1 to 2.5:1.

[0010] Furthermore, the electrolyte-resistant special monomer is selected from at least one of trifluoroethyl acrylate, trifluoroethyl methacrylate, and hexafluoroisopropyl methacrylate.

[0011] Furthermore, the silane coupling monomer containing polymerizable double bonds is γ-(methacryloyloxy)propyltrimethoxysilane.

[0012] Further, the polyisocyanate crosslinking agent is at least one of toluene diisocyanate trimer, diphenylmethane diisocyanate adduct, or hexamethylene diisocyanate biuret; the metal chelating crosslinking agent is at least one of aluminum acetylacetonate or titanium acetylacetonate; the silane coupling agent is γ-glycidyl etheroxypropyltrimethoxysilane; and the fully hydrogenated tackifying resin is a DCPD fully hydrogenated petroleum resin or a fully hydrogenated terpene resin with a softening point greater than or equal to 135°C.

[0013] The second aspect of the present invention provides a high electrolyte-resistant lithium battery tape, which comprises, from bottom to top: a polyimide substrate layer, a release layer coated on the back side of the polyimide substrate layer, and a pressure-sensitive adhesive layer coated on the front side of the polyimide substrate layer. The thickness of the polyimide substrate layer is 19–25 μm; The coating thickness of the release layer is 0.2–1.0 μm; The pressure-sensitive adhesive layer is formed by drying, curing and aging of the high electrolyte-resistant modified acrylic pressure-sensitive adhesive as described above. The dry adhesive thickness of the pressure-sensitive adhesive layer is 10-25 μm, preferably 10 μm or 25 μm.

[0014] A third aspect of this invention provides a method for preparing a high electrolyte-resistant lithium battery tape, comprising the following steps: S1. Soft acrylic acid monomers, hard acrylic acid monomers, polar functional monomers, electrolyte-resistant special monomers, and silane coupling monomers containing polymerizable double bonds are dissolved in anhydrous ethyl acetate and reacted at 75–85°C for 6–10 hours under the action of an initiator to obtain an acrylic acid copolymer resin solution with a weight-average molecular weight of 600,000 to 1,000,000. S2. Add the polyisocyanate crosslinking agent, metal chelate crosslinking agent, silane coupling agent, fully hydrogenated tackifying resin and antioxidant to the acrylic copolymer resin solution in proportion, stir for 20 to 40 minutes, adjust the solid content to 30% to 45%, and degas under vacuum to obtain the pressure-sensitive adhesive solution. S3. Apply a release agent to the back of a polyimide substrate with a thickness of 19–25 μm, and dry and cure at 120–140°C to form a release layer with a thickness of 0.2–1.0 μm; S4. The pressure-sensitive adhesive prepared in step S2 is micro-coated on the front side of the polyimide substrate, and the solvent is removed by a gradient temperature-controlled drying tunnel to control the dry adhesive thickness to be 10~25 μm, preferably 10 μm or 25 μm. S5. The coated tape is bonded to the release film and rolled up, and cured in a curing chamber at 45-55°C for 48-72 hours to obtain a high electrolyte-resistant lithium battery tape.

[0015] Furthermore, in step S4, the temperature regime of the gradient temperature control oven is as follows: first bake at 80°C for 2 minutes, then bake at 110°C for 1 minute, and finally bake at 130°C for 2 minutes.

[0016] Compared with the prior art, the present invention has the following significant advantages: 1. This invention introduces a specific amount of fluorinated acrylate monomers into the acrylic acid backbone through copolymerization. Utilizing the extremely low surface free energy and extremely high CF bond energy of fluorine atoms, the fluorinated side chains spontaneously migrate to the surface of the adhesive layer and align themselves during the coating gradient drying process, forming a fluorinated, solvent-repellent miniature layer of several nanometers to tens of nanometers. This barrier layer exhibits a strong repulsion and barrier effect against highly polar carbonate solvents (such as DMC, EC, and EMC), significantly inhibiting the diffusion and penetration of small electrolyte molecules into the adhesive layer.

[0017] 2. This invention abandons traditional rosin-based or small-molecule tackifying resins that are easily dissolved by carbonate solvents, and instead uses a fully hydrogenated alicyclic tackifying resin with a softening point ≥ 135℃ that is resistant to electrolytes. Combined with the physical locking effect of a covalent-coordinative dual crosslinking network on low-molecular-weight species, it achieves no discoloration, no turbidity, and no leaching after immersion in electrolyte at 85℃ for 24 hours, completely eliminating the potential for traditional tapes to contaminate battery electrodes and trigger side reactions.

[0018] 3. Traditional acrylic pressure-sensitive adhesives, when pursuing high peel strength, typically require reducing the crosslinking density, but this leads to a sharp deterioration in holding power at 150℃ and residual adhesive. Increasing the crosslinking density, however, causes the adhesive to harden, resulting in a significant drop in initial tack and peel strength. This invention constructs a multi-layered three-dimensional interpenetrating crosslinked network by adding polyisocyanate and a metal chelating agent in a mass ratio of 3:1 to 6:1, combined with the side-group condensation of the molecular chain of γ-glycidyl etheroxypropyltrimethoxysilane monomer. This allows the adhesive layer to maintain good viscoelastic deformation and flow wettability at room temperature, stably achieving a high peel strength of 800–1100 gf / 25mm and initial tack strength for balls of sizes 1–8. Simultaneously, it provides strong network support at 150℃, ensuring adhesion to steel plates at 150℃ / 60min without detachment, edge warping, or residual adhesive, with a holding power >72h.

[0019] 4. This invention directly introduces γ-(methacryloyloxy)propyltrimethoxysilane into the acrylic resin backbone during the polymerization stage, and synergistically adds γ-glycidyloxypropyltrimethoxysilane in the formulation. During the drying and curing stages, silanoxy groups accumulate at the interface between the tape and the PI substrate and the interface between the tape and the metal electrode under polar action, and undergo hydrolytic condensation with trace amounts of surface hydroxyl groups to form a strong Si-OM (M=Si, Cu, Al, Fe) covalent bond. This chemical anchoring effect fundamentally prevents wet peeling and edge warping caused by the penetration of small electrolyte molecules along the "adhesive layer-substrate" interface gaps, ensuring that the flat-laid copper / aluminum foil remains tightly bonded even after long-term immersion in electrolyte at 85°C. Detailed Implementation

[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0021] The present invention will be further described below with reference to specific embodiments and comparative examples. Example 1

[0022] 1. Synthesis of acrylic copolymer resin: In a 1L four-necked flask equipped with an electric stirrer, a condenser, a titration funnel, and a nitrogen inlet, add 150g of dehydrated ethyl acetate, 62g of isooctyl acrylate (2-EHA), 20g of methyl methacrylate (MMA), 5g of acrylic acid (AA), 2g of 2-hydroxyethyl acrylate (HEA), 10g of trifluoroethyl acrylate (TFEA), and 1g of γ-(methacryloyloxy)propyltrimethoxysilane (KBM-503).

[0023] After purging oxygen with high-purity nitrogen for 30 minutes, the temperature was raised to 80°C, and 0.3g of azobisisobutyronitrile (AIBN) was added to initiate polymerization. The reaction was maintained at 80°C for 8 hours to obtain an acrylic copolymer resin solution with a solid content of 40.2% and a weight average molecular weight of approximately 820,000.

[0024] 2. Rubber Mixing: Based on 100g of resin dry weight, add 0.45g of toluene diisocyanate (TDI) trimer crosslinking agent (L-75), 0.10g of aluminum acetylacetonate (TDI to aluminum chelating agent mass ratio 4.5:1), 0.5g of γ-glycidyl etheroxypropyltrimethoxysilane (KBM-403), 10g of fully hydrogenated DCPD alicyclic petroleum resin (SU-400) with a softening point of 140℃, and 0.2g of antioxidant 1010 to the above resin solution. Stir at 1200rpm for 30min using a high-speed disperser, add dehydrated ethyl acetate to adjust the solid content to 35%, and degas under vacuum for 20min.

[0025] 3. Tape coating and curing: A 25μm thick polyimide (PI) film was selected, and a silicone-fluorine modified release agent was micro-coated on its back side. After drying and curing at 130℃, a release layer with a thickness of 0.5μm was formed. The prepared pressure-sensitive adhesive was coated on the front side of the PI film, and the solvent was removed and cured by passing it through a three-stage gradient temperature-controlled drying tunnel (80℃ / 2min→110℃ / 2min→130℃ / 2min), and the dry adhesive thickness was controlled to be 25μm.

[0026] After laminating the release film, the tape is cured in a curing chamber at 50°C for 60 hours to obtain a high electrolyte-resistant lithium battery tape. Example 2

[0027] The difference between Example 2 and Example 1 is as follows: In the synthesis of the acrylic copolymer resin, the feed ratio was adjusted as follows: 150g of dehydrated ethyl acetate, 60g of 2-EHA, 20g of MMA, 5g of AA, 2g of HEA, 12g of hexafluoroisopropyl methacrylate (HFIMA), 1g of KBM-503, and 0.3g of initiator AIBN. The polymerization process was the same as in Example 1, yielding a resin solution with a solid content of approximately 40.0%. Example 3

[0028] The difference between Example 3 and Example 1 is as follows: When preparing the adhesive, add 0.60g of TDI trimer, 0.20g of aluminum acetylacetonate (TDI to aluminum chelating agent mass ratio 3:1), 0.5g of KBM-403, 8g of fully hydrogenated terpene resin with a softening point of 135℃, and 0.2g of antioxidant per 100g of dry resin.

[0029] During coating and curing, a 19μm PI film was selected, with a 0.3μm release layer on the back side and a 10μm dry adhesive thickness on the front side. The film was cured at 50℃ for 72 hours. Example 4

[0030] The difference between Example 4 and Example 1 is as follows: When preparing the adhesive, add 0.30g of TDI trimer, 0.05g of aluminum acetylacetonate (TDI to aluminum chelating agent mass ratio 6:1), 0.5g of KBM-403, 12g of fully hydrogenated DCPD petroleum resin with a softening point of 140℃, and 0.2g of antioxidant per 100g of dry resin.

[0031] During coating and curing, a 25μm PI film is selected, with a 0.8μm release layer on the back side and a 25μm dry adhesive thickness on the front side. Curing is carried out at 50℃ for 48 hours. Example 5

[0032] The difference between Example 5 and Example 1 is: The feed ratio for the synthesis of acrylic copolymer resin is: 2-EHA 67g, MMA 20g, AA 5g, HEA 2g, TFEA 5g, KBM-503 1g. Comparative Example 1

[0033] The difference between Comparative Example 1 and Example 1 is as follows: Do not add TFEA during polymerization; replace it with an equal amount of 2-EHA. Comparative Example 2

[0034] The difference between Comparative Example 2 and Example 1 is as follows: When preparing the adhesive, replace the fully hydrogenated DCPD petroleum resin with 10g of ordinary hydrogenated rosin glycerol ester with a softening point of 100℃. Comparative Example 3

[0035] The difference between Comparative Example 3 and Example 1 is as follows: When preparing the adhesive, do not add aluminum acetylacetonate, but only add 0.55g of TDI trimer. Comparative Example 4

[0036] The difference between Comparative Example 4 and Example 1 is as follows: During resin synthesis, KBM-503 silane monomer is not added; it is replaced with an equal amount of MMA.

[0037] Do not add KBM-403 silane coupling agent when preparing the adhesive. Comparative Example 5

[0038] The difference between Comparative Example 5 and Example 1 is as follows: When preparing the adhesive, add 0.60g of TDI trimer and only 0.05g of aluminum acetylacetonate (the mass ratio of TDI to aluminum chelating agent is 12:1). Comparative Example 6

[0039] The difference between Comparative Example 5 and Example 1 is as follows: When preparing the adhesive, add 0.3g of TDI trimer and only 0.2g of aluminum acetylacetonate (the mass ratio of TDI to aluminum chelating agent is 1.5:1). Performance testing

[0040] The adhesive tape samples prepared in Examples 1-5 and Comparative Examples 1-6 were subjected to performance tests. The test items and methods are as follows: 1. 180° peel force test Test standard: Refer to GB / T 2792-2014 "Test method for 180° peel strength of pressure sensitive adhesive tape".

[0041] Sample preparation: Cut the tape into samples with a width of 25 mm and a length of 200 mm.

[0042] 1. 180° peel force test Test standard: Refer to GB / T 2792-2014 "Test method for 180° peel strength of pressure sensitive adhesive tape".

[0043] Sample preparation: Cut the tape into samples with a width of 25 mm and a length of 200 mm.

[0044] Test procedure: Using a standard 2.0 kg rubber roller, roll back and forth 3 times on the stainless steel plate (standard SUS304 plate) to be bonded at a speed of approximately 300 mm / min. After bonding, let stand for 20 min in a standard environment (23℃±3℃).

[0045] Test conditions: Fix the stainless steel plate on a tensile testing machine (such as the HT-101 high-speed rail testing instrument), bend the free end of the tape 180° in the opposite direction, peel it off at a tensile speed of 300 mm / min, and record the average tensile force value during the peeling process, expressed in gf / 25mm.

[0046] 2. Tensile strength test Test standard: Refer to GB / T 7753-1987 "Test method for tensile properties of adhesive tapes".

[0047] Sample preparation: Cut the tape into samples with a width of 25 mm and a length of 150 mm, and set the clamping distance to 00 mm.

[0048] Test procedure: Clamp both ends of the specimen in the upper and lower fixtures of the universal tensile testing machine, ensuring that the longitudinal axis of the specimen coincides with the center line of the fixture.

[0049] Test conditions: The specimen is stretched at a tensile speed of 300 mm / min until it breaks. The maximum load (breaking force) at which the specimen breaks is recorded, and the unit is expressed as kgf / 25 mm.

[0050] 3. Initial tack test Test standard: Refer to GB / T 4852-2002 "Test method for initial tack of pressure sensitive adhesive tape (rolling ball method)".

[0051] Testing equipment: Inclined plate initial adhesion tester, with the inclination angle set to 30°.

[0052] Test procedure: Fix the tape with the adhesive side facing up on the inclined plate. At the specified starting point, release the standard steel balls of different groups (1# to 32#) from rest and let them roll down the inclined plane over the surface of the tape.

[0053] Judgment criteria: The number of the largest steel ball (#) that can stop sticking on the adhesive surface of the tape for more than 5 seconds is used as the initial adhesion index of the sample.

[0054] 4. Holding power test Test standard: Refer to GB / T 4851-2014 "Test method for holding power of pressure sensitive adhesive tape".

[0055] Test conditions: The tape was laid flat on a stainless steel plate, with the bonding area controlled at 25 mm × 25 mm. It was rolled three times with a 2.0 kg roller and left to stand for 20 minutes. The steel plate was vertically fixed on the tackiness tester, and a 1.0 kg (10 N) standard weight was suspended from the lower end of the tape. The test environment was maintained at 23℃±2℃ and 50%±5%RH.

[0056] Judgment criteria: The automatic recording of the time (in hours) it takes for the weight to detach from the tape and fall off. If the weight does not fall off after 72 hours, it is recorded as >72 hours.

[0057] 5. Temperature resistance test at 150℃ Test procedure: Cut the tape into 25 mm × 100 mm pieces, apply it flat to a clean stainless steel plate surface using a 2.0 kg pressure roller, let it stand for 20 minutes, and then hang it vertically in a precision forced-air drying oven at 150℃.

[0058] Test conditions: After heating at 150℃ for 60 minutes, remove and cool to room temperature.

[0059] Judgment criteria: Visually inspect the edges of the tape for warping, bulging, displacement, or detachment. After peeling, observe the surface of the steel plate for any residual adhesive. Requirements: no detachment, no edge warping, and no residual adhesive.

[0060] 6. Electrolyte resistance test Test sample: The tape (25 mm × 100 mm) is flatly applied to the clean surface of rolled copper foil and battery-grade aluminum foil, and compacted with a 2.0 kg pressure roller to ensure that no air bubbles remain.

[0061] Test conditions: The copper / aluminum foil with tape was completely immersed in a sealed fluoroplastic bottle containing standard lithium battery electrolyte (electrolyte formula: 1.0M LiPF6 / EC+DMC+EMC = 1:1:1 v / v, water content < 20 ppm), and then placed in an 85℃ constant temperature drying oven for 24 h to soak.

[0062] Criteria for judgment: Appearance and detachment: After removal, observe whether the tape has curled edges, bubbles, or has detached from the metal foil; Discoloration and dissolution: Observe whether the electrolyte solution is cloudy or discolored (such as turning yellow), and whether the tape substrate and adhesive layer fade or change color.

[0063] The test results of Examples 1-5 and Comparative Examples 1-6 are shown in Table 1.

[0064] Table 1

[0065] Please refer to Table 1. The tape samples in Examples 1-5 all exhibited excellent high temperature resistance and resistance to electrolyte at 85°C.

[0066] The tape sample in Comparative Example 1 lacked fluorinated monomer copolymerization, which prevented it from self-assembling on the adhesive surface to form a highly hydrophobic / solvent-repellent barrier layer, resulting in rapid electrolyte penetration and severe swelling and peeling.

[0067] In Comparative Example 2, the tape sample used ordinary hydrogenated rosin resin. After being immersed in electrolyte at 85°C for a long time, it was extracted and dissolved by small molecule carbonate solvent, causing the electrolyte to become cloudy and yellow. This verifies the importance of selecting fully hydrogenated alicyclic petroleum resin with a softening point ≥135°C for ensuring the safety of the battery cell.

[0068] The tape sample in Comparative Example 3 only used isocyanate covalent crosslinking and lacked dynamic reversible coordination bonds formed by metal chelating agents. The colloid lacked stress relaxation and network elastic support at a high temperature of 150°C, resulting in creep and detachment, with a holding power of only 16h.

[0069] The tape sample in Comparative Example 4 lacked silane monomer (KBM-503) and added coupling agent (KBM-403). The adhesive layer could not form Si-OM covalent bond anchoring with the copper / aluminum foil electrode surface, and "wet peeling" occurred when immersed in electrolyte, resulting in the tape edge warping and falling off.

[0070] In the tape sample of Comparative Example 5, the mass ratio of TDI to metal chelating agent was as high as 12:1. Due to excessive covalent cross-linking, the internal rigidity of the colloid was too large and the coagulation force was too high, resulting in the loss of polar flow wettability. This caused the peel force to drop sharply to 420 gf / 25mm and almost lost the initial tack.

[0071] In the tape sample of Comparative Example 6, the mass ratio of TDI to metal chelating agent was only 1.5:1. The excessive metal chelating agent over-consumed the polar carboxyl groups (-COOH) on the main chain of acrylic resin, which not only caused a sharp drop in the polar anchoring force of the colloid to the metal interface (peel force only 550 gf / 25mm), but also made the coordination bonds easy to be competitively dissociated by the polar molecules of the electrolyte when immersed in the electrolyte at 85℃, causing wet detachment of the interface.

[0072] The above-described embodiments are merely preferred embodiments provided to fully illustrate the present invention, and the scope of protection of the present invention is not limited thereto. Equivalent substitutions or modifications made by those skilled in the art based on the present invention are all within the scope of protection of the present invention. The scope of protection of the present invention is defined by the claims.

Claims

1. A high electrolyte-resistant modified acrylic pressure-sensitive adhesive, characterized in that, The following raw materials are included in the preparation by mass parts: 100 parts of acrylic copolymer resin; 0.2–0.8 parts of polyisocyanate crosslinking agent; 0.05–0.2 parts of metal chelating crosslinking agent; 0.1 to 1.0 parts of silane coupling agent; 5-15 parts of fully hydrogenated tackifying resin; Antioxidant 0.1–0.5 parts; The mass ratio of the polyisocyanate crosslinking agent to the metal chelate crosslinking agent is 3:1 to 6:

1.

2. The high electrolyte resistance modified acrylic pressure-sensitive adhesive according to claim 1, characterized in that, The acrylic copolymer resin is produced by free radical solution polymerization of the following monomers in the presence of an organic solvent and an initiator: 55-70 parts of acrylic acid soft monomer; 15-25 parts of hard acrylic monomer; 3-8 parts of polar functional monomers; 5-15 parts of electrolyte-resistant special monomer; 0.5 to 2.0 parts of silane coupling monomer containing polymerizable double bonds.

3. The high electrolyte-resistant modified acrylic pressure-sensitive adhesive according to claim 2, characterized in that, The acrylic soft monomer is selected from at least one of isooctyl acrylate, n-butyl acrylate, and isostearate acrylate; The acrylic hard monomer is selected from at least one of methyl methacrylate, isopropyl acrylate, isobornyl acrylate, and cyclohexyl methacrylate.

4. The high electrolyte resistance modified acrylic pressure-sensitive adhesive according to claim 2, characterized in that, The polar functional monomers include carboxyl monomers and hydroxyl monomers; The carboxyl monomer is selected from at least one of acrylic acid and methacrylic acid, and the hydroxyl monomer is selected from at least one of 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; the mass ratio of the carboxyl monomer to the hydroxyl monomer is 1.5:1 to 2.5:

1.

5. The high electrolyte-resistant modified acrylic pressure-sensitive adhesive according to claim 2, characterized in that, The electrolyte-resistant special monomer is selected from at least one of trifluoroethyl acrylate, trifluoroethyl methacrylate, and hexafluoroisopropyl methacrylate.

6. The high electrolyte resistance modified acrylic pressure-sensitive adhesive according to claim 2, characterized in that, The silane coupling monomer containing polymerizable double bonds is γ-(methacryloyloxy)propyltrimethoxysilane.

7. The high electrolyte resistance modified acrylic pressure-sensitive adhesive according to claim 1, characterized in that, The polyisocyanate crosslinking agent is at least one of toluene diisocyanate trimer, diphenylmethane diisocyanate adduct, or hexamethylene diisocyanate biuret. The metal chelating crosslinking agent is at least one of aluminum acetylacetonate and titanium acetylacetonate; The silane coupling agent is γ-glycidoxypropyltrimethoxysilane; The fully hydrogenated tackifying resin is a DCPD fully hydrogenated petroleum resin or a fully hydrogenated terpene resin with a softening point ≥135℃.

8. A high electrolyte-resistant lithium battery tape, characterized in that, From bottom to top, it includes: a polyimide substrate layer, a release layer coated on the back side of the polyimide substrate layer, and a pressure-sensitive adhesive layer coated on the front side of the polyimide substrate layer. The thickness of the polyimide substrate layer is 19–25 μm; The coating thickness of the release layer is 0.2–1.0 μm; The pressure-sensitive adhesive layer is formed by drying, curing and aging the high electrolyte-resistant modified acrylic pressure-sensitive adhesive as described in any one of claims 1 to 7, and the dry adhesive thickness of the pressure-sensitive adhesive layer is 10~25um.

9. A method for preparing a high electrolyte-resistant lithium battery tape as described in claim 8, characterized in that, Includes the following steps: S1. Soft acrylic acid monomers, hard acrylic acid monomers, polar functional monomers, electrolyte-resistant special monomers, and silane coupling monomers containing polymerizable double bonds are dissolved in anhydrous ethyl acetate and reacted at 75–85°C for 6–10 hours under the action of an initiator to obtain an acrylic acid copolymer resin solution with a weight-average molecular weight of 600,000 to 1,000,000. S2. Add the polyisocyanate crosslinking agent, metal chelate crosslinking agent, silane coupling agent, fully hydrogenated tackifying resin and antioxidant to the acrylic copolymer resin solution in proportion, stir for 20 to 40 minutes, adjust the solid content to 30% to 45%, and degas under vacuum to obtain the pressure-sensitive adhesive solution. S3. Apply a release agent to the back of a polyimide substrate with a thickness of 19–25 μm, and dry and cure at 120–140°C to form a release layer with a thickness of 0.2–1.0 μm; S4. The pressure-sensitive adhesive prepared in step S2 is micro-coated on the front side of the polyimide substrate, and the solvent is removed by a gradient temperature-controlled drying tunnel to control the dry adhesive thickness to 10~25um. S5. The coated tape is bonded to the release film and rolled up, and cured in a curing chamber at 45-55°C for 48-72 hours to obtain a high electrolyte-resistant lithium battery tape.

10. The method for preparing the high electrolyte-resistant lithium battery tape according to claim 9, characterized in that, In step S4, the temperature regime of the gradient temperature control oven is as follows: first bake at 80°C for 2 minutes, then bake at 110°C for 1 minute, and finally bake at 130°C for 2 minutes.