A method for preparing yttrium phosphate thin films by cathodic electrodeposition, its products and applications
The preparation of yttrium phosphate and rare earth-doped yttrium phosphate thin films under normal pressure by cathodic electrodeposition solves the problems of high equipment investment and poor controllability in the high-temperature and high-pressure preparation of existing technologies, and realizes low-cost, controllable film preparation and industrial application of high-performance films.
Patent Information
- Application Number
- CN202611261800.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
Existing processes for preparing yttrium phosphate and rare-earth-doped yttrium phosphate films require stringent conditions such as high-temperature heating, high-vacuum sealing, and high-pressure reactions. These processes involve high equipment investment, high costs, and poor process controllability, making it difficult to achieve mass production and industrial applications.
By employing cathodic electrodeposition under normal pressure and controlling electrolyte concentration, pH value, and deposition parameters, yttrium phosphate and rare earth-doped yttrium phosphate nanofilms are prepared. A dense film is formed on the surface of ITO conductive glass using a cathodic reduction reaction, avoiding the use of organic complexing agents and improving process controllability and product consistency.
It has achieved low-cost and controllable thin film preparation. The film is dense and has good crystallinity, making it suitable for industrial production. It also has high-intensity fluorescence properties and wide applicability.
Smart Images

Figure CN123108686A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional nanofilm material preparation technology, specifically relating to a cathodic electrodeposition method for preparing yttrium phosphate films, its products and applications. The prepared film materials can be widely used in high-end optoelectronic technology fields such as optical display devices, photoelectric conversion devices, laser material preparation, biological fluorescent labeling, and fluorescence sensing detection. Background Technology
[0002] Yttrium phosphate is a high-performance inorganic matrix functional material, mostly exhibiting monoclinic or tetragonal crystal structures. It possesses outstanding advantages such as high melting point, high photon yield, excellent optical stability, and intrinsic absence of fluorescence interference, making it an ideal substrate material for rare-earth ion doping modification. Rare-earth-doped yttrium phosphate composites can fully combine the structural stability of the yttrium phosphate matrix with the characteristic fluorescence properties of rare-earth ions, exhibiting excellent optoelectronic coupling performance. It is a core candidate material in fields such as optical displays, precision optoelectronic devices, laser fabrication, and fluorescence sensing.
[0003] Currently, the mainstream preparation processes for yttrium phosphate and rare-earth-doped yttrium phosphate thin films include hydrothermal methods, sol-gel methods, sonochemical methods, chemical precipitation methods, and microemulsion methods. These traditional processes have inherent technical drawbacks: they generally require stringent preparation conditions such as high-temperature heating, high-vacuum sealing, and high-pressure reactions, placing extremely high demands on the precision, airtightness, and high-temperature resistance of experimental equipment, resulting in high equipment investment and energy consumption costs. Furthermore, traditional processes are complex and have poor process controllability, making it impossible to precisely control film thickness, microstructure, and crystallinity, leading to inconsistent product quality and severely limiting the mass production and industrial-scale application of yttrium-based functional thin films.
[0004] Currently, existing reports on the preparation of rare earth phosphate films by electrochemical deposition (such as CN101962805A) employ an anodic oxidation-complex dissociation deposition pathway: in a near-neutral electrolyte, rare earth ions (La)... 3+ It needs to form a stable complex with EDTA, and release H through oxidation with H2O at the anodic potential. + This lowers the pH value at the electrode surface, thereby disrupting the complex structure and releasing free La. 3+ And then with PO4 3+ Combined deposition. This technical route has the following inherent defects: (1) Organic complexing agents such as EDTA must be added, which increases the cost of raw materials and the difficulty of subsequent purification; (2) The anodic reaction is accompanied by O2 precipitation, which easily causes the film to be porous, loose and insufficient in density; (3) The deposition process is constrained by multiple factors of complexation-dissociation equilibrium, the process window is narrow and the controllability is poor.
[0005] Therefore, there is an urgent need for a simple and controllable electrodeposition method for preparing yttrium phosphate and rare earth-doped yttrium phosphate thin films. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of existing yttrium phosphate and rare earth-doped yttrium phosphate thin film preparation processes, such as stringent conditions, expensive equipment, poor process controllability, and difficulty in large-scale production. This invention provides a simple, low-cost, parameter-controllable, and product-stable cathode electrodeposition method that can efficiently prepare yttrium phosphate and rare earth-doped yttrium phosphate nanofunctional thin films with uniform morphology, excellent crystallinity, and superior fluorescence performance.
[0007] To achieve the above-mentioned objectives, the present invention adopts the following technical solution:
[0008] In a first aspect, the present invention provides a method for preparing a yttrium phosphate thin film by cathodic electrodeposition, comprising:
[0009] 1) Pre-treat the surface of the ITO conductive glass to serve as a conductive substrate;
[0010] 2) Prepare an aqueous solution of yttrium ions with a concentration of 0.005–0.5 mol / L and adjust the pH to acidity; then add an ammonium dihydrogen phosphate solution with a concentration of 0.01–1 mol / L to the solution, stir well, and adjust the pH of the solution to acidity to obtain the yttrium phosphate electrodeposition electrolyte;
[0011] 3) Construct a three-electrode electrochemical deposition system. Use the conductive substrate obtained in step 1) as the working electrode, the platinum electrode as the counter electrode, and the Ag / AgCl electrode as the reference electrode. Immerse the three-electrode electrochemical deposition system in the yttrium phosphate electrodeposition electrolyte obtained in step 2). Under normal pressure, control the deposition temperature at 20-80℃ and the cathode deposition potential relative to the Ag / AgCl electrode at -0.6--1.1 V for isothermal and isoelectric deposition. After deposition, remove the conductive substrate, clean and dry it to obtain a dense yttrium phosphate film with nanoparticles.
[0012] Preferably, the pretreatment in step 1) includes: degreasing with organic solvents, ultrasonic removal of impurities with pure water, activation with dilute nitric acid, rinsing with pure water and drying, to thoroughly remove impurities from the substrate surface, activate the conductive interface, effectively improve the adhesion between the film and the ITO substrate, and avoid film detachment and cracking defects.
[0013] During electrolyte preparation, a stable yttrium-phosphate coordination system is constructed by precisely controlling the pH value step by step, which effectively avoids electrolyte precipitation and stratification problems, and ensures the continuity and stability of the electrodeposition process.
[0014] The cathode electrodeposition process adopts a standardized three-electrode system. By dividing multiple temperature and potential parameter ranges, it can prepare ultra-thin uniform films, high-flatness general-purpose films, and high-crystallinity and high-strength films to meet the needs of different applications. The process is highly adaptable.
[0015] Preferably, in step 3), the deposition temperature is selected from any one of the temperature ranges of 20–40°C, 40–60°C, or 60–80°C; and the cathode deposition potential is selected from any one of the potential ranges of -0.6–-0.9V, -0.9–-1.0V, or -1.0–-1.1V (relative to the Ag / AgCl electrode).
[0016] Preferably, in step 3), the isothermal and constant potential deposition time is 60 to 180 min.
[0017] Preferably, in step 2), the yttrium ion aqueous solution is an yttrium nitrate aqueous solution.
[0018] Preferably, in step 2), the electrolyte is a rare earth-doped electrolyte, which is prepared by mixing a yttrium nitrate solution with a concentration of 0.005–0.5 mol / L and a europium nitrate solution with a concentration of 0.0001–0.1 mol / L evenly, adjusting the pH to acidic, then adding an ammonium dihydrogen phosphate solution with a concentration of 0.01–1 mol / L, stirring evenly, and adjusting the pH of the solution to acidic to obtain a rare earth europium-doped electrodeposition electrolyte.
[0019] Preferably, the molar ratio of europium nitrate to yttrium nitrate is 0.0002:1 to 0.2:1.
[0020] Preferably, when the electrolyte is a rare earth-doped electrolyte, the isothermal and constant potential deposition time in step 3) is 60 to 180 minutes to obtain a rare earth europium-doped yttrium phosphate film.
[0021] Preferably, in step 2), the pH value is adjusted to 1.1 to 1.5 for the first time and to 1.2 to 1.5 for the second time.
[0022] This method enables uniform doping of rare earth ions within the yttrium phosphate lattice, effectively avoiding rare earth ion aggregation and segregation problems, maximizing the excitation of rare earth ion fluorescence characteristics, and obtaining functional thin films with excellent morphology and stable fluorescence performance. This invention utilizes a cathodic reduction method to electrodeposit YPO4:Eu thin films. In acidic solution, when the deposition potential is less than -0.8 V vsAg / AgCl, O2 and NO... 3- and H + The reduction causes the pH value on the ITO electrode surface to increase, Y3 + Eu 3+ and PO4 produced by hydrolysis 3- Combine to form YPO4:Eu 3+ It is deposited on the surface of ITO conductive glass. The reaction mechanism is as follows:
[0023] O2 + 4H + + 4e- →2H2O (1)
[0024] NO3 3- +2H + +e - →NO2 + H2O (2)
[0025] 2H + + 2e - → H2 (3)
[0026] H2PO4 - + 2OH - →2H2O + PO4 3- (4)
[0027] Y 3+ + PO4 3- →YPO4 ↓ (5)
[0028] Eu 3+ + PO4 3- →EuPO4 ↓ (6)
[0029] Secondly, the present invention provides a yttrium rare earth doped thin film, which is prepared by the above method.
[0030] Thirdly, the present invention provides the application of the above-mentioned yttrium rare earth doped thin film in optical display devices, photoelectric conversion devices, laser materials, biological fluorescent labels or fluorescent sensors.
[0031] Compared with the prior art, the present invention has the following significant advantages:
[0032] 1. Mild process conditions and wide adaptability: The entire process of this invention is completed in a low temperature and normal pressure environment, without the need for harsh process conditions such as high temperature sintering, high pressure reaction, and high vacuum sealing. This greatly reduces the investment in special equipment and production energy consumption. The operation is safe and simple, which can meet the needs of precise laboratory research and development, and can also be adapted to large-scale industrial mass production.
[0033] 2. Low production cost and high efficiency: The raw materials used in this invention are readily available and the proportions are flexible and controllable. The preparation equipment has a simple structure and low maintenance cost. The electrodeposition rate is fast and the preparation cycle is short. The production efficiency is much higher than that of traditional preparation processes, and it has excellent industrialization economic benefits.
[0034] 3. Excellent product performance and high consistency: The pure yttrium phosphate film prepared by this invention has a regular microstructure, with a uniform and dense nanoparticle structure, high crystal purity, good structural stability, and strong adhesion to the substrate; the rare earth europium doped film has no ion agglomeration or segregation defects, and the rare earth ions are uniformly dissolved in the film lattice, which has stable and high-intensity characteristic fluorescence emission performance and excellent optical consistency.
[0035] 4. Strong process controllability and high scalability: This invention can precisely control the film thickness, microstructure, crystallization performance and fluorescence performance by simply adjusting parameters such as electrolyte concentration, rare earth doping ratio, deposition temperature and deposition potential. It can be adapted to the differentiated application needs of multiple fields such as optical display, photoelectric detection, laser materials, and biological fluorescent labeling. The technology has extremely high scalability and application value. Attached Figure Description
[0036] Figure 1 The images shown are field emission scanning electron microscope (SEM) images of the 5% europium yttrium doped thin film prepared in Example 6 of this invention; where a is a scanning electron microscope image magnified 5000 times with a scale bar of 2 μm; and b is a scanning electron microscope image magnified 20000 times with a scale bar of 500 nm.
[0037] Figure 2 The X-ray diffraction pattern of the 5% europium yttrium doped thin film prepared in Example 6 of this invention;
[0038] Figure 3 The fluorescence emission spectrum of the 5% europium yttrium doped thin film prepared in Example 6 of this invention is shown below.
[0039] Figure 4 This is a comparison of the emission colors of the 5% europium yttrium phosphate thin film prepared in Example 6 of the present invention before and after excitation by 395 nm light.
[0040] Figure 5 The fluorescence lifetime test results of the 5% europium yttrium phosphate thin film prepared in Example 6 of the present invention after excitation by 395 nm light are shown, where a is the fluorescence lifetime at 593 nm and b is the fluorescence lifetime at 620 nm; the average times are 2.67 ms and 2.72 ms, respectively. Detailed Implementation
[0041] The technical solution will now be described in detail and completely with reference to preferred embodiments of the present invention. These described embodiments are only some, not all, of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0042] Example 1: Low-temperature preparation of ultrathin uniform yttrium phosphate films
[0043] 1) Substrate pretreatment: Clean the ITO conductive glass twice with acetone to remove surface oil and organic impurities; ultrasonically clean the ITO conductive glass in deionized water for 10 minutes to remove surface dust and attached impurities; activate the conductive surface by immersing it in a 10% nitric acid solution for 10 seconds; rinse thoroughly with deionized water and air dry at room temperature for later use.
[0044] 2) Electrolyte preparation: Prepare a 0.005 mol / L yttrium ion aqueous solution and adjust the pH of the solution to 1.3; add a 0.01 mol / L ammonium dihydrogen phosphate solution, stir continuously until homogeneous, and adjust the pH of the system to 1.5 again to obtain a stable yttrium phosphate electrodeposition electrolyte;
[0045] 3) Cathodic electrodeposition: A three-electrode electrochemical system was constructed, with pretreated ITO conductive glass as the working electrode, a platinum electrode as the counter electrode, and Ag / AgCl as the reference electrode. The three-electrode system was immersed in the electrolyte. The cathode deposition potential was controlled at -0.6 and the deposition temperature at 30℃. The deposition was carried out at ambient pressure, constant temperature and constant potential for 120 min. After deposition, the substrate was removed, washed with deionized water, and dried at room temperature to obtain an ultrathin, uniform, defect-free nanoparticle yttrium phosphate film.
[0046] Example 2: High-Temperature Preparation of Highly Crystalline Yttrium Phosphate Thin Films
[0047] 1) Substrate pretreatment: ITO conductive glass was cleaned with acetone 3 times, ultrasonically cleaned with deionized water for 30 min, activated with 10% nitric acid solution for 30 s, rinsed with deionized water and air-dried at room temperature for later use.
[0048] 2) Electrolyte preparation: Prepare a 0.5 mol / L yttrium ion aqueous solution and adjust the pH to 1.3; add a 1 mol / L ammonium dihydrogen phosphate solution, stir evenly, and then precisely adjust the pH to 1.4 to obtain the yttrium phosphate electrodeposition electrolyte;
[0049] 3) Cathodic electrodeposition: A three-electrode system was constructed, and the cathode deposition potential was controlled at -1.0V and the deposition temperature at 80℃. The deposition was carried out under constant temperature and potential at ambient pressure for 60 min. After cleaning and drying, a thick yttrium phosphate film with high crystallinity and high structural stability was obtained.
[0050] Example 3: Preparation of Yttrium Phosphate Thin Films with Optimal Overall Performance at Medium Temperature
[0051] 1) Substrate pretreatment: ITO conductive glass was cleaned twice with acetone, ultrasonically cleaned with deionized water for 15 min, activated with 10% nitric acid solution for 15 s, rinsed with deionized water and dried for later use.
[0052] 2) Electrolyte preparation: Prepare a 0.01 mol / L yttrium ion aqueous solution, adjust the pH to 1.3, add a 0.02 mol / L ammonium dihydrogen phosphate solution, stir evenly, and then adjust the pH to 1.5 to obtain a stable electrolyte;
[0053] 3) Cathodic electrodeposition: By controlling the deposition potential to -0.9V and the deposition temperature to 50℃, and depositing at a constant temperature and potential for 120 min, a yttrium phosphate functional film with optimal synergistic smoothness, density and crystallinity was prepared.
[0054] Example 4: Low-doped uniform europium-doped yttrium phosphate fluorescent thin film
[0055] 1) Substrate pretreatment: Same as the pretreatment process in Example 1;
[0056] 2) Preparation of doped electrolyte: Prepare a 0.005 mol / L yttrium nitrate solution, add a 0.0001 mol / L europium nitrate solution, stir and mix thoroughly, and adjust the pH value to 1.3; add a 0.01 mol / L ammonium dihydrogen phosphate solution, and adjust the pH value to 1.5 again to obtain a low-doped rare earth doped electrolyte;
[0057] 3) Cathode electrodeposition: The deposition potential was controlled at -0.6V and the deposition temperature at 30℃. The deposition was carried out at a constant temperature and potential for 180 min to obtain a low-concentration europium-doped yttrium phosphate fluorescent film with uniform doping and no agglomeration defects.
[0058] Example 5: Europium-doped yttrium phosphate thin film with high fluorescence intensity
[0059] 1) Substrate pretreatment: Same as the pretreatment process in Example 2;
[0060] 2) Preparation of doped electrolyte: Prepare a 0.5 mol / L yttrium nitrate solution, add a 0.1 mol / L europium nitrate solution, stir well and adjust the pH to 1.3; add a 1.2 mol / L ammonium dihydrogen phosphate solution and adjust the pH to 1.45 to obtain a high-concentration doped electrolyte;
[0061] 3) Cathodic electrodeposition: By controlling the deposition potential to -1.0V and the deposition temperature to 80℃, and performing isothermal and constant potential deposition for 90 min, a rare earth-doped functional thin film with excellent crystallinity and high fluorescence emission intensity was prepared.
[0062] Example 6: High-stability europium-doped yttrium phosphate thin film with moderate doping
[0063] 1) Substrate pretreatment: Same as the pretreatment process in Example 3;
[0064] 2) Preparation of doped electrolyte: Prepare a 0.01 mol / L yttrium nitrate solution, add a 0.001 mol / L europium nitrate solution, stir well and adjust the pH to 1.3; add a 0.02 mol / L ammonium dihydrogen phosphate solution and adjust the pH to 1.46 to obtain a medium-concentration stable doped electrolyte;
[0065] 3) Cathodic electrodeposition: The deposition potential was controlled at -0.9V and the deposition temperature at 50℃. The deposition was carried out at a constant temperature and potential for 120 min to obtain a highly stable doped film with highly synergistic morphology, crystallinity and fluorescence properties.
[0066] Performance test analysis
[0067] Systematic performance characterization was performed on the films prepared in Examples 1-6 of this invention: Field emission scanning electron microscopy (FE-SEM) tests showed that all sample films were uniformly dense, free of pores, detachment, and cracks, exhibiting a regular nanoparticle microstructure; X-ray diffraction (XRD) tests confirmed that the pure yttrium phosphate film had a high-purity tetragonal crystal structure without impurity phase formation. The crystal structure of the film did not change after rare earth doping, and the dopant ions successfully dissolved into the crystal lattice. Based on the Scherrer equation, the grain size of the film was calculated to be approximately 30 nm, and the SEM results also corroborated that the nanoparticles ranged from 20 to 50 nm. The FE-SEM image, X-ray diffraction pattern, and fluorescence emission spectrum of the 5% europium-doped yttrium phosphate film prepared in Example 6 are shown below. Figure 1 , Figure 2 , Figure 3 As shown.
[0068] Fluorescence emission spectroscopy (PL) test results are as follows Figure 5 , Figure 5 The results show that the europium-doped yttrium phosphate thin film prepared by this invention exhibits a clear and stable characteristic fluorescence emission peak of europium ions under 395 nm excitation light, with good luminescence uniformity and high intensity. Optical comparison experiments show that the film has significant color difference before and after ultraviolet light excitation, the luminescence effect is intuitive, and the fluorescence response performance is excellent. Meanwhile, the film prepared by the hydrothermal method was tested, and its fluorescence lifetime was 2.29 ms, with a calculated quantum yield of 45%, indicating that the method of this invention is superior.
[0069] Thin films prepared with different process parameters exhibit significant performance differences, allowing for precise matching of application requirements in various scenarios: low-temperature, low-potential processes are suitable for high-precision ultrathin optical films, medium-temperature, medium-potential processes are suitable for general-purpose stable functional films, and high-temperature, high-potential processes are suitable for highly crystalline, high-brightness optoelectronic functional films. The process control is highly flexible and practical.
[0070] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, or improvements made to the process parameters, raw material ratios, and doping systems of the present invention within the spirit and principles of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing a yttrium phosphate thin film by cathodic electrodeposition, characterized in that, Includes the following steps: 1) Pre-treat the surface of the ITO conductive glass to serve as a conductive substrate; 2) Prepare an aqueous solution of yttrium ions with a concentration of 0.005–0.5 mol / L and adjust the pH to acidity; then add an ammonium dihydrogen phosphate solution with a concentration of 0.01–1 mol / L to the solution, stir well, and adjust the pH of the solution to acidity to obtain the yttrium phosphate electrodeposition electrolyte; 3) Construct a three-electrode electrochemical deposition system. Use the conductive substrate obtained in step 1) as the working electrode, the platinum electrode as the counter electrode, and the Ag / AgCl electrode as the reference electrode. Immerse the three-electrode electrochemical deposition system in the yttrium phosphate electrodeposition electrolyte obtained in step 2). Under normal pressure, control the deposition temperature at 20-80℃ and the cathode deposition potential relative to the Ag / AgCl electrode at -0.6--1.1 V to perform isothermal and isoelectric deposition. After deposition, the conductive substrate is removed, cleaned, and dried to obtain a yttrium phosphate film.
2. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 1, characterized in that, Step 1) The pretreatment includes: degreasing with organic solvents, ultrasonic removal of impurities with pure water, activation with dilute nitric acid, rinsing with pure water, and drying.
3. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 2, characterized in that, In step 3), the deposition temperature is selected from any temperature range of 20-40℃, 40-60℃, or 60-80℃; the cathode deposition potential is selected from any potential range of -0.6--0.9V, -0.9--1.0V, or -1.0--1.1V.
4. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 3, characterized in that, In step 3), the isothermal and constant potential deposition time is 60 to 180 minutes.
5. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 4, characterized in that, In step 2), the yttrium ion aqueous solution is an yttrium nitrate aqueous solution.
6. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 4, characterized in that, In step 2), the electrolyte is a rare earth-doped electrolyte, which is prepared by mixing a yttrium nitrate solution with a concentration of 0.005–0.5 mol / L and a europium nitrate solution with a concentration of 0.0001–0.1 mol / L evenly, adjusting the pH to acidic, then adding an ammonium dihydrogen phosphate solution with a concentration of 0.01–1 mol / L, stirring evenly, and adjusting the pH of the solution to acidic to obtain a rare earth europium-doped electrodeposition electrolyte; in step 3), the isothermal and constant potential deposition time is 60–180 min to obtain a rare earth europium-doped yttrium phosphate film.
7. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 1, characterized in that, The molar ratio of europium nitrate to yttrium nitrate is 0.0002:1 to 0.2:
1.
8. The method for preparing yttrium phosphate thin films by cathodic electrodeposition according to claim 6, characterized in that, In step 2), the pH value is adjusted to 1.1-1.5 for the first time and to 1.2-1.5 for the second time.
9. A yttrium rare earth-doped thin film, prepared by the method described in any one of claims 6-8.
10. The application of the yttrium rare earth doped thin film as described in claim 9 in optical display devices, photoelectric conversion devices, laser materials, biofluorescent labeling, or fluorescence sensing.
Citation Information
Patent Citations
Electrochemical preparation method of lanthanum phosphate or rare earth doped lanthanum phosphate film
CN101962805A