An iron oxide-coated carbon aerogel composite material, its preparation method and application

By coating the surface of MOFs-derived carbon aerogel with iron oxide, an iron oxide-coated carbon aerogel composite material was prepared, which solved the capacity and fast-charging performance problems of existing lithium-ion battery anode materials and improved the electrochemical performance and cycle stability of the material.

CN123120604APending Publication Date: 2026-11-17SOOCHOW MOFS SCI & TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611276912.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The theoretical specific capacity of graphite, an existing lithium-ion battery anode material, is low. Under fast charging conditions, the diffusion kinetics of lithium ions are limited, which easily leads to lithium dendrite deposition. Furthermore, the intrinsic conductivity and interfacial reactivity of MOFs-derived carbon aerogels are insufficient, which restricts the improvement of their electrochemical performance.

Method used

Iron oxide-coated carbon aerogel composites were prepared by coating the surface of MOFs-derived carbon aerogels with iron oxide, thereby constructing a stable SEI film, regulating interfacial reactions, and improving the conductivity and cycle stability of the materials.

Benefits of technology

It achieves a balance between high specific surface area and pore size, enhances the cycling stability and electrochemical performance of the material, improves the first coulombic efficiency and rate performance, and inhibits the irreversible decomposition of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120604A_ABST
    Figure CN123120604A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of lithium-ion battery anode materials, and more specifically relates to an iron oxide-coated carbon aerogel composite material, its preparation method, and its application. This invention coats the surface of MOF-derived carbon aerogel with an iron oxide layer. The iron oxide regulates the interface between the carbon aerogel and the electrolyte, constructing a stable SEI film, inhibiting continuous electrolyte decomposition, reducing irreversible lithium loss, and improving the material's initial coulombic efficiency, rate performance, and cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of lithium-ion battery anode material technology, and more specifically relates to an iron oxide-coated carbon aerogel composite material, its preparation method and application. Background Technology

[0002] Faced with the dual challenges of fossil fuel depletion and ecological degradation, lithium-ion batteries, with their superior energy density and environmental compatibility, have become an indispensable core energy storage technology in modern society. However, the graphite anode widely used in commercial lithium-ion batteries currently has a theoretical specific capacity of only 372 mAh / g, which is insufficient to meet the needs of future high-energy-density energy storage devices. At the same time, the small interlayer spacing of graphite (0.335 nm) restricts lithium-ion diffusion kinetics under fast charging conditions, easily leading to lithium dendrite deposition and posing safety hazards.

[0003] Metal-organic framework (MOF)-derived carbon aerogels exhibit large reversible capacity and excellent cycle stability in the field of lithium-ion battery anodes due to their combination of high specific surface area, tunable porous structure, and stable three-dimensional carbon framework network. However, the insufficient intrinsic conductivity and limited interfacial reactivity of MOF-derived carbon aerogels restrict further improvement in their electrochemical performance.

[0004] Therefore, developing novel anode materials that combine high capacity and high rate performance is of great significance. Summary of the Invention

[0005] The purpose of this invention is to provide an iron oxide-coated carbon aerogel composite material, its preparation method, and its application, so as to solve the problems existing in the prior art.

[0006] To achieve the above objectives, the present invention provides the following solution: One of the technical solutions of this invention: provides a method for preparing an iron oxide-coated carbon aerogel composite material, comprising the following steps: Iron salts were dissolved in water to prepare an iron salt solution. Carbon aerogel was added and stirred to disperse the solution. While stirring, alkali solution was added dropwise to adjust the pH to 7-8 (so that iron hydroxide was generated in situ and coated on the carbon aerogel). Stirring was continued, followed by washing, drying, and calcination (the pyrolysis of iron hydroxide into iron oxide) to obtain an iron oxide-coated carbon aerogel composite material.

[0007] Furthermore, the iron salt includes at least one of ferric chloride hexahydrate, ferrous chloride tetrahydrate, and ferric nitrate nonahydrate.

[0008] Furthermore, the carbon aerogel is a MOF-derived carbon aerogel.

[0009] Furthermore, the mass ratio of the iron salt to the carbon aerogel is 0.03~0.04:0.2, preferably 0.0313:0.2.

[0010] Furthermore, the amount of iron salt and water used is 0.03~0.04 g: 4~6 mL, preferably 0.0313 g: 5 mL.

[0011] Furthermore, the stirring and dispersion time is 20-40 min, preferably 30 min.

[0012] Furthermore, the alkaline solution is ammonia water with a concentration of 25-28 wt%.

[0013] Furthermore, the stirring time is 20-40 minutes, preferably 30 minutes.

[0014] Furthermore, the drying temperature is 50~70 ℃, and the time is 10~14 h.

[0015] Optionally, the drying temperature is 60 °C and the time is 12 h.

[0016] Furthermore, the calcination heating rate is 3~8 ℃ / min, the temperature is 250~350 ℃ (within this temperature range, there will be no incomplete decomposition of iron salts and no residues, nor will high-oxidation-state iron oxides be generated to destroy the porous framework of carbon aerogel), the time is 1~3 h, and the atmosphere is an inert atmosphere (nitrogen or argon).

[0017] Optionally, the calcination heating rate is 5 °C / min, the temperature is 300 °C, and the time is 2 h.

[0018] The second technical solution of the present invention provides an iron oxide-coated carbon aerogel composite material, which is prepared by the above preparation method.

[0019] The third technical solution of the present invention provides an application of the above-mentioned iron oxide-coated carbon aerogel composite material as an active ingredient in the preparation of lithium-ion battery electrodes.

[0020] The fourth technical solution of the present invention provides an electrode, wherein the active component of the electrode is the above-mentioned iron oxide-coated carbon aerogel composite material.

[0021] Fifth technical solution of the present invention: A lithium-ion battery is provided, wherein the lithium-ion battery uses the above-mentioned electrode as the negative electrode.

[0022] The present invention discloses the following technical effects: The iron oxide-coated carbon aerogel composite material provided by this invention uses MOFs-derived carbon aerogel. This MOFs-derived carbon aerogel maintains a large interlayer spacing while possessing a larger pore size than traditional carbon materials, and its stable structure ensures ultra-long cycling stability. Based on this, by coating the surface of the MOFs-derived carbon aerogel with an iron oxide layer, the iron oxide regulates the interface between the carbon aerogel and the electrolyte, constructing a stable SEI film, inhibiting continuous electrolyte decomposition, reducing irreversible lithium loss, and improving the material's initial coulombic efficiency, rate performance, and cycling stability.

[0023] The iron oxide-coated carbon aerogel composite material provided by this invention has both high specific surface area and iron oxide surface activity, and the material has excellent electrochemical performance. Attached Figure Description

[0024] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 The image shows a SEM image of the iron oxide-coated carbon aerogel prepared in Example 1.

[0025] Figure 2 The CV curve of the iron oxide-coated carbon aerogel of Example 1 is shown at a scan rate of 0.1 mV / s.

[0026] Figure 3 The image shows the EIS impedance spectrum of the iron oxide-coated carbon aerogel from Example 1.

[0027] Figure 4 This is a comparison chart of the rate performance of iron oxide-coated carbon aerogel (iron-coated carbon aerogel) and MOFs-derived carbon aerogel in Example 1.

[0028] Figure 5 This is a comparison chart of the long-cycle performance of electrodes prepared in Example 1 using iron oxide-coated carbon aerogel (iron-coated carbon aerogel) and MOFs-derived carbon aerogel (MOFs-derived carbon aerogel in step S1) at a rate of 0.5C. Detailed Implementation

[0029] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0030] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Any stated value or intermediate value within a stated range, as well as each smaller range between any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0031] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0032] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0033] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0034] Unless otherwise specified, all raw materials and reagents involved in the specific embodiments of this invention are commercially available products.

[0035] The MOFs-derived carbon aerogel used in the specific embodiments of the present invention is the MOFs-derived carbon aerogel of Suzhou Maofushi Technology Co., Ltd.

[0036] Unless otherwise specified, room temperature and normal temperature in the specific embodiments of the present invention refer to 20-30℃.

[0037] It should be noted that any aspects not described in detail in this invention are conventional practices in the field and are not the focus of this invention.

[0038] Example 1 The preparation steps of iron oxide-coated carbon aerogel composite materials include: S1. Preparation of ferric hydroxide-coated carbon aerogel: Weigh 0.2 g of MOFs-derived carbon aerogel, dissolve 0.0313 g of ferric chloride hexahydrate in 5 mL of deionized water to prepare an iron salt solution, add the MOFs-derived carbon aerogel and stir at room temperature for 30 min to disperse it fully. Then, while stirring, add ammonia water (25 wt%) dropwise to adjust the pH to between 7 and 8, so that iron is generated in situ and coated on the MOFs-derived carbon aerogel. After stirring for 30 min, wash with deionized water and dry under vacuum at 60 °C for 12 h to obtain ferric hydroxide-coated carbon aerogel powder.

[0039] S2. Preparation of iron oxide-coated carbon aerogel composite material: The iron hydroxide-coated carbon aerogel powder prepared in step S1 was calcined in a tube furnace under nitrogen atmosphere at a temperature of 5 °C / min to 300 °C and held for 2 h. The iron hydroxide was pyrolyzed into iron oxide to obtain the iron oxide-coated carbon aerogel composite material.

[0040] Test case Figure 1 The image shows a SEM image of the iron oxide-coated carbon aerogel prepared in Example 1. As can be seen from the image, the material retains the typical three-dimensional cross-linked hierarchical porous carbon skeleton of carbon aerogel. The sheet-like wrinkled carbon matrix overlaps to form a continuous conductive network. A large number of high-contrast iron oxide-based nanoparticles are uniformly attached and embedded on the surface of the carbon matrix and the inner wall of the pores, without obvious agglomeration or clumping. The overall structure presents a loose and porous composite microstructure.

[0041] The materials prepared in the examples and comparative examples were used as active materials in the preparation of lithium-ion battery anodes: The active material, binder (CMC:SBR=2:1) ​​and superconducting carbon black were mixed in a mass ratio of 68:22:10 to obtain a slurry. The slurry was then uniformly coated onto copper foil using a coater to a thickness of 100 micrometers. The coating was then dried in a vacuum oven at 120 °C for 12 h and cut into electrode sheets with a diameter of 13 mm to obtain the negative electrode of the lithium-ion battery.

[0042] The lithium-ion battery negative electrode prepared above was used as the working electrode. PP was used as the separator, and lithium metal sheet was used as the counter electrode. The electrolyte was 1.0 mol / L lithium hexafluorophosphate (LiPF6) dissolved in a mixed solvent system of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1. Simultaneously, 10.0% (v / v) of fluoroethylene carbonate (FEC) and 1.0% (v / v) of vinylene carbonate (VC) were added as functional additives. A coin cell was assembled in a glove box filled with high-purity argon.

[0043] The electrochemical performance of the coin cells prepared above was measured at room temperature using a Shanghai Chenhua electrochemical workstation (CHI660E) and a Blue Electric system. The results are as follows: Figures 2-5 As shown.

[0044] The electrochemical characterization (CV) of iron oxide-coated carbon aerogel was performed using a Shanghai Chenhua CHI660E electrochemical workstation at a scan rate of 0.1 mV / s. The test results are as follows: Figure 2 As shown.

[0045] Figure 2 The figure shows the CV curves of the iron oxide-coated carbon aerogel of Example 1 at a scan rate of 0.1 mV / s. As can be seen from the figure, except for the irreversible process of the electrode material in the first scan (mainly due to the formation of the SEI film and the decomposition of the electrolyte), there were no significant changes in the second and third scans, demonstrating good cycling stability and reversibility.

[0046] Electrochemical impedance spectroscopy (EIS) was performed using a Shanghai Chenhua CHI660E electrochemical workstation. The test results are as follows: Figure 3 As shown.

[0047] Figure 3 The image shows the EIS impedance spectrum of the iron oxide-coated carbon aerogel from Example 1. As can be seen from the figure, the low-frequency region exhibits a steeply sloping line, representing the ion diffusion process, while the mid-frequency region shows a distinct semicircle, corresponding to charge transfer impedance. The low charge transfer impedance of this iron oxide-coated carbon aerogel electrode indicates low charge transport resistance at the material interface and excellent electrode interface dynamics.

[0048] The performance of two materials, iron oxide-coated carbon aerogel and MOFs-derived carbon aerogel (MOFs-derived carbon aerogel in step S1), was compared using rate charge-discharge tests. The test results are as follows: Figure 4 As shown.

[0049] Figure 4 This is a comparison of the rate performance of iron oxide-coated carbon aerogel and MOFs-derived carbon aerogel in Example 1. As can be seen from the figure, both materials exhibit extremely high initial discharge specific capacity during the first discharge cycle, with the MOFs-derived carbon aerogel achieving a first-cycle discharge capacity of 2970.45 mAh g⁻¹. -1 The initial discharge of iron oxide-coated carbon aerogel was 3036.85 mAh g. -1 The irreversible capacity in the first cycle originates from the formation of the SEI film and the decomposition of the electrolyte. During the test, the specific capacity of both materials decreased to some extent at high rates, but the discharge specific capacity of the iron oxide-coated carbon aerogel was consistently higher than that of the MOF-derived carbon aerogel. Under a high current charge-discharge of 5C, the iron oxide-coated carbon aerogel could achieve a discharge capacity of 800 mAh g. -1The reversible capacity is around 100 mAh / g, while MOF-derived carbon aerogels only have 700 mAh / g. -1 The reversible capacity of the iron oxide-coated carbon aerogel, even when returning to a current of 0.1C, still maintains approximately 1800 mAh g⁻¹. -1 The reversible capacity fully demonstrates that the iron oxide-coated modified carbon aerogel remains intact even after a large current passes through it, exhibiting excellent rate performance.

[0050] Long-cycle charge-discharge tests were conducted on iron oxide-coated carbon aerogel (iron-coated carbon aerogel) and MOFs-derived carbon aerogel (MOFs-derived carbon aerogel in step S1) electrodes at a 0.5C rate. The test results are as follows: Figure 5 As shown.

[0051] Figure 5 This figure compares the long-cycle performance of electrodes prepared in Example 1 using iron oxide-coated carbon aerogel (iron-coated carbon aerogel) and MOFs-derived carbon aerogel (MOFs-derived carbon aerogel in step S1) at 0.5C rate. As can be seen from the figure, both materials exhibit high initial discharge specific capacity in the first cycle, with the iron oxide-coated carbon aerogel reaching a first-cycle discharge specific capacity of 3000 mAh g⁻¹. -1 The MOF-derived carbon aerogel exhibits an initial discharge specific capacity of approximately 2900 mAh g. -1 The initial efficiency (IQ) of iron oxide-coated carbon aerogel reached 84.4%, while that of MOF-derived carbon aerogel was only 67.39%. In subsequent cycles, the capacity of iron oxide-coated carbon aerogel was consistently higher than that of MOF-derived carbon aerogel. These results indicate that iron oxide coating modification can effectively improve the IQ of carbon aerogel and enhance the reversible capacity of the electrode.

[0052] The comparison results above show that this invention, through the design and synthesis of iron oxide-coated carbon aerogel and its preparation via calcination-pyrolysis, utilizes the prepared iron oxide-coated carbon aerogel as a negative electrode. The performance in terms of CV, impedance, rate charge-discharge, and constant current charge-discharge was then tested. In summary, this invention provides a simple method for modifying carbon aerogel materials and offers a new approach for improving lithium-ion batteries using carbon aerogel as the negative electrode.

[0053] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.

[0054] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing an iron oxide-coated carbon aerogel composite material, characterized by the steps of The application relates to a preparation method of an iron oxide coated carbon aerogel composite material. The iron salt is dissolved in water to form an iron salt solution, and the carbon aerogel is dispersed by stirring after being added into the solution; an alkali solution is added dropwise under stirring to adjust the pH value to 7-8; the stirring is continued; and then the iron oxide coated carbon aerogel composite material is obtained through washing, drying and calcination.

2. The production method according to claim 1, wherein The iron salt comprises at least one of ferric chloride hexahydrate, ferrous chloride tetrahydrate and nitric acid iron nine hydrate; The mass ratio of the iron salt to the carbon aerogel is 0.03-0.04:0.2; The amount of the iron salt and water is 0.03-0.04 g:4-6 mL; The carbon aerogel is MOFs derived carbon aerogel.

3. The production method according to claim 1, wherein The stirring and dispersing time is 20-40 min.

4. The production method according to claim 1, wherein The alkali solution is ammonia water with a concentration of 25-28 wt%; The stirring time is 20-40 min.

5. The production method according to claim 1, wherein The drying temperature is 50-70 DEG C, and the time is 10-14 h.

6. The production method according to claim 1, wherein The calcination temperature is 250-350 DEG C, the time is 1-3 h, the heating rate is 3-8 DEG C / min, and the atmosphere is inert atmosphere.

7. An iron oxide-coated carbon aerogel composite material, characterized by, The iron oxide coated carbon aerogel composite material is prepared by the preparation method in any one of claims 1-6.

8. The iron oxide coated carbon aerogel composite material in claim 7 is used as an active ingredient in the preparation of a lithium ion battery electrode.

9. An electrode characterized by, The active ingredient of the electrode is the iron oxide coated carbon aerogel composite material in claim 7.

10. A lithium-ion battery, characterized by, The lithium ion battery uses the electrode in claim 9 as a negative electrode.