A positive electrode, a secondary battery and its preparation method

By adding a specific lithium salt additive S to the positive electrode slurry, the problems of electrolyte wetting of thick electrodes and interface stability of negative electrodes were solved, achieving high energy density and long life performance of the battery.

CN123120637APending Publication Date: 2026-11-17GREEN ENERGY ORIGIN TECHNOLOGY (JIANGSU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611618098.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to improve electrolyte wetting of thick electrodes, compensate for initial irreversible lithium loss, and stabilize the negative electrode interface without reducing electrode loading and compaction density, leading to a decline in battery rate performance and cycle life.

Method used

A specific type of ionic lithium salt additive S, such as lithium sulfate or lithium sulfonate, is added to the positive electrode slurry. It is then retained inside the positive electrode active material film layer through coating, drying, and rolling. Subsequently, it dissolves into the electrolyte during battery use, improving electrolyte wetting and lithium ion transport.

Benefits of technology

Without changing the electrode loading and compaction density, the battery's initial coulombic efficiency, cycle performance, and high-temperature storage performance are improved by the synergistic effect of additive S, which compensates for irreversible lithium loss and stabilizes the negative electrode interface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a positive electrode sheet, a secondary battery, and a method for preparing the same, relating to the field of battery preparation technology. The positive electrode slurry includes a positive electrode active material, a conductive agent, a binder, an additive S, and a solvent. The additive S is an ionic lithium salt containing lithium and sulfur elements, with sulfur atoms connected to lithium ions via bridging atoms X, where X is selected from at least one of oxygen and nitrogen atoms. The additive S does not decompose, produce gas, or volatilize under drying conditions of 80–120°C, and remains in a solid phase within the positive electrode active material film. Based on the total mass of the positive electrode active material film, the content of additive S is 0.01 wt%–5 wt%. Using this method, the effects of improving electrolyte wetting of thick electrodes, compensating for initial irreversible lithium loss, and stabilizing the negative electrode interface are achieved without reducing the electrode loading and compaction density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery manufacturing technology, and in particular to a positive electrode sheet, a secondary battery, and a method for preparing the same. Background Technology

[0002] With the rapid development of the new energy vehicle and energy storage industries, the market is constantly demanding higher energy density, stronger fast charging capabilities, longer cycle life, and better high-temperature storage performance from lithium-ion batteries. Lithium iron phosphate (LFP) has become one of the mainstream cathode materials in energy storage and power applications due to its abundant raw material reserves, low cost, good thermal stability, and excellent cycle life. However, limited by its specific capacity, increasing the coating thickness and compaction density of the electrode to improve the active material loading has become the mainstream technical route for improving battery energy density and reducing unit capacity cost, making thick electrode structures a research hotspot.

[0003] However, thick-coated, high-pressure solid electrode preparation results in low porosity and poor internal pore connectivity, making it difficult for the electrolyte to fully penetrate the active material layer near the current collector. This leads to a longer lithium-ion migration path and obstructed transport, easily causing concentration polarization and resulting in a decline in battery rate performance and cycle life. Simultaneously, the SEI film formed at the negative electrode interface during the initial battery formation irreversibly consumes a large amount of active lithium, causing initial capacity loss and a low initial coulombic efficiency. In thick electrode systems, these wetting difficulties and irreversible lithium losses are further amplified.

[0004] In existing technologies, functional additives are typically introduced into the electrolyte system to improve the initial coulombic efficiency, cycle life, and high-temperature storage performance of batteries. However, this approach can only improve interface stability through negative electrode film formation and is ineffective for thick electrodes with poor wettability and insufficient pore connectivity. Another approach focuses on electrode structure or processes, improving electrolyte penetration and retention by adjusting coating and rolling conditions, but this often comes at the cost of reducing electrode compaction density or active material loading. It is evident that both approaches address only one aspect of the negative electrode interface and electrolyte wetting: the thick coating and high compaction required for high energy density are difficult to reconcile with good wetting, high initial coulombic efficiency, and a stable negative electrode interface. Therefore, how to simultaneously improve electrolyte wetting of thick electrodes, compensate for initial irreversible lithium loss, and stabilize the negative electrode interface without reducing electrode loading and compaction density has become a pressing technical challenge in this field. Summary of the Invention

[0005] The purpose of this invention is to provide a positive electrode sheet, a secondary battery, and a method for preparing the same, in order to solve the technical problem in the prior art of how to improve the electrolyte wetting of thick electrodes, compensate for the first irreversible lithium loss, and stabilize the negative electrode interface without reducing the electrode loading and compaction density.

[0006] To achieve the above objectives, the technical solution of the present invention is as follows: A positive electrode sheet includes a positive current collector and a positive active material film layer disposed on at least one side surface of the positive current collector, wherein the positive active material film layer is formed by coating, drying and rolling a positive electrode slurry; The positive electrode slurry includes a positive electrode active material, a conductive agent, a binder, an additive S, and a solvent; the positive electrode active material is a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate. The additive S is an ionic lithium salt containing lithium and sulfur elements, and the sulfur atoms are connected to the lithium ions via bridging atoms X, wherein X is selected from at least one of oxygen and nitrogen atoms. The additive S does not decompose, produce gas, or volatilize under drying conditions of 80–120°C, and remains in solid form inside the positive electrode active material film layer during the coating, drying, and rolling processes; based on the total mass of the positive electrode active material film layer, the content of the additive S is 0.01 wt%–5 wt%.

[0007] Preferably, the additive S comprises at least one of the following (i) and (ii): (i) Lithium sulfate or lithium sulfonate as represented by the general formula R¹-SO₂-O-Li; (ii) Lithium bis(sulfonyl)imide represented by the general formula (R²-SO₂)(R³-SO₂)N-Li; R¹, R², and R³ are each independently selected from halogens, unsubstituted or fluorinated C1-C4 saturated alkyl groups, C2-C6 unsaturated hydrocarbon groups, unsubstituted or fluorinated C1-C4 saturated alkoxy groups, C2-C6 unsaturated alkoxy groups, and trifluoromethyl groups.

[0008] Furthermore, the positive electrode active material is lithium iron phosphate, the thickness of the positive electrode active material film is 120-190 μm, and the compaction density is 2.4-2.8 g / cm³.

[0009] Further, the additive S is selected from lithium sulfate or lithium sulfonate as represented by the general formula R¹-SO2-O-Li, wherein R¹ is selected from at least one of trifluoromethyl, halogen, unsubstituted or fluorinated C1-C4 saturated alkoxy and C2-C6 unsaturated alkoxy.

[0010] Furthermore, the additive S is selected from lithium bis(sulfonyl)imide represented by the general formula (R²-SO2)(R³-SO2)N-Li, wherein R² and R³ are each independently selected from fluorine atoms and trifluoromethyl groups.

[0011] Furthermore, the additive S is selected from at least one of lithium allyl sulfate, lithium trifluoromethanesulfonate, lithium bisfluorosulfonylimide, and lithium trifluoromethanesulfonylimide.

[0012] Furthermore, the mass ratio of the positive electrode active material, the conductive agent, the binder and the additive S is (92-97): (1-3): (1-3): (0.5-2).

[0013] This invention also provides a method for preparing a positive electrode sheet, comprising the following steps: S1. Prepare a positive electrode slurry, wherein the positive electrode slurry is the positive electrode slurry in the above-mentioned positive electrode sheet; S2. The positive electrode slurry is coated on at least one side of the positive electrode current collector and dried at 80°C to 120°C for 15 minutes to obtain the positive electrode substrate; S3. The positive electrode substrate is cold-pressed, then slit and die-cut to obtain the above-mentioned positive electrode sheet; The additive S does not decompose, produce gas, volatilize, or leak under the drying temperature of S2 and the cold pressing conditions of S3, and remains in the solid form inside the obtained positive electrode active material film.

[0014] Preferably, S1 includes: first dissolving the binder in N-methylpyrrolidone to obtain a glue solution, then adding the conductive agent and stirring to disperse, then adding the positive electrode active material and the additive S and continuing to stir, and obtaining the positive electrode slurry after vacuum degassing treatment; wherein, the additive S is added to the positive electrode slurry during the slurry mixing stage.

[0015] Furthermore, in step S1, the viscosity of the positive electrode slurry at 25°C is 3000–8000 mPa·s, and the fineness is less than 30 μm; in step S3, the positive electrode substrate is cold-pressed to a compaction density of 2.4–2.8 g / cm³.

[0016] The present invention also provides a secondary battery, comprising the above-mentioned positive electrode, negative electrode, separator, electrolyte and casing; the electrolyte contains lithium hexafluorophosphate, and the concentration of lithium hexafluorophosphate in the electrolyte is 0.7-1.5 mol / L; the additive S dissolves from the inside of the positive electrode active material film layer and enters the electrolyte after being injected into the electrolyte.

[0017] Preferably, the concentration of lithium hexafluorophosphate in the electrolyte is 1.0 to 1.5 mol / L.

[0018] Furthermore, the positive electrode active material film layer has pores formed by the dissolution of the additive S, and at least a portion of the additive S has dissolved from the interior of the positive electrode active material film layer.

[0019] This invention also provides a method for preparing a secondary battery, comprising the following steps: T1. Prepare a positive electrode using the above-mentioned method for preparing a positive electrode sheet; T2. Add the negative electrode active material, conductive agent, thickener and binder to deionized water and stir to disperse evenly to obtain a negative electrode slurry; coat the negative electrode slurry onto the surface of the negative electrode current collector, and then dry, roll and cut to obtain a negative electrode sheet; T3. Stack or wind the positive electrode sheet, the separator and the negative electrode sheet in sequence to obtain a battery cell pack, and encapsulate the battery cell pack in the battery casing; T4. Inject electrolyte into the packaged cell. After injection, let it stand at room temperature or 30℃~45℃ for 12~48h to allow the additive S to dissolve from the inside of the positive electrode active material film. The electrolyte contains lithium hexafluorophosphate at a concentration of 0.7~1.5mol / L. T5. The cells that have been left to stand are pre-charged, aged, and tested for capacity in sequence to obtain the secondary battery.

[0020] Preferably, in step T3, the electrolyte includes a lithium salt, an organic solvent, and optional electrolyte additives; the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium bis(oxalate borate), lithium difluorooxalate phosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide, and the concentration of the lithium salt is 0.7–1.5 mol / L; The organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, butenyl carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, 1,4-butyrolactone, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, or ethyl butyrate, and the total mass fraction of the solvent accounts for 70% to 90% of the total mass fraction of the electrolyte. The electrolyte additive is selected from at least one of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, methanedisulfonate, 1,3-propanesulfonate lactone, and tris(trimethylsilane) phosphate, and the total mass fraction of the additive accounts for 0.5% to 5% of the total mass fraction of the electrolyte.

[0021] Furthermore, the mass ratio of negative electrode active material, conductive agent, thickener and binder in the negative electrode slurry is (94-98):(0-2):(1-2):(1-3).

[0022] The present invention provides a positive electrode sheet, a secondary battery, and a method for preparing the same, which have the following advantages compared to the prior art: This invention introduces a specific structured ionic lithium salt additive S into the positive electrode slurry of a positive electrode active material containing lithium transition metal oxides or lithium transition metal phosphates. The additive S is designed to remain stable in a solid phase within the positive electrode active material film during coating, drying, and rolling processes, preventing decomposition, gas generation, and volatilization. This allows the additive S to be pre-introduced into the positive electrode active material film and play a corresponding role during subsequent battery use. Because the additive S contains lithium and sulfur, and sulfur atoms are connected to lithium ions via bridging atoms X, the additive S provides a source of lithium and sulfur for the battery system. This helps compensate for irreversible lithium loss during the first charge-discharge cycle and improves the initial coulombic efficiency of the battery, while also improving the stability of the negative electrode interface. On the other hand, by pre-dispersing the additive S in solid form and retaining it inside the positive electrode active material film, the additive S can come into contact with the electrolyte during subsequent electrolyte injection and gradually enter the battery system, which is beneficial to improving the electrolyte wetting and lithium-ion transport conditions inside the thick electrode. Therefore, this invention can achieve synergistic improvement of initial irreversible lithium loss, internal battery transport, and interface stability through the additive S without changing the positive electrode active material or reducing the positive electrode loading and compaction density, thereby improving the initial coulombic efficiency, cycle performance, and high-temperature storage performance of the secondary battery. Detailed Implementation

[0023] The technical solutions of this application will be clearly and completely described below with reference to the embodiments therein. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0024] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "connected" and "linked" should be interpreted broadly. For example, they can refer to a direct connection or an indirect connection through an intermediate medium, or the internal connection of two elements or the interaction between two elements. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances. In the description of this application, "multiple" means two or more, unless otherwise expressly specified. Furthermore, the terms "first," "second," "third," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features.

[0025] For lithium iron phosphate batteries, thick electrode design is the core means to improve energy density. However, problems such as difficulty in electrolyte wetting, large initial irreversible lithium loss, and unstable negative electrode interface caused by thick coating and high compaction have always restricted the overall performance of thick electrode systems. In the existing technology, electrolyte functional additives can only improve the negative electrode interface, and electrode structure control often comes at the cost of energy density, making it difficult to achieve both simultaneously.

[0026] The applicant discovered that by introducing a specific sulfur-containing lithium salt additive into the positive electrode slurry during the slurry mixing stage, its thermal stability and non-volatile properties under drying conditions of 80–120°C allow it to remain in solid form within the positive electrode active material film layer. After battery electrolyte injection, the additive gradually dissolves and is released from the film layer in situ, simultaneously achieving a triple synergistic effect of in-situ pore formation to improve wetting, releasing active lithium to compensate for initial efficiency loss, and sulfur-containing anions participating in negative electrode film formation. By introducing only one substance, multiple pain points of thick electrodes can be solved simultaneously without reducing electrode loading and compaction density.

[0027] Based on the above findings, a first aspect of this application provides a positive electrode sheet, comprising a positive current collector and a positive active material film layer disposed on at least one surface of the positive current collector, wherein the positive active material film layer is formed by coating, drying, and rolling a positive electrode slurry. The positive electrode slurry comprises a positive active material, a conductive agent, a binder, an additive S, and a solvent.

[0028] The positive electrode active material is a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate. Specifically, the positive electrode active material is selected from one or more of lithium cobalt oxide, nickel-cobalt-manganese ternary materials, lithium iron phosphate, and lithium manganese oxide. Preferably, the positive electrode active material is lithium iron phosphate. Lithium iron phosphate has an olivine-type crystal structure, a theoretical specific capacity of approximately 170 mAh / g, and an operating voltage plateau of approximately 3.4 V (vs Li / Li). + Due to its abundant raw material reserves, low cost, good thermal stability, and long cycle life, it is widely used in the fields of energy storage and power.

[0029] The additive S is an ionic lithium salt containing lithium and sulfur elements, with sulfur atoms connected to lithium ions via bridging atoms X, where X is selected from at least one of oxygen and nitrogen atoms. It is understood that bridging atoms X can be entirely oxygen atoms, entirely nitrogen atoms, or a combination of oxygen and nitrogen atoms (e.g., using a mixture of two additives, one containing O bridging and the other containing N bridging). When X is an oxygen atom, additive S can be of the type lithium sulfonate or lithium sulfate; when X is a nitrogen atom, additive S can be of the type lithium sulfonamide or lithium sulfimide.

[0030] The additive S does not decompose, produce gas, or volatilize under drying conditions of 80–120°C, and remains in solid form within the positive electrode active material film layer during the coating, drying, and rolling processes. These characteristics are crucial: if the additive decomposes during drying, it may produce gas, leading to defects such as pores and bulging on the electrode sheet; if the additive volatilizes at high temperatures, it will be lost in the drying oven and unable to perform its subsequent function within the film layer. Therefore, the thermal stability of additive S is a prerequisite for achieving solid-phase retention and liquid dissolution.

[0031] Based on the total mass of the positive electrode active material film, the content of additive S is 0.01wt% to 5wt%. It is understood that the content of additive S (unit: wt%) can be any value from 0.01, 0.1, 0.2, 0.5, 1, 1.5, 2, 3, 4, 5, or any value within a range of any two values. When the content of additive S is too low, the pore-forming effect and lithium replenishment effect after dissolution are insufficient, making it difficult to show significant performance improvement; when the content of additive S is too high, on the one hand, it will reduce the mass ratio of the active material, leading to a decrease in capacity; on the other hand, excessive sulfur-containing species may trigger side reactions, increasing interfacial impedance. Preferably, the content of additive S is 0.5wt% to 2wt%, within which the optimal pore-forming effect and interfacial modification effect can be achieved.

[0032] In some embodiments, the additive S comprises at least one of the following (i) and (ii): (i) Lithium sulfate or lithium sulfonate as represented by the general formula R¹-SO₂-O-Li; (ii) Lithium bis(sulfonyl)imide of general formula (R²-SO₂)(R³-SO₂)N-Li.

[0033] Wherein, R¹, R², and R³ are each independently selected from halogens, unsubstituted or fluorinated C1-C4 saturated alkyl groups, C2-C6 unsaturated hydrocarbon groups, unsubstituted or fluorinated C1-C4 saturated alkoxy groups, C2-C6 unsaturated alkoxy groups, and trifluoromethyl groups. It is understood that the halogen can be any one of fluorine, chlorine, bromine, and iodine, preferably a fluorine atom. The C1-C4 saturated alkyl group can be any one of methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, and tert-butyl. The C2-C6 unsaturated hydrocarbon group can be any one of vinyl, allyl, and propynyl. The C1-C4 saturated alkoxy group can be any one of methoxy, ethoxy, propoxy, and butoxy. The C2-C6 unsaturated alkoxy group can be any one of allyloxy and vinyloxy.

[0034] Different substituents affect the solubility, thermal stability, reduction potential, and film-forming properties of additive S. For example, substituents containing fluoroalkyl or trifluoromethyl groups have a stronger electron-withdrawing effect, reducing the electron cloud density on the sulfonyl group and making it easier for sulfur-containing anions to be reduced and decomposed on the negative electrode surface, thereby promoting the formation of the SEI film. Substituents containing unsaturated bonds, such as allyl groups, can participate in the polymerization reaction during the formation process, contributing to the formation of a denser interfacial film.

[0035] In some embodiments, the additive S is selected from lithium sulfate or lithium sulfonate of the general formula R¹-SO2-O-Li, wherein R¹ is selected from at least one of trifluoromethyl, halogen, unsubstituted or fluorinated C1-C4 saturated alkoxy and C2-C6 unsaturated alkoxy.

[0036] In some embodiments, the additive S is selected from lithium bis(sulfonyl)imide of the general formula (R²-SO₂)(R³-SO₂)N-Li, wherein R² and R³ are each independently selected from fluorine atoms and trifluoromethyl groups.

[0037] In some embodiments, the additive S is selected from at least one of lithium allyl sulfate, lithium trifluoromethanesulfonate, lithium bisfluorosulfonylimide, and lithium trifluoromethanesulfonylimide. All four substances are commercially available battery-grade lithium salts, widely available, with controllable purity, and convenient for industrial application. Specifically: lithium allyl sulfate belongs to the lithium sulfate ester class (X=O), R¹ is an allyloxy group, and the molecule contains both a sulfur-oxygen bridging structure and an unsaturated double bond, possessing pore-forming, lithium replenishment, and film-forming functions; lithium trifluoromethanesulfonate belongs to the lithium sulfonate ester class (X=O), R¹ is a trifluoromethyl group, exhibiting excellent thermal and electrochemical stability; lithium bisfluorosulfonylimide (LiFSI) belongs to the lithium bissulfonylimide class (X=N), R² and R³ are both fluorine atoms, exhibiting high ionic conductivity and good film-forming performance; lithium trifluoromethanesulfonylimide (LiTFSI) belongs to the lithium bissulfonylimide class (X=N), R² and R³ are both trifluoromethyl groups, exhibiting excellent thermal stability and good hydrolytic stability.

[0038] In some embodiments, the thickness of the positive electrode active material film is 120–190 μm, and the compaction density is 2.4–2.8 g / cm³. It is understood that the film thickness (unit: μm) can be any value from 120, 130, 140, 150, 160, 170, 180, 190, or any value within a range of any two values. The compaction density (unit: g / cm³) can be any value from 2.4, 2.5, 2.6, 2.7, 2.8, or any value within a range of any two values. The above thickness and compaction density range correspond to the design of thick electrodes for high-energy-density lithium iron phosphate batteries, which is also the application scenario where the technical effect of this invention is most significant. The thicker the film and the higher the compaction density, the greater the difficulty of electrolyte wetting, and the more prominent the improvement effect brought by the dissolution and pore-forming effect of additive S.

[0039] In some embodiments, the mass ratio of the positive electrode active material, the conductive agent, the binder, and the additive S is (92–97):(1–3):(1–3):(0.5–2). It is understood that the mass fraction of the positive electrode active material can be any value among 92, 93, 94, 95, 96, and 97; the mass fraction of the conductive agent can be any value among 1, 1.5, 2, 2.5, and 3; the mass fraction of the binder can be any value among 1, 1.5, 2, 2.5, and 3; and the mass fraction of the additive S can be any value among 0.5, 1, 1.5, and 2.

[0040] The conductive agent is selected from at least one of conductive carbon black, acetylene black, conductive graphite, carbon nanotubes (CNTs), and graphene. Based on the total mass of the positive electrode active material film, the content of the conductive agent is 0.5% to 5%, preferably 1% to 3%.

[0041] The binder is selected from at least one of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), and polytetrafluoroethylene (PTFE), preferably polyvinylidene fluoride (PVDF). Based on the total mass of the positive electrode active material film layer, the content of the binder is 0.5% to 5%, preferably 1% to 3%.

[0042] The positive current collector is an aluminum foil with a thickness of 5–30 μm, preferably 12 μm.

[0043] A second aspect of this application provides a method for preparing a positive electrode sheet, comprising the following steps: S1. Prepare a positive electrode slurry, wherein the positive electrode slurry is the positive electrode slurry in the above-mentioned positive electrode sheet; S2. The positive electrode slurry is coated on at least one side of the positive electrode current collector and dried at 80°C to 120°C to obtain the positive electrode substrate; S3. The positive electrode substrate is cold-pressed, then slit and die-cut to obtain the positive electrode sheet.

[0044] The additive S does not decompose, produce gas, volatilize, or leak under the drying temperature of S2 and the cold pressing conditions of S3, and remains in the solid form inside the obtained positive electrode active material film.

[0045] In some embodiments, step S1 includes: first dissolving the binder in N-methylpyrrolidone to obtain a slurry, then adding the conductive agent and stirring to disperse it, followed by adding the lithium iron phosphate and the additive S and continuing to stir, and finally obtaining the positive electrode slurry after vacuum degassing. The additive S is added to the positive electrode slurry during the slurry mixing stage, that is, during the active material feeding stage, so that the additive S can be fully and uniformly mixed with the active material, conductive agent and other solid components, and finally uniformly distributed inside the film layer.

[0046] In some embodiments, the viscosity of the positive electrode slurry in S1 at 25°C is 3000–8000 mPa·s, and the fineness is less than 30 μm. It is understood that the viscosity of the slurry (unit: mPa·s) can be any value from 3000, 4000, 5000, 6000, 7000, and 8000, or any value within a range of any two values. Viscosity and fineness are key indicators for evaluating the uniformity and coating applicability of the slurry. Excessive viscosity can lead to poor coating flowability and defects such as streaks; excessively low viscosity can easily lead to sedimentation. Excessive fineness indicates the presence of large particle agglomerates, which may cause particle scratches on the coating surface.

[0047] In some embodiments, in step S3, the positive electrode substrate is cold-pressed to a compaction density of 2.4 to 2.8 g / cm³.

[0048] A third aspect of this application provides a secondary battery, including the aforementioned positive electrode, negative electrode, separator, electrolyte, and casing. The electrolyte contains lithium hexafluorophosphate, and the concentration of lithium hexafluorophosphate in the electrolyte is 0.7–1.5 mol / L. It is understood that the concentration of lithium hexafluorophosphate (unit: mol / L) can be any value from 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a value within a range of any two values. Lithium hexafluorophosphate is currently the most widely commercially available lithium salt, possessing excellent film-forming properties and ion transport performance. When the lithium salt concentration is too low, the electrolyte conductivity is insufficient, affecting rate performance; when the lithium salt concentration is too high, the electrolyte viscosity increases, which is also detrimental to ion transport.

[0049] The additive S dissolves from the inside of the positive electrode active material film layer and enters the electrolyte after the electrolyte is injected. During the electrode preparation stage (coating, drying, rolling), the additive S exists stably in solid form inside the film layer; after the battery is injected with electrolyte, as the electrolyte gradually penetrates into the film layer, the additive S gradually dissolves and diffuses into the electrolyte, thereby leaving a porous structure in situ.

[0050] In some embodiments, the concentration of lithium hexafluorophosphate in the electrolyte is 1.0–1.5 mol / L. Within this concentration range, the electrolyte exhibits high ionic conductivity and good overall performance.

[0051] In some embodiments, the positive electrode active material film layer has pores formed by the dissolution of the additive S, and at least a portion of the additive S has dissolved from the interior of the positive electrode active material film layer. These in-situ formed pores and interconnected channels provide pathways for electrolyte penetration and are key structural features for improving the wettability of thick electrodes.

[0052] In some embodiments, the electrolyte comprises a lithium salt, an organic solvent, and optional electrolyte additives. The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium bis(oxalate borate), lithium difluorooxalate phosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide, and the concentration of the lithium salt is 0.7–1.5 mol / L. It is understood that a single lithium salt can be used, or two or more can be used in combination. Mixed lithium salt systems often combine the advantages of different lithium salts; for example, adding a small amount of lithium bis(fluorosulfonyl)imide to lithium hexafluorophosphate can improve the high-temperature stability of the electrolyte.

[0053] The organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, butenyl carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, 1,4-butyrolactone, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, or ethyl butyrate, and the total mass fraction of the solvent accounts for 70% to 90% of the total mass fraction of the electrolyte. It is understood that the organic solvent is typically a mixture of cyclic carbonates and chain carbonates. Cyclic carbonates (such as EC) have a higher dielectric constant, which is beneficial for the dissociation of lithium salts; chain carbonates (such as DMC, EMC, DEC) have lower viscosity, which is beneficial for ion migration. Using a mixture of both can balance dielectric constant and viscosity, achieving ideal ionic conductivity.

[0054] The electrolyte additive is selected from at least one of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, methylene disulfonate, 1,3-propanesulfonate lactone, and tris(trimethylsilane)phosphate, and the total mass fraction of the additive accounts for 0.5% to 5% of the total mass fraction of the electrolyte. Although the content of the electrolyte additive is very low, it can preferentially undergo reduction or oxidation reactions on the electrode surface during battery formation to form a protective interfacial film, which has a crucial impact on the cycle life and storage performance of the battery.

[0055] The diaphragm is a polyolefin-based diaphragm (PE or PP), and optionally has a ceramic heat-resistant coating and / or a PVDF adhesive coating coated on at least one side surface, with a diaphragm thickness of 9–20 μm.

[0056] In some embodiments, the secondary battery includes a square stacked battery, a pouch stacked battery, a square wound battery, or a cylindrical wound battery.

[0057] The fourth aspect of this application provides a method for preparing a secondary battery, comprising the following steps: T1. Prepare a positive electrode using the above-mentioned method for preparing a positive electrode sheet; T2. Add the negative electrode active material, conductive agent, thickener and binder to deionized water and stir to disperse evenly to obtain a negative electrode slurry; coat the negative electrode slurry onto the surface of the negative electrode current collector, and then dry, roll and cut to obtain a negative electrode sheet; T3. Stack or wind the positive electrode sheet, the separator and the negative electrode sheet in sequence to obtain a battery cell pack, and encapsulate the battery cell pack in the battery casing; T4. Inject electrolyte into the packaged cell. After injection, let it stand at room temperature or 30℃~45℃ for 12~48h to allow the additive S to dissolve from the inside of the positive electrode active material film. The electrolyte contains lithium hexafluorophosphate at a concentration of 0.7~1.5mol / L. T5. The cells that have been left to stand are pre-charged, aged, and tested for capacity in sequence to obtain the secondary battery.

[0058] In some embodiments, the mass ratio of negative electrode active material, conductive agent, thickener, and binder in the negative electrode slurry is (94-98):(0-2):(1-2):(1-3). It is understood that the mass fraction of the negative electrode active material can be any value among 94, 95, 96, 97, and 98; the mass fraction of the conductive agent can be any value among 0, 0.5, 1, 1.5, and 2 (a conductive agent content of 0 indicates that no additional conductive agent is added to the negative electrode slurry); the mass fraction of the thickener can be any value among 1, 1.5, and 2; and the mass fraction of the binder can be any value among 1, 1.5, 2, 2.5, and 3.

[0059] The negative electrode active material includes, but is not limited to, at least one of carbon-based negative electrode materials, silicon-based negative electrode materials, tin-based negative electrode materials, silicon-containing alloy negative electrode materials, and tin-containing alloy negative electrode materials. More preferably, the negative electrode active material is graphite. The thickener is sodium carboxymethyl cellulose (CMC). The binder is styrene-butadiene rubber (SBR). The negative electrode current collector is copper foil with a thickness of 6–12 μm, preferably 8 μm.

[0060] The positive electrode sheet and secondary battery provided in this application break through the technical limitations of traditional electrolytes that only add functional additives. By placing lithium salt-based sulfide compound additive S in the pre-processing of lithium iron phosphate positive electrode slurry, a working mechanism is achieved where the additive is pre-placed in situ on the positive electrode and gradually dissolved later. With only one substance, it innovatively integrates the three functions of positive electrode pore-forming modification, active lithium compensation, and negative electrode interface film-forming modification. Without reducing the electrode coating thickness and compaction density, or sacrificing the battery energy density, it simultaneously solves multiple technical problems such as poor wettability of thick lithium iron phosphate electrodes, large initial irreversible capacity loss, unstable negative electrode interface, and poor cycle and high-temperature storage performance.

[0061] The following description, in conjunction with specific embodiments, illustrates the positive electrode sheet, secondary battery, and their preparation method provided in this application: Example 1 This embodiment provides a lithium iron phosphate positive electrode sheet containing lithium allyl sulfate additive, and an LFP / graphite soft-pack lithium-ion battery prepared using the positive electrode sheet.

[0062] Preparation of positive electrode sheet: Raw material mass ratio: Lithium iron phosphate (LFP): Conductive carbon black: Binder PVDF: Additive S = 96:1:2:1. Additive S is lithium allyl sulfate, with the molecular formula CH2=CH-CH2-O-SO2-O-Li, belonging to the lithium sulfate ester category represented by the general formula R¹-SO2-O-Li. R¹ stands for allyloxy (C2-C6 unsaturated alkoxy group), and the sulfur atom is bridged to the lithium ion via an oxygen atom.

[0063] The preparation steps are as follows: S1. Preparation and Homogenization: PVDF binder is dissolved in NMP solvent and stirred to prepare a slurry with a solid content of 7wt%. Conductive carbon black is added to the slurry and dispersed uniformly under vacuum. Then, LFP active material and lithium allyl sulfate are added, and vacuum stirring is continued until the solid content reaches 75%, obtaining a uniform positive electrode slurry. Additive S is added to the positive electrode slurry during the slurry mixing stage. The resulting positive electrode slurry has a viscosity of 3000–8000 mPa·s at 25°C and a fineness of less than 30 μm.

[0064] S2. Coating and Drying: The positive electrode slurry is coated onto the surface of a 12μm thick aluminum foil current collector, and then dried at a gradient temperature of 80–120℃ to remove the NMP solvent, thus obtaining the positive electrode substrate. During the drying process, lithium allyl sulfate is uniformly dispersed in solid form within the positive electrode active material film layer without decomposition, gas generation, or volatilization.

[0065] S3. Roll pressing and slitting: The dried positive electrode substrate is cold-pressed to control the compaction density of the positive electrode active material film layer to be 2.6 g / cm³ and the film layer thickness to be 169.2 μm; the positive electrode sheet is obtained by cutting and welding the tabs.

[0066] Negative electrode preparation: Raw material mass ratio: artificial graphite ∶ SBR ∶ CMC = 96 ∶ 2 ∶ 2. Artificial graphite, CMC, SBR, and deionized water are mixed and stirred evenly to obtain a negative electrode slurry. The negative electrode slurry is coated onto the surface of an 8μm copper foil current collector, dried, cold-pressed, and then cut and welded to obtain the negative electrode sheet.

[0067] Electrolyte preparation: Under a dry argon atmosphere, a base solvent was prepared by mixing DMC:EC:EMC in a mass ratio of 1:1:1; dissolving 1 mol / L LiPF6; and then adding 3% VC by mass to prepare the base electrolyte.

[0068] Battery assembly: A 12μm thick porous polymer separator (PE) is used. The positive electrode, separator, and negative electrode are stacked sequentially and packaged in an aluminum-plastic outer foil, with a pre-reserved electrolyte injection port. The electrolyte is then injected and sealed. Sequential processes of electrolyte injection and settling, pre-charge formation, and capacity sorting are performed to obtain an LFP / graphite soft-pack lithium-ion battery.

[0069] After electrolyte injection, the electrode is allowed to stand at 30–45°C for 12–48 hours to allow the electrolyte to fully wet the electrode. Simultaneously, additive S gradually dissolves and diffuses from within the positive electrode active material film, entering the electrolyte. A porous structure formed in the positive electrode active material film is created by the dissolution of additive S, and at least a portion of additive S has dissolved from within the film.

[0070] Examples 2-10 The preparation methods of the positive electrode sheets and batteries provided in Examples 2-10 are basically the same as those in Example 1, with the only differences being the compaction density of the positive electrode active material film, the film thickness, and the type and amount of additive S. Specific parameters for each example are shown in Table 1.

[0071] Comparative Examples 1-6 Comparative Examples 1 to 6 are used to illustrate the technical effects of the present invention.

[0072] Comparative Examples 1-4 are blank comparative examples, with no additive S added to the positive electrode slurry. They correspond to different compaction densities and film thickness conditions, and are used to examine the baseline performance without additives.

[0073] Comparative Example 5 uses vinyl sulfate (DTD) as the positive electrode additive. DTD molecules contain sulfur but no lithium ions, and are used to verify the necessity of the "lithium replenishment" function.

[0074] Comparative Example 6 uses ammonium dihydrogen carbonate as the positive electrode additive. Its molecules contain neither sulfur nor lithium, and can only play a role in physical pore formation.

[0075] The specific parameters for each comparative example are shown in Table 1: Table 1

[0076] The performance testing method is as follows: Electrolyte wettability: Using the electrolyte climb height method, after vacuum baking at 80℃ for 4 hours, the lower end of the electrode is immersed in the electrolyte, and the electrolyte climb height H is read after 10 minutes. The higher the height, the better the wettability. Initial coulombic efficiency: Charged to 3.4V at 0.05C→0.2C at 45℃, then constant voltage, and then discharged to 2.5V at 1 / 3C. Initial efficiency = discharge capacity / charge capacity × 100%. DC internal resistance DCR: Voltage difference / current value after applying a 1C discharge pulse for 30s at 25℃ and 50% SOC. 25℃ cycle performance: Capacity retention rate after 800 charge-discharge cycles at 0.5P. 60℃ storage performance: Capacity retention rate after 30 days of storage at 60℃ in a fully charged state.

[0077] Based on the data in Table 1, the following conclusions can be drawn: A comparison of the data from Examples 1-3 with Comparative Example 1 shows that, under the same compaction density (2.6 g / cm³) and film thickness (169.2 μm), the addition of three different types of sulfur-containing lithium salts (lithium allyl sulfate, LiTFSI, and LiFSI) significantly improved electrode wettability, increased initial coulombic efficiency, reduced DC internal resistance, and enhanced cycle and high-temperature storage performance. Specifically, the electrolyte creep height increased from 17 mm to 31 mm, 29 mm, and 28 mm, respectively, and the initial coulombic efficiency increased from 85.89% to 89.59%, 89.14%, and 89.33%, respectively. This indicates that sulfur-containing lithium salts in which X is an oxygen atom (lithium sulfate / sulfonate) or a nitrogen atom (lithium bissulfonylimide) can exert a triple synergistic effect through solid-phase retention and liquid-injection dissolution mechanisms.

[0078] A comparison of the data from Examples 1, 4-7, and Comparative Example 1 shows that as the amount of additive S increases from 0.2% to 4%, the electrolyte rise height continuously increases (22mm → 38mm), but the initial coulombic efficiency shows a trend of first increasing and then decreasing, reaching a peak of 89.59% when the addition amount is 1% (Example 1). Cyclic and high-temperature storage performance also exhibit a similar pattern of first increasing and then decreasing. Insufficient addition results in limited dissolution of active lithium and sulfur-containing anions, leading to insufficient pore-forming and film-forming effects; excessive addition increases interfacial impedance due to excessive sulfur-containing byproducts, resulting in performance degradation. Therefore, it is necessary to control the content of additive S within the range of 0.01wt% to 5wt%, preferably 0.5wt% to 2wt%. This doping ratio can balance the optimal pore-forming and interfacial modification effects, avoiding insufficient pore-forming and film-forming effects due to too low a doping amount, or problems such as decreased slurry stability, excessive electrode porosity leading to decreased mechanical properties, and increased battery side reactions due to too high a doping amount.

[0079] A comparison of the data from Examples 1, 8-10 and Comparative Examples 1-4 shows that as the film thickness increases (109.6 μm → 131.9 μm → 169.2 μm → 184 μm), the performance of the blank comparative examples deteriorates sharply. While the performance of the examples with additive S also decreases, the decrease is much smaller than that of the comparative examples, and both are significantly better than the comparative examples of the same specifications. Especially in the thickest 184 μm electrode (Example 10 vs. Comparative Example 4), the electrolyte creep height increases from 11 mm to 26 mm, and the first-efficiency increases from 83.02% to 89.17%, showing the most significant improvement. This indicates that additive S of the present invention has a more prominent application value in thick electrode systems.

[0080] A comparison of the data from Example 1 and Comparative Examples 5 and 6 shows that while vinyl sulfate (DTD) can dissolve to create pores and participate in film formation, it lacks lithium ions and cannot replenish lithium, resulting in limited improvement in first-efficiency (88.69% vs 89.59%). Ammonium dihydrogen carbonate can only physically create pores (climb height similar to Example 1), but it cannot replenish lithium or form films, resulting in minimal improvement in first-efficiency and cycle performance. In contrast, the additive S of this invention possesses both sulfur-containing anions and lithium ions, achieving a synergistic effect of lithium replenishment, in-situ pore creation, and negative electrode film formation, with overall performance significantly superior to single-function additive systems.

[0081] In summary, this application introduces additive S into the slurry mixing process of the positive electrode slurry in advance, allowing additive S to be pre-dispersed in solid form and retained inside the positive electrode active material film during the preparation of the positive electrode sheet. During battery electrolyte injection and subsequent charge-discharge activation, additive S gradually dissolves into the electrolyte and is then leached out in situ from within the positive electrode active material film. This achieves synergistic control over the internal pore structure of the thick electrode, the supply of active lithium, and the film formation at the negative electrode interface without sacrificing the compaction density and active material loading of the positive electrode sheet. On the one hand, after additive S gradually dissolves from within the positive electrode film, it can form pores or enlarge local channels at its original retention location, which is beneficial for improving the porosity within the positive electrode active material film. The additive S improves the connectivity of the pores, promoting electrolyte penetration into the active material layer near the current collector and shortening the lithium-ion transport path, thereby reducing ion migration resistance in thick electrode systems. On the other hand, the lithium element in additive S provides active lithium during the first charge-discharge cycle to compensate for irreversible lithium loss during SEI film formation at the negative electrode, thus reducing initial capacity loss and improving initial coulombic efficiency. Simultaneously, the sulfur element in additive S migrates with the electrolyte to the negative electrode surface and participates in the negative electrode interface reaction during charge-discharge activation, facilitating the formation of a stable sulfur-containing SEI film, suppressing continuous side reactions between the negative electrode and electrolyte, and reducing active lithium consumption, thereby improving negative electrode interface stability. Therefore, this invention utilizes the different roles of the same additive S at different stages of the battery to achieve a triple synergistic effect of in-situ pore formation on the positive electrode, improved electrolyte wetting, active lithium compensation, and SEI stabilization at the negative electrode.

[0082] In some other embodiments, the additive S in this application is not limited to the application of the positive electrode sheet, but can also be added to the negative electrode slurry to form the negative electrode sheet; in some other embodiments, the secondary battery in this application is not limited to the lithium-ion battery, but can also be applied to the sodium-ion battery, by replacing the lithium salt in the additive S with the sodium salt.

[0083] The foregoing has provided a detailed description of the positive electrode sheet, secondary battery, and its preparation method provided in the embodiments of this application. Specific examples have been used in this application to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are merely for the purpose of helping to understand the technical solutions and core ideas of this application. Those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A positive electrode sheet, comprising a positive current collector and a positive active material film layer disposed on at least one surface of the positive current collector, wherein the positive active material film layer is formed by coating, drying and rolling a positive electrode slurry, characterized in that: The positive electrode slurry includes a positive electrode active material, a conductive agent, a binder, an additive S, and a solvent; The positive electrode active material is a lithium-containing transition metal oxide or a lithium-containing transition metal phosphate. The additive S is an ionic lithium salt containing lithium and sulfur elements, and the sulfur atoms are connected to the lithium ions via bridging atoms X, wherein X is selected from at least one of oxygen and nitrogen atoms. The additive S does not decompose, produce gas, or volatilize under drying conditions of 80–120°C, and remains in solid form inside the positive electrode active material film during the coating, drying, and rolling processes. Based on the total mass of the positive electrode active material film, the content of the additive S is 0.01wt% to 5wt%.

2. The positive electrode sheet according to claim 1, characterized in that, The additive S includes at least one of the following (i) and (ii): (i) Lithium sulfate or lithium sulfonate as represented by the general formula R¹-SO₂-O-Li; (ii) Lithium bis(sulfonyl)imide of the general formula (R²-SO₂)(R³-SO₂)N-Li; R¹, R², and R³ are each independently selected from halogens, unsubstituted or fluorinated C1-C4 saturated alkyl groups, C2-C6 unsaturated hydrocarbon groups, unsubstituted or fluorinated C1-C4 saturated alkoxy groups, C2-C6 unsaturated alkoxy groups, and trifluoromethyl groups.

3. A positive electrode sheet according to claim 2, characterized in that, The positive electrode active material is lithium iron phosphate, and the thickness of the positive electrode active material film layer is 120-190 μm, and the compaction density is 2.4-2.8 g / cm³.

4. A positive electrode sheet according to claim 2, characterized in that, The additive S is selected from lithium sulfate or lithium sulfonate as represented by the general formula R¹-SO2-O-Li, wherein R¹ is selected from at least one of trifluoromethyl, halogen, unsubstituted or fluorinated C1-C4 saturated alkoxy and C2-C6 unsaturated alkoxy.

5. A positive electrode sheet according to claim 2, characterized in that, The additive S is selected from lithium bis(sulfonyl)imide represented by the general formula (R²-SO₂)(R³-SO₂)N-Li, wherein R² and R³ are each independently selected from fluorine atoms and trifluoromethyl groups.

6. A positive electrode sheet according to claim 2, characterized in that, The additive S is selected from at least one of lithium allyl sulfate, lithium trifluoromethanesulfonate, lithium bisfluorosulfonylimide, and lithium trifluoromethanesulfonylimide.

7. A positive electrode sheet according to claim 2, characterized in that, The mass ratio of the positive electrode active material, the conductive agent, the binder and the additive S is (92-97): (1-3): (1-3): (0.5-2).

8. A method for preparing a positive electrode sheet, characterized in that, Includes the following steps: S1. Prepare a positive electrode slurry, wherein the positive electrode slurry is the positive electrode slurry in the positive electrode sheet according to claim 1; S2. The positive electrode slurry is coated on at least one side of the positive electrode current collector and dried at 80°C to 120°C for 15 minutes to obtain the positive electrode substrate; S3. The positive electrode substrate is cold-pressed, then slit and die-cut to obtain the positive electrode sheet as described in claim 1; The additive S does not decompose, produce gas, volatilize, or leak under the drying temperature of S2 and the cold pressing conditions of S3, and remains in the solid form inside the obtained positive electrode active material film.

9. The method for preparing a positive electrode sheet according to claim 8, characterized in that, The S1 includes: first dissolving the binder in N-methylpyrrolidone to prepare a slurry, then adding the conductive agent and stirring to disperse it, then adding the positive electrode active material and the additive S and continuing to stir, and finally obtaining the positive electrode slurry after vacuum degassing treatment; The additive S is added to the positive electrode slurry during the slurry mixing stage.

10. A method for preparing a positive electrode sheet according to claim 9, characterized in that, In step S1, the viscosity of the positive electrode slurry at 25°C is 3000–8000 mPa·s, and the fineness is less than 30 μm; and / or, in step S3, the positive electrode substrate is cold-pressed to a compaction density of 2.4–2.8 g / cm³.

11. A secondary battery, characterized in that, Includes the positive electrode, negative electrode, separator, electrolyte, and casing as described in any one of claims 1 to 7; The electrolyte contains lithium hexafluorophosphate, and the concentration of lithium hexafluorophosphate in the electrolyte is 0.7–1.5 mol / L; The additive S dissolves from inside the positive electrode active material film and enters the electrolyte after the electrolyte is injected.

12. The secondary battery according to claim 11, characterized in that, The concentration of lithium hexafluorophosphate in the electrolyte is 1.0–1.5 mol / L.

13. The secondary battery according to claim 11, characterized in that, The positive electrode active material film layer has pores formed by the dissolution of the additive S, and at least a portion of the additive S has dissolved from the interior of the positive electrode active material film layer.

14. A method for preparing a secondary battery, characterized in that, Includes the following steps: T1. Prepare a positive electrode sheet using the method described in any one of claims 8 to 10; T2. Add the negative electrode active material, conductive agent, thickener and binder to deionized water and stir to disperse evenly to obtain a negative electrode slurry; coat the negative electrode slurry onto the surface of the negative electrode current collector, and then dry, roll and cut to obtain a negative electrode sheet; T3. Stack or wind the positive electrode sheet, the separator and the negative electrode sheet in sequence to obtain the battery cell pack, and encapsulate the battery cell pack in the battery casing; T4. Inject electrolyte into the packaged cell. After injection, let it stand at room temperature or 30℃~45℃ for 12~48h to allow the additive S to dissolve from the inside of the positive electrode active material film. The electrolyte contains lithium hexafluorophosphate at a concentration of 0.7~1.5mol / L. T5. The cells that have been left to stand are sequentially pre-charged, aged, and tested for capacity to obtain the secondary battery.

15. The method for preparing a secondary battery according to claim 14, characterized in that, In step T3, the electrolyte includes lithium salt, organic solvent, and optional electrolyte additives; The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium difluorooxalate borate, lithium bis(oxalate borate), lithium difluorooxalate phosphate, lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethanesulfonyl)imide, and the concentration of the lithium salt is 0.7 to 1.5 mol / L. The organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, butenyl carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, 1,4-butyrolactone, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, or ethyl butyrate, and the total mass fraction of the solvent accounts for 70% to 90% of the total mass fraction of the electrolyte. The electrolyte additive is selected from at least one of vinylene carbonate, fluoroethylene carbonate, vinyl sulfate, methanedisulfonate, 1,3-propanesulfonate lactone, and tris(trimethylsilane) phosphate, and the total mass fraction of the additive accounts for 0.5% to 5% of the total mass fraction of the electrolyte.

16. The method for preparing a secondary battery according to claim 14, characterized in that, The mass ratio of negative electrode active material, conductive agent, thickener and binder in the negative electrode slurry is (94-98):(0-2):(1-2):(1-3).