Synergistic high-silicon anode sheet with single-walled carbon nanotube gradient conductive network and ion-selective surface layer, preparation method and lithium-ion battery

By constructing a single-walled carbon nanotube gradient conductive network and setting an ion-selective surface layer in the active layer of the silicon-based anode, the problems of conductive network breakage and electrolyte side reactions caused by volume expansion and contraction during the charging and discharging process of silicon-based anode materials are solved, thereby improving the internal resistance and cycle life of the battery.

CN123120643APending Publication Date: 2026-11-17DANYANG XINGYUAN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611623351.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively solve the problems of conductive network breakage and electrolyte side reactions caused by volume expansion and contraction during the charging and discharging process of silicon-based anode materials. In particular, in high areal capacity thick electrodes, the lack of conductive framework near the current collector and the exposure of surface carbon nanotubes lead to increased internal resistance and reduced cycle life.

Method used

A gradient conductive network of single-walled carbon nanotubes is constructed in the active layer of a silicon-based anode, with a high content on the side closer to the current collector and a low content on the side farther from the current collector. An ion-selective surface layer is set on the outer surface to block the electrolyte solvent molecules from contacting the silicon-based active material. Combined with pre-lithiation treatment, a synergistic effect is formed between the gradient conductive network and the ion-selective surface layer.

Benefits of technology

It significantly reduces the internal resistance of the electrode, reduces side reactions, improves structural stability and cycle life, and extends the battery cycle capacity retention rate, thus solving the technical pain points of high areal capacity thick silicon anode electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120643A_ABST
    Figure CN123120643A_ABST
Patent Text Reader

Abstract

This invention belongs to the technical field of modified high-silicon anode plates, and particularly relates to a high-silicon anode plate, its preparation method, and a lithium-ion battery, which is a combination of a single-walled carbon nanotube gradient conductive network and an ion-selective surface layer. The plate includes a copper foil current collector, a silicon-based anode active layer, and an ion-selective surface layer. The silicon-based anode active layer is disposed on the surface of the copper foil current collector. The single-walled carbon nanotubes within the silicon-based anode active layer are distributed in a gradient decreasing direction along the thickness of the plate. The side closer to the copper foil current collector is a high-single-walled carbon nanotube framework region, and the side closer to the electrolyte is a low-single-walled carbon nanotube reaction region. The ion-selective surface layer is coated on the outer surface of the silicon-based anode active layer away from the copper foil current collector. The ion-selective surface layer allows lithium ions to pass through while inhibiting electrolyte solvent molecules from contacting the silicon-based active material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of modified high-silicon anode plates, and particularly relates to a high-silicon anode plate with a single-walled carbon nanotube gradient conductive network and an ion-selective surface layer working synergistically, its preparation method, and a lithium-ion battery. Background Technology

[0002] Silicon-based anodes, with their theoretical specific capacity far exceeding that of traditional graphite anodes, are core candidate anode materials for high-energy-density lithium-ion batteries. However, silicon materials undergo significant volume expansion and contraction during charging and discharging, which can easily lead to the breakage of the internal conductive network and the pulverization and shedding of active material particles. Especially when preparing high-area-capacity thick silicon anode sheets, the increased sheet thickness further exacerbates the internal electron transport resistance. If the conductive agent is uniformly distributed, insufficient conductive framework near the current collector will increase the internal resistance of the sheet. Furthermore, excessive carbon nanotubes on the surface will expose a large amount of high specific surface area, inducing continuous decomposition side reactions in the electrolyte, resulting in a continuous increase in battery interface impedance and a rapid decline in cycle life.

[0003] Existing methods for improving silicon anodes mostly focus on modifying the silicon material itself or optimizing the overall electrode conductivity system, with few methods specifically designed to create differentiated conductive structures along the thickness of thick electrodes. At the same time, relying solely on material modification is still insufficient to prevent direct contact between the electrolyte solvent and the silicon active material, resulting in significant initial irreversible capacity loss. The side reaction problems caused by repeated breakage and reconstruction of the SEI film remain prominent. Furthermore, pre-lithiation technology is difficult to effectively coordinate with the internal conductive structure and surface protection strategies in high-silicon thick electrodes, thus limiting the practical application of high areal capacity silicon anodes. Summary of the Invention

[0004] In view of the aforementioned problems, and in conjunction with the first aspect of the present invention, the present invention provides a high-silicon anode electrode sheet in which a single-walled carbon nanotube gradient conductive network and an ion-selective surface layer work together, comprising a copper foil current collector, a silicon-based anode active layer, and an ion-selective surface layer. The silicon-based anode active layer is disposed on the surface of the copper foil current collector. The single-walled carbon nanotubes inside the silicon-based anode active layer are distributed in a gradient decreasing direction along the thickness of the electrode sheet. The side closer to the copper foil current collector is a high single-walled carbon nanotube framework region, and the side closer to the electrolyte is a low single-walled carbon nanotube reaction region. The ion-selective surface layer is coated on the outer surface of the silicon-based negative electrode active layer away from the copper foil current collector. The ion-selective surface layer allows lithium ions to pass through and inhibits electrolyte solvent molecules from contacting the silicon-based active material.

[0005] Preferably, the high-silicon anode electrode surface area capacity is 4.5-6.2 mAh / cm². 2 The compacted density is 1.55 g / cm³. 3 ; The mass content ratio of single-walled carbon nanotubes in the high single-walled carbon nanotube framework region to that in the low single-walled carbon nanotube reaction region is 5:1.

[0006] Preferably, the thickness of the ion-selective surface layer is 0.3-1.2 μm; The ion-selective surface layer is an organic lithium polymer composite inorganic lithium salt particle system. The organic lithium polymer is selected from at least one of lithium polyacrylic acid and lithium alginate, and the inorganic lithium salt particles are selected from at least one of nano lithium phosphate and lithium niobate nanoparticles. The solid mass ratio of the organic lithium polymer to the inorganic lithium salt particles is 7:3 to 8:2.

[0007] Preferably, based on the total solid mass of the silicon-based anode active layer, it comprises 55-85 parts of silicon-based active material, 0.08-0.90 parts of single-walled carbon nanotubes, 0.20-1.50 parts of auxiliary conductive agent, and 2-18 parts of binder; The silicon-based active material is selected from one or more of nano-silicon, silicon suboxide, silicon-carbon composite materials, and carbon-coated silicon-based materials; The auxiliary conductive agent is selected from one or more of conductive carbon black, Ketjen black, graphene, and carbon nanofibers; The adhesive is selected from one or more of lithium-ion polyacrylic acid, sodium carboxymethyl cellulose-styrene-butadiene rubber composite, lithium-ion alginate, and polyimide.

[0008] Preferably, the adhesive is a composite adhesive of lithium-ion polyacrylic acid and styrene-butadiene rubber, wherein the solid mass ratio of lithium-ion polyacrylic acid to styrene-butadiene rubber is 2:1-6:1. The high-silicon anode sheet undergoes a stable lithium powder contact pre-lithiation treatment, with the amount of lithium replenishment corresponding to 15%-40% of the initial irreversible capacity of the electrode sheet.

[0009] A method for preparing the high-silicon negative electrode sheet includes the following steps: S1. Preparation of single-walled carbon nanotube dispersion: Single-walled carbon nanotubes, bile salt dispersant, and cellulose thickener are dispersed in deionized water, and then dispersed under high shear and ultrasonic conditions. Large agglomerates are removed by filtration to obtain single-walled carbon nanotube dispersion. S2. Prepare high single-walled carbon nanotube slurry A and low single-walled carbon nanotube slurry B respectively. The amount of single-walled carbon nanotubes added in slurry A is greater than that in slurry B. S3. Gradient coating: Wet-on-wet coating, co-extrusion coating, multiple coating, penetration or electric field-assisted orientation coating are used on the copper foil current collector. Slurry A is close to the copper foil current collector, and slurry B is facing the outside of the electrode to form a silicon-based negative electrode active wet film with a gradient distribution of single-walled carbon nanotubes. S4. Drying and calendering: After the wet film is pre-dried in sections and vacuum dried, it is rolled to obtain a gradient conductive negative electrode substrate; S5. Constructing an ion-selective surface layer: Prepare a surface treatment solution and spray it onto the surface of a gradient conductive negative electrode substrate. After curing, a high-silicon negative electrode sheet is obtained.

[0010] Preferably, in step S1, the single-walled carbon nanotubes have a purity ≥90%, an average diameter of 1.4 nm, and a length of 5-20 μm. The mass ratio of single-walled carbon nanotubes, sodium cholate, and sodium carboxymethyl cellulose is 6:3:1. High shearing speed 1500-2500 r / min, shearing for 30 min; Ultrasonic frequency 20-40kHz, power 100-300W, ultrasonic treatment for 20 minutes; Aggregation was removed by filtration using a 5μm filter membrane, and the temperature of the dispersion system was controlled at 15-30℃.

[0011] Preferably, the total thickness of the wet film in step S3 is 150-220 μm; When using double-layer slit synchronous co-extrusion, the flow ratio of slurry A to slurry B is 1:1-3:1; When using three-layer co-extrusion, the mass ratio of single-walled carbon nanotubes near the current collector layer, the middle layer, and the surface layer is 5:2:1, and the wet film thickness ratio of the three layers is 2:2:1. When using electric field-assisted orientation, apply a DC or pulsed electric field of 0.1-5V / mm for 10s-5min.

[0012] Preferably, the segmented pre-drying temperatures in step S4 are 60-80℃, 80-100℃, and 100-120℃ respectively; Vacuum drying conditions: 110-130℃, drying for 6-12 hours; In step S5, the surface treatment liquid content is 1.5%, the solvent is deionized water and isopropanol with a mass ratio of 8:2, the curing temperature is 90℃, and the curing time is 30min. After calendering and before spraying the surface treatment liquid, pre-lithiation is performed: under an inert environment with a dew point ≤ -40℃, stabilized lithium powder is added at a concentration of 0.3-1.5 mg / cm³. 2 Apply the areal density to the electrode surface, apply a light pressure of 0.5-2.0 MPa for 1-5 minutes, and let it stand in an inert atmosphere for 2-12 hours to remove unreacted lithium powder.

[0013] A lithium-ion battery comprising a positive electrode, an electrolyte, and a high-silicon negative electrode sheet in synergy between a single-walled carbon nanotube gradient conductive network and an ion-selective surface layer.

[0014] Based on the above, a conductive network of single-walled carbon nanotubes with a gradient decreasing along the thickness direction is constructed inside the active layer of the silicon-based negative electrode. The high content of single-walled carbon nanotubes on the current collector side constructs a long-range continuous conductive framework, which can buffer the volume deformation caused by the charging and discharging of silicon-based materials, maintain the electron transport path inside the thick electrode, and reduce the overall internal resistance of the electrode. At the same time, the low single-walled carbon nanotube reaction zone on the surface reduces the exposure of high specific surface area carbon materials, effectively weakens the electrolyte side reactions induced by carbon materials, alleviates the generation and propagation of electrode cracks during charging and discharging, and improves the structural stability and peel strength of the electrode.

[0015] An ion-selective surface layer on the outer surface of the electrode enables selective lithium-ion permeability, preventing electrolyte solvent molecules from directly contacting the silicon-based active material and inhibiting repeated breakage and reconstruction of the SEI film. Combined with optional pre-lithiation treatment to compensate for the initial irreversible capacity loss, the gradient conductive network, the ion-selective surface layer, and the pre-lithiation process work synergistically to achieve a capacity of 4.5-6.2 mAh / cm³. 2 Under high areal capacity conditions, it effectively slows down the growth of battery interface impedance, significantly improves battery cycle capacity retention, and solves the technical pain points of high areal capacity thick silicon anode sheets such as high internal resistance, serious side reactions and poor cycle life. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of a high-silicon anode electrode sheet, a preparation method thereof, and a thickness direction gradient structure of a high-silicon anode electrode sheet for lithium-ion batteries, provided by an embodiment of the present invention, which is a synergistic structure of a single-walled carbon nanotube gradient conductive network and an ion-selective surface layer. Figure 2 This is a schematic diagram of the process of preparing a high-silicon anode electrode, a preparation method, and a lithium-ion battery, which is provided by an embodiment of the present invention, through the synergistic effect of a single-walled carbon nanotube gradient conductive network and an ion-selective surface layer. Figure 3 This is a schematic diagram illustrating the synergistic effect of the gradient distribution of single-walled carbon nanotubes and the ion-selective surface layer in a high-silicon anode electrode, its preparation method, and the lithium-ion battery provided by an embodiment of the present invention. Detailed Implementation

[0017] The present invention will now be described in detail with reference to the accompanying drawings.

[0018] The following examples are used to further illustrate the present invention, but should not be construed as limiting the scope of protection of the present invention.

[0019] Example 1: Preparation of high-silicon anode sheet using gradient single-walled carbon nanotubes; (1) Preparation of single-walled carbon nanotube dispersion: Single-walled carbon nanotubes with a purity of over 90%, an average tube diameter of about 1.4 nm, and a length of 5 to 20 μm were added to deionized water; a dispersion system was constructed with bile salt dispersant and a small amount of cellulose thickener, and the dispersion was subjected to high shear dispersion for 30 minutes, low-power ultrasonication for 20 minutes, and large agglomerates were removed by 5 μm filtration membrane to obtain a single-walled carbon nanotube dispersion with a solid content of 0.3% by weight.

[0020] (2) Preparation of high single-walled carbon nanotube slurry A: By weight, take 35 parts of silicon-carbon composite material, 50 parts of artificial graphite, 0.60 parts of single-walled carbon nanotube, 0.40 parts of conductive carbon black, and 14 parts of lithium-ionized polyacrylic acid and styrene-butadiene rubber composite binder, add an appropriate amount of deionized water, and stir under vacuum to obtain slurry A.

[0021] (3) Preparation of low single-walled carbon nanotube slurry B: By weight, take 35 parts of silicon-carbon composite material, 50 parts of artificial graphite, 0.12 parts of single-walled carbon nanotube, 0.30 parts of conductive carbon black, and 14.58 parts of lithium-ionized polyacrylic acid and styrene-butadiene rubber composite binder, add an appropriate amount of deionized water, and stir under vacuum to obtain slurry B.

[0022] (4) Gradient coating: On a copper foil current collector with a thickness of 8 micrometers, slurry A is first coated, and then slurry B is continuously coated by wet-on-wet method, so that slurry A is close to the current collector and slurry B is close to the electrode surface. The total thickness of the wet film is controlled to be between 150 micrometers and 220 micrometers.

[0023] (5) Drying and calendering: After pre-drying at 80 degrees Celsius and vacuum drying at 120 degrees Celsius, the electrode sheet is calendered to an areal capacity of about 4.5 mA / cm² and a compaction density of 1.55 g / cm³.

[0024] (6) Construction of ion-selective surface layer: Prepare a surface treatment solution containing lithium-ionized polyacrylic acid and nano-lithium phosphate particles with a solid mass ratio of 7:3. The solution is precisely sprayed onto the electrode surface to form an ion-selective surface layer of about 0.6 micrometers, and then cured at 90 degrees Celsius for 30 minutes.

[0025] In the resulting negative electrode, a region rich in single-walled carbon nanotube framework is formed near the current collector, while a relatively sparse region of single-walled carbon nanotubes is formed near the electrolyte. This structure ensures the continuity of the conductive network in the thick electrode while reducing the surface side reaction interface.

[0026] Example 2: High areal capacity, high silicon anode sheet; The negative electrode sheet was prepared according to the method of Example 1, but the silicon-carbon composite material was adjusted to 45 parts by weight, the artificial graphite was adjusted to 40 parts by weight, the amount of single-walled carbon nanotubes in slurry A was 0.90 parts by weight, the amount of single-walled carbon nanotubes in slurry B was 0.18 parts by weight, and the capacity of the negative electrode sheet after calendering was controlled at 6.2 mA / cm².

[0027] The surface ion-selective layer employs a composite system of lithium-ionized alginate and lithium niobate nanoparticles, with a thickness of approximately 1.2 micrometers. After assembling a full cell using the NCM811 cathode, the capacity retention rate can reach over 80% after 200 cycles at 0.5C. Compared with a comparative electrode with the same total single-walled carbon nanotube content but uniform distribution, the interfacial impedance increases more slowly, and the surface cracks of the electrode are significantly reduced.

[0028] Example 3: Pre-lithiation gradient electrode After the negative electrode sheet was prepared according to Example 1, it was pre-lithiated by a light pressure contact method with stabilized lithium powder, so that the amount of lithium replenishment corresponded to 15% to 40% of the initial irreversible capacity. After pre-lithiation, a lithium phosphate / lithiated polyacrylic acid composite surface layer with a thickness of about 0.3 micrometers was constructed.

[0029] The full cell assembled with lithium iron phosphate cathode showed better capacity retention than the un-pre-lithiated sample after 300 cycles under 1C charge-discharge conditions; and it also maintained low polarization under 2C fast charging conditions, indicating that the gradient single-walled carbon nanotube network can synergize with the surface layer and the pre-lithiation strategy.

[0030] Comparative illustration; Comparative Example 1 used the same total amount of single-walled carbon nanotubes as Example 1, but the nanotubes were uniformly distributed throughout the entire electrode thickness direction, and no ion-selective surface layer was provided. Test results showed that while this comparative example improved initial conductivity, after 100 cycles, the accumulation of side reaction products on the electrode surface was significant, and the interfacial impedance increased more rapidly.

[0031] Comparative Example 2 uses low single-walled carbon nanotubes with uniform distribution and a surface layer, but the conductive framework on the current collector side is insufficient, the internal resistance of the thick electrode is high, and the polarization is obvious under high rate and high areal capacity conditions.

[0032] Therefore, it can be seen that the present invention can significantly improve the overall performance of high silicon anode by combining the design of "high single-walled carbon nanotube framework on the current collector side + low single-walled carbon nanotube reaction zone on the electrolyte side + ion-selective surface layer".

[0033] Process deformation methods; This invention is not limited to the specific embodiments described above. Without departing from the concept of this invention, the following modifications can be made: 1. Gradient formation can be achieved through double-layer slit synchronous co-extrusion, triple-layer co-extrusion, continuous multiple coatings, local penetration migration, or electric field-assisted directional construction.

[0034] 2. Single-walled carbon nanotubes can be used in composite systems with different length gradations or different degrees of surface functionalization to further optimize the mechanical and electrical balance between the framework region and the reaction region.

[0035] 3. The surface ion-selective surface layer can be further incorporating fluoropolymers, borates, sulfonates, lithium salt complex monomers, or inorganic ionic conductors to adapt to different electrolyte systems.

[0036] 4. This invention is also applicable to various silicon-based anode systems such as silicon-oxygen, silicon-tin, silicon-graphite, and silicon-hard carbon.

[0037] Material definition and preferred range; The binder can be one or more selected from lithium-ion polyacrylic acid, polyacrylic acid, sodium carboxymethyl cellulose and styrene-butadiene rubber composite, lithium-ion alginate, polyimide, or polyvinylidene fluoride. Based on 100 parts by weight of the total solid mass of the negative electrode active layer, the binder is preferably 2 to 18 parts by weight, more preferably 5 to 15 parts by weight. The solid mass ratio of the aqueous lithium-ion polyacrylic acid and styrene-butadiene rubber composite binder is preferably 2:1 to 6:1.

[0038] The auxiliary conductive agent can be selected from one or more of conductive carbon black, acetylene black, Ketjen black, graphene, carbon nanofibers, or vapor-grown carbon fibers; its dosage is preferably 0.10 to 5.00 parts by weight, more preferably 0.20 to 1.50 parts by weight. The auxiliary conductive agent is used to establish short-range particle contact, and single-walled carbon nanotubes are used to establish long-range conductive and tough networks across particles and layers.

[0039] Silicon-based active materials can be nano-silicon, silicon suboxide, silicon-carbon composite materials, silicon-based materials with a carbon coating, or combinations thereof; graphite materials can be natural graphite, artificial graphite, soft carbon, hard carbon, or combinations thereof. To provide specific implementation examples to support the above concepts, the following supplementary examples cover combinations of silicon suboxide and natural graphite, nano-silicon and hard carbon, and coated silicon and soft carbon, respectively.

[0040] Example 1 Parameter Supplement; In the single-walled carbon nanotube dispersion, the mass ratio of single-walled carbon nanotubes, sodium cholate, and sodium carboxymethyl cellulose was 6:3:1; the mass fractions of the three components, based on the total mass of the dispersion, were 0.30%, 0.15%, and 0.05%, respectively. The dispersion was first subjected to high shear at 1500–2500 rpm for 30 minutes, followed by ultrasonication at 20–40 kHz and 100–300 W for 20 minutes, and finally filtered through a 5-micron filter membrane. The dispersion temperature was controlled between 15 and 30 degrees Celsius.

[0041] In Example 1, 14 parts by weight of the composite adhesive consisted of 10.5 parts by weight of lithium-ionized polyacrylic acid and 3.5 parts by weight of styrene-butadiene rubber. The ion-selective surface treatment solution had a solid content of 1.5%, and the solvent was deionized water and isopropanol in a mass ratio of 8:2. The solid mass ratio of lithium-ionized polyacrylic acid to lithium phosphate particles with an average particle size of 50 to 200 nanometers was 7:3.

[0042] Wet-on-wet coating is carried out in an environment of 20 to 28 degrees Celsius and relative humidity of 30% to 60%. Slurry B is applied within 5 to 30 seconds after slurry A is applied. The viscosities of slurry A and slurry B are controlled at 3000 to 8000 mPa·s and 2000 to 6000 mPa·s, respectively, and the coating speed is 0.5 to 5 m / min. The staged drying temperatures are 60 to 80 degrees Celsius, 80 to 100 degrees Celsius, and 100 to 120 degrees Celsius, respectively, followed by drying under vacuum at 110 to 130 degrees Celsius for 6 to 12 hours.

[0043] Supplement to the pre-lithiation step; Stabilized lithium powder contact pre-lithiation is performed in a dry environment with a dew point not exceeding -40°C. Stabilized lithium powder is evenly spread or transferred onto the surface of the rolled electrode at a rate of 0.3 to 1.5 mg / cm², and gently pressed for 1 to 5 minutes with a linear pressure of 0.5 to 2.0 MPa to ensure sufficient contact between the stabilized lithium powder and the surface. After standing in an inert atmosphere for 2 to 12 hours, unreacted particles are removed, and then the ion-selective surface layer is constructed. The lithium replenishment is targeted at 15% to 40% of the initial irreversible capacity, calculated using the areal density of the stabilized lithium powder.

[0044] Supplementary Examples; Example 4 uses a silica-substrate and natural graphite system. The high single-walled carbon nanotube slurry contains 30 parts by weight of silica-substrate, 55 parts by weight of natural graphite, 0.50 parts by weight of single-walled carbon nanotubes, 0.50 parts by weight of conductive carbon black, and 14.00 parts by weight of composite binder; the low single-walled carbon nanotube slurry contains 0.10 parts by weight of single-walled carbon nanotubes, 0.40 parts by weight of conductive carbon black, and 14.50 parts by weight of composite binder, with the remaining active materials unchanged. A gradient layer is formed by simultaneous co-extrusion of two slits, and the surface is coated with a composite layer of lithium-ion alginate and lithium phosphate in a mass ratio of 8:2.

[0045] Example 5 uses a nano-silicon and hard carbon system. The high single-walled carbon nanotube slurry contains 20 parts by weight of nano-silicon, 65 parts by weight of hard carbon, 0.40 parts by weight of single-walled carbon nanotubes, 0.40 parts by weight of Ketjen black, and 14.20 parts by weight of lithium-ionized polyacrylic acid binder; the low single-walled carbon nanotube slurry contains 0.08 parts by weight of single-walled carbon nanotubes, 0.30 parts by weight of Ketjen black, and 14.62 parts by weight of binder. A three-layer continuous coating is used, with the ratio of single-walled carbon nanotubes in the high, medium, and low single-walled carbon nanotube layers being 5:2:1.

[0046] Example 6 uses a silicon-based material with a carbon-coated surface and a soft carbon system. The high single-walled carbon nanotube slurry contains 40 parts by weight of coated silicon, 45 parts by weight of soft carbon, 0.80 parts by weight of single-walled carbon nanotubes, 0.30 parts by weight of graphene, and 13.90 parts by weight of polyimide binder; the low single-walled carbon nanotube slurry contains 0.16 parts by weight of single-walled carbon nanotubes, 0.20 parts by weight of graphene, and 14.64 parts by weight of binder. A gradient infiltration method is used to allow the single-walled carbon nanotube dispersion to infiltrate from the current collector side to the upper layers.

[0047] Double-layer slit synchronous co-extrusion: High single-walled carbon nanotube slurry and low single-walled carbon nanotube slurry are fed into a dual-channel die head, with the flow ratio controlled between 1:1 and 3:1. The total thickness of the wet film is 150 to 220 micrometers. The two layers are coated synchronously after merging at the die lip.

[0048] Three-layer co-extrusion: Three slurries were prepared with single-walled carbon nanotube contents of 0.60, 0.25 and 0.08 parts by weight in the current collector layer, the middle layer and the surface layer, respectively. The wet film thickness ratio of each layer was 2:2:1. The slurries were simultaneously extruded and then dried in stages.

[0049] Multiple coatings are applied consecutively: first, a high single-walled carbon nanotube slurry is applied and pre-dried until the solvent residue is 20% to 50%, then a low single-walled carbon nanotube slurry is applied; the interval between the two coatings is 10 seconds to 5 minutes to maintain interpenetration of the interface without complete mixing.

[0050] Localized penetration or electric field-assisted orientation: First, a bottom layer containing single-walled carbon nanotubes is formed on the current collector side, and then a top layer with low single-walled carbon nanotubes is coated; while the top layer is still wet, a DC or pulsed electric field of 0.1 to 5 V / mm is applied for 10 seconds to 5 minutes, or a dispersion is added from the current collector side and the penetration depth is controlled to form a continuous concentration gradient.

[0051] The high content of single-walled carbon nanotubes on the current collector side bridges silicon-based particles, graphite particles, and copper foil, maintaining long-range conductive pathways and dispersing interfacial stresses during silicon volume changes. The lower content of single-walled carbon nanotubes on the electrolyte side reduces the exposure of high-surface-area carbon, and the ion-selective surface layer further restricts the continuous contact of solvent molecules with the active surface. The combined effect of these three factors should be verified through comparative studies with the same areal capacity, same compaction density, and same total solids composition.

[0052]

[0053] The above ranges are given under the conditions of the same isal capacity, same compaction density, and same silicon content. Publicly available studies have demonstrated that porous / hierarchical structures, gradient conductive networks, gradient binders, and pre-lithiation can mitigate silicon volumetric effects or first irreversible losses; therefore, the evaluation focus of this application should be on the improvement in resistance, cracking, and cycle retention relative to a uniform SWCNT network, rather than pursuing a single absolute capacity record. It should be noted that, in order to simplify the description of the present invention and thus help to understand one or more embodiments of the invention, multiple features may sometimes be grouped into one embodiment, drawing or description thereof in the foregoing description of the embodiments of the present invention.

[0054] The embodiments of this application have been described above with reference to the accompanying drawings. Unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other. This application is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of this application without departing from the spirit and scope of the claims, and all of these forms are within the protection scope of this application.

Claims

1. A high-silicon anode electrode sheet with a synergistic single-walled carbon nanotube gradient conductive network and an ion-selective surface layer, characterized in that: It includes a copper foil current collector, a silicon-based negative electrode active layer, and an ion-selective surface layer; The silicon-based anode active layer is disposed on the surface of the copper foil current collector. The single-walled carbon nanotubes inside the silicon-based anode active layer are distributed in a gradient decreasing direction along the thickness of the electrode sheet. The side closer to the copper foil current collector is a high single-walled carbon nanotube framework region, and the side closer to the electrolyte is a low single-walled carbon nanotube reaction region. The ion-selective surface layer is coated on the outer surface of the silicon-based negative electrode active layer away from the copper foil current collector. The ion-selective surface layer allows lithium ions to pass through and inhibits electrolyte solvent molecules from contacting the silicon-based active material.

2. The high-silicon negative electrode sheet according to claim 1, characterized in that, The high-silicon negative pole piece has a surface capacity of 4.5-6.2 mAh / cm 2 , and a compacted density of 1.55 g / cm 3 ; The mass content ratio of single-walled carbon nanotubes in the high single-walled carbon nanotube framework region to that in the low single-walled carbon nanotube reaction region is 5:

1.

3. The high-silicon negative electrode sheet according to claim 1, characterized in that, The thickness of the ion-selective surface layer is 0.3-1.2 μm; The ion-selective surface layer is an organic lithium polymer composite inorganic lithium salt particle system. The organic lithium polymer is selected from at least one of lithium polyacrylic acid and lithium alginate, and the inorganic lithium salt particles are selected from at least one of nano lithium phosphate and lithium niobate nanoparticles. The solid mass ratio of the organic lithium polymer to the inorganic lithium salt particles is 7:3 to 8:

2.

4. The high-silicon negative electrode sheet according to claim 1, characterized in that, Based on the total solid mass of the silicon-based anode active layer, it contains 55-85 parts of silicon-based active material, 0.08-0.90 parts of single-walled carbon nanotubes, 0.20-1.50 parts of auxiliary conductive agent, and 2-18 parts of binder; The silicon-based active material is selected from one or more of nano-silicon, silicon suboxide, silicon-carbon composite materials, and carbon-coated silicon-based materials; The auxiliary conductive agent is selected from one or more of conductive carbon black, Ketjen black, graphene, and carbon nanofibers; The adhesive is selected from one or more of lithium-ion polyacrylic acid, sodium carboxymethyl cellulose-styrene-butadiene rubber composite, lithium-ion alginate, and polyimide.

5. The high-silicon negative electrode sheet according to claim 4, characterized in that, The adhesive is a composite adhesive of lithium-ion polyacrylic acid and styrene-butadiene rubber, with a solid mass ratio of lithium-ion polyacrylic acid to styrene-butadiene rubber of 2:1-6:

1. The high-silicon anode sheet undergoes a stable lithium powder contact pre-lithiation treatment, with the amount of lithium replenishment corresponding to 15%-40% of the initial irreversible capacity of the electrode sheet.

6. A method for preparing a high-silicon negative electrode sheet according to any one of claims 1-5, characterized in that, Includes the following steps: S1. Preparation of single-walled carbon nanotube dispersion: Single-walled carbon nanotubes, bile salt dispersant, and cellulose thickener are dispersed in deionized water, and then dispersed under high shear and ultrasonic conditions. Large agglomerates are removed by filtration to obtain single-walled carbon nanotube dispersion. S2. Prepare high single-walled carbon nanotube slurry A and low single-walled carbon nanotube slurry B respectively. The amount of single-walled carbon nanotubes added in slurry A is greater than that in slurry B. S3. Gradient coating: Wet-on-wet coating, co-extrusion coating, multiple coating, penetration or electric field-assisted orientation coating are used on the copper foil current collector. Slurry A is close to the copper foil current collector, and slurry B is facing the outside of the electrode to form a silicon-based negative electrode active wet film with a gradient distribution of single-walled carbon nanotubes. S4. Drying and calendering: After the wet film is pre-dried in sections and vacuum dried, it is rolled to obtain a gradient conductive negative electrode substrate; S5. Constructing an ion-selective surface layer: Prepare a surface treatment solution and spray it onto the surface of a gradient conductive negative electrode substrate. After curing, a high-silicon negative electrode sheet is obtained.

7. The preparation method according to claim 6, characterized in that, In step S1, the single-walled carbon nanotubes have a purity ≥90%, an average diameter of 1.4 nm, and a length of 5-20 μm. The mass ratio of single-walled carbon nanotubes, sodium cholate, and sodium carboxymethyl cellulose is 6:3:

1. High shearing speed 1500-2500 r / min, shearing for 30 min; Ultrasonic frequency 20-40kHz, power 100-300W, ultrasonic treatment for 20 minutes; Aggregation was removed by filtration using a 5μm filter membrane, and the temperature of the dispersion system was controlled at 15-30℃.

8. The preparation method according to claim 6, characterized in that, In step S3, the total thickness of the wet film is 150-220 μm; When using double-layer slit synchronous co-extrusion, the flow ratio of slurry A to slurry B is 1:1-3:1; When using three-layer co-extrusion, the mass ratio of single-walled carbon nanotubes near the current collector layer, the middle layer, and the surface layer is 5:2:1, and the wet film thickness ratio of the three layers is 2:2:

1. When using electric field-assisted orientation, apply a DC or pulsed electric field of 0.1-5V / mm for 10s-5min.

9. The preparation method according to claim 6, characterized in that, The segmented pre-drying temperatures in step S4 are 60-80℃, 80-100℃, and 100-120℃ respectively. Vacuum drying conditions: 110-130℃, drying for 6-12 hours; In step S5, the surface treatment liquid content is 1.5%, the solvent is deionized water and isopropanol with a mass ratio of 8:2, the curing temperature is 90℃, and the curing time is 30min. After the rolling is completed, before the surface treatment liquid is sprayed, pre-lithiation is carried out: under the inert environment with a dew point ≤-40℃, the stabilized lithium powder is 0.3-1.5 mg / cm 2 The surface density of the electrode piece is applied to the surface, and the surface is lightly pressed for 1-5 min under a pressure of 0.5-2.0 MPa, and then is placed in an inert atmosphere for 2-12 h, and the unreacted lithium powder is removed.

10. A lithium-ion battery, characterized in that, It includes a positive electrode, an electrolyte, and a high-silicon negative electrode sheet as described in any one of claims 1-5, which combines a single-walled carbon nanotube gradient conductive network with an ion-selective surface layer.