Titanium-based compound-coated Prussian blue compounds, their preparation methods and applications
By coating the surface of Prussian blue compounds with titanium-based compounds to form a protective layer, the problem of structural instability of Prussian blue compounds was solved, thus improving the electrochemical performance of sodium-ion batteries.
Patent Information
- Application Number
- CN202611424098.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
Prussian blue compounds are prone to introducing lattice water molecules and interstitial water molecules during synthesis, leading to structural instability and affecting the electrochemical performance of sodium-ion batteries.
A titanium-based compound coating layer is used to cover Prussian blue compounds, forming a dense protective layer that reduces interstitial water content and promotes sodium ion diffusion kinetics.
It effectively stabilizes the crystal structure, suppresses structural collapse, improves the sodium storage capacity and cycle life of sodium-ion batteries, reduces interfacial impedance, and optimizes the electrode/electrolyte interface.
Smart Images

Figure CN123120720A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion battery cathode materials, and in particular to a titanium-based compound-coated Prussian blue compound, its preparation method, and its application. Background Technology
[0002] Sodium-ion batteries have become a competitive new type of energy storage battery due to their advantages such as abundant sodium resources, low cost, and long lifespan. Sodium is abundant in the Earth's crust, with a more even distribution than lithium resources. Moreover, sodium-based raw materials are inexpensive, and production equipment can be reused from lithium-ion battery production lines, reducing costs. At the same time, sodium-ion batteries have a long cycle life, slow capacity decay, and also feature rapid charging and discharging and wide temperature range operation, making them a promising candidate for large-scale energy storage and other fields.
[0003] Prussian blue analogues (PBAs) have become highly competitive cathode active materials for sodium-ion batteries due to their open three-dimensional framework structure, low cost, ease of preparation, and high theoretical capacity. However, the synthesis of Prussian blue analogues easily introduces a large number of lattice water molecules and interstitial water molecules. These water molecules are distributed on the surface or in the interstices of the material, occupying sodium ion migration channels. After decomposition at high potentials, they continue to react with the electrolyte, causing a decline in battery cycle performance. Furthermore, during battery charging and discharging, lattice water molecules migrate or are removed during the insertion / extraction of sodium ions. The migration of lattice water molecules generates stress, while the loss of water molecules disrupts the stability of the original structure, leading to the collapse of the skeletal structure of the Prussian blue analogues. This results in initial capacity loss and long-cycle capacity decay, severely affecting the electrochemical performance of sodium-ion batteries.
[0004] To address the aforementioned problems, existing technologies mainly employ modification strategies such as oxide coating, carbon coating, sulfide coating, or element doping. However, oxide coatings have extremely low electrical conductivity, which is detrimental to electron transport; carbon coating processes are complex, and high-temperature treatment may damage the Prussian blue structure; sulfide coatings are easily oxidized and decomposed at high potentials; and element doping cannot completely eliminate the influence of interstitial water. Therefore, there is an urgent need to develop a novel surface modification technology that can effectively reduce interstitial water content, stabilize the crystal structure, and promote sodium ion diffusion kinetics. Summary of the Invention
[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a titanium-based compound-coated Prussian blue compound, its preparation method and application, aiming to solve the problems of poor crystal structure stability and high interstitial water content in the existing coating modification methods of Prussian blue compounds, which lead to poor electrochemical performance.
[0006] To achieve the above objectives, the present invention adopts the following technical solution: Firstly, a Prussian blue-like compound coated with a titanium-based compound, the chemical formula of which is: A x M a [M b (CN)6] 1-y ·□ y ·nH₂O; where 0 ≤ x ≤ 3, 0 ≤ y < 1, 0 ≤ n ≤ 20; in this chemical formula, A is an alkali metal, alkaline earth metal, or a mixture thereof, M a and M b These represent different transition metal elements, and □ represents [M]. b The vacancies are created by the absence of the (CN)6] group; the surface of the Prussian blue compounds is coated with a titanium-based compound coating layer, with a coverage of 80%-100%.
[0007] Secondly, a method for preparing a Prussian blue-like compound coated with a titanium-based compound, the method comprising: Step 1: Add a cyanide containing A to the first solvent and stir at room temperature to obtain a first solution; wherein, A is an alkali metal or an alkaline earth metal; Step 2: Add a transition metal M salt and a chelating agent to the second solvent, and stir at room temperature to obtain a second solution; wherein, M is M a Or M b At least one of them; Step 3: Mix the first solution and the second solution in a water bath, stir, and then age. After aging, centrifuge, wash, and vacuum dry to prepare the Prussian blue matrix material. Step 4: Weigh the Prussian blue matrix material and disperse it in anhydrous ethanol to form a suspension. Weigh the titanium source material to prepare a titanium source precursor solution. Slowly add the titanium source precursor solution to the suspension and add deionized water to fully hydrolyze the titanium source. Continue stirring to uniformly coat the Prussian blue matrix material with titanium-based compounds. After filtration and drying, obtain the Prussian blue-like compound coated with titanium-based compounds.
[0008] Further, in step 1, the first solvent includes one or more of deionized water, ethanol, and ethylene glycol; in step 2, the second solvent includes one or more of deionized water, ethanol, and ethylene glycol, the transition metal M salt includes one or more of sulfate, gluconate, citrate, chloride, and nitrate, and the chelating agent includes sodium citrate.
[0009] Further, in step 3, the second solution is poured into a 250mL three-necked flask and placed in a 50℃ water bath; the first solution is slowly added dropwise to the second solution at a flow rate of 3mL / min using a peristaltic pump, with continuous stirring at a stirring speed of 400rpm during the addition; the centrifugation speed is 8000rpm, the separation time is 5 minutes, and the solution is washed 3 times each with deionized water and ethanol, and then vacuum dried at 80℃ for 12 hours; the aging treatment temperature is 20-80℃, and the aging treatment time is 4h-24h.
[0010] Furthermore, in step 4, the mass ratio of the titanium source material to the Prussian blue matrix material is 1:100-1:10.
[0011] Furthermore, in step 4, the drying temperature is 100-140℃ and the time is 8-16 hours.
[0012] Further, in step 4, the dried Prussian blue matrix material is placed in a mortar and ground thoroughly. 2.0g of the ground Prussian blue matrix material is weighed and added to 30mL of anhydrous ethanol and ultrasonically dispersed for 20 minutes.
[0013] Furthermore, in step 4, the titanium source material includes one or more of isopropyl titanate, tetraethyl titanate, and tetrabutyl titanate.
[0014] Furthermore, in step 4, the molar ratio of deionized water to titanium source material is (2-10):1, the hydrolysis reaction time is 1-4 hours, and the temperature is ambient temperature and pressure.
[0015] The titanium-based compounds include, but are not limited to, titanium dioxide (TiO2) and lithium titanate (Li4Ti5O). 12 One or more of sodium titanate (Na2Ti3O7) or sodium titanate (Na2Ti3O7).
[0016] Thirdly, the application of a titanium-based compound-coated Prussian blue compound, wherein the titanium-based compound-coated Prussian blue compound is used to prepare a positive electrode sheet for a sodium-ion battery, the positive electrode sheet comprising a current collector and a positive electrode active material layer located on at least one side of the current collector, the positive electrode active material layer comprising a Prussian blue compound; the surface of the Prussian blue compound is coated with a titanium-based compound coating layer, the coverage of the titanium-based compound coating layer is 80%-100%, and the titanium-based compound coating layer is in direct contact with the surface of the Prussian blue compound particles; the thickness of the titanium-based compound coating layer is 1-50 nm.
[0017] The technical solution adopted in this invention has the following beneficial effects: In this invention, a titanium-based compound coating forms a dense protective layer on the surface of Prussian blue-like compounds, preventing moisture from entering the material interstices and reducing the formation of interstitial water. Simultaneously, the titanium source reacts with adsorbed water on the material surface during the coating process, further reducing the material's water content. During cycling, the coating layer suppresses the collapse of the Prussian blue framework structure, maintaining the integrity of the crystal structure and effectively mitigating volume changes during sodium ion insertion / extraction. Furthermore, the titanium-based compound coating layer possesses moderate ionic conductivity, which is beneficial for the rapid transport of sodium ions, optimizing the electrode / electrolyte interface, reducing interfacial impedance, and promoting sodium ion diffusion kinetics.
[0018] Furthermore, this invention can coat Prussian blue prepared with different metal elements to form Prussian blue-like compounds with different metal elements, thereby ensuring the universality of this invention. Attached Figure Description
[0019] Figure 1 These are the X-ray diffraction (XRD) patterns of the Prussian blue matrix material and the titanium source-coated Prussian blue material prepared in Example 1 of this application; Figure 2 This is a comparison of the first charge-discharge curves of the cathode materials prepared in Example 1 and Comparative Example 1 of this application at a rate of 0.1C. Detailed Implementation
[0020] To make the objectives, technical solutions, and effects of this invention clearer and more explicit, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the invention.
[0021] Firstly, the chemical formula of Prussian blue compounds is: A x M a [M b (CN)6] 1-y ·□ y ·nH₂O; where 0 ≤ x ≤ 3, 0 ≤ y < 1, 0 ≤ n ≤ 20; in this chemical formula, A is an alkali metal, an alkaline earth metal, or a mixture thereof, M a and M b These represent different transition metal elements, and □ represents [M]. b The vacancies are created by the absence of the (CN)6] group; the surface of the Prussian blue compounds is coated with a titanium-based compound coating layer, with a coverage of 80%-100%.
[0022] Prussian blue compounds, through surface coating with titanium-based compounds, effectively reduce interstitial water content, stabilize the crystal structure during cycling, and promote sodium ion diffusion kinetics. This not only enhances the sodium storage capacity of the battery but also effectively suppresses the capacity decay problem of sodium-ion batteries during long-term cycling.
[0023] Secondly, a method for preparing a Prussian blue-like compound coated with a titanium-based compound, the method comprising: Step 1: Add a cyanide containing A to the first solvent and stir at room temperature to obtain a first solution; wherein, A is an alkali metal or an alkaline earth metal; Step 2: Add a transition metal M salt and a chelating agent to the second solvent, and stir at room temperature to obtain a second solution; wherein, M is M a Or M b At least one of them; Step 3: Mix the first solution and the second solution in a water bath, stir, and then age. After aging, centrifuge, wash, and vacuum dry to prepare the Prussian blue matrix material. Step 4: Weigh the Prussian blue matrix material and disperse it in anhydrous ethanol to form a suspension. Weigh the titanium source material to prepare a titanium source precursor solution. Slowly add the titanium source precursor solution to the suspension and add deionized water to fully hydrolyze the titanium source. Continue stirring to uniformly coat the Prussian blue matrix material with titanium-based compounds. After filtration and drying, obtain the Prussian blue-like compound coated with titanium-based compounds.
[0024] During the coating process, titanium-based materials can react with adsorbed water on the material surface, further reducing the water content of the material.
[0025] In this embodiment, in step 1, the first solvent includes one or more of deionized water, ethanol, and ethylene glycol; these first solvents can dissolve sodium ferrocyanide.
[0026] In step 2, the second solvent includes one or more of deionized water, ethanol, and ethylene glycol, which can dissolve the ferrous source and the chelating agent; the transition metal M salt includes one or more of sulfate, gluconate, citrate, chloride, and nitrate, which can provide electrochemical reactivity; the chelating agent includes sodium citrate; as a strong complexing agent, sodium citrate can rapidly complex with ferrous ions through carboxyl groups in the early stage of the reaction, reducing the concentration of free ferrous ions in the reaction system, thereby effectively controlling the nucleation rate of Prussian blue-like compound crystals in the early stage of the reaction and promoting uniform growth of crystal nuclei.
[0027] In this embodiment, in step 3, the second solution is poured into a 250 mL three-necked flask and placed in a 50 °C water bath. The first solution is slowly added dropwise to the second solution using a peristaltic pump at a flow rate of 3 mL / min, with continuous stirring at a stirring speed of 400 rpm during the addition process. The centrifugation speed is 8000 rpm, and the separation time is 5 minutes. The solution is washed three times each with deionized water and ethanol, and then vacuum dried at 80 °C for 12 hours. The aging temperature is 20-80 °C, and the aging time is 4-24 hours, preferably 20 °C for 12 hours. This allows the reaction to proceed fully, giving the crystals sufficient time to grow and perfect their structure.
[0028] In this embodiment, in step 4, the mass ratio of titanium source material to Prussian blue matrix material is 1:1000-1:10; this can control the thickness and content of the coating layer, avoiding insufficient protection due to an excessively thin coating layer or hindering ion transport due to an excessively thick coating layer. Preferably, the ratio is 1:20, which can stabilize the protection effect at the optimal level and ensure the electro-ion transport capability and the conductivity of Prussian blue compounds.
[0029] In this embodiment, in step 4, the drying temperature is 100-140℃ and the time is 8-16h, preferably 120℃ and preferably 12h, which can completely remove the solvent and residual moisture and obtain a dry coated product.
[0030] In this embodiment, in step 4, the dried Prussian blue matrix material is placed in a mortar and ground thoroughly. 2.0g of the ground Prussian blue matrix material is weighed and added to 30mL of anhydrous ethanol and ultrasonically dispersed for 20 minutes to prepare a suspension.
[0031] In this embodiment, in step 4, the titanium source material includes one or more of isopropyl titanate, tetraethyl titanate, and tetrabutyl titanate. These titanium sources can form a uniform titanium-based compound coating layer on the Prussian blue surface.
[0032] In this embodiment, in step 4, the molar ratio of deionized water to titanium source material is (2-10):1, the hydrolysis reaction time is 1-4 hours, and the temperature is normal temperature and pressure, which can fully hydrolyze the titanium source and uniformly adsorb it on the surface of the material particles to form a stable coating layer.
[0033] Thirdly, the application of a titanium-based compound-coated Prussian blue compound, wherein the titanium-based compound-coated Prussian blue compound is used to prepare a positive electrode sheet for a sodium-ion battery, the positive electrode sheet comprising a current collector and a positive electrode active material layer located on at least one side of the current collector, the positive electrode active material layer comprising a Prussian blue compound; the surface of the Prussian blue compound is coated with a titanium-based compound coating layer, the coverage of the titanium-based compound coating layer is 80%-100%, and the titanium-based compound coating layer is in direct contact with the surface of the Prussian blue compound particles; the thickness of the titanium-based compound coating layer is 1-50 nm.
[0034] The following specific embodiments illustrate the solution of this application. It should be noted that, unless otherwise specified in the embodiments, the techniques or conditions described in the literature in this field or in accordance with the product instructions are followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional products.
[0035] Example 1
[0036] The preparation of Prussian blue compounds includes the following steps: S100. Add 4.84 g of sodium ferrocyanide decahydrate (Na4Fe(CN)6·10H2O) to 100 mL of deionized water and stir at room temperature for 30 minutes to obtain the first solution. S200. Add 2.78g of ferrous sulfate heptahydrate (FeSO4·7H2O) and 1.47g of sodium citrate to 100mL of deionized water, and stir at room temperature for 30 minutes to obtain the second solution. S300. Pour the second solution into a 250 mL three-necked flask and place it in a 50 °C water bath. Use a peristaltic pump to slowly add the first solution dropwise to the second solution at a flow rate of 3 mL / min, while continuously stirring at a speed of 400 rpm. After the addition is complete, stop stirring and age at room temperature for 12 hours. After aging, centrifuge (8000 rpm, 5 minutes), wash three times each with deionized water and ethanol, and then vacuum dry at 80 °C for 12 hours to obtain the Prussian blue matrix material. S400. The dried Prussian blue matrix material was thoroughly ground in a mortar. 2.0 g of the ground Prussian blue matrix material was weighed and added to 30 mL of anhydrous ethanol and ultrasonically dispersed for 20 minutes. 0.1 g of isopropyl titanate was measured with a pipette and dissolved in anhydrous ethanol. The solution was stirred to form a uniform and transparent precursor solution. The precursor solution was slowly added dropwise to the Prussian blue suspension. Deionized water in the same proportion as isopropyl titanate was added to fully hydrolyze the isopropyl titanate into titanium dioxide (amorphous titanium dioxide). The mixture was stirred continuously at room temperature and pressure for 1 h to allow the titanium source to be uniformly adsorbed onto the surface of the material particles. Subsequently, the suspension was filtered, and the resulting filter cake was transferred to a vacuum drying oven and dried at 120 °C for 12 h to obtain a titanium source-coated Prussian blue compound (denoted as PB@Ti-1).
[0037] Example 2
[0038] The difference from Example 1 is that the amount of isopropyl titanate used in step S400 is 0.2g, while the remaining steps are the same as in Example 1, to obtain a titanium source coated Prussian blue compound (denoted as PB@Ti-2).
[0039] Example 3
[0040] The difference from Example 1 is that the amount of isopropyl titanate used in step S400 is 0.05g, while the remaining steps are the same as in Example 1, to obtain a titanium source coated Prussian blue compound (denoted as PB@Ti-0.5).
[0041] Example 4
[0042] The difference from Example 1 is that in step S400, 0.15g of tetrabutyl titanate is used to replace an equal amount of isopropyl titanate, while the remaining steps are the same as in Example 1, to obtain a titanium source coated Prussian blue compound (denoted as PB@Ti(OBu)4).
[0043] Example 5
[0044] The difference from Example 1 is that in step S400, 0.15g of tetraethyl titanate is used to replace an equal amount of isopropyl titanate, while the remaining steps are the same as in Example 1, to obtain a titanium source coated Prussian blue compound (denoted as PB@Ti(OEt)4).
[0045] Comparative Example 1 The difference from Example 1 is that the titanium source coating treatment in step S400 is not performed, and only the Prussian blue matrix material is ground and used as the positive electrode material (denoted as PB).
[0046] Preparation of positive electrode sheet The Prussian blue compound, conductive agent Super P carbon black, and binder polyvinylidene fluoride (PVDF) prepared above were added to N-methylpyrrolidone (NMP) solvent in a weight ratio of 8:1:1 and stirred evenly to prepare a positive electrode slurry. The positive electrode slurry was coated on aluminum foil and dried under vacuum at 80°C for 12 hours to obtain a positive electrode sheet.
[0047] Battery assembly The positive electrode, sodium metal negative electrode, electrolyte, and separator prepared above were assembled into a CR2032 coin cell in a glove box with oxygen and water content both below 0.1 ppm. The separator was made of glass fiber (Whatman GF / D); the electrolyte was a 1M NaPF6 solution with propylene carbonate (PC) as the solvent and 5 wt% fluoroethylene carbonate (FEC) as an additive.
[0048] Performance testing 1. The interstitial water content of the Prussian blue compounds in Examples 1-5 and Comparative Example 1 was tested using thermogravimetric analysis (TGA) at a temperature range of 25-300°C and a heating rate of 10°C / min.
[0049] 2. Sodium storage capacity test: At a 0.1C rate, the voltage range is 2.0-4.0V (vs. Na). + / Na), test the first discharge specific capacity.
[0050] 3. Cycle life test: At 1C rate, voltage range 2.0-4.0V (vs. Na) + / Na), and after 100 cycles, the capacity retention rate is tested.
[0051] 4. Rate performance test: Cycle 5 times at each of the following rates: 0.1C, 0.2C, 0.5C, 1C, 2C and 5C, and test the discharge specific capacity at different rates.
[0052] 5. Electrochemical Impedance Spectroscopy (EIS) Test: Before cycling and after 100 cycles, test the AC impedance in the frequency range of 100kHz-10mHz.
[0053] Test method for coverage The coating coverage rate was obtained by analyzing images from scanning electron microscopy (SEM) or transmission electron microscopy (TEM). At least 10 fields of view were randomly selected, and the ratio of the coating area to the particle surface area was calculated and the average value was taken.
[0054] Test Results The test results of Examples 1-5 and Comparative Example 1 are shown in Table 1.
[0055]
[0056] As shown in Table 1, the interstitial water content of Examples 1-5 was significantly lower than that of Comparative Example 1, indicating that the titanium-based compound coating effectively improved the electrochemical performance of Prussian blue compounds. The sodium storage capacity and cycle life of Examples 1-5 were superior to those of Comparative Example 1, with the sodium storage capacity increasing from 104.0 mAh g⁻¹. -1 Increased to 120.7 mAh g -1 After 100 cycles, the capacity retention rate increased from 78.2% to 93.5%.
[0057] Figure 1 It is an XRD pattern, composed of Figure 1 It can be seen that the titanium source-coated Prussian blue material prepared in Example 1 and the Prussian blue matrix material in Comparative Example 1 both maintained the typical crystal structure of Prussian blue and no obvious impurity phase peaks appeared. This indicates that the titanium source coating did not destroy the crystal structure of Prussian blue and effectively suppressed the collapse of the Prussian blue framework structure, maintaining the integrity of the crystal structure.
[0058] Figure 2 It is a comparison chart of charge and discharge curves, from Figure 2 It can be seen that, at a rate of 0.1C and a voltage range of 2.0-4.0V, the initial discharge specific capacity of Example 1 is 120.7 mAh g. -1 It exhibits a higher reversible discharge specific capacity. The titanium-based compound modified Prussian blue effectively suppressed structural distortion during the charge and discharge process, reduced electrochemical polarization, made the voltage plateau more stable, and improved the discharge specific capacity.
Claims
1. A Prussian blue-like compound coated with a titanium-based compound, characterized in that, The chemical formula of Prussian blue compounds is: A x M a [M b (CN)6] 1-y ·□ y ·nH2O; Wherein, 0 ≤ x ≤ 3, 0 ≤ y < 1, 0 ≤ n ≤ 20; in this chemical formula, A is an alkali metal, an alkaline earth metal, or a mixture thereof, and M... a and M b These represent different transition metal elements, and □ represents [M]. b The vacancies are created by the absence of the (CN)6] group; the surface of the Prussian blue compounds is coated with a titanium-based compound coating layer, with a coverage of 80%-100%.
2. A method for preparing a Prussian blue-like compound coated with a titanium-based compound as described in claim 1, characterized in that, Preparation methods include: Step 1: Add a cyanide containing A to the first solvent and stir at room temperature to obtain a first solution; wherein, A is an alkali metal or an alkaline earth metal; Step 2: Add a transition metal M salt and a chelating agent to the second solvent, and stir at room temperature to obtain a second solution; wherein, M is M a Or M b At least one of them; Step 3: Mix the first solution and the second solution in a water bath, stir, and then age. After aging, centrifuge, wash, and vacuum dry to prepare the Prussian blue matrix material. Step 4: Weigh the Prussian blue matrix material and disperse it in anhydrous ethanol to form a suspension. Weigh the titanium source material to prepare a titanium source precursor solution. Slowly add the titanium source precursor solution to the suspension and add deionized water to fully hydrolyze the titanium source. Continue stirring to uniformly coat the Prussian blue matrix material with titanium-based compounds. After filtration and drying, obtain the Prussian blue-like compound coated with titanium-based compounds.
3. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 1, the first solvent includes one or more of deionized water, ethanol, and ethylene glycol; in step 2, the second solvent includes one or more of deionized water, ethanol, and ethylene glycol, the transition metal M salt includes one or more of sulfate, gluconate, citrate, chloride, and nitrate, and the chelating agent includes sodium citrate.
4. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 3, the second solution is poured into a 250 mL three-necked flask and placed in a 50 °C water bath. The first solution is slowly added dropwise to the second solution using a peristaltic pump at a flow rate of 3 mL / min, with continuous stirring at a stirring speed of 400 rpm during the addition process. The centrifugation speed is 8000 rpm, the separation time is 5 minutes, and the solution is washed 3 times each with deionized water and ethanol. Then, it is vacuum dried at 80 °C for 12 hours. The aging treatment temperature is 20-80 °C, and the aging treatment time is 4-24 hours.
5. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 4, the mass ratio of titanium source material to Prussian blue matrix material is 1:1000-1:
10.
6. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 4, the drying temperature is 100-140℃ and the time is 8-16 hours.
7. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 4, the dried Prussian blue matrix material is placed in a mortar and ground thoroughly. 2.0g of the ground Prussian blue matrix material is weighed and added to 30mL of anhydrous ethanol and ultrasonically dispersed for 20 minutes.
8. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 4, the titanium source material includes one or more of isopropyl titanate, tetraethyl titanate, and tetrabutyl titanate.
9. The method for preparing Prussian blue-like compounds coated with titanium-based compounds according to claim 2, characterized in that, In step 4, the molar ratio of deionized water to titanium source material is (2-10):1, the hydrolysis reaction time is 1-4 hours, and the temperature is ambient temperature and pressure.
10. The application of a Prussian blue compound coated with a titanium-based compound as described in claim 1, characterized in that, A titanium-based compound coated with Prussian blue-like compounds is used to prepare a positive electrode sheet for a sodium-ion battery. The positive electrode sheet includes a current collector and a positive active material layer located on at least one side of the current collector. The positive active material layer includes a Prussian blue-like compound. The surface of the Prussian blue-like compound is coated with a titanium-based compound coating layer, which is 80%-100% thick and in direct contact with the surface of the Prussian blue-like compound particles. The thickness of the titanium-based compound coating layer is 1-50 nm.