Battery cells, battery packs and electrical devices

By introducing additives such as SeS2 and SeO2 into the positive electrode film layer to react with the electrolyte to generate selenium/lithium sulfate, forming a CEI film and long-chain polymer, the capacity decay problem caused by the instability of the positive electrode and electrolyte interface in traditional battery systems is solved, and the cycle performance and safety performance of the battery are improved.

CN123120730APending Publication Date: 2026-11-17CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510633476.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional battery systems generally face capacity decay during long-term cycling, mainly due to instability caused by interfacial side reactions between the cathode and electrolyte, and structural degradation caused by electrolyte penetration.

Method used

Introducing positive electrode additives such as SeS2, SeO2, and metal selenides into the positive electrode film layer allows them to react with sulfur-containing additives in the electrolyte to generate selenium/lithium sulfate, forming a fast ion conductor CEI film. This enhances interfacial stability and Li ion transport performance, and the resulting long-chain polymers further enhance mechanical strength and suppress interfacial side reactions.

Benefits of technology

It improves the interfacial stability between the cathode and the electrolyte, reduces structural degradation, improves the cycle performance of individual cells, reduces internal resistance, and enhances electrochemical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120730A_ABST
    Figure CN123120730A_ABST
Patent Text Reader

Abstract

This application provides a battery cell, a battery device, and an electrical device. The battery cell includes a positive electrode and an electrolyte. The positive electrode includes a positive current collector and a positive electrode film. The positive electrode film includes a positive active material and a positive additive. The positive additive includes one or more of SeS2, SeO2, and metal selenides. The electrolyte includes an electrolyte additive, which includes sulfur-containing additives, including one or more of sulfate esters, thiols, or thiocarbonates. The combination of the above-mentioned positive electrode additive and electrolyte additive can improve the interfacial mechanical strength and stability between the positive electrode and the electrolyte, improve Li-ion transport performance, and improve the cycle performance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a battery cell, a battery device, and an electrical device. Background Technology

[0002] With the rapid development of new energy vehicles and the energy storage industry, the demand for high-energy-density lithium-ion batteries is becoming increasingly urgent. However, traditional battery systems generally face the challenge of capacity decay during long-term cycling, which severely restricts battery life. In existing technologies, improvements to the cathode are mostly focused on surface coating or bulk doping. Although these can suppress structural degradation in the short term, they are difficult to prevent capacity decay caused by interfacial side reactions triggered by electrolyte penetration. Summary of the Invention

[0003] This application provides a battery cell, a battery device, and an electrical device to improve the interfacial stability between the positive electrode and the electrolyte and improve the cycle performance of the battery cell.

[0004] The first aspect of this application provides a battery cell, which includes a positive electrode sheet and an electrolyte. The positive electrode sheet includes a positive current collector and a positive electrode film. The positive electrode film includes a positive active material and a positive additive. The positive additive includes one or more of SeS2, SeO2, and metal selenides. The electrolyte includes an electrolyte additive. The electrolyte additive includes a sulfur-containing additive. The sulfur-containing additive includes one or more of sulfate ester additives, thiol additives, or thiocarbonate additives.

[0005] The aforementioned cathode additives can react with residual lithium on the surface of the cathode active material during formation and early charge / discharge cycles, transforming into selenium / lithium sulfate. Selenium / lithium sulfate, acting as a fast-ion conductor CEI film, can improve the interfacial stability between the cathode and the electrolyte, as well as Li-ion transport performance. Simultaneously, selenium / lithium sulfate can also polymerize with sulfur-containing additives in the electrolyte, generating a structure with long-chain polymers. This structure not only enhances the mechanical strength and stability of the cathode-electrolyte interface and reduces structural degradation of the cathode material, thus improving interfacial stability and enhancing the cycle performance of the battery cell.

[0006] In any embodiment of the first aspect, the mass content of Se element in the positive electrode film layer is 0.05%-7%. Introducing Se element within the above-mentioned mass range into the positive electrode film layer can form a relatively sufficient selenium / lithium sulfate and CEI film on the positive electrode surface. On the one hand, selenium / lithium sulfate promotes interfacial charge transfer, and on the other hand, the CEI film better suppresses the occurrence of interfacial side reactions, thereby improving the cycle performance of the battery cell based on better lithium-ion transport.

[0007] In any embodiment of the first aspect, the mass content of the positive electrode additive in the positive electrode film layer is 0.02%-5%. The presence of a positive electrode additive within this range in the positive electrode film layer enables dynamic consumption-residue balance of the positive electrode additive, continuously compensating for and constructing a new CEI film during subsequent long-term cyclic charge-discharge processes, maintaining structural stability, and simultaneously avoiding excessive film formation leading to impedance growth.

[0008] In any embodiment of the first aspect, the average particle size of the positive electrode additive is 0.005 μm to 2.5 μm. Optionally, the average particle size of the positive electrode additive is 5 nm to 520 nm. An average particle size within the above range allows for sufficient dispersion of the positive electrode additive and the positive electrode active material, which is beneficial for fully realizing their aforementioned effects.

[0009] In any embodiment of the first aspect, the electrolyte additive includes a sulfate ester additive, which includes a chain sulfate ester or a cyclic sulfate ester. The sulfate ester additive undergoes a chemical cross-linking reaction with lithium selenate and / or lithium sulfate formed on the positive electrode surface, thereby improving electrochemical and mechanical stability, reducing interfacial impedance, and providing lithium-ion conduction channels, thus synergistically improving the safety and cycle performance of the battery cell.

[0010] In any embodiment of the first aspect, the chain sulfate comprises a compound having the following general formula I:

[0011] General Formula I: R 1 -O-SO2R 2 ,

[0012] Among them, R 1 and R 2 Independently comprising any one of substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, or substituted or unsubstituted C6-C12 aryl, R 1 and R 2 The substituents include any one of halogens and C1-C3 alkyl groups.

[0013] In any implementation of the first aspect, R 1 and R 2 Independently comprising any one of substituted or unsubstituted C1-C6 alkyl groups or substituted or unsubstituted C2-C4 alkenyl groups, R 1 and R 2 The substituents include any one of halogens and C1-C3 alkyl groups.

[0014] In any embodiment of the first aspect, the chain sulfate ester includes one or more of monoethyl sulfate, dimethyl sulfate, methyl ethyl sulfate, diethyl sulfate, triethyl sulfate, bis(trifluoromethyl) sulfate, dipropyl sulfate, isopropyl sulfate, dibutyl sulfate, dipentyl sulfate, dihexyl sulfate, or dipropylene sulfate.

[0015] In any embodiment of the first aspect, the cyclic sulfate additive comprises a compound having the following general formula II:

[0016]

[0017] Among them, R 3 R 4 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C6 alkyl group, Any one of them; R 5 Including any one of substituted or unsubstituted C1-C6 alkyl groups, R 3 R 4 and R 5 The substituents include any one of halogens and C1-C3 alkyl groups.

[0018] In any implementation of the first aspect, R 3 R 4 Each independently includes a hydrogen atom, a C1-C3 alkyl group, Any one of them; R 5 Including any one of C1-C3 alkyl groups.

[0019] In any embodiment of the first aspect, the cyclic sulfate additive includes one or two of vinylene sulfate (DTD), divinylene sulfate, and trivinylene sulfate.

[0020] In any embodiment of the first aspect, the thiol additive includes one or more of methanethiol, ethanethiol, propanethiol, isopropanethiol, butanethiol, pentathiol, or halothiol; and / or the thiocarbonate additive includes one or more of trithiocarbonate, dithiocarbonate, monothiocarbonate, bis(trifluoromethyl)thiocarbonate, dimethylthiocarbonate, diethylthiocarbonate, and methylethylthiocarbonate.

[0021] In any embodiment of the first aspect, the mass content of the sulfur-containing additive in the electrolyte is 0.05%-0.3%, and / or the mass content of the sulfur-containing additive in the electrolyte is 0.1%-1%. The above-mentioned mass content of sulfur-containing additive can form a sufficient CEI film during the formation stage, thereby suppressing the interfacial reaction between the positive electrode and the electrolyte, and also avoids the increase in electrolyte viscosity caused by the addition of excessive sulfur-containing additive.

[0022] In any embodiment of the first aspect, the electrolyte further includes a solvent. Optionally, the solvent includes cyclic carbonates and chain carbonates; optionally, the cyclic carbonate includes one or more of ethylene carbonate and propylene carbonate, and the chain carbonate includes one or more of dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate.

[0023] In any embodiment of the first aspect, the cyclic carbonate in the solvent accounts for 30%-70% by mass.

[0024] In any embodiment of the first aspect, the positive electrode film layer further includes a conductive polymer, optionally at least partially coated on the surface of the positive electrode additive. Adding a conductive polymer to the positive electrode film layer can significantly improve electron conduction efficiency and further suppress direct contact between the positive electrode active material and the electrolyte, reducing interfacial side reactions. Its flexible long-chain structure can also buffer volume changes during charging and discharging, reducing the risk of particle breakage and enhancing the mechanical strength of the electrode.

[0025] In any embodiment of the first aspect, the conductive polymer includes one or more of polyaniline, polypyrrole, polythiophene, or polyacrylonitrile.

[0026] In any embodiment of the first aspect, the positive electrode film layer includes a conductive polymer with a mass content of 0.001%-1%.

[0027] In any embodiment of the first aspect, the positive electrode active material comprises a nickel-containing lithium transition metal oxide. Optionally, the nickel-containing lithium layered transition metal oxide comprises a lithium-containing nickel-cobalt-manganese oxide or a lithium-containing nickel-cobalt-aluminum oxide.

[0028] In any embodiment of the first aspect, the nickel-containing lithium transition metal oxide includes the compound Li a Ni b Co c Mn d M e O 2-fWherein, M includes one or more elements selected from Al, Fe, Ti, Mg, Zr, Cr, Ga, Cu, Zn, Nb, and B; a is any value in the range of 0.4-1.2, and can be selected as any value in the range of 0.8-1.2; b is any value in the range of 0.45-0.95, and can be selected as any value in the range of 0.5-0.85; c is any value in the range of 0.02-0.25, and can be selected as any value in the range of 0.02-0.2; d is any value in the range of 0.05-0.5, and can be selected as any value in the range of 0.05-0.48; e is any value in the range of 0-0.2, and can be selected as any value in the range of 0.001-0.2; f is any value in the range of 0-0.3, and can be selected as any value in the range of 0-0.2.

[0029] A second aspect of this application provides a battery device including a battery cell, the battery cell including any embodiment of the battery cell provided in the first aspect.

[0030] A third aspect of this application provides an electrical device, including a battery cell or a battery device, wherein the battery cell includes the battery cell provided in any embodiment of the first aspect, and the battery device is the battery device provided in any embodiment of the second aspect. Attached Figure Description

[0031] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.

[0032] Figure 1 This is a schematic diagram of a secondary battery according to one embodiment of this application.

[0033] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of this application is shown.

[0034] Figure 3 This is a schematic diagram of a battery module according to one embodiment of this application.

[0035] Figure 4 This is a schematic diagram of a battery pack according to one embodiment of this application.

[0036] Figure 5 yes Figure 4 An exploded view of a battery pack according to one embodiment of this application is shown.

[0037] Figure 6This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.

[0038] The accompanying drawings are not drawn to scale.

[0039] Explanation of reference numerals in the attached figures:

[0040] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery cell; 51 Housing; 52 Electrode assembly; 53 Top cover assembly. Detailed Implementation

[0041] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.

[0042] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the positive electrode, negative electrode, battery cell, battery module, battery pack, and power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.

[0043] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0044] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.

[0045] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.

[0046] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0047] Unless otherwise specified, the terms "comprising" and "including" as used in this application are open-ended. For example, "comprising" and "including" may mean that other components not listed may also be included or contained.

[0048] Unless otherwise specified, the term "or" is inclusive in this application. For example, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0049] [Battery cell]

[0050] Due to their high surface activity, positive electrode materials are prone to irreversible side reactions with the electrolyte, leading to problems such as the formation of an unstable CEI film at the positive electrode-electrolyte interface, continuous electrolyte decomposition causing gas production, and ultimately capacity decay. To address these issues, the first embodiment of this application provides a battery cell comprising a positive electrode sheet and an electrolyte. The positive electrode sheet includes a positive current collector and a positive electrode film. The positive electrode film includes a positive electrode active material and a positive electrode additive. The positive electrode additive includes one or more of SeS2, SeO2, and metal selenides. The electrolyte includes an electrolyte additive, which includes sulfur-containing additives, including one or more of sulfate esters, thiols, or thiocarbonates.

[0051] The applicant unexpectedly discovered:

[0052] During the formation process and early charge / discharge stages, the aforementioned cathode additives can undergo in-situ chemical reactions with residual lithium (such as Li₂O and Li₂CO₃) on the cathode material surface to generate lithium selenate (Li₂SeO₄) and / or lithium sulfate (Li₂SO₄). This selenium / lithium sulfate acts as a fast ion conductor CEI layer, improving the interfacial stability between the cathode and the electrolyte, enhancing Li ion transport performance, and reducing battery internal resistance. Simultaneously, lithium selenate and / or lithium sulfate can polymerize with sulfur-containing additives in the electrolyte to form long-chain polymers with cross-linked structures. These polymers can suppress CEI film rupture caused by mechanical stress concentration, strengthening the mechanical properties of the interface. Furthermore, due to the enhanced CEI stability, interfacial side reactions can be better suppressed, gas generation can be inhibited, and electrochemical stability can be improved, thereby improving the cycle performance of the battery cell.

[0053] As analyzed above, the aforementioned positive electrode additives containing Se undergo chemical reactions during formation and cycling, leading to changes in their form. However, Se remains stable in the positive electrode. In some embodiments, the mass content of Se in the positive electrode film is 0.05%-7%, for example, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, or any two of the above values. Se content within the above mass range allows for the formation of a sufficiently thick selenium / lithium sulfate and CEI film on the positive electrode surface. This facilitates interfacial charge transfer using selenium / lithium sulfate and better suppresses interfacial side reactions using the CEI film, thereby improving the cycle performance of the battery cell while maintaining good lithium-ion transport.

[0054] The Se element content can be tested using the following method: After disassembling the positive electrode sheet from the battery cell, thoroughly clean the positive electrode sheet with DMC (dimethyl carbonate), and then dry and calcine the positive electrode sheet before collecting the positive electrode material in the positive electrode active layer. The positive electrode material is then tested using inductively coupled plasma atomic emission spectrometry (ICP-OES) or inductively coupled plasma mass spectrometry (ICP-MS). In some embodiments, the mass content of the positive electrode additive in the positive electrode film layer is 0.1%-10%, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any two of the above values. During the preparation of the positive electrode film, controlling the mass content of the positive electrode additive in the raw materials within the above-mentioned range is beneficial to the regulation of the selenium / lithium sulfate and long-chain polymers formed subsequently, thereby constructing a richer fast ion conductor CEI film and an organic long-chain CEI film, and realizing the synergistic effect of the two.

[0055] During the formation process and initial charge-discharge cycles, some of the positive electrode additive is consumed. In some embodiments, the mass content of the positive electrode additive in the positive electrode film is 0.02%-5%, for example, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.15%, 0.19%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 2%, 3%, 4%, 5%, or any two of the above values. Controlling the mass content of the positive electrode additive in the positive electrode film within the above range enables a dynamic consumption-residue balance of the positive electrode additive, continuously compensating for the formation of a new CEI film during subsequent long-term charge-discharge cycles, maintaining structural stability, and avoiding impedance growth caused by excessive film formation.

[0056] The mass content of the positive electrode additive in the positive electrode film can be detected by the following methods:

[0057] After the positive electrode sheet is disassembled from the battery cell, it is thoroughly cleaned with DMC (dimethyl carbonate), dried, and the positive electrode material in the positive active layer is collected. The positive electrode material is tested with an X-ray diffractometer, and the mass content of the positive electrode additive in the positive electrode film is calculated based on the spectrum obtained from the XRD test and the lattice parameter refinement (Rietveld method).

[0058] In some embodiments, the average particle size of the positive electrode additive is 0.005 μm-2.5 μm, for example 0.005 μm, 0.006 μm, 0.007 μm, 0.008 μm, 0.009 μm, 0.01 μm, 0.02 μm, 0.03 μm, 0.04 μm, 0.05 μm, 0.06 μm, 0.07 μm, 0.08 μm, 0.09 μm, 0.1 μm, 0.2 μm. The particle size ranges from 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2.0μm, 2.1μm, 2.2μm, 2.3μm, 2.4μm, 2.5μm, or any two of the above values. Using positive electrode additives within these particle size ranges allows for thorough dispersion with the positive electrode active material, facilitating the full realization of its aforementioned effects.

[0059] In some embodiments, the average particle size of the cathode additive is 5nm-520nm, for example, 5nm, 6nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm, 16nm, 17nm, 18nm, 19nm, 20nm, 23nm, 25nm, 27nm, 30nm, 35nm, 36nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 510nm, 520nm, or any two of the above values. Using nanoscale cathode additives can achieve full dispersion of cathode additives in cathode slurry, which is beneficial to the reaction of cathode additives with residual lithium on the surface of cathode active material; moreover, the same amount of cathode additives dispersed in smaller particles is beneficial to uniform dispersion in cathode film layer and provides a larger specific surface area, which is conducive to more efficient formation of denser and more uniform CEI film on cathode surface.

[0060] The average particle size of the positive electrode additive was measured using the following method:

[0061] The average particle size of the aforementioned positive electrode additive can be tested using equipment and methods known in the art. For example, a scanning electron microscope (e.g., ZEISS Sigma 300) can be used, referring to JY / T010-1996, to obtain a scanning electron microscope (SEM) image of the negative electrode sheet. As an example, the test can be performed as follows: Randomly select a test sample of length × width = 50 mm × 100 mm on the positive electrode sheet. Randomly select multiple test areas (e.g., 5 areas) within the test sample, and at a certain magnification (e.g., 1000x when measuring the positive electrode additive), read the particle size of each positive electrode additive particle in each test area (i.e., take the distance between the two farthest points on the positive electrode additive particle as the particle size). Count the number and particle size values ​​of the positive electrode additive particles in each test area, and take the arithmetic mean of the positive electrode additive particles in each test area, which is the number-average particle size of the positive electrode additive particles in the test sample. To ensure the accuracy of the test results, multiple test samples (e.g., 10) can be used to repeat the above test, and the average value of each test sample can be taken as the final test result. In some embodiments, the positive electrode active material may include at least one of the following materials: lithium phosphate, lithium transition metal oxide, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium phosphate may include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4, also referred to as LFP), lithium iron phosphate and carbon composites, lithium manganese phosphate (e.g., LiMnPO4), lithium manganese phosphate and carbon composites, lithium iron manganese phosphate, and lithium iron manganese phosphate and carbon composites. Examples of lithium transition metal oxide may include, but are not limited to, lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, and lithium nickel cobalt manganese oxide (e.g., LiNi). 1 / 3Co 1 / 3 Mn 1 / 3 O2, also known as NCM 333 LiNi 0.5 Co 0.2 Mn 0.3 O2, also known as NCM 523 LiNi 0.5 Co 0.25 Mn 0.25 O2, also known as NCM 211 LiNi 0.6 Co 0.2 Mn 0.2 O2, also known as NCM622 LiNi 0.8 Co 0.1 Mn 0.1 O2, also known as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.05 Al 0.05 At least one of O2 and its modified compounds. Modified compounds refer to substances obtained by modification methods such as doping or coating based on the above-mentioned substances.

[0062] In some embodiments, the positive electrode active material includes a nickel-containing lithium transition metal oxide. In some embodiments, the nickel-containing lithium layered transition metal oxide includes a lithium-containing nickel-cobalt-manganese oxide or a lithium-containing nickel-cobalt-aluminum oxide.

[0063] In some embodiments, the nickel-containing lithium transition metal oxide includes the compound Li. a Ni b Co c Mn d M e O 2-f Wherein, M includes one or more elements selected from Al, Fe, Ti, Mg, Zr, Cr, Ga, Cu, Zn, Nb, and B;

[0064] a can be any value in the range of 0.4-1.2, or any value in the range of 0.8-1.2; b can be any value in the range of 0.45-0.95, or any value in the range of 0.5-0.85; c can be any value in the range of 0.02-0.25, or any value in the range of 0.02-0.2; d can be any value in the range of 0.05-0.5, or any value in the range of 0.05-0.48; e can be any value in the range of 0-0.2, or any value in the range of 0.001-0.2; f can be any value in the range of 0-0.3, or any value in the range of 0-0.2.

[0065] In some embodiments, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0066] As an example, the positive current collector can be a metal foil, a conductive polymer material, a carbon material, or a composite current collector. For example, as a metal foil, pure metals, alloys, or surface-treated metals can be used, including but not limited to stainless steel, copper, aluminum, nickel, titanium, or silver. The composite current collector may include a polymer material base layer and a metal layer. The composite current collector can be formed by forming a metal material (aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0067] In the examples of positive electrode active materials in this application, the molar content of oxygen is only a theoretical value. Oxygen release from the crystal lattice will cause changes in the molar content of oxygen, and the actual molar content of oxygen will fluctuate.

[0068] In some embodiments, the positive electrode film layer also includes a conductive polymer. Adding a conductive polymer to the positive electrode film layer can significantly improve electron conduction efficiency, further suppress direct contact between the positive electrode active material and the electrolyte, reduce interfacial side reactions, and its flexible long-chain structure can also buffer volume changes during charging and discharging, reduce the risk of particle breakage, and enhance the mechanical strength of the electrode.

[0069] In some embodiments, at least a portion of the conductive polymer is coated on the surface of the positive electrode additive. When the conductive polymer is partially coated on the surface of the positive electrode additive, in addition to the inner layer of the positive electrode additive performing the functions described above, the coated conductive polymer shell can further reduce the contact resistance between the positive electrode active material and the positive electrode additive, improve charge transfer efficiency, and buffer volume strain through its elasticity.

[0070] In some embodiments, the conductive polymer includes one or more of polyaniline, polypyrrole, polythiophene, or polyacrylonitrile.

[0071] In some embodiments, the positive electrode film layer includes a conductive polymer with a mass content of 0.001%-1%, such as 0.001%, 0.002%, 0.003%, 0.004%, 0.005%, 0.006%, 0.007%, 0.008%, 0.009%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, or any two of the above values. This content range avoids excessive polymer blocking ion transport paths and effectively alleviates stress cracking during positive electrode cycling through its flexible molecular chains, ultimately optimizing both the rate performance and cycle life of the battery cell.

[0072] In some implementations, a conductive polymer can be first coated on the surface of the positive electrode additive, and then mixed with the positive electrode active material to form a positive electrode slurry. On the one hand, the conductive polymer can be used to improve the surface stability of the positive electrode additive in air, and on the other hand, the conductive polymer can be used to more effectively improve the impedance problem between the positive electrode additive and the positive electrode active material.

[0073] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0074] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0075] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, positive additive, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.

[0076] Electrolyte

[0077] The electrolyte plays a role in conducting ions between the positive and negative electrode plates.

[0078] In some embodiments, the electrolyte additive includes sulfate ester additives, which include chain sulfate esters or cyclic sulfate esters. The sulfate ester additives undergo a chemical cross-linking reaction with lithium selenate and / or lithium sulfate formed on the positive electrode surface, resulting in a CEI film comprising organic sulfate ester segments -[R-SO2-O-] that provide a flexible framework and adapt to volume changes. n - By incorporating an inorganic selenium / lithium sulfate moiety that enhances mechanical strength and thermal stability, this structure not only improves electrochemical and mechanical stability and reduces interfacial impedance, but also provides lithium-ion conduction channels, synergistically improving the safety and cycle performance of the battery cell. Chain-like sulfate additives can rapidly form a two-dimensional layered CEI film on the cathode surface, while cyclic sulfates, after ring-opening activation, can form a dense three-dimensional network CEI film on the cathode surface.

[0079] In some embodiments, the chain sulfate esters comprise compounds having the following general formula I:

[0080] General Formula I: R 1 -O-SO2R 2 ,

[0081] Among them, R 1 and R 2 Independently comprising any one of substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, or substituted or unsubstituted C6-C12 aryl, R 1 and R 2 The substituents include any one of halogens and C1-C3 alkyl groups.

[0082] In some implementations, R 1 and R 2 Independently comprising any one of substituted or unsubstituted C1-C6 alkyl groups or substituted or unsubstituted C2-C4 alkenyl groups, R 1 and R 2 The substituents include any one of halogens and C1-C3 alkyl groups.

[0083] In some embodiments, the chain sulfate esters include one or more of monoethyl sulfate, dimethyl sulfate, methyl ethyl sulfate, diethyl sulfate, bis(trifluoromethyl) sulfate, dipropyl sulfate, diisopropyl sulfate, dibutyl sulfate, dipentyl sulfate, dihexyl sulfate, or dipropylene sulfate.

[0084] In some embodiments, the cyclic sulfate additives include compounds having the following general formula II:

[0085]

[0086] Among them, R 3 R 4 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C6 alkyl group, Any one of them; R 5 Including any one of substituted or unsubstituted C1-C6 alkyl groups, said R 3 R 4 and R 5 The substituents include any one of halogens and C1-C3 alkyl groups.

[0087] In some implementations, R 3 R 4 Each independently includes a hydrogen atom, a C1-C3 alkyl group, Any one of them; R 5 Including any one of C1-C3 alkyl groups.

[0088] In some embodiments, the cyclic sulfate additives include one or two of vinylene sulfate (DTD), divinylene sulfate, and trivinylene sulfate.

[0089] In some embodiments, the thiol additive includes one or more of methanethiol, ethanethiol, propanethiol, isopropanethiol, butanethiol, pentathiol, or halothiols. The thiol additive can chemically crosslink with lithium selenate and / or lithium sulfate formed on the cathode surface. The resulting polydisulfide segments -[RSS-]n- provide elasticity, effectively buffering volume changes, while the selenium / sulfur crosslinking points enhance mechanical strength and stability.

[0090] In some embodiments, the thiocarbonate additives include one or more of trithiocarbonate, dithiocarbonate, monothiocarbonate, bis(trifluoromethyl)thiocarbonate, dimethylthiocarbonate, diethylthiocarbonate, and methyl ethylthiocarbonate. These thiocarbonate additives can chemically crosslink with lithium selenate and / or lithium sulfate formed on the cathode surface to generate a thiocarbonate polymer -[ROC(=S)-O-]n-, where the thiocarbonyl group (C=S) exhibits high reactivity, enhancing interfacial lithium-ion conductivity, guiding uniform Li+ deposition, and reducing lithium dendrites.

[0091] In some embodiments, the mass content of sulfur-containing additives in the electrolyte is 0.05%-0.3%, for example, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.15%, 0.17%, 0.18%, 0.19%, 0.2%, 0.25%, 0.3%, or any two of the above values. Controlling the mass content of sulfur-containing additives in the electrolyte within the above range enables the continuous formation of a suitable and dense interfacial film during the long-term charge-discharge cycle of the battery cell, while avoiding impedance increases due to excessive addition, thus achieving a balance between improved cycle performance and enhanced charging capacity.

[0092] The analysis of the above organic components in the electrolyte can be performed using gas chromatography. Standard solutions are prepared according to the formula, and both the standard solution and the sample are directly injected into the gas chromatography system for FID detection. After processing by the chromatograph, a chromatogram is obtained. Based on the retention time, peak shape, and other characteristics of each peak on the chromatogram, different components in the sample are identified. The content of each component is determined using methods such as peak area (peak height) percentage method, normalization method, internal standard method, external standard method, or standard addition method.

[0093] As an example, the types and contents of inorganic components / electrolyte salts in the electrolyte can be qualitatively or quantitatively analyzed using ion chromatography, referring to standard JY / T020-1996 "General Rules for Ion Chromatography Analysis". In the embodiments of this application, freshly prepared electrolytes can be used as samples, or the free electrolyte from a fresh battery can be used as a sample. Alternatively, a fully discharged battery (discharged to the lower cutoff voltage so that the battery's state of charge is approximately 0% SOC) can be disassembled in reverse, and the free electrolyte obtained from the battery can be used as a sample for detection using ion chromatography.

[0094] As an example, the types and contents of organic components in the electrolyte can be qualitatively and quantitatively analyzed by gas chromatography, referring to GB / T9722-2006 "General Rules for Gas Chromatography of Chemical Reagents". In the embodiments of this application, freshly prepared electrolytes can be used as samples, free electrolytes from fresh batteries can be used as samples, or batteries that have been completely discharged (discharged to the lower limit cutoff voltage so that the battery's state of charge is approximately 0% SOC) can be disassembled in reverse, and the free electrolytes obtained from the batteries can be used as samples for detection by ion chromatography.

[0095] Considering the consumption of sulfur-containing additives during formation and cycling, in some embodiments, the mass content of sulfur-containing additives in the electrolyte is 0.1%-1%, for example, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, or any two of the above values. The above-mentioned amounts of sulfur-containing additives can form a sufficient CEI film during the formation stage, thereby suppressing the interfacial reaction between the positive electrode and the electrolyte, and also avoid increasing the electrolyte viscosity due to excessive addition of sulfur-containing additives.

[0096] In some embodiments, the electrolyte may optionally include other additives. For example, the additives may include negative electrode film-forming additives, other positive electrode film-forming additives, and additives that can improve certain properties of the battery cell, such as additives that improve the overcharge / fast charge performance of the battery cell, additives that improve the high-temperature performance of the battery cell, and additives that improve the low-temperature performance of the battery cell.

[0097] In some embodiments, the electrolyte also includes a solvent. The solvent in the electrolyte can dissolve and transport electrolyte salts, construct Li+ transport channels, and regulate electrode interface chemistry.

[0098] In some embodiments, the solvent includes cyclic carbonates and linear carbonates. Cyclic carbonates possess high dielectric constants and strong lithium salt dissociation capabilities, preferentially participating in the formation of a dense inorganic interfacial film and improving interfacial stability. Linear carbonates have lower viscosity and a wide liquid phase range (-20 to 90°C), which can improve electrolyte wettability and ion migration rates. When used synergistically, the mixed solvent can balance high dielectric constant and low viscosity, ultimately simultaneously improving the battery's rate performance and cycle life.

[0099] In some embodiments, cyclic carbonates include one or more of ethylene carbonate and propylene carbonate, and chain carbonates include one or more of dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate.

[0100] In some embodiments, the mass percentage of cyclic carbonates in the solvent is 30%-70%, for example, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, or any two of the above values. Controlling the mass percentage of cyclic carbonates within this range balances the requirements for high dielectric properties and low viscosity: a higher proportion of cyclic carbonates (50%-70%) enhances lithium salt dissociation and interfacial film stability, while a lower proportion (30%-50%) optimizes low-temperature fluidity and ion migration rate. This ratio range allows the electrolyte to possess the combined advantages of high ionic conductivity, capacity retention, and low transition metal dissolution.

[0101] In some embodiments, the electrolyte also includes an electrolyte salt.

[0102] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.

[0103] [Negative electrode plate]

[0104] The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer including a negative electrode active material.

[0105] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0106] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0107] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0108] In some embodiments, the negative electrode film layer may optionally include a binder. As an example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0109] In some embodiments, the negative electrode film may optionally include a conductive agent. As an example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0110] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).

[0111] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.

[0112] [Isolation Component]

[0113] In some embodiments, the secondary battery also includes a separator disposed between the positive and negative electrodes.

[0114] In some embodiments, the separator is a separator membrane. This application does not have any particular restrictions on the type of separator membrane, and any well-known porous structure separator membrane with good chemical and mechanical stability can be selected.

[0115] As an example, the main material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, and ceramic. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation. The separator can be a single component located between the positive and negative electrodes, or it can be attached to the surfaces of the positive and negative electrodes. An inorganic particle coating, an organic particle coating, or an organic / inorganic composite coating can also be applied to the surface of the separator.

[0116] In some embodiments, the separator is a solid electrolyte. The solid electrolyte is disposed between the positive and negative electrodes, serving both to transport ions and to isolate the positive and negative electrodes.

[0117] [Electrode Assembly]

[0118] In some embodiments, the electrode assembly can be cylindrical, flat, or polygonal, etc.

[0119] In some embodiments, the electrode assembly is provided with tabs that allow current to be drawn from the electrode assembly. The tabs include a positive tab and a negative tab.

[0120] [shell]

[0121] In some embodiments, the battery cell may include a casing. The casing may be a steel casing, an aluminum casing, a plastic casing (such as a polypropylene casing), a composite metal casing (such as a copper-aluminum composite casing), or an aluminum-plastic film, etc. In some embodiments, the casing may be a sealed structure or a non-sealed structure. As an example, when the casing is a non-sealed structure, the casing serves to protect the electrode assembly, and a sealing bag is included between the casing and the electrode assembly to encapsulate the electrode assembly and electrolyte. Specifically, the sealing bag may be a bag-shaped insulating component or an aluminum-plastic film. When the casing is a sealed structure, it is used to encapsulate components such as the electrode assembly and electrolyte.

[0122] As an example, the battery cell can be a cylindrical battery cell, a prismatic battery cell, a pouch battery cell, or a battery cell of other shapes. Prismatic battery cells include prismatic battery cells, blade-shaped battery cells, and multi-prismatic batteries, such as hexagonal prismatic batteries. This application does not have any particular limitations.

[0123] In some embodiments, the housing includes an end cap and a housing, the housing having an opening, and the end cap covering the opening. The housing may have one or more openings. The end cap may also have one or more.

[0124] Figure 1 The example shown is a square-structured battery cell 5.

[0125] In some implementations, refer to Figure 2 The outer packaging may include a housing 51 and an end cap 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the end cap 53 can be placed over the opening to close the receiving cavity. The positive electrode, negative electrode, and separator can be formed into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in a single battery cell 5 can be one or more, which can be selected by those skilled in the art according to specific practical needs.

[0126] Electrode terminals

[0127] In some embodiments, at least one electrode terminal is provided on the housing, and the electrode terminal is electrically connected to the tab. The electrode terminal can be directly connected to the tab, or it can be indirectly connected to the tab through a current collector. The electrode terminal can be provided on the end cap or on the housing.

[0128] Pressure relief mechanism

[0129] In some embodiments, a pressure relief mechanism is provided on the casing. The pressure relief mechanism is used to release the internal gas of the battery cell.

[0130] As an example, the internal pressure or temperature of a battery cell is actuated to release the internal pressure or temperature when it reaches a predetermined threshold. When the internal pressure or temperature of the battery cell reaches the predetermined threshold, the pressure relief mechanism is activated or a weak structure in the pressure relief mechanism is broken, thereby forming an opening or channel for the internal pressure or temperature to be released. The threshold design varies depending on the design requirements. The threshold may depend on the materials of one or more of the positive electrode, negative electrode, electrolyte, and separator in the battery cell.

[0131] As an example, the pressure relief mechanism can be integrally molded with the housing.

[0132] As an example, the pressure relief mechanism can also be separately installed and connected to the housing.

[0133] The term "actuation" as used in this application refers to the activation or actuation of the pressure relief mechanism to a certain state, thereby releasing the internal pressure and temperature of the battery cell. The actions of the pressure relief mechanism may include, but are not limited to: movement of components within the mechanism to form an exhaust channel, rupture, breakage, tearing, or opening of at least a portion of the mechanism, etc. When the pressure relief mechanism is activated, the high-temperature, high-pressure substances inside the battery cell are discharged as waste from the activated portion. This method allows for pressure and temperature relief of the battery cell under controllable pressure or temperature, thereby preventing potentially more serious accidents.

[0134] In some embodiments, when the housing is a non-sealed structure, the pressure relief mechanism can be configured as a through hole for venting gas inside the battery cell.

[0135] The emissions from battery cells mentioned in this application include, but are not limited to: electrolyte, dissolved or split positive and negative electrode plates, fragments of separators, high-temperature and high-pressure gases generated by the reaction, flames, etc.

[0136] The battery apparatus mentioned in the embodiments of this application may include one or more battery cell assemblies for providing voltage and capacity. A battery cell assembly may include multiple battery cells connected in series, parallel, or mixed connections via a busbar.

[0137] In some embodiments, a battery cell assembly is typically formed by arranging multiple battery cells.

[0138] As an example, a battery cell assembly can be a battery module, which is formed by arranging and fixing multiple battery cells together to form an independent module. As another example, a battery module can be formed by bundling multiple battery cells together with cable ties.

[0139] Figure 3 This is battery module 4 as an example. (See reference...) Figure 3 In the battery module 4, multiple battery cells 5 can be arranged sequentially along the length of the battery module 4. Of course, they can also be arranged in any other way. Furthermore, these multiple secondary battery cells 5 can be fixed in place using fasteners.

[0140] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.

[0141] In some embodiments, the battery device may be a battery pack, which includes a housing and one or more individual battery cells housed within the housing.

[0142] As an example, the battery cell assembly can be a battery module, which can be housed in a housing by fixing the battery module in the housing.

[0143] As an example, battery cell assemblies can also be housed in a housing by directly fixing multiple battery cells to the housing.

[0144] As an example, the enclosure may include a first enclosure and a second enclosure. The first enclosure and the second enclosure are fastened together to form a closed space inside the enclosure to house the individual battery cells. Here, "closed" refers to covering or closing, and can be either sealed or unsealed. The first enclosure may be a top cover or a bottom plate.

[0145] As an example, the enclosure may include a top cover, a frame, and a bottom plate. The top cover and bottom plate are connected to the frame, creating an enclosed space inside the enclosure to house the individual battery cells.

[0146] Figure 4 and Figure 5 This is battery pack 1 as an example. (See reference...) Figure 4 and Figure 5 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.

[0147] In some embodiments, the housing may be part of the vehicle's chassis structure. For example, a portion of the housing may be at least a part of the vehicle's floor, or a portion of the housing may be at least a part of the vehicle's crossbeams and longitudinal beams.

[0148] The technical solutions described in the embodiments of this application are applicable to various electrical devices that use individual battery cells, such as mobile phones, portable devices, laptops, electric vehicles, electric toys, power tools, vehicles, ships, and spacecraft. For example, spacecraft include airplanes, rockets, space shuttles, and spacecraft.

[0149] As the electrical device, a single secondary battery cell, a battery module, or a battery pack can be selected according to its usage requirements.

[0150] Figure 6This is an example of an electrical device. The device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used. [Example]

[0151] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0152] [Example]

[0153] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.

[0154] Example 1

[0155] Preparation of positive electrode sheet :

[0156] LiNi, the positive electrode active material 0.9 Co 0.05 Mn 0.05 O2 (Dv50 is 5μm), conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeS2 (Dv50 is 23.7nm) are dry-mixed in a weight ratio of 93:3:2:2. Then, N-methylpyrrolidone (NMP) is added and dispersed evenly. The resulting slurry is coated on aluminum foil, dried, cold-pressed, and slit to obtain the positive electrode sheet.

[0157] Preparation of negative electrode sheet :

[0158] The negative electrode active material artificial graphite, conductive agent acetylene black, binder SBR and thickener CMC are mixed in a mass ratio of 97:1:0.8:1.2, deionized water is added and stirred to form a uniform slurry, and then the slurry is coated on copper foil, dried, cold pressed and cut to obtain the negative electrode sheet.

[0159] Preparation of electrolyte :

[0160] Electrolyte was prepared in an argon-filled glove box (water content < 0.1 ppm, oxygen content < 0.1 ppm). The solvent of the electrolyte was a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1. The content of the additive monoethyl sulfate (DES) was 0.5 wt%, and the concentration of lithium salt LiPF6 was 1 mol / L.

[0161] Separation membrane: Made of polyethylene film.

[0162] The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in sequence, with the separator in the middle of the positive and negative electrode sheets, and then wound to obtain a bare cell. The bare cell is placed in the outer packaging of the battery, and then the electrolyte is injected, encapsulated, and formed to obtain a lithium-ion battery cell.

[0163] test:

[0164] The mass content of the positive electrode additive and the mass content of Se element in the positive electrode film were tested in accordance with the method described above.

[0165] The sulfur-containing additives in the electrolyte are analyzed qualitatively and quantitatively using gas chromatography, in accordance with GB / T9722-2006 "General Rules for Gas Chromatography of Chemical Reagents".

[0166] Storage Gas Generation Test Method :

[0167] 1) Adjust the battery cell to 100% SOC: charge at a constant rate of 1 / 3C to the upper voltage limit, then charge at a constant voltage to a rate of 0.05C;

[0168] 3) Store the battery cells at 60℃ for 100 days and record the internal pressure data of the battery cells. The internal pressure data is obtained as follows: Install a pressure pipe at the sealing nail position of the battery cell cover. After ensuring that the sealing meets the standard, connect the pressure pipe to a piezoresistive pressure sensor and record the pressure change during the storage process in a constant temperature environment of 25℃. The final equilibrium pressure at the end of the storage period is recorded as the internal pressure of the battery cell.

[0169] DC internal resistance test method :

[0170] First, adjust the battery cells to 50% SOC: charge the battery cells at a constant rate of 1 / 3C to the upper voltage limit, then charge them at a constant voltage to a rate of 0.05C, and then discharge them at 1 / 3C for 30 minutes.

[0171] Then, connect the positive and negative probes of the AC internal resistance tester to the positive and negative terminals of the battery respectively to read the battery's internal resistance value.

[0172] Battery capacity test :

[0173] (1) Loop test process:

[0174] Charge the battery cells to the upper voltage limit at a constant 1C rate, then charge them to a constant voltage rate of 0.05C; let them stand for 10 minutes; discharge them to the lower voltage limit at a constant 1C rate; let them stand for 10 minutes; repeat the above steps until the cycle count reaches 200.

[0175] Examples 2-4

[0176] The only difference from Example 1 is the type and amount of the positive electrode additive. In Example 2, the positive electrode additive used is SeO2, and the positive electrode active material is LiNi. 0.9 Co 0.05 Mn 0.05 The weight ratio of O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeO2 (Dv50 of 18.4 nm) is 93.2:3:2:1.8; the positive electrode additive used in Example 3 is Li2Se, and the positive electrode active material is LiNi. 0.9 Co 0.05 Mn 0.05 The weight ratio of O2, conductive agent carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive Li2Se (Dv50 of 16.9 nm) is 93.2:3:2:1.8; the positive electrode additive used in Example 4 is NiSe, and the positive electrode active material is LiNi. 0.9 Co 0.05 Mn 0.05 The weight ratio of O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and cathode additive NiSe (Dv50 is 35.2nm) is 93.5:3:2:1.5.

[0177] Comparative Example 1

[0178] The only difference from Example 1 is that the positive electrode additive is replaced with Se powder with a Dv50 of 27.5 nm, and the positive electrode active material is LiNi. 0.9 Co 0.05 Mn 0.05 The weight ratio of O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive Se powder is 93.8:3:2:1.2.

[0179] Comparative Example 2

[0180] The difference from Example 1 is that it does not contain a positive electrode additive, namely the positive electrode active material LiNi. 0.9 Co 0.05 Mn 0.05 O2 (Dv50 is 5μm), conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) are dry-mixed at a weight ratio of 95:3:2.

[0181] Comparative Example 3

[0182] The only difference from Example 1 is that the electrolyte additive is replaced with fluoroethylene carbonate (FEC) at a mass content of 0.5 wt%.

[0183] The internal resistance, internal pressure, and capacity retention of the battery cells in the above embodiments and comparative examples were tested, and the mass content of positive electrode additives, the mass content of Se element in the positive electrode film, and the mass content of sulfur-containing additives in the electrolyte of each battery cell were recorded in Table 1.

[0184] Table 1

[0185]

[0186] According to the data in Table 1, the content of the positive electrode additive obtained in the test was reduced compared to the content at the time of addition because the positive electrode additive underwent an in-situ chemical reaction with the residual lithium on the surface of the positive electrode active material during formation. Similarly, the content of the sulfur-containing additive obtained in the test was also reduced compared to the content at the time of addition because the lithium selenate or lithium sulfate formed by the positive electrode additive reacted with the monoethyl sulfate. Compared with Comparative Examples 1-2, Examples 1-4 show that the battery cells in Comparative Example 2, which does not contain positive electrode additives, have higher internal resistance and lower cycle performance. Compared with Comparative Example 2, Comparative Example 1, which uses Se powder as the positive electrode additive, shows improved internal resistance and capacity retention, but the battery cell internal pressure data shows that it generates gas severely during cycling. Comparative Example 3, which uses FEC as the electrolyte additive, is similar to Example 1, but the gas generation is slightly increased and the capacity retention performance is significantly reduced. In Examples 1-4, when the positive electrode additive is SeS2, SeO2 or metal selenide, the internal resistance of the battery cell is significantly reduced and the capacity retention rate is also improved. At the same time, the gas production caused by the continuous decomposition of the electrolyte is reduced, and the cycle performance of the battery cell is improved.

[0187] The following examines the impact of the parameter characteristics of cathode additives on the performance of individual battery cells.

[0188] Examples 5-9, Comparative Example 4

[0189] The only difference from Example 1 is that the content or particle size of the positive electrode additive has been changed.

[0190] In Example 5, the positive electrode active material LiNi 0.9 Co 0.05 Mn 0.05 O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeS2 (Dv50 of 23.7nm) are mixed in a weight ratio of 94.9:3:2:0.1.

[0191] In Example 6, the positive electrode active material LiNi0.9 Co 0.05 Mn 0.05 O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeS2 (Dv50 of 23.7nm) are mixed in a weight ratio of 85:3:2:10.

[0192] In Example 7, the positive electrode active material LiNi 0.9 Co 0.05 Mn 0.05 O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeS2 (Dv50 is 514nm) are mixed in a weight ratio of 93.2:3:2:1.8.

[0193] In Example 8, the positive electrode active material LiNi 0.9 Co 0.05 Mn 0.05 O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeS2 (Dv50 of 6.2nm) are mixed in a weight ratio of 92.6:3:2:2.4.

[0194] In Example 9, the positive electrode active material LiNi 0.9 Co 0.05 Mn 0.05 O2, conductive carbon black, binder polyvinylidene fluoride (PVDF), and positive electrode additive SeS2 (Dv50 of 2.9μm) are mixed in a weight ratio of 93.5:3:2:1.5.

[0195] Comparative Example 4

[0196] Based on Example 9, the electrolyte additive ethyl sulfate (DES) was removed from the electrolyte, and the rest was the same as in Example 9.

[0197] The internal resistance, internal pressure, and capacity retention of the battery cells in the above embodiments were tested, as well as the mass content of the positive electrode additive and the mass content of Se element in the positive electrode film of each battery cell obtained in each group, and the results are recorded in Table 2.

[0198] Table 2

[0199]

[0200] The data in Table 2 show that the battery cells prepared using the cathode additive parameters of Examples 5-9 all achieved good cycle performance and produced less gas. Data from Examples 1 and 7-9 show that as the average particle size of the cathode additive increased from 5 nm to 2.5 μm, the cycle capacity retention rate of the battery cells first increased and then decreased, indicating that the particle size range of the above-mentioned cathode additives (5 nm-500 nm) is the optimal range; particles that are too small or too large may weaken the capacity retention during cycling.

[0201] The following examines the influence of electrolyte additive parameters on the performance of individual battery cells.

[0202] Examples 10-16, Comparative Example 5

[0203] The only difference from Example 1 is that the type or content of electrolyte additives has been changed.

[0204] The electrolyte additive added in Example 10 was 0.5 wt% dimethyl sulfate;

[0205] The electrolyte additive added in Example 11 was 0.5 wt% vinylene sulfate;

[0206] The electrolyte additive added in Example 12 was 0.5 wt% methanethiol;

[0207] The electrolyte additive added in Example 13 was 0.5 wt% monothiocarbonate;

[0208] The electrolyte additive added in Example 14 was 0.1 wt% DES;

[0209] The electrolyte additive added in Example 15 was 0.65 wt% DES;

[0210] The electrolyte additive added in Example 16 was 1 wt% DES.

[0211] The difference between Comparative Example 5 and Example 16 is that no positive electrode additive was added to the positive electrode, and the positive electrode active material LiNi was used. 0.9 Co 0.05 Mn 0.05 The weight ratio of O2, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) is 95:3:2.

[0212] The internal resistance, internal pressure, and capacity retention of the battery cells in each of the above embodiments were tested, and the mass content of sulfur-containing additives in the electrolyte of each battery cell was recorded in Table 3.

[0213] Table 3

[0214]

[0215] The data in Table 3 show that the battery cells prepared using the electrolyte additive parameters of Examples 10-16 all achieved good cycle performance. Data from Examples 1 and 14-16 show that when the concentration of the electrolyte additive increases from 0.1 wt% to 1 wt%, the cycle capacity retention of the battery cells initially increases and then decreases. Furthermore, the internal pressure data at a concentration of 1 wt% indicates severe gas generation during cycling. This demonstrates a threshold effect in electrolyte additive concentration; the above-mentioned concentration range can achieve a balance between improving cycle performance and enhancing charging capacity. Excessive addition may trigger side reactions and damage the electrodes.

[0216] The following examines the influence of electrolyte solvent parameters on the performance of individual battery cells.

[0217] Examples 17-18

[0218] The only difference from Example 1 is the change in the electrolyte solvent. The electrolyte solvent used in Example 17 was a mixture of EC and EMC in a volume ratio of 4:6, and the electrolyte solvent used in Example 18 was a mixture of EC and EMC in a volume ratio of 6:4.

[0219] The internal resistance, internal pressure, and capacity retention of the battery cells in the above embodiments were tested and recorded in Table 4.

[0220] Table 4

[0221] Battery cell internal resistance / mΩ Battery cell internal pressure / MPa 200-cycle capacity retention rate / % Example 17 211 0.166 98.4 Example 18 220 0.178 98.0

[0222] The data in Table 5 show that the battery cells prepared using the solvent parameters of the electrolytes in Examples 17-18 all achieved good cycle performance and produced less gas.

[0223] The following investigation examines the effect of coating the cathode additive on the performance of the battery cell.

[0224] Examples 19-21

[0225] Example 19: The difference from Example 1 lies in the coating treatment of the positive electrode additive. In this example, the positive electrode additive SeS2 (Dv50 of 23.7 nm) was dispersed in water, and then surfactant PVP and 1 wt% conductive polymer polyaniline were added (the mass of conductive polymer polyaniline relative to the mass of positive electrode additive SeS2 is 1%, and the mass of surfactant PVP relative to the mass of positive electrode additive SeS2 is 1%). The mixture was dispersed evenly, heated at 100°C, and stirred for 6 hours. The resulting product was filtered, washed, and dried to obtain the positive electrode additive with a conductive polymer coating.

[0226] Example 20: The difference from Example 19 is that the conductive polymer is changed to polypyrrole.

[0227] Example 21: The difference from Example 19 is that the mass of the conductive polymer polyaniline relative to the positive electrode additive SeS2 is 10 wt%.

[0228] The internal resistance, internal pressure, and capacity retention of the battery cells in the above embodiments were tested, and the mass content of the positive electrode additive, the mass content of Se element in the positive electrode film, and the mass content of sulfur-containing additive in the electrolyte of each battery cell were recorded in Table 5.

[0229] Table 5

[0230]

[0231] As can be seen from the data in Table 5, in Example 19, coating the positive electrode additive with a conductive polymer further reduced the internal resistance of the battery cell and improved the cycle capacity retention. Data from Examples 19-21 show that the battery cells prepared under the above conditions all exhibit good electronic conductivity and cycle performance.

[0232] The following examines the impact of positive electrode active materials on the performance of individual battery cells.

[0233] Example 22

[0234] The only difference from Example 1 is that the positive electrode active material is changed to LiFePO4 with a Dv50 of 1 μm.

[0235] The internal resistance, internal pressure, and capacity retention of the battery cells in Test Example 22, as well as the mass content of the positive electrode additive and the mass content of Se element in the positive electrode film of each battery cell, are recorded in Table 6.

[0236] Table 6

[0237]

[0238] As shown in Table 6, when the positive electrode active material is changed to LiFePO4, the intrinsic conductivity is lower than that of Example 1, resulting in a significant increase in the internal resistance of the battery cell. However, it still maintains good overall cycle performance, with a capacity retention rate of 97.2% after 200 cycles.

[0239] Although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A battery cell, the battery cell comprising a positive electrode sheet and an electrolyte, the positive electrode sheet comprising a positive current collector and a positive electrode film layer, the positive electrode film layer comprising a positive electrode active material and a positive electrode additive, the positive electrode additive comprising one or more of SeS2, SeO2, and metal selenides, the electrolyte comprising an electrolyte additive, the electrolyte additive comprising a sulfur-containing additive, the sulfur-containing additive comprising one or more of sulfate ester additives, thiol additives, or thiocarbonate additives.

2. The battery cell according to claim 1, wherein, The mass content of Se element in the positive electrode film is 0.05%-7%.

3. The battery cell according to claim 1 or 2, wherein, The mass content of the positive electrode additive in the positive electrode film layer is 0.02%-5%.

4. The battery cell according to any one of claims 1-3, wherein, The average particle size of the positive electrode additive is 0.005μm-2.5μm, and optionally, the average particle size of the positive electrode additive is 5nm-520nm.

5. The battery cell according to any one of claims 1-4, wherein, The electrolyte additives include sulfate ester additives, which include chain sulfate esters or cyclic sulfate esters.

6. The battery cell according to claim 5, wherein, The chain sulfates include compounds having the following general formula I: General style I:R 1 -O-SO2R 2 , Wherein, the R 1 and R 2 Independently comprising any one of substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted C2-C6 alkenyl, or substituted or unsubstituted C6-C12 aryl, wherein the R 1 and R 2 The substituents include any one of halogens and C1-C3 alkyl groups.

7. The battery cell according to claim 6, wherein, The R 1 and R 2 Independently comprising any one of substituted or unsubstituted C1-C6 alkyl groups or substituted or unsubstituted C2-C4 alkenyl groups, wherein the R 1 and R 2 The substituents include any one of halogens and C1-C3 alkyl groups.

8. The battery cell according to any one of claims 5-7, wherein, The chain sulfate esters include one or more of monoethyl sulfate, dimethyl sulfate, methyl ethyl sulfate, diethyl sulfate, triethyl sulfate, bis(trifluoromethyl) sulfate, dipropyl sulfate, isopropyl sulfate, dibutyl sulfate, dipentyl sulfate, dihexyl sulfate, or dipropylene sulfate.

9. The battery cell according to claim 5, wherein, The cyclic sulfate additives include compounds having the following general formula II: Among them, R 3 R 4 Each independently includes a hydrogen atom, a substituted or unsubstituted C1-C6 alkyl group, Any one of them; R 5 Including any one of substituted or unsubstituted C1-C6 alkyl groups, said R 3 R 4 and R 5 The substituents include any one of halogens and C1-C3 alkyl groups.

10. The battery cell according to claim 9, wherein, R 3 R 4 Each independently includes a hydrogen atom, a C1-C3 alkyl group, Any one of them; R 5 Including any one of C1-C3 alkyl groups.

11. The battery cell according to any one of claims 9-10, wherein, The cyclic sulfate additives include one or two of vinylene sulfate (DTD), divinylene sulfate, and trivinylene sulfate.

12. The battery cell according to any one of claims 1-11, wherein, The thiol additives include one or more of methanethiol, ethanethiol, propanethiol, isopropanethiol, butanethiol, pentamethanethiol, or halothiols; and / or The thiocarbonate additives include one or more of the following: trithiocarbonate, dithiocarbonate, monothiocarbonate, bis(trifluoromethyl)thiocarbonate, dimethylthiocarbonate, diethylthiocarbonate, and methyl ethylthiocarbonate.

13. The battery cell according to any one of claims 1-12, wherein, The sulfur-containing additive in the electrolyte has a mass content of 0.05%-0.3%, and / or the sulfur-containing additive in the electrolyte has a mass content of 0.1%-1%.

14. The battery cell according to any one of claims 1-13, wherein, The electrolyte also includes a solvent. Optionally, the solvent includes cyclic carbonates and chain carbonates; Optionally, the cyclic carbonate includes one or more of ethylene carbonate and propylene carbonate, and the chain carbonate includes one or more of dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate.

15. The battery cell according to claim 14, wherein, The cyclic carbonate in the solvent accounts for 30%-70% by mass.

16. The battery cell according to any one of claims 1-15, wherein, The positive electrode film layer also includes a conductive polymer, and optionally at least a portion of the conductive polymer is coated on the surface of the positive electrode additive.

17. The battery cell according to claim 16, wherein, The conductive polymer includes one or more of polyaniline, polypyrrole, polythiophene, or polyacrylonitrile.

18. The battery cell according to claim 16 or 17, wherein, The positive electrode film layer includes the conductive polymer at a mass content of 0.001%-1%.

19. The battery cell according to any one of claims 1-18, wherein, The positive electrode active material includes a nickel-containing lithium transition metal oxide. Optionally, the nickel-containing lithium layered transition metal oxide includes a lithium-containing nickel-cobalt-manganese oxide or a lithium-containing nickel-cobalt-aluminum oxide.

20. The battery cell according to claim 19, wherein, The nickel-containing lithium transition metal oxide includes the compound Li a Ni b Co c Mn d M e O 2-f Wherein, M includes one or more elements selected from Al, Fe, Ti, Mg, Zr, Cr, Ga, Cu, Zn, Nb, and B; The value of 'a' is any value within the range of 0.4-1.2, and can be selected as any value within the range of 0.8-1.2; the value of 'b' is any value within the range of 0.45-0.95, and can be selected as any value within the range of 0.5-0.85; the value of 'c' is any value within the range of 0.02-0.25, and can be selected as any value within the range of 0.02-0.2; the value of 'd' is any value within the range of 0.05-0.5, and can be selected as any value within the range of 0.05-0.48; the value of 'e' is any value within the range of 0-0.2, and can be selected as any value within the range of 0.001-0.2; the value of 'f' is any value within the range of 0-0.3, and can be selected as any value within the range of 0-0.

2.

21. A battery device comprising one or more battery cells according to any one of claims 1 to 20.

22. An electrical device comprising a battery cell according to any one of claims 1 to 20, or a battery device according to claim 21.