A method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery
By employing a combination of pH gradient control, oxidation treatment, and selective chelating resin impurity removal in the failed vanadium electrolyte of a vanadium redox flow battery, the problems of impurity removal and valence state restoration in the prior art have been solved, achieving efficient and clean electrolyte regeneration, which is suitable for the recycling of vanadium redox flow batteries.
Patent Information
- Application Number
- CN202611235484.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for the recovery and regeneration of vanadium electrolyte in failed vanadium redox flow batteries suffer from problems such as poor solubility of solid raw materials, complex processes, high energy consumption, introduction of exogenous materials or organic impurities, and difficulty in simultaneously achieving deep removal of impurities and accurate restoration of valence state.
A method combining oxidation/precipitation/adsorption sequence for impurity removal under pH gradient control with electrolytic fine-tuning is adopted. The failed electrolyte is mixed in a protective atmosphere, oxidized, and then the pH value is gradually adjusted. Impurities are removed using a selective chelating cation exchange resin. Finally, the electrolyte is regenerated by adjusting the vanadium ion ratio and valence state through proton exchange membrane electrolysis.
Without significantly altering the total vanadium concentration, a variety of key impurity ions were systematically removed, and the average valence state of the electrolyte was precisely restored to +3.5, achieving an efficient and clean regeneration process while reducing process complexity and energy consumption.
Smart Images

Figure CN123120766A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of recycling and regeneration technology of electrolyte in vanadium redox flow batteries, aiming to restore electrolyte performance and recycle resources. Specifically, it relates to a method for restoring and regenerating failed vanadium electrolyte in vanadium redox flow batteries. Background Technology
[0002] Vanadium redox flow batteries have broad application prospects in large-scale energy storage due to their advantages such as high safety, long cycle life, and flexible capacity configuration. However, the cost of the electrolyte accounts for 40% to 50% of the total cost of the battery system. Moreover, during long-term operation, the electrolyte will gradually fail due to factors such as vanadium ion valence imbalance, accumulation of impurity ions (such as Fe, Al, and Si), and hydrolysis precipitation of pentavalent vanadium (V₂O₅), leading to battery capacity decay and decreased energy efficiency.
[0003] CN201811279095.X discloses a method for regenerating failed vanadium electrolyte in a sulfuric acid system. This method involves directly adding tetravalent or trivalent vanadium electrolyte to adjust the average valence state to +3.5 by detecting the average valence state of the failed electrolyte. However, this method requires the preparation of a large quantity of tetravalent or trivalent vanadium electrolyte at a specific concentration as a correction solution. These raw materials may require complex preparation processes or be purchased, increasing recycling costs. Furthermore, this method is essentially a mixing and dilution process; by adding a large amount of external electrolyte to adjust the valence state, it cannot achieve a net increase in electrolyte capacity (i.e., the total vanadium content does not increase).
[0004] CN202310176659.1 discloses a method for recycling electrolyte from spent vanadium battery batteries, which involves mixing and reacting the failed positive and negative electrode solutions, and then adding solid vanadium sulfate (III), vanadium oxysulfate (IV), sulfuric acid, and hydrochloric acid for further preparation. This method still requires the addition of solid vanadium sulfate and vanadium oxysulfate, posing risks of solubility issues and the introduction of insoluble substances. It involves the sequential addition of multiple solid and liquid raw materials, resulting in numerous steps and complex quality control points.
[0005] CN202411849058.3 discloses a method for recycling and reusing failed electrolyte from a vanadium redox flow battery. The method involves electrolyzing the failed electrolyte from the positive and negative electrodes separately to obtain pure tetravalent and trivalent electrolytes, followed by evaporation and crystallization to obtain VOSO4 and V2(SO4)3 crystals. This method includes two electrolysis systems and subsequent evaporation and crystallization processes, resulting in high equipment investment and energy consumption. Its output is a high-purity crystalline product, not directly regenerated battery electrolyte. If the goal is to regenerate the electrolyte, this method requires redissolving and preparing the crystals, making the process circuitous. The crystallization produces a mother liquor containing vanadium and sulfuric acid, requiring additional steps (such as ion exchange and adsorption) for recovery, increasing the process and cost.
[0006] CN202510008488.0 discloses a method for recovering failed vanadium battery electrolyte. The method involves electrolytically reducing a vanadium solution to its tetravalent state, followed by extraction and back-extraction to ultimately obtain vanadium oxalate. The final product of this method is vanadium oxalate, a chemical product that deviates from the scope of "battery electrolyte regeneration" and represents another path for resource recovery. However, the use of extractants and sulfonated kerosene presents problems such as organic phase entrainment, solvent loss, and potential pollution. Furthermore, it involves multiple chemical unit operations including electrolysis, pH adjustment, extraction, back-extraction, and crystallization, resulting in a complex process and low economic efficiency.
[0007] In summary, current methods for regenerating spent vanadium redox flow battery electrolytes still face challenges such as poor solubility of solid raw materials, complex processes, high energy consumption, introduction of exogenous materials or organic impurities, and difficulty in simultaneously achieving deep impurity removal and precise valence state restoration. Therefore, developing an efficient, low-cost, and pollution-free spent electrolyte regeneration process is of great significance for promoting the large-scale application of vanadium redox flow batteries and sustainable resource development. Summary of the Invention
[0008] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for the recovery and regeneration of vanadium electrolyte in a vanadium redox flow battery. The present invention can systematically remove a variety of key impurity ions without significantly changing the total vanadium concentration and avoiding vanadium precipitation, and finally accurately restore the average valence state of vanadium ions in the electrolyte to +3.5, thereby achieving efficient and clean regeneration.
[0009] To achieve the above objectives, the present invention adopts the following technical solution: A method for recovering and regenerating vanadium electrolyte from a failed vanadium redox flow battery includes the following steps: The positive and negative electrolytes of the failed vanadium battery were mixed in a protective atmosphere at a volume ratio of (0.5-1.5):(0.5-1.5) to obtain mixture A. Oxygen is introduced into the mixture A and stirred to carry out oxidation treatment, resulting in mixture B. Add ammonia to the mixture B to adjust the pH to 2.0-3.0, thus obtaining mixture C; The mixture C is subjected to solid-liquid separation to obtain the first filtrate; Add alkali solution to the first filtrate to adjust the pH value to 3.0-3.5 to obtain mixture D; The mixture D is aged, and after aging, solid-liquid separation is performed to obtain a second filtrate. The second filtrate is passed through a selective chelating cation exchange resin to remove the impurity metal ions that remain after hydrolysis and precipitation, thus obtaining a deeply purified electrolyte. Using the deep-purified electrolyte as the cathode liquid, and separating the deep-purified electrolyte from the anolyte through a proton exchange membrane, electrolysis is performed to adjust the vanadium ion ratio to the target state of V(III):V(IV)=1:1. Then, the vanadium ion concentration and sulfate concentration are adjusted to the target values, thereby realizing the recovery and regeneration of the failed vanadium electrolyte in the vanadium redox flow battery.
[0010] Preferably, the positive and negative electrolytes of the failed vanadium battery are mixed in equal volume ratio under a protective atmosphere to obtain mixture A.
[0011] Preferably, when oxygen is introduced into the mixture A and stirred to perform oxidation treatment, resulting in mixture B: The oxygen flow rate is 0.05-0.20 vvm, the preferred treatment time is 25-35 min, and the temperature of the mixed solution A during oxidation treatment is 20-40℃.
[0012] Preferably, when ammonia is added to the mixture B to adjust the pH to 2.0-3.0, resulting in mixture C: Use ammonia water with a mass fraction of 1%-5% (that is, the mass concentration of ammonia water is 1%-5%). Ammonia solution is added dropwise to mixture B, and the rate of pH change during the addition of ammonia solution is controlled to not exceed 0.2 pH units / min.
[0013] Preferably, the alkaline solution added to the first filtrate is ammonia water with a mass fraction of 1%-5% (that is, the mass concentration of ammonia water is 1%-5%).
[0014] Preferably, when aging the mixture D, the aging temperature is 20-30℃ and the aging time is 30-90 min.
[0015] Preferably, the selective chelating cation exchange resin is a chelating cation exchange resin containing iminodiacetic acid groups or aminophosphonic acid groups; the chelating resin is an H-type resin; the H-type resin is Purolite S930 Plus, Lewatit TP 207 or Amberlite IRC748.
[0016] Preferably, when the second filtrate is passed through a selective chelating cation exchange resin to remove residual impurity metal ions after hydrolysis and precipitation, resulting in a deeply purified electrolyte: The second filtrate was subjected to deep purification by passing it through a fixed bed packed with selective chelating cation exchange resin. The resin bed was filled with 0.02-0.06 L of resin per 1 L of wet resin volume. The height-to-diameter ratio of the resin bed was (5-10):1. The influent pH was controlled at 3.0-3.1, and the processing flow rate was 2-5 BV / h, where BV is the wet resin bed volume. Influent and effluent samples were collected after processing 0.45-0.55 BV of electrolyte, and the total vanadium concentration and the concentration of the target impurity ions were measured. When the ratio of the effluent concentration to the influent concentration of any target impurity ion reached 0.05, the resin was considered to have reached the impurity penetration endpoint. After the resin reaches the breakthrough endpoint, the residual liquid is first replaced with 1-2 BV of deionized water, and then regenerated with sulfuric acid solution of concentration 1.0-2.0 mol / L at a flow rate of 1-2 BV / h, with a regeneration solution volume of 2-4 BV. Subsequently, it is washed with 3-5 BV of deionized water until the effluent is free of metal ions, and then transformed and equilibrated with 1-2 BV of sulfuric acid solution of concentration 1.5-2.0 mol / L to obtain a reusable H-type chelating resin.
[0017] Preferably, the deeply purified electrolyte is used as the cathode liquid, and the deeply purified electrolyte and the anolyte are separated by a proton exchange membrane during electrolysis: The electrolyte temperature is controlled at 20-40℃; the current density for constant current electrolysis, based on the effective projected area of the electrodes, is 20-80 mA / cm². 2 The electrolyte is circulated into the electrolytic cell.
[0018] Preferably, the anolyte is a pretreated vanadium sulfate reference electrolyte, or an inert anode is used with sulfuric acid electrolyte as the anolyte; both the cathode and anode are made of acid-resistant conductive carbon material, which includes graphite felt electrode and carbon paper electrode; During electrolysis, the theoretical charge flow rate is determined by the following formula: Q = F × C v ×V e ×|3.5-Z0| / η In the formula, Q is the theoretical charge, in C; F is the Faraday constant; C v V represents the total vanadium concentration in the electrolyte, expressed in mol / L. e Z0 is the volume of the electrolyte to be treated, in L; Z0 is the average valence state of vanadium ions before electrolysis; η is the current efficiency. When the initial average valence state is lower than +3.5, the electrolyte to be treated is used as the anolyte for oxidation electrolysis. When the initial average valence state of the deep-purified electrolyte is higher than +3.5, the deep-purified electrolyte is used as the cathode liquid for reduction electrolysis. The electrolysis time is determined by the theoretical charge and the actual current, i.e., t = Q / I. The single electrolysis time is controlled to be 0.5-8 h, and adjusted according to the electrolyte volume, electrode area and initial valence state. When the initial average valence state is equal to +3.5 and the molar ratio of V(III) to V(IV) meets the target state, the vanadium ion concentration and sulfate concentration are adjusted to the target values. During electrolysis, online redox potential monitoring was used, and samples were taken every 25-35 minutes for potentiometric titration analysis. Electrolysis was stopped when the molar ratio of V(III) to V(IV) reached 1:1 and the average valence state of vanadium ions reached +3.3 to +3.7. After electrolysis, the electrolyte was circulated for 5-15 minutes to ensure that the electrolyte composition was homogeneous. When the vanadium ion concentration and sulfate concentration are adjusted to the target values, according to the measurement results, a pre-prepared sulfuric acid standard solution or deionized water is added to the electrolyte under stirring conditions, or vanadium sulfate reference electrolyte is added to restore the total vanadium concentration, sulfate concentration and electrolyte volume to the preset target values, and finally realize the recovery and regeneration of the failed vanadium electrolyte in the vanadium redox flow battery.
[0019] The present invention has the following beneficial effects: In the method for recovering and regenerating failed vanadium electrolyte in a vanadium redox flow battery of the present invention, the failed positive electrode electrolyte and negative electrode electrolyte of the vanadium battery are mixed under a protective atmosphere at a volume ratio of (0.5... 1.5): (0.5) 1.5) Mixing yields mixture A. A protective atmosphere prevents the oxidation of low-valence vanadium ions by external air. During mixing, redox reactions occur between vanadium ions of different valence states, eliminating local extreme valence states within the electrolyte and resulting in a homogeneous mixture A. This eliminates the need for pre-adjusting the valence state with additional trivalent or tetravalent vanadium correction solutions, avoiding the increased costs associated with introducing external materials in existing technologies. Introducing oxygen into mixture A and stirring oxidizes it to obtain mixture B. The oxygen can neutralize Fe in the system. 3+ Oxidized into Fe, which is more easily hydrolyzed 3+ This process unifies the valence state of iron impurities, creating conditions for precipitation and impurity removal under subsequent pH adjustment. It also oxidizes some organic degradation products, reducing the adverse effects of organic components on the electrolyte and subsequent processes. Ammonia is added to mixture B to adjust the pH to 2.0. 3.0 After obtaining the mixed solution C, solid-liquid separation is performed to obtain the first filtrate. Adjusting the pH with ammonia water will not introduce difficult-to-remove alkali metal impurities. Within this pH range, Fe... 3+Preemptive hydrolysis forms an iron-containing hydroxide precipitate, which can remove some metal impurities through adsorption and co-precipitation. Solid-liquid separation further removes the precipitated impurities. Alkali solution is then added to the first filtrate to adjust the pH to 3.0. 3.5 The resulting mixture D is aged and then separated into solid and liquid solutions to obtain the second filtrate. Stepwise pH adjustment avoids localized over-alkalinity caused by a one-time pH increase, thus preventing vanadium precipitation and achieving a minimal change in the total vanadium concentration. Aging promotes the aggregation and growth of hydrolysis products, further enhancing adsorption and co-precipitation to capture residual impurities. The second filtrate is then treated with a selective chelating cation exchange resin to remove residual metal ions that are difficult to completely remove through hydrolysis precipitation. The combination of precipitation and resin can remove various key impurity ions. This treatment method does not use extraction-type organic reagents, thus avoiding the introduction of organic impurities. This process achieves clean treatment by using a deeply purified electrolyte as the cathode solution. Electrolysis is carried out by separating the cathode solution and the anolyte through a proton exchange membrane. The vanadium ion ratio is adjusted to V(III):V(IV)=1:1, which corresponds to the average valence state of vanadium ions being restored to +3.5, thus restoring the valence state. This electrolysis valence adjustment method does not add exogenous solid vanadium salts, thereby overcoming the defect of poor solubility of solid raw materials. At the same time, it eliminates high-energy-consuming and roundabout processes such as evaporation crystallization and crystal redissolution, reducing process complexity and energy consumption. After electrolysis, the vanadium ion concentration and sulfate concentration are adjusted to the target values to directly obtain the regenerated electrolyte. The technical solution of this invention can simultaneously solve the problems of poor solubility of solid raw materials, complex processes, high energy consumption, introduction of exogenous materials or organic impurities, and difficulty in achieving deep removal of impurities and accurate restoration of valence state in the prior art, while reducing the loss of vanadium components. It achieves the invention objective of removing multiple key impurity ions and efficiently and cleanly regenerating failed vanadium electrolyte without significantly changing the total vanadium concentration and avoiding vanadium precipitation. The regenerated electrolyte can be directly used in vanadium redox flow batteries, which is conducive to realizing the recycling of failed vanadium electrolyte. Attached Figure Description
[0020] Figure 1 This is the vanadium ion potential titration diagram (EV) of the failed vanadium electrolyte in Example 1 of this application. Figure 2 The potentiometric titration first-order differential curve (ΔE / ΔV-V) of Example 1 of this application is shown. Figure 3 This is the vanadium ion potential titration diagram (EV) of the failed vanadium electrolyte in Example 2 of this application. Figure 4 The potentiometric titration first-order differential curve (ΔE / ΔV-V) of Example 2 of this application; Figure 5 This is the vanadium ion potential titration diagram (EV) of the failed vanadium electrolyte in Example 3 of this application. Figure 6The potentiometric titration first-order differential curve (ΔE / ΔV-V) of Example 3 of this application is shown. Figure 7 The diagram shows the energy efficiency of the vanadium electrolyte obtained from the recovery and regeneration in Examples 1, 2, and 3 of this application. Figure 8 The diagram shows the voltage efficiency of the vanadium electrolyte obtained from the recovery and regeneration in Examples 1, 2, and 3 of this application. Figure 9 The coulombic efficiency diagrams of the vanadium electrolytes obtained from the recovery and regeneration in Examples 1, 2, and 3 of this application are shown. Figure 10 The charge-discharge curves of the vanadium electrolyte obtained from the regeneration in Examples 1, 2, and 3 of this application are shown. Detailed Implementation
[0021] The present invention will be further described clearly and in detail below with reference to specific embodiments and the accompanying drawings. Those skilled in the art will be able to implement the present invention based on these descriptions. Furthermore, the embodiments of the present invention described below are generally only some, not all, of the embodiments of the present invention. Therefore, all other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort should fall within the scope of protection of the present invention.
[0022] This invention utilizes a process that combines sequential purification through oxidation / precipitation / adsorption under pH gradient control with electrolytic fine-tuning. This process systematically removes multiple key impurity ions without significantly altering the total vanadium concentration or avoiding vanadium precipitation. Ultimately, it precisely restores the average valence state of vanadium ions in the electrolyte to +3.5, achieving efficient and clean regeneration.
[0023] Based on the above ideas, the method for recovering and regenerating failed vanadium electrolyte in a vanadium redox flow battery provided by the present invention includes the following steps: S1. Pretreatment and Initial Valence State Homogenization: The positive and negative electrolytes of the failed vanadium battery are mixed and stirred uniformly at a volume ratio of (0.5-1.5):(0.5-1.5) under inert gas protection, allowing vanadium ions of different valence states to undergo redox reactions, eliminating local extreme valence states, and obtaining mixture A. Among them, the V in the negative electrolyte... 2+ VO2 in the positive electrode electrolyte can + Restore to V 3+ This reduces the risk of side reactions caused by excessive local oxidation or reduction during subsequent impurity removal processes.
[0024] S2, Mild Oxidation: Oxygen is introduced into the mixture A obtained in S1 and stirred. Oxidation is carried out at 20-40℃ to obtain mixture B. The preferred oxygen introduction rate is 0.05-0.20 vvm, and the preferred treatment time is 25-35 min. During the oxygen introduction process, oxygen enters the electrolyte via gas-liquid mass transfer, oxidizing Fe... 2+ Oxidized into Fe, which is more easily hydrolyzed 3+ This facilitates subsequent stepwise precipitation and removal, while also reducing the adverse effects of some easily oxidized organic degradation products on electrolyte stability and subsequent electrolysis processes. By placing the oxidation step before the pH adjustment step, the valence state of iron impurities can be standardized before utilizing Fe... 3+ Selective impurity removal is achieved by leveraging the preferential hydrolysis characteristics under weakly acidic conditions.
[0025] S3, pH gradient control for impurity removal: S3.1, First-stage selective hydrolysis for impurity removal: Add 1%-5% (w / w) dilute ammonia solution to the mixture B after S2 treatment to adjust the pH of the solution to 2.0-3.0. During the addition process, control the pH change rate to not exceed 0.2 pH units / min to obtain mixture C. The amount of dilute ammonia solution added should be based on achieving the predetermined pH and should not be limited to a fixed volume. Choosing dilute ammonia solution as a neutralizing agent can achieve slow and uniform pH adjustment, reducing the risk of vanadium hydrolysis precipitation caused by local high pH; at the same time, the introduced ammonium ions do not form alkali metal impurities that are difficult to remove, and the introduction of new impurities such as alkali metals can be avoided.
[0026] Within this pH range, Fe 3+ Hydrolysis preferentially occurs, forming iron-containing hydroxide or hydroxyl polymer precipitates; these precipitates can further adsorb or co-precipitate some colloidal silicon, aluminum impurities, and other trace metal impurities. For Ca... 2+ When the sulfate concentration in the system reaches the solubility product condition of the corresponding sulfate, a slightly soluble sulfate can be formed and removed through solid-liquid separation. After this stage, the mixture C is subjected to a first precision filtration to obtain the first filtrate.
[0027] S3.2 Second Stage Aging and Adsorption Removal: Continue adding alkaline solution to the first filtrate, preferably using 1%-5% dilute ammonia water to adjust the pH to 3.0-3.5, obtaining mixture D. Using dilute ammonia water avoids introducing new impurities such as alkali metals. Then, age at 20-30℃ for 30-90 min and perform a second precision filtration to obtain the second filtrate. During aging, the iron-containing hydrolysis product Fe(OH)3 further aggregates, grows, and plays an adsorption and co-precipitation role to capture residual colloidal silicon and some trace metal impurities (including Cu). 3+ Al 3+By dividing the pH adjustment into two interconnected intervals, the localized overly alkaline environment caused by a one-time increase in pH can be avoided, thus balancing the efficiency of iron impurity removal with the stability of vanadium components.
[0028] S3.3, Resin Deep Purification: The second filtrate obtained in S3.2 is subjected to deep purification using a selective chelating cation exchange resin to remove residual metal ions (such as Cu) remaining after hydrolysis and precipitation. 2+ Al 3+ Fe 3+ Ca 2+ Pb 3+ The resulting deeply purified electrolyte is obtained. The resin is preferably a chelating cation exchange resin containing iminodiacetic acid groups or aminophosphonic acid groups. The second filtrate is deeply purified by passing it through a fixed bed packed with iminodiacetic acid-type macroporous chelating cation exchange resin. This method can achieve high removal efficiency for divalent and trivalent heavy metal ions. The chelating resin is an H-type resin, preferably one of Purolite S930Plus, Lewatit TP 207, or Amberlite IRC748.
[0029] Based on the wet resin volume, 0.02-0.06 L of resin is added per 1 L of electrolyte to be treated (i.e., the aforementioned second filtrate); the preferred height-to-diameter ratio of the resin bed is (5-10):1. The influent pH is controlled at 3.0-3.1, and the treatment flow rate is 2-5 BV / h, where BV is the wet resin bed volume. Under these conditions, the iminodiacetic acid functional groups in the resin are utilized to react with Cu... 2+ Fe 3+ Al 3+ Pb 2+ The coordination adsorption of these metal impurity ions further reduces the concentration of residual metal impurities. For every 0.5 ± 0.05 BV of electrolyte treated, influent and effluent samples were collected, and the total vanadium concentration and the concentration of the target impurity ions were measured. When the ratio of the effluent concentration to the influent concentration of any target impurity ion (C / C0) reached 0.05, the resin was considered to have reached the impurity penetration endpoint.
[0030] After the resin reaches the breakthrough endpoint, the residual liquid is first replaced with 1-2 BV of deionized water, and then regenerated with sulfuric acid solution of concentration 1.0-2.0 mol / L at a flow rate of 1-2 BV / h, with a regeneration solution volume of 2-4 BV. Subsequently, it is washed with 3-5 BV of deionized water until the effluent is free of metal ions, and then transformed and equilibrated with 1-2 BV of sulfuric acid solution of concentration 1.5-2.0 mol / L to obtain a reusable H-type chelating resin.
[0031] The entire regeneration process is carried out under a closed or inert atmosphere to prevent the oxidation of low-valent vanadium by air.
[0032] S4. Fine-tuning of electrolytic valence state: The electrolyte after deep purification in S3 (i.e., the deeply purified electrolyte) is transferred into the electrolytic cell as the cathode liquid. The anolyte is a pretreated vanadium sulfate reference electrolyte, or an inert anode with sulfuric acid electrolyte as the anolyte. The cathode liquid and anolyte are separated by a proton exchange membrane. Both the cathode and anode are preferably made of graphite felt electrode, carbon paper electrode, or other acid-resistant conductive carbon material.
[0033] During electrolysis, the electrolyte temperature is controlled at 20-40℃, preferably 25℃; the current density for constant current electrolysis is 20-80 mA / cm², based on the effective projected area of the electrodes. 2 Preferably 50 mA / cm 2 The electrolyte is circulated into the electrolytic cell, and the circulation flow rate should ensure that there are no obvious air bubbles trapped on the electrode surface or concentration polarization.
[0034] Before electrolysis, the total vanadium concentration, volume, and average vanadium ion valence state of the electrolyte are measured. The theoretical charge is calculated based on the difference between the initial and target average valence states. The theoretical charge is determined by the following formula: Q = F × C v ×V e ×|3.5-Z0| / η In the formula, Q is the theoretical charge, in C; F is the Faraday constant; C v V represents the total vanadium concentration in the electrolyte, expressed in mol / L. e Z0 represents the volume of the electrolyte to be treated, in liters (L); Z0 represents the average valence state of vanadium ions before electrolysis; and η represents the current efficiency.
[0035] When the initial average valence state is below +3.5, the electrolyte to be treated is used as the anolyte for oxidation electrolysis; when the initial average valence state is above +3.5, the electrolyte to be treated is used as the catholyte for reduction electrolysis. The theoretical charge is calculated according to the formula, and the electrolysis time is determined by the theoretical charge and the actual current, i.e., t = Q / I; preferably, the single electrolysis time is controlled to be 0.5-8 h, and adjusted according to the electrolyte volume, electrode area and initial valence state. When the initial average valence state is equal to +3.5 and the molar ratio of V(III) to V(IV) meets the preset requirements, no valence state adjustment electrolysis is performed, and the process proceeds directly to the subsequent component compounding step.
[0036] Online redox potential monitoring was employed during electrolysis, with samples taken every 25-35 minutes (preferably 0.5 hours) for potentiometric titration analysis to monitor the vanadium valence state changes in real time. Electrolysis time and charge were controlled accordingly. Electrolysis was stopped when the molar ratio of V(III) to V(IV) reached the target state of 1:1 and the average vanadium ion valence state reached +3.5 ± 0.02. After electrolysis, the electrolyte was circulated for another 5-15 minutes to ensure homogeneity of the electrolyte composition.
[0037] S5. Component Combination and Performance Verification: During electrolysis, water molecules can migrate across the ion exchange membrane under the influence of concentration gradient, electroosmotic drag, and ion migration, causing changes in the volume, density, and acidity of the cathode and anolyte. The minute changes in vanadium concentration are calculated. After electrolysis, the volume, density, total vanadium concentration, and sulfate concentration of the regenerated electrolyte are measured under the same temperature conditions. Volume and density are used to establish a material balance before and after electrolysis. The total vanadium concentration is determined using potentiometric titration, UV-Vis spectrophotometry, or inductively coupled plasma atomic emission spectrometry. The sulfate concentration is determined using ion chromatography, titration, or other calibrated analytical methods.
[0038] Based on the measurement results, pre-prepared sulfuric acid standard solution or deionized water was added to the electrolyte under stirring conditions. If necessary, a confirmed vanadium sulfate reference electrolyte was added to restore the total vanadium concentration, sulfate concentration, and electrolyte volume to the preset target values. The total vanadium concentration and sulfate concentration were remeasured after each addition until all indicators met the target range.
[0039] The reconstituted electrolyte was assembled into a vanadium redox flow battery, and constant current charge-discharge cycle tests were conducted under the same battery structure, membrane materials, electrode materials, current density, cutoff voltage, and temperature conditions as with a fresh reference electrolyte. The charging capacity, discharging capacity, average charge-discharge voltage, and capacity retention during cycling were recorded, and the capacity recovery rate, coulombic efficiency, voltage efficiency, energy efficiency, and cycle stability were calculated.
[0040] This invention combines a scientific impurity removal sequence with electrolytic fine-tuning, which efficiently removes various metal ion impurities without losing vanadium or introducing new impurities, and precisely restores the chemical state of the electrolyte. The process is clean, efficient, and produces a regenerated electrolyte with excellent performance.
[0041] Example 1: This embodiment describes a method for restoring and regenerating vanadium electrolyte in a failed vanadium redox flow battery. Experiments were conducted at 20°C. Unless otherwise specified, all pH values were measured using a calibrated pH meter, the total vanadium concentration was determined by potentiometric titration, and the concentration of metallic impurities was determined by ICP-OES. The method includes the following steps: S1. Take 200 mL each of the positive and negative electrolytes from the failed vanadium redox flow battery. The vanadium concentration of this failed electrolyte is 1.67 mol / L. Figure 1 As shown, the potentiometric titration curve exhibits two potential change ranges corresponding to different vanadium valence states as the potassium permanganate titration volume increases; for example... Figure 2 As shown, the two peaks of the first-order differential curve correspond to V. 3+ and V 4+ The titration endpoint. (By...) Figure 1 and Figure 2 Determine the volume consumed in the potentiometric titration of potassium permanganate: V1 = 5.06 mL (V 3+ V2 = 10.18 mL (V 4+ ), mole fraction: X V 3+ =0.332, X V 4+ =0.668, molar concentrations of each valence state: C(V) 3+ = C_total (V) × X V 3+ =0.5532mol / L C(V) 4+ = C_total (V) × X V 4+ =1.1130mol / L The calculated average valence state of the failed vanadium electrolyte was +3.7. The initial composition of the failed vanadium electrolyte in Example 1 is shown in Table 1. The impurities exceeded the standard: Fe 3+ =89.32mg / L, Al 3+ =60.05mg / L, Cu 2+ =10.21mg / L, Ca 2+ =30.21mg / L, Si 4+ =16.43mg / L.
[0042] Table 1
[0043] Nitrogen gas was introduced for protection, and mechanical stirring (200 rpm) was performed for 30 minutes to ensure complete homogeneous mixing of the positive and negative electrode liquids, eliminate local differences in valence state, and obtain a homogeneous mixture A.
[0044] S2. Slowly introduce pure oxygen into the homogeneous mixture A, controlling the oxygen flow rate at 0.10 vvm, maintaining the temperature at 20℃ and the stirring speed at 150 rpm, and controlling the oxidation endpoint through online potential monitoring. The oxidation time was 2.5 h, during which organic degradation impurities were oxidized into CO2 and H2O; the Fe in the system was reduced. 2+ Completely oxidized to Fe 3+ After oxidation, Fe becomes Fe3+ The solution is present, and its turbidity is significantly reduced, resulting in mixture B.
[0045] S3. Add 5% (w / w) dilute ammonia to the mixture B to adjust the pH of the electrolyte and remove Al. 3+ Cu 2+ Ca 2+ Some Si impurities.
[0046] Dilute ammonia was slowly added dropwise, and the pH of the solution was monitored in real time with a pH meter until the pH was adjusted to 2.5. The mixture was stirred for 15 minutes to obtain mixture C. Mixture C was aged at 20°C for 2 hours, and then filtered precisely (using a 0.22μm filter membrane) to remove precipitates such as hydroxides, silica colloids, and calcium sulfate to obtain the first filtrate.
[0047] Add 5% (w / w) dilute ammonia solution dropwise to the first filtrate to adjust the pH to 3.0, and stir for 15 minutes to obtain mixture D. Then, age mixture D at 20°C for 3 hours to form Fe(OH)3 flocs, which adsorb residual trace amounts of Al, Cu, and Si colloids. Perform a second precision filtration to obtain the second filtrate. Pass the second filtrate through a fixed bed of H-type iminodiacetic acid macroporous chelating cation exchange resin (Purolite S930Plus) at a flow rate of 5 BV / h for adsorption at room temperature, deeply removing residual heavy metal ions to obtain a deeply purified electrolyte.
[0048] Effluent detection: Filtrate analysis via ICP-OES: Al 3+ =12mg / L<50mg / L, Cu 2+ =0.22mg / L < 1mg / L, Ca 2+ =7.64mg / L < 30mg / L, Si 4+ =1.56 mg / L < 10 mg / L, Fe 2+ / 3+ =6.89mg / L < 50mg / L, impurity removal rate ≥ 99%, and all impurity ions meet the national standard (GB / T37204—2018).
[0049] S4. The purified electrolyte is used as the cathode liquid, and the anolyte is 3.0 mol / L high-purity sulfuric acid. The cathode and anode are separated by a proton exchange membrane, and the electrodes are made of acid-resistant conductive carbon material.
[0050] At 40mA / cm 2 Constant current electrolysis was performed at a controlled temperature of 20°C, with nitrogen protection maintained throughout the process. Based on the measured total vanadium concentration, volume, and average valence state before electrolysis, the equation Q = F × C was used. v ×V eThe calculated charge is 3.17 A·h, and the electrolysis time is determined to be 95 min using the formula t=Q / I.
[0051] During electrolysis, samples were taken and titrated every 0.5 hours. Electrolysis was stopped when V(III):V(IV) was 1:1 and the average valence was +3.50±0.02. The electrolyte was then circulated for 10 minutes to make the electrolyte composition uniform.
[0052] S5. The actual measured volume after electrolysis is 400.0 mL. The calculated V... 3+ The concentration is 0.823 mol / L, V 4+ The concentration was 1.105 mol / L, the total vanadium concentration was 1.928 mol / L, and the average valence state of the electrolyte after recovery and regeneration was +3.573. The sulfate concentration fluctuated slightly. 1 mL of high-purity sulfuric acid (concentration 3.0 mol / L) and 5.90 mL of deionized water were added to adjust the total vanadium concentration to 1.9 mol / L and the sulfuric acid concentration to 3.0 mol / L.
[0053] Example 2: The method for restoring and regenerating the vanadium electrolyte in a failed vanadium redox flow battery in this embodiment was tested at 25°C. The remaining testing methods are the same as in Example 1, and include the following steps: S1. Take 300 mL each of the positive and negative electrolytes from the failed vanadium redox flow battery, with an initial total vanadium concentration of 1.72 mol / L; If Figure 3 As shown, the potentiometric titration curve exhibits two potential change ranges corresponding to different vanadium valence states as the potassium permanganate titration volume increases; for example... Figure 4 As shown, the two peaks of the first-order differential curve correspond to V. 3+ and V 4+ The titration endpoint. (By...) Figure 3 and Figure 4 Determine the volume consumed in the potentiometric titration of potassium permanganate: V1 = 4.72 mL (V 3+ V2 = 10.56 mL (V 4+ Total titration volume: 15.28 mL. Mole fraction: X V 3+ =4.72 / 15.28≈0.3089, X V 4+ =10.56 / 15.28≈0.6911, Average vanadium valence state of the failed liquid: z = (3 × 0.5313 + 4 × 1.1887) ÷ 1.72 ≈ 3.691, impurities exceed the standard: Fe 3+ =126mg / L, Al 3+ =88mg / L, Cu 2+ =16mg / L, Ca 2+ =42mg / L, Si4+ =24mg / L.
[0054] The failed electrolytes of the positive and negative electrodes were transferred into a sealed reactor, and high-purity nitrogen was continuously introduced to isolate the air for protection. Mechanical stirring was carried out (stirring rate of 220 rpm, constant temperature of 25℃, stirring time of 35 min) to eliminate local valence state stratification and obtain a homogeneous mixed stock solution (i.e., mixed solution A).
[0055] S2. Maintain a constant temperature of 25℃ and a stirring speed of 160 rpm. Continuously introduce pure oxygen into mixture A for 3 hours to oxidize it. The oxygen flow rate is controlled at 0.20 vvm. Monitor the oxidation endpoint in real time using online potential. Remove residual Fe from the system. 2+ Completely oxidized to Fe 3+ The organic degradation products of the electrolyte are oxidized and decomposed into CO2 and water. After oxidation, the solution turns light yellow-brown and the turbidity decreases significantly, resulting in mixture B.
[0056] S3. Slowly add 2% dilute ammonia water to the obtained mixture B, adjust the pH to 2.6, stir at 25℃ for 20 min to obtain mixture C; keep mixture C at 25℃ for 2.5 h, then filter it with a 0.22μm precision filter membrane to remove Al(OH)3, silica colloid, calcium sulfate, and silicate precipitate to obtain the first filtrate.
[0057] Secondary coprecipitation for iron removal: 5% dilute ammonia solution was added dropwise to the first filtrate to adjust the pH to 3.2. The mixture was stirred for 20 minutes to obtain a mixed solution D. The mixed solution D was then aged at 25°C for 3.5 hours to generate Fe(OH)3 flocs, which adsorbed and coprecipitated trace amounts of Al, Cu, and silica gel. The mixture was then subjected to a second precision filtration to obtain the second filtrate.
[0058] The second filtrate was subjected to deep purification at a flow rate of 3.5 BV / h through a fixed bed of H-type iminodiacetic acid macroporous chelating cation exchange resin (Lewatit TP207). Adsorption at room temperature effectively removed residual heavy metal ions, yielding a deeply purified electrolyte. ICP-OES analysis of impurities after purification showed that Al was present. 3+ =4.67mg / L < 50mg / L, Cu 2+ =0.12mg / L < 1mg / L, Ca 2+ =2.67mg / L < 30mg / L, Si 4+ =1.90 mg / L < 10 mg / L, Fe 2+ / 3+ =6.87mg / L < 50mg / L, overall impurity removal rate ≥ 99%, meeting the national standard (GB / T37204—2018) electrolyte standard.
[0059] S4. Use the purified electrolyte as the cathode solution, and select a 3 mol / L high-purity sulfuric acid solution as the anolyte; Electrolysis process parameters: current density 50 mA / cm². 2 The device features a power supply of 5.56 A·h, an energizing time of 133 min, a constant temperature of 25℃, and nitrogen inert protection throughout the process. It employs potentiometric titration for real-time online monitoring of vanadium ion valence state changes and constant current electrolysis to regulate the power supply, ensuring that V... 3+ With V 4+ The molar ratio approaches 1:1. Sampling and detection at the electrolysis endpoint: c(V) 3+ =0.861 mol / L, c(V) 4+ The concentration of vanadium is 0.857 mol / L, the total vanadium concentration is 1.718 mol / L, the average valence is 3.498, and the valence deviation is ≤0.002, which meets the target valence requirement of +3.5.
[0060] S5. During electrolysis, ion migration across the membrane causes slight fluctuations in sulfate and vanadium concentrations. Concentration deviations are calculated by monitoring changes in solution density and volume. After electrolysis, the electrolyte volume is measured to be 600.0 mL and the total vanadium concentration is 1.720 mol / L. 7.06 mL of a prepared 3.000 mol / L sulfuric acid standard solution is added, including 5.91 mL of deionized water. The concentrations are adjusted to 1.7 mol / L total vanadium and 3.0 mol / L sulfate. The solution is then precisely filtered to remove trace amounts of suspended colloids, yielding the regenerated vanadium electrolyte.
[0061] Example 3: The method for restoring and regenerating the vanadium electrolyte in a failed vanadium redox flow battery in this embodiment was tested at 30°C. The remaining testing methods are the same as in Example 1, and include the following steps: S1. Take 250 mL each of the positive and negative electrolytes from the failed vanadium battery, with an initial total vanadium concentration of 1.62 mol / L; If... Figure 5 As shown, the potentiometric titration curve exhibits two potential change ranges corresponding to different vanadium valence states as the potassium permanganate titration volume increases; for example... Figure 6 As shown, the two peaks of the first-order differential curve correspond to V. 3+ and V 4+ The titration endpoint. (By...) Figure 5 and Figure 6 Determine the volume consumed in the potentiometric titration of potassium permanganate: V1 = 4.38 mL (V 3+ V2 = 10.74 mL (V 4+ Total titration volume: 15.12 mL. Mole fraction: X V 3+ =4.38 / 15.12≈0.2897, X V 4+ =10.74 / 15.12≈0.7103 Valence concentration: c(V) 3+)=1.62×0.2897≈0.4693mol / L, c(V 4+ )=1.62×0.7103≈1.1507mol / L.
[0062] Average vanadium valence state of the failed liquid: z = (3 × 0.4693 + 4 × 1.1507) ÷ 1.62 ≈ 3.710; Initial impurities: total Fe = 142 mg / L, Al 3+ =95mg / L, Cu 2+ =19mg / L, Ca 2+ =48mg / L, Si 4+ =28mg / L.
[0063] The positive and negative electrolytes are mixed into a sealed reactor and continuously protected with nitrogen. The mixture is stirred and mixed (stirring speed is 240 rpm, constant temperature is 30℃, and stirring time is 40 min) to eliminate local enrichment of valence states and obtain a uniformly mixed failed original solution (i.e., mixture A).
[0064] S2. Under constant temperature of 30℃ and stirring speed of 180 rpm, pure oxygen was introduced into mixture A for 2 hours for oxidation, with the oxygen introduction rate controlled at 0.15 vvm. The oxidation endpoint was monitored online by potential. Fe in the system was completely oxidized. 2+ For Fe 3+ The organic degradation impurities in the electrolyte are completely decomposed, and the clarity of the solution is significantly improved after oxidation, with no suspended organic flocs, resulting in mixture B.
[0065] S3. Primary precipitation and impurity removal: Using 3% dilute ammonia water, slowly adjust the pH of mixture B to 2.8, stir at 30℃ for 15 minutes to obtain mixture C; keep mixture C at 30℃ for 2 hours, and then use a 0.22μm filter membrane for precision filtration to remove Al, Ca, and silicon-based precipitates to obtain the first filtrate.
[0066] Secondary coprecipitation for iron removal: 3% dilute ammonia solution was slowly added to the first filtrate to adjust the pH to 3.4. The mixture was stirred for 15 minutes to obtain a mixed solution D. The mixed solution D was then aged at 30°C for 3 hours to generate Fe(OH)3 flocs to coprecipitate trace heavy metals. The mixture was then subjected to a second precision filtration to obtain the second filtrate.
[0067] The second filtrate was subjected to deep purification at a flow rate of 4 BV / h through a fixed bed of H-type iminodiacetic acid macroporous chelating cation exchange resin (Amberlite IRC748) to remove residual trace heavy metals at room temperature, yielding a deeply purified electrolyte. ICP analysis after purification showed that Al... 3+ =7.12mg / L < 50mg / L, Cu 2+ =0.34mg / L < 1mg / L, Ca2+ =6.82mg / L<30mg / L, Si 4+ =1.52mg / L < 10mg / L, Fe 2+ / 3+ =9.32mg / L < 50mg / L, impurity removal rate ≥ 99.1%, which meets the national standard (GB / T37204—2018) electrolyte standard.
[0068] S4. The purified electrolyte is used as the cathode solution, and the anode uses a standard 3 mol / L sulfuric acid electrolyte; Electrolysis parameters: current density 65 mA / cm² 2 The system operates at a constant temperature of 30℃, with a current flow of 4.80 A·h and a energizing time of 89 min, under nitrogen-sealed protection throughout. Potentiometric titration tracks the vanadium ion valence state change in real time, while constant current electrolysis controls the current flow, adjusting V... 3+ / V 4+ The molar ratio is close to 1:1. Electrolysis endpoint detection: c(V) 3+ =0.812 mol / L, c(V) 4+ =0.806mol / L, total vanadium concentration 1.618mol / L, average valence 3.497, valence deviation ≤0.003, meeting the target +3.5 valence standard.
[0069] S5. Electrolysis caused slight shifts in vanadium and sulfate concentrations due to transmembrane migration. The concentration difference was calculated based on changes in solution density and volume. After electrolysis, the total electrolyte volume was measured to be 500.0 mL, and the total vanadium concentration was 1.618 mol / L. 5.6 mL of a 3.0 mol / L high-purity sulfuric acid standard solution was added, stirred thoroughly, and then measured again. After reconstitution, the total vanadium concentration was 1.600 mol / L, and the sulfuric acid concentration was 3.0 mol / L. Trace solid impurities were removed by precise filtration, yielding a qualified regenerated electrolyte.
[0070] Performance testing: The regenerated electrolytes compounded in Examples 1-3 were assembled into vanadium redox flow batteries of the same structure and subjected to 100 constant current charge-discharge cycles. The experimental results are as follows.
[0071] Example 1: As Figure 10 As shown, the initial discharge capacity is 1.67 A·h; Figure 9 As shown, the coulombic efficiency gradually decreased from 92% in the first cycle to 89% in the 100th cycle, a decrease of 3 percentage points; Figure 8 As shown, the voltage efficiency remains consistently between 88% and 89%; Figure 7 As shown, the energy efficiency decreased from 83% to 79%. Therefore, the voltage efficiency of Example 1 remained relatively stable, while the decrease in energy efficiency corresponds to a gradual decrease in coulombic efficiency. The capacity recovery rate needs to be calculated based on the initial discharge capacity of a fresh reference electrolyte under the same battery and operating conditions.
[0072] Example 2: As Figure 10 As shown, the initial discharge capacity is 1.90 A·h, which is the highest among the three embodiments illustrated; as Figure 9 As shown, the coulombic efficiency changes from 98% to 97%, a change of 1 percentage point within 100 cycles; as Figure 8 As shown, the voltage efficiency remains at 85%-86%; Figure 7 As shown, the energy efficiency is 84%. Compared with Example 1, Example 2 exhibits higher coulombic efficiency and capacity, but its voltage efficiency is 2-4 percentage points lower. This is because higher current density increases electrode reaction overpotential, ohmic voltage drop across the membrane and electrolyte, and mass transfer polarization, thereby widening the charge-discharge voltage difference and reducing voltage efficiency.
[0073] Example 3: As Figure 10 As shown, the initial discharge capacity is 1.65 A·h; Figure 9 As shown, the coulombic efficiency decreased from 98% to 96%; Figure 8 As shown, the voltage efficiency decreased from 85% to 83%-84%; Figure 7 As shown, the energy efficiency decreased from 84% to 81%. Compared to Example 2, Example 3 exhibited both lower coulombic efficiency and voltage efficiency at the end of 100 cycles, thus its energy efficiency decreased more significantly.
[0074] The efficiency of each component showed no significant decay during cycling, demonstrating excellent electrochemical performance and cycle stability, and can be used in the actual operating conditions of vanadium redox flow batteries.
[0075] The experimental results above show that the technical solution of the present invention has the following characteristics: Highly efficient and thorough impurity removal: Through a multi-stage synergistic process of oxidation-pH gradient hydrolysis precipitation-precipitation-precision filtration-chelation resin purification, key impurities such as Fe, Si, and Al are efficiently removed.
[0076] Precise valence control: Electrolysis is used instead of chemical reagents for valence adjustment, avoiding the introduction of new impurities, and the valence state of vanadium is controlled through real-time monitoring with minimal deviation.
[0077] Short process flow and low cost: The entire regeneration process does not require complex equipment, and the regeneration cost can be reduced by more than 60% compared with new electrolyte.
[0078] Excellent regeneration performance: the purity of the regenerated electrolyte is ≥99.9%, the battery capacity recovery rate is ≥95%, and the energy efficiency remains ≥80% after 100 cycles, meeting the requirements of industrial applications.
[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the specific implementation of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.
Claims
1. A method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery, characterized in that, The process includes the following: The positive and negative electrolytes of the failed vanadium battery were mixed in a protective atmosphere at a volume ratio of (0.5-1.5):(0.5-1.5) to obtain mixture A. Oxygen is introduced into the mixture A and stirred to carry out oxidation treatment, resulting in mixture B. Add ammonia to the mixture B to adjust the pH to 2.0-3.0, thus obtaining mixture C; The mixture C is subjected to solid-liquid separation to obtain the first filtrate; Add alkali solution to the first filtrate to adjust the pH value to 3.0-3.5 to obtain mixture D; The mixture D is aged, and after aging, solid-liquid separation is performed to obtain a second filtrate. The second filtrate is passed through a selective chelating cation exchange resin to remove the impurity metal ions that remain after hydrolysis and precipitation, thus obtaining a deeply purified electrolyte. Using the deep-purified electrolyte as the cathode liquid, and separating the deep-purified electrolyte from the anolyte through a proton exchange membrane, electrolysis is performed to adjust the vanadium ion ratio to the target state of V(III):V(IV)=1:
1. Then, the vanadium ion concentration and sulfate concentration are adjusted to the target values, thereby realizing the recovery and regeneration of the failed vanadium electrolyte in the vanadium redox flow battery.
2. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, The positive and negative electrolytes of a failed vanadium battery are mixed in equal volume ratio under a protective atmosphere to obtain mixture A.
3. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, When oxygen is introduced into mixture A and stirred to carry out oxidation treatment, resulting in mixture B: The oxygen flow rate is 0.05-0.20 vvm, the preferred treatment time is 25-35 min, and the temperature of the mixed solution A during oxidation treatment is 20-40℃.
4. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, When ammonia is added to mixture B to adjust the pH to 2.0-3.0, resulting in mixture C: Ammonia solution with a mass fraction of 1%-5% is used; Ammonia solution is added dropwise to mixture B, and the rate of pH change during the addition of ammonia solution is controlled to not exceed 0.2 pH units / min.
5. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, The alkaline solution added to the first filtrate is ammonia water with a mass fraction of 1%-5%.
6. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, When aging the mixture D, the aging temperature is 20-30℃ and the aging time is 30-90 min.
7. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, The selective chelating cation exchange resin is a chelating cation exchange resin containing iminodiacetic acid groups or aminophosphonic acid groups; the chelating resin is an H-type resin; the H-type resin is Purolite S930Plus, Lewatit TP 207 or Amberlite IRC748.
8. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 7, characterized in that, When the second filtrate is passed through a selective chelating cation exchange resin to remove residual impurity metal ions after hydrolysis and precipitation, a deeply purified electrolyte is obtained: The second filtrate was subjected to deep purification by passing it through a fixed bed packed with selective chelating cation exchange resin. The resin bed was filled with 0.02-0.06 L of resin per 1 L of wet resin volume. The height-to-diameter ratio of the resin bed was (5-10):
1. The influent pH was controlled at 3.0-3.1, and the processing flow rate was 2-5 BV / h, where BV is the wet resin bed volume. Influent and effluent samples were collected after processing 0.45-0.55 BV of electrolyte, and the total vanadium concentration and the concentration of the target impurity ions were measured. When the ratio of the effluent concentration to the influent concentration of any target impurity ion reached 0.05, the resin was considered to have reached the impurity penetration endpoint. After the resin reaches the breakthrough endpoint, the residual liquid is first replaced with 1-2 BV of deionized water, and then regenerated with sulfuric acid solution of concentration 1.0-2.0 mol / L at a flow rate of 1-2 BV / h, with a regeneration solution volume of 2-4 BV. Subsequently, it is washed with 3-5 BV of deionized water until the effluent is free of metal ions, and then transformed and equilibrated with 1-2 BV of sulfuric acid solution of concentration 1.5-2.0 mol / L to obtain a reusable H-type chelating resin.
9. The method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1, characterized in that, Using the aforementioned deeply purified electrolyte as the cathode liquid, and separating the deeply purified electrolyte from the anolyte through a proton exchange membrane, during electrolysis: The electrolyte temperature is controlled at 20-40℃; the current density for constant current electrolysis, based on the effective projected area of the electrodes, is 20-80 mA / cm². 2 ; The electrolyte is circulated into the electrolytic cell.
10. A method for recovering and regenerating vanadium electrolyte in a failed vanadium redox flow battery according to claim 1 or 9, characterized in that, The anolyte is a pretreated vanadium sulfate reference electrolyte, or an inert anode is used with sulfuric acid electrolyte as the anolyte; both the cathode and anode are made of acid-resistant conductive carbon material, which includes graphite felt electrode and carbon paper electrode. During electrolysis, the theoretical charge flow rate is determined by the following formula: Q=F×C v ×V e ×|3.5-Z0| / h In the formula, Q is the theoretical charge, in C; F is the Faraday constant; C v V represents the total vanadium concentration in the electrolyte, expressed in mol / L. e Z0 represents the volume of the electrolyte to be treated, in liters (L); Z0 represents the average valence state of vanadium ions before electrolysis. η is the current efficiency; When the initial average valence state is lower than +3.5, the electrolyte to be treated is used as the anolyte for oxidation electrolysis. When the initial average valence state of the deep-purified electrolyte is higher than +3.5, the deep-purified electrolyte is used as the cathode liquid for reduction electrolysis. The electrolysis time is determined by the theoretical charge and the actual current, i.e., t = Q / I. The single electrolysis time is controlled to be 0.5-8 h, and adjusted according to the electrolyte volume, electrode area and initial valence state. When the initial average valence state is equal to +3.5 and the molar ratio of V(III) to V(IV) meets the target state, the vanadium ion concentration and sulfate concentration are adjusted to the target values. During electrolysis, online redox potential monitoring was used, and samples were taken every 25-35 minutes for potentiometric titration analysis. Electrolysis was stopped when the molar ratio of V(III) to V(IV) reached 1:1 and the average valence state of vanadium ions reached +3.3 to +3.
7. After electrolysis, the electrolyte was circulated for 5-15 minutes to ensure that the electrolyte composition was homogeneous. When the vanadium ion concentration and sulfate concentration are adjusted to the target values, according to the measurement results, a pre-prepared sulfuric acid standard solution or deionized water is added to the electrolyte under stirring conditions, or vanadium sulfate reference electrolyte is added to restore the total vanadium concentration, sulfate concentration and electrolyte volume to the preset target values, and finally realize the recovery and regeneration of the failed vanadium electrolyte in the vanadium redox flow battery.
Citation Information
Patent Citations
Regeneration method of ineffective vanadium electrolyte of sulfuric acid system
CN109360997A
A method for recycling waste vanadium battery electrolyte
CN116130692B
Recycling method of failure all-vanadium redox flow battery electrolyte