A high-temperature, high-pressure cycle-stable lithium-ion battery

By combining a doped and modified LiCoO2 cathode with specific electrolyte additives, the problem of poor cycle stability of lithium-ion batteries under high temperature and high pressure was solved, and long-term stability and high performance of the battery under high temperature and high pressure were achieved.

CN123120830APending Publication Date: 2026-11-17HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611476375.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have poor cycle stability under high temperature and high pressure. Current optimization strategies are difficult to balance bulk and interface stability, resulting in a decrease in battery cycle life in complex environments.

Method used

By employing a combination design of doped and modified LiCoO2 cathode material and specific electrolyte additives, strong TM-O bonds are formed to suppress phase transitions, and a stable CEI layer blocks electrolyte erosion. Combined with silicon-carbon anode and polyethylene separator, the interface stability is improved.

Benefits of technology

It significantly improves the cycle stability and electrochemical performance of lithium-ion batteries under high temperature and high pressure, avoids electrolyte decomposition and interface failure, maintains excellent ion and electron transport dynamics, and extends battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120830A_ABST
    Figure CN123120830A_ABST
Patent Text Reader

Abstract

This invention discloses a high-temperature, high-pressure cycle-stable lithium-ion battery, belonging to the field of lithium-ion battery technology. The battery includes a LiCoO2 positive electrode, an electrolyte, a negative electrode, and a separator; wherein the LiCoO2 positive electrode contains at least one doping element selected from Mg, Al, Zr, F, and Ti; the high-temperature, high-pressure additive contains at least two selected from vinylene carbonate (VC), 1,3,6-hexanetrionitrile (HTCN), 1,3-propanesulfonyl lactone and fluoroethylene carbonate (FEC), methane disulfonyl ester (MMDS), and 1,3-propanesulfonyl lactone (PS). This invention achieves synergistic regulation of element doping and electrolyte additives, significantly improving the high-temperature, high-pressure cycle performance of LCO batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and in particular to a lithium-ion battery that is stable under high temperature and high pressure cycling. Background Technology

[0002] LiCoO2 (LCO) is one of the most widely used cathode materials in commercial lithium-ion batteries due to its high specific capacity, excellent conductivity, and mature preparation process. With the rapid development of the new energy industry, the demand for battery energy density in end-user devices continues to rise. Increasing the operating voltage of LCO-based batteries (e.g., to 4.6V) is an effective technical path to improve energy density. However, at high voltages, LCO is prone to O3 phase to H phase transformation. 1-3 Irreversible phase transitions are accompanied by lattice oxygen evolution; meanwhile, in practical applications, batteries often face high temperatures that accelerate electrolyte decomposition and exacerbate side reactions at the electrode interface, further deteriorating battery cycle stability, making it difficult for existing LCO-based batteries to meet long-term usage requirements under high temperature and high pressure conditions.

[0003] In existing technologies, stability optimization strategies for LCO are mainly divided into two categories: bulk phase control and interface optimization. For bulk phase control, elements such as Ti, Mo, W, and Mg with high bonding energies to oxygen are doped to form "oxygen anchors," enhancing bulk integrity. However, single doping is insufficient to ensure interface stability at high temperatures. For interface optimization, surface coating with polyanionic species (such as PO4) is employed. 3- (e.g., CePO4) can reduce direct contact between the material surface and the electrolyte, inhibiting the dissolution of Co / O from the material surface, or electrolyte additives can be used to optimize the CEI layer. However, the coating layer is prone to increased impedance and uneven distribution, affecting the rate performance of the battery. Optimization of a single electrolyte cannot suppress the irreversible phase transition in the bulk phase.

[0004] In addition, most existing technologies focus on normal temperature or single high voltage scenarios, lacking targeted optimization for high temperature and high voltage combined operating conditions, resulting in a significant reduction in battery cycle life in real complex environments, which cannot meet the requirements of commercial applications. Summary of the Invention

[0005] The purpose of this invention is to provide a lithium-ion battery that is stable under high temperature and high pressure, thereby improving the cycle stability under high temperature and high pressure conditions.

[0006] To achieve the above objectives, the present invention provides a high-temperature, high-pressure cycle-stable lithium-ion battery, comprising a positive electrode, an electrolyte, a negative electrode, and a separator. The positive electrode is doped and modified LiCoO2, the electrolyte comprises a base electrolyte and additives, the negative electrode is a silicon-carbon negative electrode, and the separator is a polyethylene separator. The element used in the positive electrode doping modification is at least one of Mg, Al, Zr, F, and Ti; The additive is at least two of the following: adiponitrile, 1,3,6-hexanetrionitrile, fluoroethylene carbonate, methane disulfide methyl ester, and 1,3-propane sulpholol.

[0007] Preferably, the lithium-ion battery has an operating voltage of 2.5-4.55V and an operating temperature of 60℃.

[0008] Preferably, the doping amount of each positive electrode doping modification element is 0.5-2%.

[0009] Preferably, the mass fraction of each additive in the electrolyte is 1-5%.

[0010] Preferably, the base electrolyte is a mixed solvent of ethylene carbonate / dimethyl carbonate / diethyl carbonate containing dissolved lithium salt.

[0011] Preferably, the volume ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate is 1:1:1; The lithium salt is LiPF6, and its concentration in the base electrolyte is 1.0 mol / L. The separator is a polyethylene (PE) membrane.

[0012] Preferably, the negative electrode is a silicon-carbon negative electrode (SiC).

[0013] Therefore, the present invention provides a high-temperature, high-pressure cycle-stable lithium-ion battery through the coupled design of bulk doping and electrolyte additives, which has the following beneficial effects: (1) Strong TM-O bonds inhibit phase transition and lattice oxygen activity in the bulk phase, and a stable CEI layer blocks electrolyte erosion at the interface. The dual protection works synergistically to comprehensively solve the structural degradation problem of LiCoO2 under high temperature and high pressure.

[0014] (2) The combination design of electrolyte solvent system and additives ensures that the battery can maintain stable electrochemical performance at a high temperature of 60°C, avoiding problems such as electrolyte decomposition and interface failure caused by high temperature.

[0015] (3) LiCoO2 can be prepared by commercial purchase or conventional solid-state sintering method. The electrolyte formulation is simple and easy to scale up production. No additional complex process steps are required. Furthermore, there is no need to coat the surface of LiCoO2, which avoids problems such as increased impedance and decreased rate performance caused by the coating layer. The battery maintains high stability while also having excellent ion / electron transport dynamics.

[0016] (4) The battery can maintain high and stable cycle performance in a high-temperature environment of 60°C, which is far superior to the battery performance of existing single optimization strategies.

[0017] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0018] Figure 1 The following are the elemental bonding characterization diagrams of the cathode materials used in this invention; wherein, (a) is the Mg 1s XPS spectrum of Mg-LCO; (b) is the Al 2p XPS spectrum of Al-LCO; (c) is the Zr 3d XPS spectrum of Zr-LCO; (d) is the F 1s XPS spectrum of F-LCO; and (e) is the Ti 2p XPS spectrum of Ti-LCO.

[0019] Figure 2 The graphs show the electrochemical performance curves of two sets of soft-pack batteries prepared in Example 1 and Comparative Example 1 of this invention under the conditions of 2.5-4.55V and 1C; where (a) is the high-temperature cycling performance curve at 60℃; and (b) is the charge-discharge curve corresponding to 200 cycles. Figure 3 This is a comparison of the cycle performance curves of two sets of soft-pack batteries prepared in Example 2 and Comparative Example 1 of the present invention under the conditions of 60°C, 2.5-4.55V, and 1C. Figure 4 This is a comparison chart showing the voltage changes of two sets of soft-pack batteries prepared in Example 3 and Comparative Example 1 of the present invention after being fully charged at 0.1C and stored at 60°C for 250 hours. Detailed Implementation

[0020] This invention provides a high-temperature, high-pressure cycle-stable lithium-ion battery, comprising a positive electrode, an electrolyte, a negative electrode, and a separator, the specific components of which are as follows: (1) Positive electrode material: LiCoO2 doped with at least one element such as Mg, Al, Zr, F, or Ti is used as the positive electrode active material, wherein the doping amount is 0.5-2%.

[0021] (2) Electrolyte system: The electrolyte consists of a base electrolyte and additives, wherein: Basic electrolyte: LiPF6 is used as the lithium salt, with a concentration of 1.0 mol / L in the basic electrolyte; the solvent is a mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) in a volume ratio of 1:1:1. This system has both good ionic conductivity and high-temperature stability, which can reduce solvent decomposition reactions at high temperatures.

[0022] Additives: at least two selected from vinylene carbonate (VC), 1,3,6-hexanetrionitrile (HTCN), fluoroethylene carbonate (FEC), methane disulfide (MMDS), and 1,3-propane sulpholactone (PS). The mass fraction of each additive in the electrolyte is 1-5%, preferably 2%. This allows the formation of a dense and stable CEI layer, which effectively blocks direct contact between the electrolyte and the positive electrode material, inhibiting surface oxygen evolution.

[0023] (3) Negative electrode: Silicon-carbon negative electrode (SiC) is selected. This negative electrode material has good electrochemical compatibility and can form a stable electrode interface with LiCoO2 positive electrode and electrolyte containing additives.

[0024] (4) Separator: Polyethylene (PE) separator is used, which has excellent mechanical strength and ion permeability, and can maintain structural integrity at high temperature to avoid battery short circuit.

[0025] The technical solution of the present invention will be further described below with reference to the accompanying drawings and embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention should be considered equivalent substitutions and are included within the protection scope of the present invention. Furthermore, it should be understood that after reading the contents of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims and are all within the protection scope of the present invention.

[0026] In this document, the term "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The term "embodiment" appearing in various places throughout the specification does not necessarily refer to the same embodiment, nor does it specifically limit its independence or connection with other embodiments. In principle, in this application, as long as there are no technical contradictions or conflicts, the technical features mentioned in each embodiment can be combined in any way to form corresponding implementable technical solutions.

[0027] Unless otherwise defined, the technical terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the use of related terms herein is merely for the purpose of describing particular embodiments and is not intended to limit this application.

[0028] Unless otherwise specified, the reagents, instruments, and equipment used in this invention are all commonly used by those skilled in the art, and the testing standards all use national or international standards commonly used in the field, without further explanation.

[0029] The experimental materials used in the following examples and comparative examples are as follows: Cathode material: Commercially available LiCoO2 doped with at least one element of Mg, Al, Zr, F, or Ti.

[0030] Electrolyte raw materials: LiPF6 (purity ≥99.9%), EC (purity ≥99.9%), DMC (purity ≥99.9%), DEC (purity ≥99.9%).

[0031] Other materials: silicon-carbon anode (SiC) anode sheet, polyethylene separator (20μm thick), and aluminum-plastic film for pouch batteries.

[0032] Example 1 This embodiment provides a method for assembling and preparing a high-temperature, high-pressure cycle-stable lithium-ion battery, including the following steps: (1) Preparation of composite electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. Then, 2% FEC, 3% HTCN and 3% PS electrolyte additives were added, stirred evenly and sealed for later use.

[0033] (2) Battery assembly: Soft-pack battery assembly: Using 2% Ti-LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||Ti-FEC+HTCN+PS-LCO soft-pack batteries are assembled in an argon glove box.

[0034] Example 2 This embodiment provides a method for assembling and preparing a lithium-ion battery, including the following steps: (1) Preparation of composite electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. Then, 4% VC and 2% MMDS electrolyte additives were added, stirred evenly, and sealed for later use.

[0035] (3) Battery assembly: Pouch cell assembly: Using 0.5% Al-LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||Al-VC+MMDS-LCO pouch cells are assembled in an argon glove box.

[0036] Example 3 This embodiment provides a method for assembling and preparing a lithium-ion battery, including the following steps: (1) Preparation of composite electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. Then, 3% HTCN and 2% PS electrolyte additives were added, stirred evenly, and sealed for later use.

[0037] (3) Battery assembly: Pouch cell assembly: Using 1% Zr-LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||Zr-HTCN+PS-LCO pouch cells are assembled in an argon glove box.

[0038] Example 4 This embodiment provides a method for assembling and preparing a lithium-ion battery, including the following steps: (1) Preparation of composite electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. Then, 2% MMDS electrolyte additive was added, stirred evenly, and sealed for storage for later use.

[0039] (3) Battery assembly: Pouch cell assembly: Using 0.5% Al-LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||Al-MMDS-LCO pouch cells are assembled in an argon glove box.

[0040] Example 5 This embodiment provides a method for assembling and preparing a lithium-ion battery, including the following steps: (1) Preparation of composite electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. Then, 2% PS and 3% HTCN electrolyte additives were added, stirred evenly, and sealed for later use.

[0041] (3) Battery assembly: Pouch cell assembly: Using 1% Zr-LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||Zr-PS+HTCN-LCO pouch cells are assembled in an argon glove box.

[0042] Example 6 This embodiment provides a method for assembling and preparing a lithium-ion battery, including the following steps: (1) Preparation of composite electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. Then, 4% VC and 3% MMDS electrolyte additives were added, stirred evenly, and sealed for later use.

[0043] (3) Battery assembly: Pouch cell assembly: Using 2%Mg0.5%Al-LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||MgAl-VC+MMDS-LCO pouch cells are assembled in an argon glove box.

[0044] Comparative Example 1 This comparative example provides a method for assembling and preparing a lithium-ion battery, including the following steps: (1) Preparation of electrolyte: LiPF6 was dissolved in a mixed solvent of EC / DMC / DEC (volume ratio 1:1:1) to prepare a 1.0 mol / L LiPF6 electrolyte. After stirring evenly, the solution was sealed and stored for later use.

[0045] (3) Battery assembly: Soft-pack battery assembly: Using unmodified LCO as the positive electrode, SiC electrode as the negative electrode, and polyethylene membrane as the separator, a composite electrolyte is injected, and SiC||-LCO soft-pack batteries are assembled in an argon glove box.

[0046] The doped and modified cathode material was characterized, and the results are as follows: Figure 1 As shown. By Figure 1 It can be seen that the LiCoO2 doped with different elements such as Mg, Al, Zr, F and Ti obtained the elemental characteristic peaks corresponding to Mg, Al, Zr, F and Ti respectively in the X-ray photoelectron spectroscopy (XPS) test results, indicating that the elements can be successfully doped into LiCoO2.

[0047] To verify the excellent electrochemical performance of bulk-doped anchored lattice oxygen and interface-modified LCO at a high voltage of 4.6V, the coin cells assembled in Example 1 and Comparative Example 1 were subjected to high-temperature performance testing at 60°C. The results are as follows: Figure 2 As shown.

[0048] Figure 2 (a) Shows the cycling performance curves of two sets of pouch cells, Example 1 and Comparative Example 1, at a high temperature of 60°C. The horizontal axis represents the number of cycles (0-200 cycles), and the vertical axis represents the capacity (mAh). The test conditions were: charging at 60°C with a constant current of 1C to 4.55V, maintaining a constant voltage to a current of 0.1C, resting for 5 minutes, and then discharging at a constant current of 1C to 2.5V, repeating the cycle. Figure 2 It can be seen that after 200 cycles, the capacity retention rate of Example 1 is still maintained at about 90.3%, while the battery of Comparative Example 1 has obviously failed after about 50 cycles. Figure 2 (b) shows the charge-discharge curves corresponding to 200 cycles of Example 1. No obvious voltage plateau degradation or polarization intensification was observed, indicating that Example 1 of the present invention can significantly improve the long-cycle stability of the battery at high temperatures and effectively suppress capacity decay.

[0049] Figure 3 The cycling performance curves of two sets of pouch cells, Example 2 and Comparative Example 1, at a high temperature of 60°C are shown. The horizontal axis represents the number of cycles (0-100 cycles), and the vertical axis represents the capacity (mAh). The test conditions were: charging at 60°C with a constant current of 1C to 4.55V, maintaining a constant voltage to a current of 0.1C, resting for 5 minutes, and then discharging at a constant current of 1C to 2.5V, repeating the cycle. Figure 2 It can be seen that after 100 cycles, the capacity retention rate of Example 1 remained at approximately 85.3%, while the battery in Comparative Example 1 showed significant failure after approximately 50 cycles. This indicates that the strategy can improve the high-temperature performance of LCO-SiC pouch cells, but it is difficult to achieve long-term cycling performance.

[0050] Figure 4 The self-discharge curves of two sets of pouch batteries (Example 3 and Comparative Example 1) after being fully charged and stored at 60°C are shown. The horizontal axis represents storage time (0-250h), and the vertical axis represents voltage (V). The test conditions were: fully charged at 0.1C at 60°C, then stored at high temperature for 250h, with real-time recording of voltage changes. Figure 4 It can be seen that after 250 hours of storage, the voltage of Example 3 stabilized at 4.0933V, while the voltage of Comparative Example 1 dropped to 4.0548V. This shows that Example 3 of the present invention can effectively reduce the battery self-discharge rate and significantly improve the high-temperature storage stability under full charge.

[0051] Therefore, this invention has thoroughly investigated the mechanism by which bulk doping and electrolyte additives synergistically enhance the stability of SiC||LCO pouch cells under high temperature and high pressure, thereby fundamentally breaking the vicious cycle between structural degradation and interfacial side reactions.

[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.

Claims

1. A high-temperature, high-pressure cycle-stable lithium-ion battery, comprising a positive electrode, an electrolyte, a negative electrode, and a separator, characterized in that: The positive electrode is doped and modified LiCoO2, the electrolyte contains a basic electrolyte and additives, the negative electrode is a silicon-carbon negative electrode, and the separator is a polyethylene separator. The element used in the positive electrode doping modification is at least one of Mg, Al, Zr, F, and Ti; The additive is at least two of the following: adiponitrile, 1,3,6-hexanetrionitrile, fluoroethylene carbonate, methane disulfide methyl ester, and 1,3-propane sulpholol.

2. The high-temperature, high-pressure cycle-stable lithium-ion battery according to claim 1, characterized in that: The operating voltage range of lithium-ion batteries is 2.5-4.55V; the operating temperature range is 60℃.

3. A high-temperature, high-pressure cycle-stable lithium-ion battery according to claim 1, characterized in that: The doping amount of each element used for cathode doping modification is 0.5-2%.

4. A high-temperature, high-pressure cycle-stable lithium-ion battery according to claim 1, characterized in that: The mass fraction of each additive in the electrolyte is 1-5%.

5. A high-temperature, high-pressure cycle-stable lithium-ion battery according to claim 1, characterized in that: The basic electrolyte is a mixed solvent of ethylene carbonate, dimethyl carbonate, and diethyl carbonate containing dissolved lithium salts.

6. A high-temperature, high-pressure cycle-stable lithium-ion battery according to claim 5, characterized in that: The volume ratio of ethylene carbonate, dimethyl carbonate, and diethyl carbonate is 1:1:1; The lithium salt is LiPF6, and its concentration in the basic electrolyte is 1.0 mol / L.