Battery cells and their preparation methods, battery devices, energy storage devices and electrical equipment
By introducing piezoelectric materials and film-forming agents into the electrodes in a coupled manner, a stress-polarization-preferred film-forming mechanism is constructed, which solves the problem of uneven interface rupture caused by electrode volume changes, realizes precise repair and efficient film formation of the battery interface layer, and improves the cycle life and efficiency of the battery.
Patent Information
- Application Number
- CN202611517815.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to achieve precise interface repair when electrode volume changes, leading to uneven rupture and consumption of the interface film, which affects the battery's cycle life and efficiency.
By introducing piezoelectric materials into the electrode and coupling the piezoelectric effect with the interfacial electrochemical reaction, a ternary response mechanism of "stress-polarization-preferential film formation" is constructed. The piezoelectric particles generate local potential disturbances in the stress concentration area, and the film-forming agent is used in conjunction to preferentially generate a dense protective layer in the damaged area.
It enables precise repair of the electrode interface layer, improves the interface stability and coulombic efficiency during battery cycling, and reduces the consumption of film-forming agents and production costs.
Smart Images

Figure CN123120832A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of energy storage technology, and in particular to battery cells and their preparation methods, battery devices, energy storage devices, and electrical equipment. Background Technology
[0002] With the rapid development of electric vehicles and large-scale energy storage technologies, the requirements for energy density, cycle life, and safety of lithium-ion batteries are constantly increasing. The theoretical specific capacity of traditional graphite anodes is only 372 mAh / g, which is insufficient to meet the needs of next-generation high-energy-density batteries. Silicon-based anodes, due to their extremely high theoretical specific capacity (4200 mAh / g, more than 11 times that of graphite), have become the most promising next-generation anode material. Meanwhile, high-nickel ternary cathode materials (such as the NCM811 and NCM90 series) have also attracted widespread attention due to their high specific capacity and high operating voltage. However, these high-capacity electrode materials face severe challenges in interfacial stability during practical applications.
[0003] The core problem with silicon-based anodes lies in their enormous volume changes during charge and discharge. Silicon expands by 300-400% during lithiation, and this repeated volume change causes the solid electrolyte interphase (SEI) film on the electrode surface to repeatedly rupture and regenerate. The continuous rupture of the SEI film exposes fresh silicon surface, continuously consuming electrolyte and active lithium, resulting in low initial coulombic efficiency and rapid capacity decay during cycling. Similarly, high-nickel cathodes at high voltages (greater than 4.3 V vsLi / Li)... + During cycling, lattice oxygen release, surface phase transition, and lattice strain occur, leading to instability at the positive electrode electrolyte interface, continuous increase in interface impedance, and degradation of battery performance.
[0004] Against this backdrop, electrode interface stabilization has become a key technological bottleneck for improving the performance of lithium-ion batteries. How to construct a dynamic interface layer that can adapt to changes in electrode volume while continuously providing effective protection is an important direction in current battery materials research. Although traditional interface optimization strategies have made some progress, they still have significant limitations when dealing with the complex operating conditions of high-strain electrodes, necessitating the development of novel interface regulation technologies with damage recognition and adaptive repair capabilities. Summary of the Invention
[0005] This application proposes a battery cell and its preparation method, battery device, energy storage device and electrical equipment, aiming to improve the repair accuracy of the electrode interface layer during battery cell cycling and achieve precise interface maintenance of "where there is damage, repair is prioritized".
[0006] In a first aspect, embodiments of this application provide a battery cell including a positive electrode, a negative electrode, and an electrolyte. The negative electrode includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material and piezoelectric particles coexisting in the form of a separated phase. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the negative electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a first film-forming agent, wherein the highest reduction potential of the organic solvent is [missing value]. The reduction potential of the first film-forming agent is , .
[0007] In some embodiments, the negative electrode active material is a silicon-based material, and the first film-forming agent includes at least one of difluoromalononitrile and fluorobutadiene.
[0008] In some embodiments, the piezoelectric particles in the negative electrode active layer account for 0.1 to 5.0 wt% of the total mass.
[0009] Secondly, embodiments of this application provide a battery cell including a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive electrode current collector coexisting in the form of a separated phase and a positive electrode active layer disposed on the surface of the positive electrode current collector. The positive electrode active layer includes a positive electrode active material and piezoelectric particles. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the positive electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a second film-forming agent, wherein the lowest oxidation potential of the organic solvent is... The oxidation potential of the second film-forming agent is , .
[0010] In some embodiments, the positive electrode active material is a high-nickel ternary material, and the second film-forming agent includes at least one of tris(trimethylsilyl)borate and lithium difluorooxalate borate.
[0011] In some embodiments, the piezoelectric particles in the positive electrode active layer account for 0.1 to 5.0 wt% of the total mass.
[0012] In some embodiments, the equivalent piezoelectric strain constant of the piezoelectric particles is 80~150 pC / N.
[0013] In some embodiments, the median particle size D50 of the piezoelectric particles is 50 nm to 300 nm.
[0014] In some embodiments, the piezoelectric material includes at least one of barium titanate and sodium bismuth titanate.
[0015] In some embodiments, the material of the ion-conducting layer includes at least one of lithium phosphate, lithium borate, lithium aluminate, or LISICON-type solid electrolytes.
[0016] In some embodiments, the ion-conducting layer includes an inner layer and an outer layer, the inner layer including lithium phosphate and the outer layer including lithium fluoride and lithium carbonate.
[0017] In some embodiments, the ionic conductivity of the ion-conducting layer is 10 at 25°C. -8 S / cm~10 -7 S / cm; In some embodiments, the thickness of the ion-conducting layer is 2 nm to 10 nm.
[0018] Thirdly, embodiments of this application propose a method for preparing a single battery cell, comprising the following steps: The positive electrode, negative electrode, separator, and casing are assembled into a battery cell; Electrolyte is injected into the battery cell to obtain a post-electrolyte-injected battery cell. The post-electrolyte-injected battery cell is then subjected to formation treatment to obtain a single battery cell. The negative electrode includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material and piezoelectric particles coexisting in the form of a separated phase. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the negative electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a first film-forming agent, wherein the highest reduction potential of the organic solvent is [missing value]. The reduction potential of the first film-forming agent is , .
[0019] In some embodiments, the content of the first film-forming agent in the electrolyte is 0.2 to 3 wt%.
[0020] In some embodiments, the piezoelectric particles in the negative electrode active layer account for 0.1 to 5.0 wt% of the total mass.
[0021] In some embodiments, the mass percentage of the first film-forming agent in the electrolyte is w1, and the mass percentage of the piezoelectric particles in the negative electrode active layer is M1, where w1:M1 = (0.3~5):1.
[0022] In some embodiments, the preparation step of the negative electrode includes: The lithium source and phosphorus source were mixed evenly at a molar ratio of Li:P = (2.7~3.3):1 to obtain the coating solution; The piezoelectric material is mixed with the coating liquid and stirred at 50-80°C for 2-6 hours to obtain a pre-coated product. The pre-coated product is heat-treated in an inert atmosphere at a temperature of 500-700°C to obtain the piezoelectric particles. A negative electrode current collector is provided, and a negative electrode active layer containing the piezoelectric particles and the negative electrode active material is disposed on the negative electrode current collector.
[0023] Fourthly, this application proposes a method for preparing a single battery cell, comprising the following steps: The positive electrode, negative electrode, separator, and casing are assembled into a battery cell; Electrolyte is injected into the battery cell to obtain a post-electrolyte-injected battery cell. The post-electrolyte-injected battery cell is then subjected to formation treatment to obtain a single battery cell. The positive electrode includes a positive current collector and a positive active layer disposed on the surface of the positive current collector. The positive active layer includes a positive active material and piezoelectric particles coexisting in the form of a separated phase. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the positive electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a second film-forming agent, wherein the lowest oxidation potential of the organic solvent is... The oxidation potential of the second film-forming agent is , .
[0024] In some embodiments, the content of the second film-forming agent in the electrolyte is w2, where w2 = 0.2~3 wt%.
[0025] In some embodiments, the piezoelectric particles in the positive electrode active layer account for 0.1 to 5.0 wt% of the total mass.
[0026] In some embodiments, the mass percentage of the second film-forming agent in the electrolyte is w2, and the mass percentage of the piezoelectric particles in the positive electrode active layer is M2, where w2:M2 = (0.3~5):1.
[0027] In some embodiments, the preparation steps of the positive electrode include: The lithium source and phosphorus source were mixed evenly at a molar ratio of Li:P = (2.7~3.3):1 to obtain the coating solution; The piezoelectric material is mixed with the coating liquid and stirred at 50-80°C for 2-6 hours to obtain a pre-coated product. The pre-coated product is heat-treated in an inert atmosphere at a temperature of 500-700°C to obtain the piezoelectric particles. A positive current collector is provided, and a positive active layer containing the piezoelectric particles and the positive active material is disposed on the positive current collector.
[0028] In some embodiments, the molar ratio of phosphorus in the phosphorus source to the piezoelectric material is (0.01~0.30):1.
[0029] In some embodiments, the phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, lithium dihydrogen phosphate, triethyl phosphate, trimethyl phosphate, and phosphorus pentoxide.
[0030] In some embodiments, the lithium source includes at least one of lithium acetate and lithium hydroxide.
[0031] Fifthly, embodiments of this application provide a battery device comprising a battery cell as described in the first and / or second aspects, or a battery cell manufactured by a preparation method as described in the third and / or fourth aspects.
[0032] Sixthly, embodiments of this application also propose an energy storage device, including the battery device as described in the fifth aspect.
[0033] In a seventh aspect, embodiments of this application also propose an electrical device, including a battery device as described in the fifth aspect, or including an energy storage device as described in the fifth aspect.
[0034] Compared with the prior art, this technical solution has at least the following technical advantages: In this application, by introducing piezoelectric materials into the electrodes (positive and negative electrodes), a ternary response mechanism of "stress-polarization-preferential film formation" is constructed by coupling the piezoelectric effect with the interfacial electrochemical reaction kinetics. This achieves precise interfacial maintenance by prioritizing repair where damage occurs, effectively improving the accuracy of electrode interfacial layer repair during battery cycling. Specifically, piezoelectric particles with an ion-conductive layer are introduced into the electrodes. When the electrode undergoes volume changes during charging and discharging, the piezoelectric particles in the stress concentration area are subjected to greater mechanical stress, generating stronger surface polarization charges according to the piezoelectric constitutive relationship. These bound charges form local potential disturbances at the nanoscale, which can modulate the local overpotential of the interfacial electrochemical reaction. By synergistically using film-forming agents (first and second film-forming agents), electrochemical reduction or oxidative decomposition preferentially occurs in the areas of enhanced piezoelectric polarization, generating a dense protective layer rich in inorganic components such as LiF and Li3N. This statistically achieves a precise interfacial maintenance effect of "where the stress is high, the polarization is strong, and film formation is preferential." Attached Figure Description
[0035] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0036] Figure 1 A schematic diagram of the structure of a battery cell and a schematic diagram of the core-shell structure of piezoelectric particles provided in an embodiment of this application; Figure 2 This is a schematic diagram of the stress-polarization-preferential film formation mechanism in the negative electrode provided in an embodiment of this application; Figure 3 The diagram illustrates three distribution patterns of piezoelectric particles in the negative electrode active layer provided in the embodiments of this application, wherein (a) is a uniform mixed distribution, (b) is a gradient distribution, and (c) is a surface piezoelectric layer. Figure 4 A schematic diagram illustrating a spatial selectivity verification method and a spatial selectivity index definition provided in an embodiment of this application; Figure 5 The following is a performance comparison chart between Example 1 and the comparative example of this application, where (a) is a two-factor comparison chart of capacity retention rate at 500 cycles, and (b) is a curve showing the change of capacity retention rate with the number of cycles.
[0037] Figure label: 100. Battery cell; 111. Negative electrode current collector; 112. Negative electrode active layer; 112a1. Negative electrode active material; 112a2. Piezoelectric particles; 112a 21 Piezoelectric materials; 112a 22112a3, Ion-conducting layer; 112b1, Conductive agent; 112b2, Piezoelectric layer; 112b2, Functional layer; 120, Separator; 131, Positive current collector; 132, Positive active layer; 140, Electrolyte; 141, First film-forming agent. Detailed Implementation
[0038] To better understand the technical solution of the present invention, the embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0039] It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0040] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a,” “the,” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.
[0041] It should be understood that the term "and / or" used in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this article generally indicates that the preceding and following related objects have an "or" relationship.
[0042] To address the interfacial stability problem of high-strain electrodes in the battery field, existing technologies mainly focus on electrolyte additive optimization, artificial interfacial film preconstruction, binder modification, and electrode structure design.
[0043] Regarding electrolyte additive optimization: Film-forming additives are added to the electrolyte. During the first charge of the battery, these additives decompose on the electrode surface to form an initial interfacial film. Widely used film-forming additives include fluoroethylene carbonate (FEC) and vinylene carbonate (VC). Among them, FEC can be preferentially reduced on the negative electrode surface to form a dense SEI film rich in LiF. Its working principle is to utilize the polarity of the FC bond and its low reduction potential, so that the decomposition potential of FEC on the negative electrode surface is lower than that of the main solvent (such as ethylene carbonate EC), thus preferentially undergoing electrochemical reduction. VC forms a flexible polymer layer on the negative electrode surface through polymerization, improving the mechanical strength and flexibility of the SEI film (solid electrolyte interfacial film).
[0044] Artificial interface film pre-construction technology improves interfacial stability by pre-depositing a protective layer on the surface of electrode materials. Typical methods include atomic layer deposition (ALD) of alumina (Al₂O₃) or zirconium oxide thin films, chemical vapor deposition (CVD) of carbon coatings, or solution deposition of polymer protective layers. These artificial interface films are typically a few nanometers to tens of nanometers thick and are designed to isolate the electrode material from direct contact with the electrolyte and suppress side reactions. For example, ALD alumina coatings reduce electrolyte decomposition on the electrode surface through their density and chemical inertness; carbon coatings improve electron conduction and stress dispersion of the electrode by providing a conductive network and buffer space.
[0045] In terms of binder modification, researchers have developed a variety of functionalized binders to enhance the mechanical stability and interfacial properties of electrodes. For example, polyacrylic acid (PAA) is widely used because its carboxyl groups can form strong hydrogen bonds with the hydroxyl groups on the silicon surface; carboxymethyl cellulose / styrene-butadiene rubber (CMC / SBR) composite binders combine the strong adhesion of CMC with the elasticity of SBR, providing mechanical strength while maintaining a certain degree of flexibility. In recent years, binders with self-healing functions have also been developed, such as polymers containing dynamic covalent bonds or supramolecular interactions, with the expectation of spontaneous repair when electrode interface damage occurs.
[0046] Although existing technologies have made some progress in improving the stability of high-strain electrode interfaces, they still have inherent limitations in dealing with complex volume changes and stress concentration problems, for example: Traditional electrolyte additives lack spatial selectivity in their film-forming processes. The decomposition of film-forming additives such as FEC and VC on the electrode surface is based on a uniform reaction driven by the overall potential, failing to identify and respond to localized stress concentrations or interfacial damage areas. Volume changes at the negative electrode often create stress concentrations at specific locations, causing preferential rupture of the SEI film in these areas. However, the decomposition and repair of traditional additives occur uniformly across the entire electrode surface. This spatial mismatch leads to an inefficient allocation of repair resources: severely damaged areas are not prioritized for protection, while intact areas consume valuable additives. This inefficient repair mechanism necessitates higher additive concentrations to maintain interfacial stability, increasing electrolyte costs and potentially causing other side effects.
[0047] Traditional electrolyte additive-based interface maintenance strategies suffer from durability issues due to their continuous decomposition. Relying on the continuous decomposition of electrolyte additives to repair the interface film (SEI or CEI film) is essentially a consumable process. As the number of cycles increases, the additives in the electrolyte are gradually depleted, reducing the interface repair capacity and accelerating capacity decay. This is especially true under harsh conditions such as high temperature or high rate, where the additive consumption rate is even faster. Moreover, the continuous decomposition of excessive additives leads to a continuous thickening of the interface film, resulting in a sustained increase in interfacial impedance and ultimately affecting the battery's rate performance and energy efficiency. This "the more it's repaired, the thicker it gets" dilemma is a bottleneck that traditional additive strategies struggle to overcome.
[0048] The static nature of pre-fabricated artificial interface films limits their adaptability to dynamic damage. While protective layers prefabricated using methods such as ALD and CVD exhibit excellent initial performance, these static coatings are prone to cracking or peeling at stress concentration points when faced with volume changes such as 300-400% in the negative electrode. Once the protective layer is damaged, the exposed fresh surface rapidly reacts with the electrolyte, forming an uneven interface film. Because artificial interface films are prepared before battery assembly, they cannot dynamically respond to newly generated damage sites during cycling, thus offering limited improvement to long-term cycle stability. Furthermore, the preparation of artificial interface films typically requires expensive vacuum equipment and complex processes, increasing production costs and process complexity, which is detrimental to large-scale industrial applications.
[0049] As can be seen from the above, existing technologies lack a closed-loop mechanism for damage identification and proactive response. Both additive optimization and surface coating are based on a passive strategy of "preset protection," meaning that the interface protection scheme is determined during the battery manufacturing stage and cannot be adaptively adjusted according to the actual damage situation during operation.
[0050] Therefore, how to provide a highly accurate electrode interface maintenance solution that prioritizes repair where damage occurs, and how to solve problems such as spatial mismatch, continuous consumption, static protection, and lack of response mechanism in existing technologies, are urgent technical issues that need to be addressed.
[0051] Based on this, this application proposes a battery cell 100.
[0052] Please see Figure 1 In this embodiment of the application, the battery cell 100 includes a positive electrode, a negative electrode, and an electrolyte 140; wherein, The negative electrode includes a negative electrode current collector 111 and a negative electrode active layer 112 disposed on the surface of the negative electrode current collector 111. The negative electrode active layer 112 includes a negative electrode active material 112a1 and piezoelectric particles 112a2 coexisting in the form of a separated phase. The piezoelectric particles 112a2 include piezoelectric material 112a 21 and coated with piezoelectric material 112a 21Surface ion-conducting layer 112a 22 In the negative electrode, the local potential disturbance generated by the piezoelectric particle 112a2 under a stress of 100 MPa is on the order of magnitude. , =10~50mV; Electrolyte 140 includes an organic solvent and a first film-forming agent 141, the highest reduction potential of the organic solvent is... The reduction potential of the first film-forming agent 141 is , ; and / or, The positive electrode includes a positive current collector 131 and a positive active layer 132 disposed on the surface of the positive current collector 131. The positive active layer 132 includes a positive active material and piezoelectric particles 112a2 (not shown) coexisting in a separated phase. The piezoelectric particles 112a2 include piezoelectric material 112a. 21 and coated with piezoelectric material 112a 21 Surface ion-conducting layer 112a 22 In the positive electrode, the local potential disturbance generated by the piezoelectric particle 112a2 under a stress of 100 MPa is on the order of magnitude. , =10~50 mV; Electrolyte 140 includes an organic solvent and a second film-forming agent, the lowest oxidation potential of the organic solvent is The oxidation potential of the second film-forming agent is , .
[0053] In the technical solution of this application, piezoelectric material 112a is introduced into the electrodes (positive electrode and negative electrode). 21 By coupling the piezoelectric effect with interfacial electrochemical reaction kinetics, a ternary response mechanism of "stress-polarization-preferred film formation" was constructed, achieving precise interface maintenance of "where there is damage, there is preferential repair," effectively improving the repair accuracy of the electrode interface layer during battery cycling. Please refer to [link / reference]. Figure 2 Specifically, an ion-conducting layer 112a is introduced into the electrode. 22When the piezoelectric particles 112a2 undergo volume change / volume expansion during the charging and discharging process of the electrode, the piezoelectric particles 112a2 in the stress concentration region are subjected to greater mechanical stress, thereby generating stronger surface polarization charges according to the piezoelectric constitutive relationship. These bound charges form local potential disturbances in the nanoscale range, which can modulate the local overpotential of the interfacial electrochemical reaction. By synergistically using film-forming agents (first film-forming agent 141 and second film-forming agent), electrochemical reduction or oxidative decomposition is preferentially carried out in the region of enhanced piezoelectric polarization, generating a dense interfacial film rich in inorganic components such as LiF and Li3N, repairing the damaged area (i.e. stress concentration area) of the electrode interfacial film, thereby achieving a precise interfacial maintenance effect of "where the stress is high - where the polarization is strong - where the film is preferentially formed" in a statistical sense.
[0054] This application utilizes piezoelectric material 112a. 21 The introduction of this technology establishes a complete closed loop of damage sensing mechanism (damage generates stress), signal conversion mechanism (piezoelectric polarization), and response execution mechanism (the first film-forming agent preferentially forms a film in the damaged area under the action of local potential disturbance), transforming passive uniform protection into active adaptive repair, which significantly improves the interface stability, cycle life, and coulombic efficiency of high strain electrodes.
[0055] In this embodiment of the application, piezoelectric material 112a can be introduced into both the positive and negative electrodes simultaneously. 21 This allows for precise interface maintenance of both the positive and negative electrodes, prioritizing repair where damage occurs; alternatively, piezoelectric material 112a can be introduced into only one of the positive or negative electrodes. 21 This allows for precise interface maintenance of the corresponding electrodes, prioritizing repair where damage occurs. Those skilled in the art can select the appropriate method based on their specific application needs.
[0056] It should be noted that, with piezoelectric material 112a 21 Unlike other methods that use piezoelectric particles as the coating layer for electrode active materials, in this application, the piezoelectric particles 112a2 exist as an independently dispersed phase within the active layer (negative electrode active layer 112 or positive electrode active layer 132), and do not constitute a core-shell coating of the active material (negative electrode active material 112a1 or positive electrode active material); their main function is not to regulate the overall electrode through a continuously built-in electric field. The key lies not in migration flux, but in stress sensing and modulation of local interface reaction dynamics.
[0057] In this embodiment, the battery cell 100 is preferably a lithium secondary battery, including lithium-ion batteries and lithium metal secondary batteries; and a corresponding alkali metal ion conductive layer 112a is used. 22 When compared with a reference potential system, the stress-response preferential film formation mechanism of this application is also applicable to other alkali metal ion secondary batteries.
[0058] The piezoelectric particle 112a2 of this application embodiment is described below using the negative electrode as an example: In this embodiment of the application, the equivalent local potential disturbance characterization value of the piezoelectric particle 112a2 in the negative electrode is... Specifically, the voltage can be 10 mV, 20 mV, 30 mV, 40 mV, 50 mV, or any value in between; the typical operating stress range of the electrode is 10~200 MPa. The determination is uniformly based on the 100 MPa benchmark compressive stress.
[0059] In this embodiment of the application, the magnitude of the local potential disturbance of the piezoelectric particle 112a2 in the negative electrode is... The equivalent local potential disturbance characterization value refers to the equivalent local interface potential change amplitude calculated by the following formula, using the finally obtained piezoelectric particle 112a2 powder as the test object, under the reference compressive stress conditions of 25 ℃ and 100 MPa: In the formula, To determine the equivalent piezoelectric strain constant of piezoelectric particles 112a2, the above-mentioned piezoelectric particle 112a2 powder was isostatically pressed into a dense preform (Φ10 mm×1 mm), polarized at 120 ℃ and 3 kV / mm for 30 minutes, and then subjected to quasi-static... The measuring instrument was used to measure at 25 ℃; The equivalent relative permittivity of piezoelectric particles 112a2 was determined by dielectric impedance spectroscopy at 1 kHz, 25 ℃, and 1 V amplitude using the same raw blank. The median particle size of the piezoelectric particle 112a2 powder is determined by a laser particle size analyzer and statistically verified by transmission electron microscopy; σ is the reference compressive stress, taken as 100 MPa. Let be the vacuum permittivity, taken as 8.854 × F / m. All three input parameters are based on the same batch of final piezoelectric particles 112a2 (i.e., containing the ion-conducting layer 112a). 22 The core-shell particles are the test objects, and the sample preparation and polarization conditions of each sample should be consistent.
[0060] It should be noted that, The equivalent characterization value, measured and calculated under the aforementioned unified conditions, is used to provide a comparable and reproducible definition of the stress response capabilities of different piezoelectric particles 112a2. This value is not equivalent to the actual local interfacial potential generated in situ by the piezoelectric particles 112a2 in the electrolyte 140—the latter is also affected by the ion-conducting layer 112a. 22 The effects of electrolyte 140 double-layer shielding and particle orientation. The typical operating stress range of the electrode is 10~200 MPa; this range is for background description and not intended as a definitive conclusion. The criteria for determination; The determination shall be based on the 100 MPa reference compressive stress.
[0061] Although the local potential perturbation of piezoelectric particles 112a2 exhibits a positive and negative distribution when randomly oriented, this application relies on the spatial difference between the perturbation amplitude and the interfacial reaction rate within the electrode stress region. Since the reaction rate is exponentially related to the overpotential, the positive and negative symmetrical perturbations, after exponential averaging, still result in a net rate increase, eliminating the need for piezoelectric material 112a2. 21 Co-polarization forms a macroscopic directional electric field.
[0062] In this embodiment of the application, the equivalent local potential disturbance characterization value of the piezoelectric particle 112a2 in the negative electrode is... (The value, i.e., the value under a reference compressive stress of 100 MPa,) is set in the range of 10~50 mV, determined based on the energy scale matching principle of electrochemical interface reactions. The room temperature thermal voltage RT / F≈25.7 mV represents the intrinsic energy barrier of ion thermal motion, where the magnitude of the local potential perturbation is... When these properties are comparable to or even surpassed, the piezoelectric effect possesses the ability to resist random thermal dispersion and exert a directional driving force with controllable intensity on interfacial charge transfer. This can be rigorously demonstrated through the following electrochemical kinetic theory: According to the Butler–Volmer equation, the net electrode reaction current *i* is exponentially related to the overpotential *η*; in the transfer coefficient... α Under the condition that ≈0.5 and single-electron transfer n=1, if the piezoelectric potential disturbance is regarded as an equivalent overpotential (η= Then, the ratio of the reaction rate (current density) in the stress zone to that in the non-stress zone follows a Tafel-type relationship: ; Substituting the quantitative values into the above formula: when When the voltage is 10mV, the rate ratio is approximately exp(0.5×10 / 25.7)≈1.2 times; when At a voltage of 50 mV, the rate ratio is approximately exp(0.5 × 50 / 25.7) ≈ 2.7 times. This calculation shows that if the disturbance is much smaller than 10 mV, the exponential term can be linearly approximated as 1 + The rate change is only a weak linear increment, making it difficult to produce a distinguishable control effect; however, the 10~50 mV range is exactly in the rising segment of the exponential response, which makes the perturbation effect jump from a linear micro-perturbation to a significantly enhanced nonlinear effect, which not only ensures the effectiveness of the control, but also avoids the side reactions or material breakdown risks that may be caused by excessively high voltage.
[0063] Therefore, by controlling the equivalent local potential perturbation characterization value of the piezoelectric particles 112a2 in the negative electrode within the range of 10~50 mV, it is ensured that the nonlinear electrochemical reaction acceleration effect is sufficiently excited, thereby increasing the local decomposition rate of the stress region relative to the non-stress region by about 1.2~2.7 times. This achieves preferential film formation in the stress concentration region (near the crack of the SEI film) while keeping the piezoelectric particles 112a2 within the stable operating window.
[0064] In the embodiments of this application, the highest reduction potential of the organic solvent is: The reduction potential of the first film-forming agent 141 is , When an organic solvent consists of multiple components, This refers to the reduction potential of the component with the highest reduction potential in an organic solvent system. By making... It can limit the negative electrode piezoelectric material 112a 21 The generated local overpotential disturbance will not cross the film-forming window of the first film-forming agent 141 and induce synchronous decomposition of the organic solvent, thereby ensuring steric selectivity and film-forming product quality.
[0065] In this embodiment of the application, the main operating potential of the negative electrode is Specifically, it refers to the main potential plateau range during the discharge process of a single battery cell, where lithium-ion extraction (or insertion) occurs at the negative electrode. This plateau is typically represented by its median or lowest potential, and is relative to metallic lithium (lithium). The potential value of the reference electrode. Understandably, < <
[0066] In this embodiment of the application, the magnitude of the local potential disturbance of the piezoelectric particle 112a2 in the positive electrode is... For the meaning, test method, and value range, please refer to the above. The relevant descriptions will not be repeated here.
[0067] In this embodiment, the lowest oxidation potential of the organic solvent is The oxidation potential of the second film-forming agent is , When an organic solvent consists of multiple components, This refers to the oxidation potential of the component with the lowest oxidation potential in an organic solvent system. Similarly, by making... It can limit the positive electrode piezoelectric material 112a 21 The generated local overpotential disturbance will not cross the film-forming window of the second film-forming agent and induce synchronous decomposition of the organic solvent, thereby ensuring steric selectivity and film-forming product quality.
[0068] In the embodiments of this application, The main operating potential of the electrode Specifically, it refers to the main potential plateau range during the lithium-ion extraction (or insertion) reaction at the positive electrode in the charging process of a single battery cell (100%). This is usually represented by its median potential or highest potential, and is relative to metallic lithium (…). The potential value of the reference electrode. The charging cutoff voltage of the positive electrode is... Specifically, this refers to the maximum voltage allowed to be reached during the charging process of a single battery cell at 100%. Understandably, ≤ ,and .
[0069] In the embodiments of this application, , , , All measurements were performed as follows: a three-electrode linear scan voltammetry method was used, with lithium metal as the reference and counter electrode; glassy carbon or copper foil was used as the working electrode for measuring the reduction potential, and platinum or aluminum foil was used as the working electrode for measuring the oxidation potential; the scan rate was 0.5 mV / s, and the temperature was 25 ℃; the current density reached The potential corresponding to the initial reduction potential or initial oxidation potential of that component is recorded. All components in the same comparison group should be measured under the same electrolyte 140 system and the same determination threshold.
[0070] In this embodiment, an appropriate first film-forming agent 141 can be selected according to the type of negative electrode, such that the reduction potential of the first film-forming agent 141 is located near the film-forming window of the negative electrode, and the decomposition reaction kinetics of the first film-forming agent 141 are sensitive to local overpotential disturbances of 10-50 mV generated by the piezoelectric particles 112a2 of the negative electrode. Similarly, an appropriate second film-forming agent can be selected according to the type of positive electrode, such that the oxidation potential of the second film-forming agent is located near the film-forming window of the positive electrode, and the decomposition reaction kinetics of the second film-forming agent are sensitive to local overpotential disturbances of 10-50 mV generated by the piezoelectric particles 112a2 of the positive electrode.
[0071] In this embodiment of the application, when piezoelectric particles 112a2 are introduced into both the positive and negative electrodes, the piezoelectric particles 112a2 in the positive and negative electrodes can be the same or different.
[0072] In some embodiments, the equivalent piezoelectric strain constant of the piezoelectric particle 112a2 30 pC / N, or 50 pC / N. The determination of whether the range independently constitutes a local potential disturbance should be based on the piezoelectric particle 112a2. and Collaborative selection, so that the result calculated according to the method specified in this application or It meets the requirement of 10~50 mV.
[0073] In one specific embodiment, the equivalent piezoelectric strain constant of the piezoelectric particle 112a2 The piezoelectric coefficient ranges from 80 to 150 pC / N, specifically 80 pC / N, 100 pC / N, 120 pC / N, 140 pC / N, 150 pC / N, or any value between them. Within this piezoelectric coefficient range, piezoelectric material 112a... 21 Under typical electrode stress conditions (10~200 MPa, this is for background information only and not intended as a basis for further discussion), or Under the given conditions, it can produce approximately 0.1~3 μC / cm. 2 The surface polarization charge is on the order of magnitude; approximately 1 μC / cm under a reference compressive stress of 100 MPa. 2 Its equivalent local potential perturbation characterization value is about 10~50 mV. This perturbation amplitude is sufficient to significantly modulate the interfacial electrochemical reaction rate (about 1.2~2.7 times rate increase) through the Butler-Volmer equation, thereby achieving preferential film formation in stress concentration areas.
[0074] In the above embodiments, the piezoelectric particles 112a2 (containing an ion-conducting layer 112a) 22 ) and piezoelectric material 112a 21 (excluding ion-conducting layer 112a) 22 The equivalent piezoelectric strain constants of the materials are similar. Therefore, when selecting materials, piezoelectric materials 112a with an equivalent piezoelectric strain constant of 80~150 pC / N can be selected. 21 .
[0075] In some embodiments, piezoelectric material 112a 21 Including at least one of barium titanate, sodium bismuth titanate, etc.
[0076] In one specific embodiment, the piezoelectric material 112a in the negative electrode and the positive electrode 21 All are barium titanate, which has a tetragonal perovskite structure and exhibits a significant piezoelectric effect at room temperature.
[0077] In some embodiments, the median particle size of the piezoelectric particles 112a2 The particle size ranges from 50 nm to 300 nm, specifically 50 nm, 80 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, or any value between them. This particle size range ensures both sufficient piezoelectric response and good dispersion in the electrode.
[0078] In one specific embodiment, the median particle size of the piezoelectric particles 112a2 The wavelength is 80~150 nm.
[0079] In some embodiments, the mass percentage of piezoelectric particles 112a2 in the negative electrode active layer 112 or the positive electrode active layer 132 is 0.1~5.0 wt%, 0.5~2.0 wt%, or 0.8~1.5 wt%, specifically 0.1 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.5 wt%, 2 wt%, 3 wt%, 4 wt%, 5.0 wt%, or any value between them. Within this mass percentage range, the effects of piezoelectric response, electrode energy density, and processing performance are taken into account.
[0080] In this embodiment of the application, the piezoelectric particle 112a2 includes piezoelectric material 112a. 21 and coated with piezoelectric material 112a 21 Surface ion-conducting layer 112a 22 This forms a core-shell structure of "piezoelectric core-ion-conducting shell". Ion-conducting layer 112a 22 It can provide a continuous lithium-ion conduction channel, ensuring the piezoelectric material 112a 21 The introduction of this will not lead to a significant increase in electrode interface impedance, thus maintaining the rate performance of the electrode; ion-conducting layer 112a 22 It can also improve piezoelectric material 112a 21 Interfacial compatibility with other components in the electrode (active material, conductive agent 112a3, binder, etc.), ion-conducting layer 112a 22 Some functional groups on the surface can even form hydrogen bonds with other components in the electrode (such as PAA (polyacrylic acid), CMC (sodium carboxymethyl cellulose) and other binders), enhancing mechanical bonding; in addition, the ion-conducting layer 112a 22 It can also block piezoelectric material 112a 21 Direct contact with electrolyte 140 inhibits ion dissolution and other side reactions, ensuring long-term cycling stability.
[0081] In some embodiments, the ion-conducting layer 112a 22 The materials include at least one lithium-ion conductive phase selected from lithium phosphate, lithium borate, lithium aluminate, or LISICON (Lithium Super Ionic Conductor) solid electrolytes.
[0082] In some embodiments, the ion-conducting layer 112a 22 It includes an inner layer and an outer layer. The inner layer includes lithium phosphate, and the outer layer includes lithium fluoride (LiF) and lithium carbonate (LiF). This bilayer structure ensures both lithium-ion conductivity and allows for the transfer of lithium ions through LiF and... Improving interfacial chemical stability reduces electrolyte 140 decomposition and further enhances the long-term cycle performance of battery cell 100.
[0083] In some embodiments, the ion-conducting layer 112a 22 The ionic conductivity at 25℃ is ~ S / cm, specifically 1 S / cm, 5 S / cm, 1 S / cm or any value between them. Within this range of ionic conductivity, the ion-conducting layer 112a 22 It can provide lithium-ion conduction channels, avoiding the piezoelectric material 112a 21 The introduction of [a certain substance] significantly improves the electrode interface impedance.
[0084] In some embodiments, the ion-conducting layer 112a 22 The thickness is 2~10 nm, specifically 2 nm, 3 nm, 4 nm, 6 nm, 8 nm, 10 nm or any value between them. This is achieved by using the ion-conducting layer 112a... 22 The thickness is controlled within the above range to ensure that the ion-conducting layer 112a 22 It can effectively block piezoelectric materials 112a 21 Direct contact with the electrolyte 140 does not significantly increase interfacial impedance, thus providing sufficient chemical protection while maintaining good ionic conductivity. In one specific embodiment, the ion-conducting layer 112a 22 The thickness is 3 ~ 8 nm.
[0085] In this embodiment, the piezoelectric particles 112a2 are distributed in various ways in the negative electrode active layer 112 or the positive electrode active layer 132. The following description uses the negative electrode as an example: Please see Figure 3 In (a) of the embodiments, in the negative electrode active layer 112, piezoelectric particles 112a2 and negative electrode active material 112a1 are uniformly mixed and distributed.
[0086] Please see Figure 3 In (b) of the embodiments, the distribution concentration of piezoelectric particles 112a2 in the negative electrode active layer 112 gradually increases or decreases from the side closer to the negative electrode current collector 111 to the side farther away from the current collector.
[0087] Please see Figure 3In some embodiments, (c) of the negative electrode active layer 112 includes a functional layer 112b2 and a piezoelectric layer 112b1. The piezoelectric layer 112b1 is disposed on the side of the functional layer 112b2 facing away from the negative electrode current collector 111. The negative electrode active material 112a1 is distributed in the functional layer 112b2, and the piezoelectric particles 112a2 are distributed in the piezoelectric layer 112b1.
[0088] In this embodiment of the application, the positive electrode can be set up in the same way as the negative electrode, and will not be described again.
[0089] In some embodiments, the organic solvent includes one or more combinations of carbonate solvents such as ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC), for example, a volume ratio of EC:EMC:DEC = 1:1:1 or EC:EMC = 3:7. The organic solvent system should take into account high and low temperature performance, conductivity, and wettability to the electrode. When the negative electrode is a lithium metal negative electrode and the electrolyte 140 does not contain a second film-forming agent, the organic solvent may also be selected from a mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME); since the oxidation potential of ether solvents is lower than that of carbonate solvents, ether solvents are not selected as organic solvents in embodiments containing a second film-forming agent.
[0090] In this embodiment, the negative current collector 111 can be selected from any one of copper foil, stainless steel mesh, nickel-plated steel strip, or other common negative current collectors 111 in the art.
[0091] In this embodiment of the application, optionally, the thickness of the negative electrode current collector 111 is 8~15 μm, specifically 8μm, 10μm, 13μm, 15 μm or any value between them.
[0092] In this embodiment, the negative electrode can be any one of various negative electrodes, such as a silicon-based negative electrode, a lithium metal negative electrode, or a graphite negative electrode. The negative electrode active material 112a1 can be selected from one or more of silicon-based materials, graphite materials, metallic lithium, lithium alloys, lithium titanate, or other negative electrode active materials 112a1 in the art. Silicon-based materials refer to a class of materials with silicon (Si) as the core active material, and can be selected from elemental silicon, silicon suboxide (SiO2), etc. x ) or their respective composites with carbon (graphite); SiO x In this context, 0 < x < 2, and optionally, 0.5 ≤ x < 1.6 (typical range for commercial silicon suboxide, with x ≈ 1 predominantly); elemental silicon and SiO x It can be designed as a nanoscale or porous structure as needed.
[0093] In some embodiments, the negative electrode is a silicon-based negative electrode, meaning the negative electrode active material 112a1 is a silicon-based material. The core problem with silicon-based negative electrodes lies in their significant volume changes during charge and discharge; silicon expands by 300-400% during lithiation, and this repeated volume change causes repeated rupture and regeneration of the solid electrolyte interphase (SEI) film on the electrode surface. The continuous rupture of the SEI film exposes fresh silicon surfaces, continuously consuming the electrolyte 140 and active lithium, resulting in low initial coulombic efficiency and rapid capacity decay during cycling. By introducing the piezoelectric material 112a1 into the silicon-based negative electrode… 21 It can achieve adaptive interface repair of damaged areas of silicon-based anodes, and can solve the problems of repeated rupture and regeneration of SEI film and continuous consumption of active lithium and electrolyte 140 caused by volume changes in silicon-based anodes, significantly improving cycle stability and first coulombic efficiency.
[0094] In the above embodiments, the main operating potential of the silicon-based anode is approximately 0.2~0.5 V, and the main SEI film formation potential is approximately 0.8~1.0 V vs. .
[0095] In the above embodiments, optionally, the reduction potential of the first film-forming agent 141 is in the range of 1.0~2.0 V, specifically 1.0 V, 1.2 V, 1.5 V, 2.0 V or any value between them.
[0096] In the above embodiments, optionally, the reduction potential of the first film-forming agent 141 is about 1.0~1.3 V, and the first film-forming agent 141 can be selected from at least one of difluoromalononitrile and fluorobutadieneonitrile. The decomposition products of such fluorinated dionitrile compounds are rich in LiF and C≡N derivatives, which helps to form a dense inorganic SEI layer and improve the interfacial mechanical strength and stability.
[0097] In the above embodiments, optionally, the organic solvent in the electrolyte 140 is selected from at least one of ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC).
[0098] In some embodiments, the negative electrode is a lithium metal negative electrode, and the first film-forming agent 141 comprises lithium nitrate and fluorosulfonyl lactone (such as methyl fluorosulfonyl lactone (MFSL)). Lithium nitrate is used in piezoelectric material 112a. 21 Driven by priority restoration, it provides / An inorganic framework, with the co-decomposition of fluorosulfonyl lactones providing LiF and sulfur-containing organic-inorganic composite components, co-deposits these components in the piezoelectric enhancement region to form a two-component dense SEI film. This not only enables selective repair of the SEI film but also preferentially decomposes in dendrite-growth-prone regions to form a dense SEI film. / Protective layer.
[0099] In the above embodiments, optionally, the organic solvent in the electrolyte 140 is a mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME).
[0100] In this embodiment, the positive current collector 131 can be selected from any one of aluminum foil, stainless steel mesh, nickel-plated steel strip or other positive current collectors 131 in the art.
[0101] In this embodiment of the application, optionally, the thickness of the positive current collector 131 is 8~15 μm, specifically 8μm, 10μm, 13μm, 15 μm or any value between them.
[0102] In this embodiment, the positive electrode active material can be selected from one or more of ternary materials, quaternary materials, lithium iron phosphate, high-voltage spinel materials, or other positive electrode active materials in the art. Ternary materials include high-nickel layered oxides such as NCM811, NCM90 series, and NCA.
[0103] In some embodiments, the positive electrode is a high-nickel positive electrode, meaning the active material in the positive electrode is a high-nickel ternary material. The charge / discharge range of the high-nickel positive electrode is approximately 2.8–4.35 V, the charging cut-off voltage is approximately 4.25–4.4 V, and the CEI film formation window of the high-nickel positive electrode is approximately 3.9 V to the charging cut-off voltage range (below the oxidation potential of the organic solvent). The high-nickel positive electrode operates at high voltages (greater than 4.3 V vs Li / Li). + During cycling, lattice oxygen release, surface phase transition, and lattice strain occur, leading to instability at the cathode solid-electrolyte interface, continuous increase in interfacial impedance, and degradation of battery performance. Introducing piezoelectric material 112a into the high-nickel cathode... 21 It can achieve adaptive interface repair of high-nickel cathode damaged areas, reduce interface impedance and slow down battery performance degradation.
[0104] In the above embodiments, optionally, the second film-forming agent includes tris(trimethylsilyl)borate (TMSB) and lithium difluorooxalate borate (LiDFOB); wherein the oxidation potential of TMSB is approximately 3.9~4.1 V, and the oxidation potential of LiDFOB is approximately 4.3~4.5 V, both falling within the CEI film formation window of the piezoelectrically tunable high-nickel cathode. Under piezoelectric assistance, TMSB and LiDFOB preferentially oxidize and decompose in the lattice strain concentration region. TMSB provides a silicon-boron-containing inorganic protective component, and LiDFOB provides LiF and a boron-containing organic-inorganic composite component. The two work synergistically to form a dense CEI film with a chemical composition gradient, suppressing the dissolution of transition metals and the release of lattice oxygen under high voltage.
[0105] In the embodiments of this application, it can be understood that the negative electrode active layer 112 and the positive electrode active layer 132 also contain a binder and a conductive agent 112a3.
[0106] In some embodiments, based on a total dry weight of 100 wt% of the negative electrode active layer 112, the negative electrode active layer 112 comprises the following components in the following proportions: negative electrode active material 112a1 60~95 wt%, piezoelectric particles 112a2 0.1~5.0 wt%, conductive agent 112a3 1~20 wt%, and binder 2~15 wt%. In some specific embodiments, the proportions of each component in the negative electrode active layer 112 are: negative electrode active material 112a1 185~95 wt%, piezoelectric particles 112a2 0.5~2.0 wt%, conductive agent 112a3 1.5~5 wt%, and binder 3~8 wt%.
[0107] In some embodiments, based on a total dry weight of 100 wt% of the positive electrode active layer 132, the positive electrode active layer 132 comprises the following components in the following proportions: 90-98 wt% positive electrode active material, 0.1-5.0 wt% piezoelectric particles 112a2, 0.5-5 wt% conductive agent 112a3, and 0.5-5 wt% binder. In some specific embodiments, the proportions of each component in the positive electrode active layer 132 are: 94-97 wt% positive electrode active material, 0.5-2.0 wt% piezoelectric particles 112a2, 1-3 wt% conductive agent 112a3, and 1-2 wt% binder.
[0108] In some embodiments, the binder in the positive electrode active layer 132 is selected from one or more combinations of PVDF or other commonly used positive electrode binders in the art, and those skilled in the art can make flexible selections according to actual conditions.
[0109] In some embodiments, the binder in the negative electrode active layer 112 is independently selected from one or more combinations of polyacrylic acid (PAA), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyvinyl alcohol (PVA), sodium alginate, or other commonly used negative electrode binders in the art. Those skilled in the art can make flexible selections according to actual conditions.
[0110] In some embodiments, the conductive agent 112a3 in the positive electrode active layer 132 and the negative electrode active layer 112 may be independently selected from one or more combinations of Super P, carbon nanotubes (CNT), acetylene black, Ketjen black, graphene, carbon black, etc.
[0111] In this embodiment of the application, the battery cell 100 further includes a separator 120, which is disposed between the positive electrode and the negative electrode.
[0112] In this embodiment, the diaphragm 120 can be a single membrane layer structure or a composite membrane layer structure.
[0113] In some embodiments, the diaphragm 120 is made of one or more of the following materials: polyethylene (PE), polypropylene (PP), polyethylene terephthalate (PET), polyimide (PI), polyvinylidene fluoride (PVDF), aramid (poly(p-phenylene terephthalamide, PMIA), alumina, silica, magnesium oxide, boehmite, etc.
[0114] In this embodiment, the battery cell 100 can be a lithium-ion battery or other common rechargeable batteries.
[0115] In some embodiments, the normal operating temperature range of the battery cell 100 is -10 to 60 ℃ or 0 to 45 ℃; the charge / discharge rate range supported by the battery cell 100 is 0.2 to 5 C, with the most significant effect at the commonly used rate of 0.5 to 2 C.
[0116] In the above embodiments, the normal operating temperature range of the battery cell 100 refers to the allowable temperature range within which the battery cell 100 can safely and stably output its nominal performance. Within this range, the various performance indicators of the battery cell 100 (such as capacity, internal resistance, and cycle life) are guaranteed, and no safety issues such as thermal runaway will occur.
[0117] In the above embodiments, the range of charge / discharge rates supported by the battery cell 100 refers to the selectable range of the ratio of the charge / discharge current that the battery cell 100 can safely withstand to its rated capacity.
[0118] In some embodiments, the electrolyte 140 contains a lithium salt, the lithium salt including... LiFSI (lithium difluorosulfonylimide) LiBOB (lithium bis(oxalato)borate) LiDFOB (lithium difluorooxalate borate) or one or more other lithium salts in the art.
[0119] In the above embodiments, optionally, the lithium salt is selected from... Combined with LiFSI, composite lithium salts can comprehensively The cost advantage and the high conductivity and film-forming performance of LiFSI.
[0120] In this embodiment of the application, the method for preparing the battery cell 100 includes the following steps: S10. Assemble the positive electrode, negative electrode, separator 120 and casing into a battery cell; S20. Inject electrolyte 140 into the cell to obtain the electrolyte-injected cell. Perform formation treatment on the electrolyte-injected cell to obtain a battery cell 100.
[0121] In this embodiment, piezoelectric particles 112a2 can be introduced into only one of the positive and negative electrodes, or into both. The following description further illustrates the preparation method of the battery cell 100 using the example of introducing piezoelectric particles 112a2 into both the positive and negative electrodes: In some embodiments, the method for preparing the negative electrode includes the following steps: Provide piezoelectric material 112a 21 In piezoelectric material 112a 21 Surface coated with ion-conductive layer 112a 22 piezoelectric particles 112a2 were obtained. A negative electrode current collector 111 is provided, and a negative electrode active layer 112 containing piezoelectric particles 112a2 and negative electrode active material 112a1 is formed on the surface of the negative electrode current collector 111 to obtain a negative electrode.
[0122] In the above embodiments, piezoelectric material 112a 21 median particle size The wavelength is 80~150 nm.
[0123] In the above embodiments, in the piezoelectric material 112a 21 Surface coated with ion-conductive layer 112a 22 Previously, the process also included the step of: processing piezoelectric material 112a 21 Pretreatment is performed. That is, the commercially available or self-made piezoelectric material 112a is pretreated. 21 Perform surface cleaning to remove organic matter and impurities from the surface.
[0124] In the above embodiments, optionally, the pretreatment step is: first, the piezoelectric material 112a... 21 Alternately perform acid washing (dilute hydrochloric acid or dilute nitric acid) and alkali washing (dilute ammonia), then wash thoroughly with deionized water until neutral, and then dry at 80~120℃ for later use.
[0125] In some embodiments, the ion-conducting layer 112a 22 The material is lithium phosphate, in piezoelectric material 112a 21 Surface coated with ion-conductive layer 112a 22 The steps include: The lithium source and phosphorus source were mixed evenly at a molar ratio of Li:P = (2.7~3.3):1 to obtain the coating solution; piezoelectric material 112a 21 Mix with the coating solution and stir at 50-80℃ for 2-6 hours to obtain the pre-coated product; The pre-coated product is heat-treated in an inert atmosphere at a temperature of 500-700℃ to obtain the composite material.
[0126] In the above embodiments, the lithium source can be selected from one or more of lithium hydroxide, lithium acetate, lithium carbonate, and lithium sulfate.
[0127] In the above embodiments, the phosphorus source may be selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, lithium dihydrogen phosphate, triethyl phosphate, trimethyl phosphate, and phosphorus pentoxide. In a specific embodiment, the phosphorus source is selected from one or more of phosphoric acid, ammonium dihydrogen phosphate, and triethyl phosphate.
[0128] In the above embodiments, the molar ratio of lithium source to phosphorus source Li:P in the coating solution is 2.7:1, 3:1, 3.3:1, or any value between them. Optionally, the molar ratio of lithium source to phosphorus source Li:P in the coating solution is (2.9~3.1):1. Within this ratio range, the amount of free phosphorus source residue can be reduced, avoiding an increase in interfacial impedance.
[0129] In the above embodiments, the stirring reaction can be carried out at a temperature of 50°C, 60°C, 70°C, 80°C, or any temperature between these temperatures, and the reaction time can be 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, or any value between these times. During the reaction, the ion-conducting layer 112a can be controlled by adjusting the pH value (preferably pH 8-10) and the reaction time. 22 The thickness of the coating.
[0130] In the above embodiments, after the stirring reaction is completed, the steps further include: filtering, washing and drying the reaction product to obtain the pre-coated product.
[0131] In the above embodiments, piezoelectric material 112a 21 The molar ratio of phosphorus to phosphorus in the phosphorus source is 1:(0.01~0.30), specifically 1:0.01, 1:0.03, 1:0.05, 1:0.10, 1:0.15, 1:0.30, or any value between them. Within this ratio range, the ion-conducting layer 112a is finally fabricated. 22 Able to be basically continuously covered in piezoelectric material 112a 21 The surface, observed under a transmission electron microscope, shows no obvious large-area exposed areas. Optionally, piezoelectric material 112a... 21 The molar ratio of phosphorus in the phosphorus source to phosphorus is 1:(0.03~0.15).
[0132] In the above embodiments, the heat treatment temperature can be 500°C, 600°C, 700°C, or any value between them. The heat treatment causes the ion-conducting layer 112a to... 22 Crystallization and enhancement of its relationship with piezoelectric material 112a 21 The interface bonding of the nucleus; by controlling the temperature of the heat treatment within this range, it is beneficial to prevent grain growth and phase transition, thereby maintaining the piezoelectric material 112a.21 The crystal structure and piezoelectric properties of the 112a ion-conducting layer are simultaneously enhanced. 22 Crystallization and strong bonding with the piezoelectric core.
[0133] In the above embodiments, the inert atmosphere may be selected from one or more of argon or nitrogen.
[0134] In the above embodiments, the heat treatment duration is 1 to 3 hours, specifically 1 hour, 2 hours, 3 hours, or any value between them. This ensures the ion-conducting layer 112a... 22 Fully crystallize and strengthen the interfacial bonding with the piezoelectric core, while avoiding grain coarsening and piezoelectric performance degradation caused by excessive sintering.
[0135] In the above embodiments, the ion-conducting layer 112a 22 The relevant preparation process parameters can be adjusted adaptively according to the actual situation, and the resulting ion-conducting layer 112a 22 It should at least meet the following conditions: basically continuous, uniform thickness, and without obvious cracks or peeling.
[0136] In the above embodiments, the ion-conducting layer 112a can be observed using a transmission electron microscope (TEM). 22 Thickness and integrity; the phase composition of piezoelectric particles 112a2 can be analyzed by X-ray photoelectron spectroscopy (XPS) and X-ray diffraction (XRD).
[0137] In some embodiments, the step of forming a negative electrode active layer 112 on the surface of the negative electrode current collector 111 includes: The piezoelectric particles 112a2 are mixed evenly with the negative electrode active material 112a1, the conductive agent 112a3 and the binder to prepare a slurry. A negative electrode current collector 111 is provided, and a slurry is coated on the surface of the negative electrode current collector 111. After drying, it is rolled and pressed to form a negative electrode active layer 112 on the surface of the negative electrode current collector 111.
[0138] In the above embodiments, the piezoelectric particles 112a2 are uniformly distributed in the negative electrode active layer 112 along with the negative electrode active material 112a1. This uniform distribution allows the piezoelectric particles 112a2 to uniformly respond to volume changes throughout the entire electrode, making it suitable for general application scenarios.
[0139] In the above embodiments, the slurry also contains a solvent (such as N-methylpyrrolidone or deionized water). Those skilled in the art can adjust the solvent content in the slurry according to actual conditions.
[0140] In the above embodiments, a high-speed shear disperser or planetary mixer is used to uniformly mix the piezoelectric particles 112a2 with the negative electrode active material 112a1, the conductive agent 112a3, and the binder. To enhance the uniformity of mixing, intermittent ultrasonic-assisted dispersion can be performed during the mixing process. In one specific embodiment, the mixing time is 30-60 minutes to ensure that the piezoelectric particles 112a2 are uniformly dispersed.
[0141] In the above embodiments, the slurry is coated onto the surface of the negative electrode current collector 111 by blade coating or roller coating, and the coating thickness is controlled to obtain the target areal density (e.g., negative electrode 2~5). ).
[0142] In the above embodiments, the drying temperature is 80~120℃ (e.g., 80℃, 100℃, 120℃, etc.). Within this temperature range, the drying process is relatively mild, avoiding rapid evaporation that could lead to agglomeration of the piezoelectric particles 112a2 or the ion-conducting layer 112a. 22 rupture.
[0143] In the above embodiments, optionally, the compaction density of the negative electrode active layer 112 is controlled within the conventional negative electrode range (e.g., 1.3~1.6 for negative electrode) by rolling. ).
[0144] In the above embodiments, the rolling pressure is ≤150 MPa to ensure the ion-conducting layer 112a of the piezoelectric particles 112a2 is intact. 22 The integrity of.
[0145] In the above embodiments, after rolling, the process further includes the step of cutting and punching the rolled electrode sheet to obtain a negative electrode of the required shape and size.
[0146] In other embodiments, the step of forming a negative electrode active layer 112 on the surface of the negative electrode current collector 111 includes: Prepare a mixed slurry containing piezoelectric particles 112a2, negative electrode active material 112a1, conductive agent 112a3 and binder with multiple concentration gradients; A negative electrode current collector 111 is provided. Several portions of mixed slurry are coated onto the surface of the negative electrode current collector 111 in sequence according to the increasing or decreasing concentration of piezoelectric particles 112a2. After drying, the mixture is rolled to form a negative electrode active layer 112 on the surface of the negative electrode current collector 111.
[0147] When piezoelectric particles 112a2 are enriched on the side away from the negative electrode current collector 111, it is more conducive to enhancing the stress-response film formation capability of the negative electrode / electrolyte 140 interface; when piezoelectric particles 112a2 are enriched on the side closer to the negative electrode current collector 111, it is helpful to alleviate stress concentration near the negative electrode active layer 112 and the negative electrode current collector 111, reducing the risk of debonding, crack propagation and electrical contact failure. The gradient distribution pattern can be optimized according to the stress characteristics of specific regions of the electrode to specifically enhance the stability of key interfaces.
[0148] In some other embodiments, the step of forming a negative electrode active layer 112 on the surface of the negative electrode current collector 111 includes: A first slurry containing negative electrode active material 112a1, conductive agent 112a3 and binder was prepared. A negative electrode current collector 111 is provided, a first slurry is coated on the surface of the negative electrode current collector 111 and dried, and a negative electrode active layer 112 is formed on the surface of the negative electrode current collector 111. The piezoelectric particles 112a2 are mixed evenly with the binder to obtain a second slurry. The second slurry is coated on the surface of the negative electrode active layer 112, dried, and then rolled to form a piezoelectric layer 112b1 on the surface of the negative electrode active layer 112. The piezoelectric layer 112b1 and the active layer are combined to form the overall structure of the negative electrode active layer 112.
[0149] By concentrating piezoelectric particles 112a2 on the electrode surface to form a functionalized piezoelectric layer 112b1, the interface protection function can be concentrated. This interface layer aggregation design is particularly suitable for applications requiring key protection of the electrode / electrolyte 140 interface.
[0150] In the above embodiments, the following process points should be noted: (1) Special attention should be paid to the uniformity of the piezoelectric particles 112a2 during the mixing stage to avoid agglomeration into large particles; (2) The roller pressing pressure should be moderate to ensure both electrode density and electronic conductivity, while avoiding the formation of ion-conducting layer 112a. 22 Mechanical damage.
[0151] In this embodiment, the positive electrode can be prepared by referring to the preparation method of the negative electrode in the above embodiment, such as the preparation method of piezoelectric particles 112a2, the mixing method, etc., which will not be described in detail in this embodiment.
[0152] In this embodiment, the battery cell in step S10 refers to a semi-finished battery, that is, a structure assembled from a positive electrode, a negative electrode, a separator 120, and a casing, but without electrolyte 140 injected. At this time, there is no electrolyte 140 inside the battery cell; only physical assembly has been completed, which is the pre-processing stage before subsequent electrolyte injection and formation treatment.
[0153] In this embodiment, the battery cell 100 can be a wound battery: the positive electrode, separator 120 and negative electrode are wound into the casing; the battery cell 100 can also be a stacked battery: the positive electrode, separator 120 and negative electrode are stacked layer by layer like a "sandwich".
[0154] In this embodiment, the battery cell 100 can be any one of cylindrical battery, prismatic battery, and pouch battery.
[0155] In this embodiment, the housing can be any one of aluminum-plastic film, steel shell, aluminum shell, etc.
[0156] In this embodiment of the application, the battery cell assembly is carried out in a glove box (moisture <0.1 ppm, oxygen <0.1 ppm).
[0157] In some embodiments, prior to step S10, the preparation method of the battery cell 100 further includes the step of: vacuum drying the positive and negative electrodes at a temperature of 80~120 ℃ for 12~24 hours to ensure that the internal moisture content of the positive and negative electrodes is less than 50 ppm, and then transferring them to a glove box for the next process (cell assembly).
[0158] In some embodiments, the preparation steps of electrolyte 140 include: in a glove box (moisture <0.1 ppm, oxygen <0.1 ppm), mixing lithium salt, organic solvent (e.g., EC:EMC:DEC = 1:1:1 volume ratio), first film-forming agent 141 and second film-forming agent, etc., according to the designed formula, and letting it stand for several hours to ensure that the components are fully compatible, thereby preparing electrolyte 140, and sealing and storing electrolyte 140 to avoid moisture and air contamination.
[0159] In some embodiments, the mass ratio of the first film-forming agent 141 in the electrolyte 140 is w1, and the mass ratio of the piezoelectric particles 112a2 in the negative electrode active layer 112 is M1, where w1:M1 = (0.3~5):1, specifically 0.3:1, 1:2, 1:1, 3:1, 4:1, or 5:1. Correspondingly, the mass ratio of the second film-forming agent in the electrolyte 140 is w2, and the mass ratio of the piezoelectric particles 112a2 in the positive electrode active layer 132 is M2, where w2:M2 = (0.3~5):1. Within this ratio range, it ensures that there is sufficient film-forming agent (first film-forming agent 141 or second film-forming agent) available for preferential decomposition in the piezoelectric response region, while avoiding the non-selective uniform film formation dilution piezoelectric coupling effect caused by excessive film-forming agent (first film-forming agent 141 or second film-forming agent).
[0160] In some embodiments, the mass percentage of piezoelectric particles 112a2 in the negative electrode active layer 112 or the positive electrode active layer 132 is 0.1~5.0 wt%, 0.5~2.0 wt%, or 0.8~1.5 wt%, specifically 0.1 wt%, 0.5 wt%, 0.8 wt%, 1 wt%, 1.5 wt%, 2 wt%, 3 wt%, 4 wt%, 5.0 wt%, or any value between them. Within this mass percentage range, the effects of piezoelectric response, electrode energy density, and processing performance are taken into account.
[0161] In some embodiments, the content of the first film-forming agent 141 (or the second film-forming agent) in the electrolyte 140 is 0.2 to 3 wt%, specifically 0.2 wt%, 1 wt%, 2 wt%, 3 wt%, or any value between them. This content range ensures that a sufficient amount of the first film-forming agent 141 (or the second film-forming agent) participates in preferential film formation around the piezoelectric particles 112a2, while avoiding non-selective uniform film formation and dilution of the piezoelectric coupling effect caused by excessive first film-forming agent 141 (or the second film-forming agent).
[0162] In some embodiments, the negative electrode is a silicon-based negative electrode, and the first film-forming agent 141 is selected from at least one of difluoromalononitrile and fluorobutadiene. The decomposition products of such fluorinated dionitrile compounds are rich in LiF and C≡N derivatives, which help to form a dense inorganic SEI layer and improve the interfacial mechanical strength and stability.
[0163] In the above embodiments, optionally, the content of the first film-forming agent 141 in the electrolyte 140 is 0.2~3 wt%, specifically 0.2 wt%, 1 wt%, 2 wt%, 3 wt%, or any value between them. Preferably, the content of the first film-forming agent 141 in the electrolyte 140 is 0.5~1.5 wt%.
[0164] In the above embodiments, optionally, the electrolyte 140 further contains a first auxiliary film-forming agent, which works synergistically with the first film-forming agent 141 to jointly construct a multi-layered SEI structure (or CEI structure).
[0165] In the above embodiments, optionally, the first auxiliary film-forming agent includes at least one of fluoroethylene carbonate, vinylene carbonate, and fluorosulfonyl lactones. In a specific embodiment, taking the total content of electrolyte 140 as 100 wt%, the first auxiliary film-forming agent includes the following components in the following amounts: fluoroethylene carbonate (FEC), with a content of 1~5 wt%, preferably 1.5~3 wt%; vinylene carbonate (VC), with a content of 0.2~1.0 wt%, preferably 0.5~1.0 wt%.
[0166] In the above embodiments, it should be noted that fluoroethylene carbonate, vinylene carbonate, and fluorosulfonyl lactones can be used as first auxiliary film-forming agents in combination with the first film-forming agent 141, or they can be used as the first film-forming agent 141; their specific roles are subject to the conditions such as the components responsible for selective window determination and content statistics in the corresponding embodiments.
[0167] In some embodiments, the negative electrode is a lithium metal negative electrode, and the first film-forming agent 141 comprises lithium nitrate and fluorosulfonyl lactone (such as methyl fluorosulfonyl lactone MFSL). Lithium nitrate is used in piezoelectric material 112a. 21 Driven by priority restoration, it provides / An inorganic framework, with the co-decomposition of fluorosulfonyl lactones providing LiF and sulfur-containing organic-inorganic composite components, co-deposits these components in the piezoelectric enhancement region to form a two-component dense SEI film. This not only enables selective repair of the SEI film but also preferentially decomposes in dendrite-growth-prone regions to form a dense SEI film. / Protective layer.
[0168] In the above embodiments, optionally, the mass ratio of lithium nitrate to MFSL in the first film-forming agent 141 is 2:1 to 5:1. Specifically, it can be 2:1, 3:1, 4:1, 5:1, or any value between them.
[0169] In the above embodiments, optionally, the mass ratio of the first film-forming agent 141 in the electrolyte 140 is w1, and the mass ratio of the piezoelectric particles 112a2 in the negative electrode active layer 112 is M1, where w1:M1=1:1~5:1.
[0170] In the above embodiments, optionally, the organic solvent in the electrolyte 140 is a mixed solvent of 1,3-dioxolane (DOL) and 1,2-dimethoxyethane (DME).
[0171] In the above embodiments, optionally, the lithium salt is at least one of LiTFSI and LiFSI, and the total concentration of the lithium salt is 0.5~2.0 mol / L.
[0172] In one specific embodiment, the piezoelectric particles 112a2 in the negative electrode active layer 112 account for 0.5~3.0 wt% of the total mass.
[0173] In some embodiments, the positive electrode is a high-nickel positive electrode, and the second film-forming agent can be selected from one or more of borate esters, lithium oxalate-borate salts, dinitrile compounds, etc. In one specific embodiment, the second film-forming agent includes tris(trimethylsilyl)borate ester (TMSB) and lithium difluorooxalate-borate (LiDFOB). Under piezoelectric polarization assistance, TMSB and LiDFOB preferentially oxidize and decompose in the lattice strain concentration region. TMSB provides a silicon- and boron-containing inorganic protective component, and LiDFOB provides LiF and a boron-containing organic-inorganic composite component. The two work together to form a dense CEI film with a chemical composition gradient, suppressing the dissolution of transition metals and the release of lattice oxygen under high voltage.
[0174] In one specific embodiment, the mass percentage of the second film-forming agent in the electrolyte 140 is w2, and the mass percentage of the piezoelectric particles 112a2 in the positive electrode active layer 132 is M2, where w2:M2 = (0.3~5):1.
[0175] In this embodiment, the amount of electrolyte 140 injected into the cell is controlled by the injection coefficient, which is usually 1~3 g / Ah, depending on the electrode porosity and the amount of liquid absorbed by the diaphragm 120.
[0176] In some embodiments, prior to formation treatment, the method for preparing the battery cell 100 further includes the steps of: vacuuming and degassing the cell after liquid injection, sealing it, and then allowing it to stand at room temperature for 2 to 12 hours.
[0177] In some embodiments, the formation process is performed under the following conditions: initial charge-discharge at a low rate of 0.1~0.2 C under a constant temperature environment of 25 °C; charging to a set upper limit voltage followed by constant voltage charging until the current drops to 0.05 C; and then discharging to a lower limit voltage. During the formation process, the film-forming agent (such as the first film-forming agent 141 or the second film-forming agent) decomposes on the electrode surface to form an initial interface layer (SEI film or CEI film). The piezoelectric particles 112a2 begin to respond to the volume change of the electrode, inducing preferential film formation in stress concentration regions.
[0178] In this embodiment, the first film-forming agent 141 (or the second film-forming agent) is preferentially consumed during the formation process. The residual amount of the first film-forming agent 141 (or the second film-forming agent) in the electrolyte 140 of the finished battery cell 100 is lower than the amount added during injection and varies with the formation conditions and cycling status. Therefore, unless otherwise stated, the content of the first film-forming agent 141 (or the second film-forming agent) in the electrolyte 140 mentioned in this application refers to the initial addition amount based on the total mass of the electrolyte 140 used for injection before formation.
[0179] After formation and long cycling, the electrolyte 140 of the resulting finished battery cell 100 still contains detectable precursors of the first film-forming agent 141 (or the second film-forming agent). After disassembling the battery cell 100, the electrolyte 140 is quantitatively extracted with dimethyl carbonate, and its residual amount is determined by gas chromatography-mass spectrometry (external standard method). Fluorine- or boron-containing components can be further... 19 F, 11 B. Quantitative verification by nuclear magnetic resonance. In addition, the characteristic decomposition products of the first film-forming agent 141 (or the second film-forming agent) are solidified in the SEI film (or CEI film) and can be detected by X-ray photoelectron spectroscopy (F 1s, N 1s, B 1s) and time-of-flight secondary ion mass spectrometry, which are used to characterize that the film-forming agent has participated in the formation of the interfacial film.
[0180] The present application will be further described below through specific embodiments and comparative examples, but the present application is not limited to these specific examples.
[0181] Unless otherwise specified, all operations in the following examples and comparative examples were performed at a dew point below [insert dew point here]. The tests were conducted in a dry environment or glove box at 45 °C (moisture < 0.1 ppm, oxygen < 0.1 ppm); all potential values were determined using the three-electrode linear scanning voltammetry method specified above. , All calculations were performed under a reference compressive stress of 100 MPa, as specified in the preceding text.
[0182] Example 1 Preparation of battery cells: (1) Preparation of piezoelectric particles: Commercial barium titanate powder (tetragonal perovskite structure, purity ≥99.9%, D 50 The sample was washed with dilute hydrochloric acid and dilute ammonia water alternately, followed by alkali washing, and then washed with deionized water until neutral. It was then dried at 100 °C. A coating solution was prepared by dissolving lithium acetate and ammonium dihydrogen phosphate in deionized water at a Li:P molar ratio of 3:1. The piezoelectric material was added to the coating solution, with a phosphorus molar ratio of 1:0.08 between the piezoelectric material and the phosphorus source in the coating solution. The mixture was stirred at 70 °C for 4 hours, filtered, washed, and dried to obtain the pre-coated product. The product was then heat-treated at 600 °C for 2 hours under an argon atmosphere to obtain piezoelectric particles coated with a lithium phosphate ion-conductive layer. The thickness of the ion-conductive layer was 3–5 nm. The Di of the piezoelectric particles was [missing information]. 50 ≈100 nm.
[0183] (2) Preparation of the negative electrode: Based on a total mass of 100wt%, 93.0wt% of silicon-carbon composite negative electrode active material (a composite material of silicon suboxide and graphite, with a reversible specific capacity of 450 mAh / g), 1.0 wt% of the above-mentioned piezoelectric particles, 2.0 wt% of conductive agent Super P and 4.0 wt% of binder (sodium carboxymethyl cellulose and styrene-butadiene rubber, with a mass ratio of 1:1) were added to deionized water to form a slurry. The slurry was coated on the surface of a 10 μm copper foil (uniformly coated), dried at 85 ℃, and then rolled to a compaction density of 1.55 g / cm³. 3 A negative electrode active layer is formed on the surface of the copper foil, and the negative electrode is cut out. The piezoelectric particles and negative electrode active material are uniformly mixed and distributed in the negative electrode active layer.
[0184] (3) Preparation of positive electrode: NCM811, conductive agent Super P, and binder polyvinylidene fluoride are mixed with N-methylpyrrolidone in a mass ratio of 96.5:2.0:1.5 to form a slurry, which is then coated on the surface of 12 μm aluminum foil. After drying at 110 °C, the slurry is rolled to form a positive electrode active layer on the surface of the aluminum foil, and the positive electrode is then cut.
[0185] (4) Preparation of electrolyte: Using ethylene carbonate: methyl ethyl carbonate: diethyl carbonate = 1:1:1 (volume ratio) as organic solvent, add lithium hexafluorophosphate to make the concentration 1.0 mol / L, and then add the first film-forming agent difluoromalonium, which accounts for 1.0 wt% of the total mass of the electrolyte (w1:M1=1:1). After mixing evenly, let stand for 6 hours.
[0186] (5) Preparation of battery cell: The positive electrode, negative electrode, polypropylene separator and shell are assembled into a cell; the above electrolyte is injected into the cell with an injection coefficient of 2.5 g / Ah; after vacuuming to remove air bubbles, the cell is sealed and left to stand at room temperature for 8 hours; the cell is charged and discharged for the first time at 0.1 C at 25 ℃, charged to the upper limit voltage and then charged at constant voltage until the current drops to 0.05 C, and then discharged to the lower limit voltage to complete the formation and obtain the battery cell.
[0187] In this embodiment, the piezoelectric particles =110 pC / N =2600、 =100 nm, =48 mV, falling within the range of 10~50 mV; the initial reduction potential of the first film-forming agent, difluoromalononitrile. The highest reduction potential of the organic solvent (ethylene carbonate) is 1.15 V. It is 0.80 V. =0.35 V, which satisfies ≤ .
[0188] Example 2 The difference from Example 1 is that: In the preparation steps of the negative electrode, the content of each component in the slurry is different: based on a total solid content of 100 wt%, the slurry contains 93.5 wt% silicon-carbon composite negative electrode active material, 0.5 wt% of the above-mentioned piezoelectric particles, 2.0 wt% conductive agent Super P and 4.0 wt% binder (w1:M1=2:1), and the rest is the same as in Example 1.
[0189] Example 3 The difference from Example 1 is that: In the preparation steps of the negative electrode, the content of each component in the slurry is different: based on a total solid content of 100 wt%, the slurry contains 92 wt% silicon-carbon composite negative electrode active material, 2.0 wt% of the above-mentioned piezoelectric particles, 2.0 wt% conductive agent Super P and 4.0 wt% binder (w1:M1=0.5:1), and the rest is the same as in Example 1.
[0190] Example 4 The difference from Example 1 is that: In the negative electrode preparation step, the coating method of the slurry is changed from uniform coating to gradient coating: three mixed slurries with piezoelectric particle mass percentages (based on a total solid content of 100 wt%) of 0.4 wt%, 1.0 wt%, and 1.6 wt% are prepared and coated onto the copper foil surface in order of increasing piezoelectric particle concentration. The dry basis coating mass of the three mixed slurries is the same. After drying, they are rolled to make the distribution concentration of piezoelectric particles gradually increase from the side closer to the negative electrode current collector to the side farther away from the negative electrode current collector. The average mass percentage of piezoelectric particles in the negative electrode active layer is 1.0 wt% (w1:M1=1:1).
[0191] Example 5 The difference from Example 1 is that: In the preparation steps of the negative electrode, the preparation of the negative electrode active layer is changed from single-layer coating to double-layer coating: First, a first slurry containing negative electrode active material, conductive agent, and binder 1 (93.0:2.0:4.0) but without piezoelectric particles is coated onto the surface of copper foil and dried to form a functional layer; then, piezoelectric particles and binder 2 are mixed at a mass ratio of 90:10 to prepare a second slurry, which is coated onto the surface of the functional layer, dried, and then rolled to form a piezoelectric layer. The piezoelectric layer is a porous, discontinuous particle layer, and the areal density of piezoelectric particles on the surface of the functional layer is 0.02~0.20 mg / cm³. 2 The corresponding masses of the negative electrode active material, piezoelectric particles, conductive agent and binder 1 in the negative electrode active layer are the same as in Example 1.
[0192] Example 6 The difference from Example 1 is that: In the preparation steps of piezoelectric particles, the particle size D is... 50 Barium titanate powder with a particle size of approximately 90 nm was replaced with a particle size of D. 50 Barium titanate powder with a diameter of approximately 40 nm.
[0193] In this embodiment, the piezoelectric particles =110 pC / N =2600、 ≈50 nm, =24 mV, falling within the range of 10~50 mV, and satisfying ≤ .
[0194] Example 7 The difference from Example 1 is that: (2) Preparation of negative electrode (lithium metal negative electrode): A 50 μm thick lithium metal active layer is set on a 10 μm copper foil; a porous discontinuous transfer layer (piezoelectric layer) containing piezoelectric particles and binder (90:10) is pre-prepared on a release substrate, and after being fully vacuum dried, it is rolled and transferred to the surface of the lithium metal active layer; during the preparation process, the lithium metal active layer does not directly contact water or the organic solvent used to prepare the transfer layer; the lithium metal active layer and the piezoelectric layer together constitute the negative electrode active layer, and the piezoelectric particles account for 1.0 wt% of the total mass of the negative electrode active layer.
[0195] (4) Preparation of electrolyte: The electrolyte was changed to use 1,3-dioxolane and 1,2-dimethoxyethane (volume ratio 1:1) as organic solvent, lithium difluorosulfonylimide was added to make the concentration 1.0 mol / L, and then 1.5 wt% lithium nitrate (first film-forming agent) and 0.5 wt% methyl fluorosulfonyl lactone (first auxiliary film-forming agent) were added. After mixing evenly, the mixture was allowed to stand for 6 hours to obtain the electrolyte.
[0196] In this embodiment, the electrolyte does not contain a second film-forming agent; only the stress-response film-forming mechanism on the negative electrode side is involved. The initial reduction potential of lithium nitrate is 1.70 V, while the maximum reduction potential of the organic solvent is 1.05 V. =0.65 V, It falls within the range of 10~50 mV and satisfies ≤ .
[0197] In this embodiment, a nitrogen-containing lithium salt, lithium bisfluorosulfonylimide, is used. Since the source of nitrogen-containing signals in the interface film is not unique, the spatial selectivity index based on nitrogen-containing fragments is not measured.
[0198] Example 8 The difference from Example 1 is that: In the preparation steps of the negative electrode, no piezoelectric particles are added to the active layer of the negative electrode.
[0199] In the preparation steps of the positive electrode, the piezoelectric particles prepared in Example 1 are added to the positive electrode active layer. The mass ratio of positive electrode active material, piezoelectric particles, Super P, and polyvinylidene fluoride is 95.5:1.0:2.0:1.5.
[0200] In the electrolyte preparation step, the first film-forming agent is replaced with the second film-forming agent tris(trimethylsilyl)borate and lithium difluorooxalate borate (mass ratio 1:1), accounting for 1.0 wt% of the total electrolyte mass.
[0201] In this embodiment, =48 mV; the initial oxidation potential of tris(trimethylsilyl)borate is 4.02 V, that of lithium difluorooxalate borate is 4.38 V, and the minimum oxidation potential of organic solvents is 4.85 V. =0.47~0.83 V, which satisfies ≤ .
[0202] Example 9 Preparation of battery cells: (1) Preparation of piezoelectric particles: Same as in Example 1.
[0203] (2) Preparation of negative electrode: Same as in Example 1.
[0204] (3) Preparation of the positive electrode: Same as in Example 8.
[0205] (4) Preparation of electrolyte: Using ethylene carbonate: methyl ethyl carbonate: diethyl carbonate = 1:1:1 (volume ratio) as organic solvent, lithium hexafluorophosphate was added to make the concentration 1.0 mol / L, and then the first film-forming agent (difluoromalononitrile) and the second film-forming agent (tris(trimethylsilyl)borate and lithium difluorooxalate borate, mass ratio 1:1) were added. The first film-forming agent and the second film-forming agent each accounted for 1.0 wt% of the total mass of the electrolyte. After mixing evenly, the mixture was allowed to stand for 6 hours.
[0206] (5) Preparation of battery cells: Same as in Example 1.
[0207] Example 10 The difference from Example 1 is that: The electrolyte was modified to an engineering electrolyte system. In the electrolyte preparation steps: the lithium salt was a composite lithium salt of lithium hexafluorophosphate and lithium difluorosulfonylimide (molar ratio 8:2), with a total concentration of 1.2 mol / L; the organic solvent was ethylene carbonate: methyl ethyl carbonate: diethyl carbonate = 1:1:1 (volume ratio); the first film-forming agent was difluoromalonium 1.0 wt%; and fluoroethylene carbonate 2.0 wt% and vinylene carbonate 0.5 wt% were added as the first auxiliary film-forming agent.
[0208] In this embodiment, lithium bis(fluorosulfonyl)imide contains nitrogen and fluorine elements, and fluoroethylene carbonate contains fluorine elements. The sources of nitrogen and fluorine elements in the interface film are no longer unique. Therefore, the spatial selectivity index is not measured in this embodiment.
[0209] Example 11 The difference from Example 1 is that: In the preparation steps of the negative electrode, the content of each component in the slurry is different: based on a total solid content of 100 wt%, the slurry contains 89 wt% silicon-carbon composite negative electrode active material, 5.0 wt% of the above-mentioned piezoelectric particles, 2.0 wt% conductive agent Super P and 4.0 wt% binder; in the preparation steps of the electrolyte, the first film-forming agent difluoromalonium accounts for 1.5 wt% of the total mass of the electrolyte, w1:M1=0.3:1, and the rest is the same as in Example 1.
[0210] Comparative Example 1 The difference from Example 1 is that: No piezoelectric particles are added to the negative electrode active layer; and, No first film-forming agent is added to the electrolyte.
[0211] Comparative Example 2 The difference from Example 1 is that: No piezoelectric particles are added to the negative electrode active layer.
[0212] Comparative Example 3 The difference from Example 1 is that: No first film-forming agent is added to the electrolyte.
[0213] Comparative Examples 1-3 and Example 1 constitute a two-factor combination of piezoelectric particles and a first film-forming agent.
[0214] Comparative Example 4 The difference from Example 1 is that: Step (1) is omitted, and the piezoelectric particles in step (2) are replaced with bare barium titanate powder (D50≈100 nm) without an ion-conducting layer on the surface.
[0215] In this comparative example, the bare barium titanate has d33_eff=115 pC / N, εr_eff=2700, and ΔVpiezo1=48 mV, which are comparable to those in Example 1.
[0216] Comparative Example 5 (Piezoelectric material as a coating layer for negative electrode active material) The difference from Example 1 is as follows: Step (1) is omitted, and the silicon-carbon composite negative electrode active material and piezoelectric particles in step (2) are replaced with a composite material of the two (mutually dispersed → core-shell structure); the preparation method of this composite material is as follows: Take the same piezoelectric particles as in Example 1 (barium titanate@lithium phosphate, D50≈100 nm), and add them to the mechanical fusion equipment with silicon-carbon composite negative electrode active material at a mass ratio of 1.0:93.0. Dry process at 2000 r / min for 30 minutes to make the piezoelectric particles attach and fix them on the surface of the negative electrode active material particles to form a coating layer.
[0217] In this comparative example, the piezoelectric material forms a coating layer on the negative electrode active material and does not exist as an independent dispersed phase in the negative electrode active layer; except for this arrangement, all other variables are the same as in Example 1.
[0218] Comparative Example 6 The difference from Example 1 is as follows: No piezoelectric particles are added to the negative electrode active layer; and, Instead of adding difluoromalononitrile to the electrolyte, fluoroethylene carbonate (3.0 wt%) and vinylene carbonate (1.0 wt%) are added.
[0219] This comparative example represents a silicon-based anode electrolyte solution using conventional film-forming additives.
[0220] Comparative Example 7 The difference from Example 1 is as follows: The first film-forming agent in the electrolyte, difluoromalononitrile, was replaced with an equal amount of succinate.
[0221] In this comparative example, the initial reduction potential of succinic anionylene was 0.72 V, which is lower than the maximum reduction potential of the organic solvent, 0.80 V. = 0.08 V, not satisfied ≤ .
[0222] Comparative Example 8 The difference from Example 1 is as follows: In the preparation step of piezoelectric particles, commercial barium titanate powder with a particle size of D50≈90 nm is replaced with commercial barium titanate powder with a particle size of D50≈290 nm.
[0223] In this comparative example, the piezoelectric particles =110 pC / N =3600、 ≈300 nm, =104 mV, which is outside the range of 10~50 mV.
[0224] Comparative Example 9 The difference from Example 1 is as follows: In the preparation step of piezoelectric particles, commercially available barium titanate powder is replaced... Strontium titanate.
[0225] The strontium titanate@lithium phosphate particles (piezoelectric particles) were characterized according to the characterization method specified in this application. ≤0.5 pC / N (close to the instrument's detection limit) =300, ≤2 mV.
[0226] This comparative example is used to examine the contribution of piezoelectric response capability to the spatial selectivity of interfacial film formation, while controlling factors such as particle size, ion-conductive layer and filler addition as much as possible.
[0227] Comparative Example 10 The difference from Example 8 is as follows: No piezoelectric particles are added to the positive electrode active layer.
[0228] Comparative Example 11 The difference from Example 7 is as follows: In the preparation of the negative electrode, the composite structure of copper foil and lithium metal active layer is directly used as the negative electrode, without the need to set a piezoelectric layer on its surface.
[0229] Comparative Example 12 The difference from Example 10 is as follows: No piezoelectric particles are added to the negative electrode active layer.
[0230] Test methods 1. Initial Coulombic Efficiency of Negative Electrode: Assemble a CR2032 coin cell with a negative electrode and a lithium electrode, discharge it at 25 °C with a constant current of 0.1 C to 0.005 V, discharge it with a constant voltage until the current drops to 0.02 C, and then charge it with a constant current of 0.1 C to 1.5 V; the ratio of the initial charge capacity to the initial discharge capacity is the initial Coulombic efficiency of the negative electrode.
[0231] 2. First Coulombic Efficiency of Positive Electrode: Assemble a CR2032 coin cell with a positive electrode and a lithium electrode, and charge and discharge it at a constant current of 0.1 C in the range of 3.0~4.25 V at 25 ℃. The ratio of the first discharge capacity to the first charge capacity is the first coulombic efficiency of the positive electrode.
[0232] 3. Li‖Cu Average Coulombic Efficiency: A CR2032 coin cell was assembled using copper foil (Cu) as the working electrode and lithium metal anode as the counter electrode (and also as the reference electrode); at a current density of 1 mA / cm²... 2 Surface capacity 1 mAh / cm 2 Under the test conditions, the cycle was 50 times, and the average coulombic efficiency from the 1st to the 50th cycle was taken.
[0233] 4. Li||Li symmetric cell: Two identical lithium metal anode sheets are assembled into a CR2032 type button cell; at a current density of 1 mA / cm²... 2 Surface capacity 1 mAh / cm 2 Under the test conditions, charge and discharge cycles were performed, and the polarization voltage was recorded after 500 h.
[0234] 5. Cycle capacity retention rate: Take the battery cells of each embodiment and comparative example, and charge and discharge them at 0.5 C in the range of 2.8~4.2 V at 25 ℃; the ratio of the discharge capacity in the 200th week and the 500th week to the discharge capacity in the first week is the corresponding capacity retention rate.
[0235] 6. Interfacial Impedance and its Increase: Electrochemical impedance spectroscopy (EIS) was performed on individual cells after 2 hours of resting at 50% SOC, with a frequency range of 10 mHz to 100 kHz and an amplitude of 5 mV. The charge transfer impedance Rct was obtained by fitting the mid-frequency capacitive arc with an equivalent circuit. The values were recorded after formation and after the 200th cycle, and the values were calculated as follows: (Rct, 200 cycles) Rct (after conversion) / Rct, calculates the increase after conversion.
[0236] 7. Chemical composition of the interfacial film: The cycled battery cells were disassembled in a glove box. The negative electrode was washed three times with dimethyl carbonate and vacuum dried. The sample was then transferred to an X-ray photoelectron spectroscopy (XPS) instrument under an inert atmosphere. F 1s, N 1s, B 1s, C 1s, and O 1s spectra were collected and analyzed using Ar... + Etching is used for in-depth analysis.
[0237] 8. Residual Film-Forming Agent: Disassemble the battery cell in a glove box and determine the absolute amount of the residual first film-forming agent. The ratio of this amount to the amount added during liquid injection is the percentage of residual agent. If the film-forming agent (first or second film-forming agent) is an inorganic salt such as lithium nitrate, ion chromatography is used for determination. If the film-forming agent (first or second film-forming agent) is an organic film-forming agent, gas chromatography-mass spectrometry or high-performance liquid chromatography is used. Fluorine-containing and boron-containing components are determined separately. 19 F, 11 B-cell nuclear magnetic resonance quantitative verification.
[0238] 9. Spatial Selectivity Index (SSI): SSI is defined as the ratio of tracer signal intensity in stress concentration areas to that in flat areas, i.e., SSI = Istress area / Iflat area. The stress concentration area is the cracked region of the negative (or positive) electrode active material located by scanning electron microscopy after cycling, and its neighborhood extending within 1 μm from the crack edge. The flat area is the region on the same negative (or positive) electrode with no visible cracks and at least 5 μm from the nearest crack. Microarea distribution imaging (beam spot ≤ 1 μm) is performed using time-of-flight secondary ion mass spectrometry. At least 10 sampling points are taken from each of the above two types of regions, and the average normalized secondary ion intensity is used for calculation. (See also...) Figure 4 .
[0239] With nitrogen-containing fragments (CN) - CNO - The result calculated using tracer ions is denoted as SSI(N), which characterizes the spatial distribution of the decomposition products of the nitrogen-containing first film-forming agent; carbonate fragments (CO3) are used as the tracer ions. - CHO2 - The result calculated using boron-containing fragments (BO2) is denoted as SSI(CO3), which characterizes the spatial distribution of organic solvent decomposition products; - The result of the tracer ion calculation is denoted as SSI(B), which characterizes the spatial distribution of the decomposition products of the boron-containing second film-forming agent. The reference electrolytes of Examples 1-6, 8, 9, and their corresponding proportions did not contain other nitrogen-containing components; therefore, the nitrogen element in the interfacial film originated solely from the first film-forming agent.
[0240] 7. Piezoelectric Selectivity Enhancement Coefficient (PSE): PSE is defined as the ratio of the SSI(N) of this group to the SSI(N) of Comparative Example 2, which contains only the first film-forming agent and no piezoelectric particles. That is, PSE = SSI(N) of this group / SSI(N) of Comparative Example 2. It is used to subtract the background effect caused by the fact that the fresh surface of the crack zone is more likely to form a film.
[0241] Test Results Table 1. Piezoelectric particle parameters for each embodiment and comparative example ( or )
[0242] Potential parameters of each first film-forming agent and their relative potentials margin ( = With reference to Example 1: =48mV, =0.80 V) is shown in Table 2 below. When When V ≥ +0.10, it is judged as clearly satisfying the selective window condition; when 0.10 V < When the initial potential is < +0.10 V, it is considered a boundary case because the repeatability of the initial potential measurement is on the same order of magnitude as this margin; when ≤ The requirement of 0.10 V is considered to be clearly unmet.
[0243] Table 2. Potential parameters of various primary film-forming agents and their relative potentials. margin
[0244]
[0245] Table 3. Electrochemical performance and steric selectivity test results of each example and comparative example in the silicon-carbon anode system.
[0246] Combination Figure 5As shown in (b) and Table 3 above, the SSI(N) of Example 1 is 1.82 while the SSI(CO3) is only 1.06, indicating that the reinforcement of the interfacial film in the stress concentration region is specifically due to the decomposition products of the first film-forming agent, rather than the overall thickening of the interfacial film. In Comparative Example 9, except that the piezoelectric core material is replaced with strontium titanate instead of barium titanate, the particle size, ion-conducting layer, and addition amount are all the same as in Example 1. Its piezoelectric response capability is significantly reduced, and correspondingly, the SSI(N) drops back to 1.06 and the PSE is 0.98, comparable to Comparative Example 2 which only contains the first film-forming agent, demonstrating the aforementioned spatial selectivity. The SSI (N) of Comparative Example 7 is derived from the piezoelectric response itself, rather than from the filling effect of nanoparticles or the contribution of the ion-conducting layer. Although Comparative Example 7 contains piezoelectric particles, the first film-forming agent does not meet the selectivity window condition, and the SSI (N) is only 1.12, indicating that the piezoelectric response and the potential matching of the film-forming agent are both indispensable. Although Comparative Example 4 does not have an ion-conducting layer, its SSI (N) still reaches 1.38, indicating that the role of the ion-conducting layer is to block the direct contact between the piezoelectric material and the electrolyte and maintain long-term stability, rather than to provide the piezoelectric response itself. Therefore, its spatial selectivity is still present, but its cycling performance and interfacial impedance are significantly degraded.
[0247] Using piezoelectric particles and the first film-forming agent as two factors, the two-factor interaction effects obtained from Comparative Examples 1, 2, 3, and 1 are shown in Table 4 below. The simple superposition expected values in the table are calculated as "no baseline + only the increment of the first film-forming agent + only the increment of the piezoelectric particles", and the interaction effect is the difference between the measured value and the expected value.
[0248] Table 4. Results of the interaction between the first film-forming agent and piezoelectric particles
[0249] Combination Figure 5 As shown in (a) and Table 4 above, the interaction effect of each indicator is positive (the increase in Rct is positive when the value decreases), indicating that the improvement brought about by the joint introduction of piezoelectric particles and the first film-forming agent is greater than the sum of the improvements brought about by the introduction of the two alone, and there is a synergistic effect between the two.
[0250] Table 5. Results of the influence of piezoelectric particle content, distribution pattern and particle size on the performance of battery cells.
[0251] Analysis of Table 5 above shows that the overall performance is optimal when w1:M1 is around 1:1; in terms of distribution, the gradient enrichment distribution exhibits the best overall performance, with the surface piezoelectric layer showing the highest spatial selectivity but a slight increase in initial interface impedance; in Example 6... When the voltage was reduced to 24 mV, the spatial selectivity and cycling performance were still significantly better than those of Comparative Example 2 (see Table 3), indicating that the effects of this application can be continuously achieved in the range of 10 to 50 mV.
[0252] The residual amount of the first film-forming agent at different stages of the battery cell is shown in Table 6 below. The residual amount is calculated as 100% of the amount added during liquid injection.
[0253] Table 6. Test results of residual amount of the first film-forming agent at different stages of the battery cell
[0254] As shown in Table 6 above, after formation and long cycling, the first film-forming agent matrix is detectable in the electrolyte of each battery cell; its residual amount continues to decrease with cycling and is not constant at each stage. Therefore, the content of the first film-forming agent in the electrolyte is defined based on the total mass of the electrolyte used for injection before formation.
[0255] Table 7. Test results of lithium metal anode system, high-nickel cathode system, dual-sided anode and cathode system, and engineering electrolyte system.
[0256] In Table 7 above, comparing Example 7 with Comparative Example 11, in the lithium metal anode system, the introduction of a piezoelectric layer can improve the average coulombic efficiency of Li‖Cu (98.8% vs. 97.2%) and reduce the polarization voltage of the Li‖Li symmetric cell (32 mV vs. 78 mV). Comparing Example 8 with Comparative Example 10, in the high-nickel cathode system, the introduction of a piezoelectric layer can show spatial selectivity and performance improvement. In Example 9, spatial selectivity on both the anode and cathode sides can be observed simultaneously, indicating that the stress-response film formation mechanisms on both sides can function in parallel. Comparing Example 10 with Comparative Example 12, in an engineered electrolyte system containing both composite lithium salt and conventional auxiliary film-forming agents, the introduction of piezoelectric particles can still improve cycle performance and interfacial impedance.
[0257] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A battery cell, characterized in that, It includes a positive electrode, a negative electrode, and an electrolyte. The negative electrode includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material and piezoelectric particles coexisting in the form of a separated phase. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the negative electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a first film-forming agent, wherein the highest reduction potential of the organic solvent is [missing value]. The reduction potential of the first film-forming agent is , .
2. The battery cell as described in claim 1, characterized in that, Includes at least one of the following features: (1) The negative electrode active material is a silicon-based material, and the first film-forming agent includes at least one of difluoromalononitrile and fluorobutadiene; (2) The piezoelectric particles in the negative electrode active layer account for 0.1~5.0 wt% of the total mass.
3. A single battery cell, characterized in that, It includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode includes a positive electrode current collector that coexists in the form of a separated phase and a positive electrode active layer disposed on the surface of the positive electrode current collector. The positive electrode active layer includes a positive electrode active material and piezoelectric particles. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the positive electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a second film-forming agent, wherein the lowest oxidation potential of the organic solvent is... The oxidation potential of the second film-forming agent is , .
4. The battery cell as described in claim 3, characterized in that, Includes at least one of the following features: (1) The positive electrode active material is a high-nickel ternary material, and the second film-forming agent includes at least one of tris(trimethylsilyl)borate and lithium difluorooxalate borate; (2) The piezoelectric particles in the positive electrode active layer account for 0.1~5.0 wt% of the total mass.
5. The battery cell according to any one of claims 1-4, characterized in that, Includes at least one of the following features: (1) The equivalent piezoelectric strain constant of the piezoelectric particles is 80~150 pC / N; (2) The median particle size D50 of the piezoelectric particles is 50 nm to 300 nm; (3) The piezoelectric material includes at least one of barium titanate and sodium bismuth titanate.
6. The battery cell according to any one of claims 1-4, characterized in that, Includes at least one of the following features: (1) The material of the ion-conducting layer includes at least one of lithium phosphate, lithium borate, lithium aluminate or LISICON-type solid electrolyte; (2) The ion-conducting layer includes an inner layer and an outer layer, wherein the inner layer includes lithium phosphate and the outer layer includes lithium fluoride and lithium carbonate; (3) The ionic conductivity of the ion-conducting layer at 25°C is 10. -8 S / cm~10 -7 S / cm; (4) The thickness of the ion-conducting layer is 2 nm to 10 nm.
7. A method for preparing a single battery cell, characterized in that, Includes the following steps: The positive electrode, negative electrode, separator, and casing are assembled into a battery cell; Electrolyte is injected into the battery cell to obtain a post-electrolyte-injected battery cell. The post-electrolyte-injected battery cell is then subjected to formation treatment to obtain a single battery cell. The negative electrode includes a negative electrode current collector and a negative electrode active layer disposed on the surface of the negative electrode current collector. The negative electrode active layer includes a negative electrode active material and piezoelectric particles coexisting in the form of a separated phase. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the negative electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a first film-forming agent, wherein the highest reduction potential of the organic solvent is [missing value]. The reduction potential of the first film-forming agent is , .
8. The method for preparing a single battery cell as described in claim 7, characterized in that, Includes at least one of the following features: (1) The content of the first film-forming agent in the electrolyte is 0.2~3 wt%; (2) The piezoelectric particles in the negative electrode active layer account for 0.1~5.0 wt% by mass. (3) The mass percentage of the first film-forming agent in the electrolyte is w1, and the mass percentage of the piezoelectric particles in the negative electrode active layer is M1, w1:M1=(0.3~5):
1.
9. The method for preparing a single battery cell as described in claim 7, characterized in that, The preparation steps of the negative electrode include: The lithium source and phosphorus source were mixed evenly at a molar ratio of Li:P = (2.7~3.3):1 to obtain the coating solution; The piezoelectric material is mixed with the coating liquid and stirred at 50-80°C for 2-6 hours to obtain a pre-coated product. The pre-coated product is heat-treated in an inert atmosphere at a temperature of 500-700°C to obtain the piezoelectric particles. A negative electrode current collector is provided, and a negative electrode active layer containing the piezoelectric particles and the negative electrode active material is disposed on the negative electrode current collector.
10. A method for preparing a single battery cell, characterized in that, Includes the following steps: The positive electrode, negative electrode, separator, and casing are assembled into a battery cell; Electrolyte is injected into the battery cell to obtain a post-electrolyte-injected battery cell. The post-electrolyte-injected battery cell is then subjected to formation treatment to obtain a single battery cell. The positive electrode includes a positive current collector and a positive active layer disposed on the surface of the positive current collector. The positive active layer includes a positive active material and piezoelectric particles coexisting in the form of a separated phase. The piezoelectric particles include a piezoelectric material and an ion-conducting layer coated on the surface of the piezoelectric material. In the positive electrode, the local potential disturbance generated by the piezoelectric particles under a stress of 100 MPa is on the order of... , =10~50 mV; The electrolyte comprises an organic solvent and a second film-forming agent, wherein the lowest oxidation potential of the organic solvent is... The oxidation potential of the second film-forming agent is , .
11. The method for preparing a single battery cell as described in claim 10, characterized in that, Includes at least one of the following features: (1) The content of the second film-forming agent in the electrolyte is w2, where w2 = 0.2~3 wt%; (2) The piezoelectric particles in the positive electrode active layer account for 0.1~5.0 wt% by mass. (3) The mass percentage of the second film-forming agent in the electrolyte is w2, and the mass percentage of the piezoelectric particles in the positive electrode active layer is M2, w2:M2=(0.3~5):
1.
12. The method for preparing a single battery cell as described in claim 10, characterized in that, The preparation steps of the positive electrode include: The lithium source and phosphorus source were mixed evenly at a molar ratio of Li:P = (2.7~3.3):1 to obtain the coating solution; The piezoelectric material is mixed with the coating liquid and stirred at 50-80°C for 2-6 hours to obtain a pre-coated product. The pre-coated product is heat-treated in an inert atmosphere at a temperature of 500-700°C to obtain the piezoelectric particles. A positive current collector is provided, and a positive active layer containing the piezoelectric particles and the positive active material is disposed on the positive current collector.
13. The method for preparing a battery cell as described in claim 9 or 12, characterized in that, Includes at least one of the following features: (1) The molar ratio of phosphorus in the phosphorus source to the piezoelectric material is (0.01~0.30):1; (2) The phosphorus source includes at least one of phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, lithium dihydrogen phosphate, triethyl phosphate, trimethyl phosphate, and phosphorus pentoxide; (3) The lithium source includes at least one of lithium acetate and lithium hydroxide.
14. A battery device, characterized in that, It includes the battery cell as described in any one of claims 1-6, or the battery cell prepared by the preparation method as described in any one of claims 7-13.
15. An energy storage device, characterized in that, Includes the battery device as described in claim 14.
16. An electrical appliance, characterized in that, It includes the battery device as described in claim 14, or the energy storage device as described in claim 15.