Solid-liquid batteries and their preparation methods

By designing a first electrolyte network and a second electrolyte network on the positive and negative electrodes of the battery, respectively, the contradiction between high-potential oxidation of the positive electrode and mechanical stability of the negative electrode is solved, thereby improving the safety and cycle performance of high-energy-density batteries and facilitating large-scale production.

CN123120834APending Publication Date: 2026-11-17WEIJIXIN ENERGY TECHNOLOGY (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611543623.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously meet the requirements of high-potential oxidation stability on the positive electrode side and mechanical stability on the negative electrode side, resulting in insufficient safety and cycle performance of batteries at high energy densities.

Method used

The solid-liquid battery structure is adopted, and a first electrolyte network and a second electrolyte network are formed on the positive electrode and the negative electrode, respectively. The first electrolyte network is formed by in-situ solidification of polymer monomers, and the second electrolyte network is a cross-linked polymer electrolyte, which respectively meet the different requirements of the positive electrode and the negative electrode, suppress side reactions and alleviate volume changes.

Benefits of technology

It improves battery safety and cycle performance, facilitates mass production through an independent electrolyte network process, and enhances cell stability and ionic conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120834A_ABST
    Figure CN123120834A_ABST
Patent Text Reader

Abstract

This invention provides a solid-liquid battery and its preparation method. The solid-liquid battery includes a positive electrode, a first electrolyte network, a negative electrode, a second electrolyte network, a separator, and a first electrolyte. The positive electrode includes a first current collector and a first coating on the surface of the first current collector; the first electrolyte network is located on the surface and within the pores of the first coating; the negative electrode includes a second current collector and a second coating on the surface of the second current collector; the second electrolyte network is located on the surface and within the pores of the second coating, and the material of the second electrolyte network includes a cross-linked polymer electrolyte; the separator is located between the positive and negative electrodes; the first electrolyte wets the positive electrode, the negative electrode, and the separator. The first and second electrolyte networks can significantly increase the lithium-ion transport channels while enhancing the stability of the electrode interface, thereby improving battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery manufacturing, and more particularly to a solid-liquid battery and its manufacturing method. Background Technology

[0002] High-energy-density full-cell systems impose extremely stringent and contradictory chemical and mechanical requirements on polymer electrolytes: the positive electrode side (such as high-nickel ternary and lithium-rich manganese-based electrodes) exhibits strong oxidative damage when charged to high potentials, requiring the electrolyte to have an extremely wide electrochemical stability window; while the negative electrode side (such as lithium metal and silicon-carbon negative electrodes) is accompanied by severe stress and volume changes during lithium insertion and extraction cycles, requiring the electrolyte to have excellent mechanical shear modulus and dimensional stability. Summary of the Invention

[0003] This invention provides a solid-liquid battery and its preparation method to meet different requirements for the positive and negative electrodes of the battery, thereby improving the battery's safety performance and cycle performance.

[0004] According to a first aspect of the present invention, a solid-liquid battery is provided, comprising: A positive electrode includes a first current collector and a first coating located on the surface of the first current collector; A first electrolyte network is located on the surface and within the pores of the first coating; The negative electrode includes a second current collector and a second coating located on the surface of the second current collector; A second electrolyte network is located on the surface and within the pores of the second coating, and the material of the second electrolyte network includes a cross-linked polymer electrolyte. A separator is located between the positive electrode and the negative electrode. The first electrolyte wets the positive electrode, the negative electrode, and the separator.

[0005] Optionally, the first electrolyte network is formed by in-situ curing of a first precursor solution, the first precursor solution comprising a polymer monomer, a first plasticizer, a first lithium salt, a high-boiling-point non-aqueous mixed solvent, and a first initiator.

[0006] Optionally, in the first precursor solution, the polymer monomer accounts for 1% to 50% by mass, the first plasticizer accounts for 0% to 70% by mass, the first lithium salt accounts for 10% to 35% by mass, the high-boiling-point non-aqueous mixed solvent accounts for 0% to 50% by mass, and the first initiator accounts for 0.1% to 3% by mass.

[0007] Optionally, the polymer monomer includes at least one selected from vinylene carbonate, vinyl ethylene carbonate, trimethylene carbonate, caprolactone, cyanoacrylate, acrylonitrile, isopropylene dimethyl benzyl isocyanate, 4-vinylphenyl isocyanate, isocyanoethyl methacrylate, and 4-cyanostyl styrene. The first plasticizer includes at least one of adiponitrile, succinic anhydride, butyrolactone, propylene carbonate, ethylene carbonate, vinylene carbonate, fluoroethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The first lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium bisfluorosulfonylimide, lithium perchlorate, lithium difluorooxalate borate, lithium difluorophosphate, lithium bisoxalate borate, and lithium tetrafluoroborate. The high-boiling-point non-aqueous mixed solvents include: Pyr14-FSI, PP13-TFSI, and EMIM-TFSI; The initiator includes at least one of a photoinitiator and a thermal initiator.

[0008] Optionally, the photoinitiator includes: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide; The thermal initiator includes: 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylpentanonitrile), 1,1'-azobis(cyclohexane-1-carbamate), dimethyl 2,2'-azobisisobutyrate, benzoyl peroxide, diisopropyl peroxide dicarbonate, dilauroyl peroxide, or di-tert-butyl peroxide.

[0009] Optionally, the second electrolyte network is formed by in-situ curing of a second precursor solution, the second precursor solution comprising a crosslinking center, a chain extender, a second plasticizer, a second initiator, and a second lithium salt.

[0010] Optionally, in the second precursor solution, the mass percentage of the crosslinking center is 1% to 30%, the mass percentage of the chain extender is 0% to 30%, the mass percentage of the second plasticizer is 40% to 95%, the mass percentage of the second initiator is 0.1% to 5%, and the mass percentage of the second lithium salt is 10% to 35%.

[0011] Optionally, the crosslinking center includes 2 to 8 first active groups, and the chain extender includes at least two second active groups. The first active groups and the second active groups are used to react under in-situ curing conditions to form the crosslinked polymer electrolyte.

[0012] Optionally, the first active group includes an epoxy ether or an isocyanate group, and the second active group includes a hydroxyl group or a lithium salt.

[0013] Optionally, the crosslinking center includes: isophorone diisocyanate, toluene diisocyanate, 2,6-TDI, dicyclohexylmethane-4,4'-diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate (HDI), HDI trimer, dimer diisocyanate, lysine diisocyanate, triphenylmethane-4,4',4''-triisocyanate, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, glycerol triglycidyl ether, dipentaerythritol hexaglycidyl ether, triglycidyl isocyanate, 4,4'-methylenebis(N,N-diglycidylaniline or octaglycidyl ether silsesquioxane); The chain extender includes at least one of the following: polypropylene glycol, polyethylene glycol (PEG, Mn<2000), polytetrahydrofuran glycol, polyglycerol, polycaprolactone diol, polyadipate polyester, polycarbonate diol, polybutadiene diol, dimer acid polyol, fluorinated polyol, silicon-containing polyol, small molecule diol, polyfunctional alcohol, lithium 2-ethylhexyl alcohol, lithium isodecanol, lithium n-octanol, and lithium polyethylene glycol.

[0014] Optionally, the second plasticizer includes at least one of polyether-based and carbonate-based plasticizers; The second initiator includes the first initiator and also includes: hydroxyl groups and NCO reaction catalyst; The second lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium bisfluorosulfonylimide, lithium perchlorate, lithium difluorooxalate borate, lithium difluorophosphate, lithium bisoxalate borate, and lithium tetrafluoroborate.

[0015] Optionally, the polyether fully etherified types include: polyethylene glycol dialkyl ether, polypropylene glycol dimethyl ether, ethylene oxide or propylene oxide copolyether dimethyl ether; The carbonates include chain carbonates and cyclic carbonates; The chain carbonates include: dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate; The cyclic carbonates include: ethylene carbonate, propylene carbonate, vinylene carbonate, or fluoroethylene carbonate.

[0016] Optionally, the first coating includes a positive electrode active material, a first conductive agent, a first solvent, and a first binder, and the second coating includes a negative electrode active material, a second conductive agent, a second solvent, and a second binder; The first electrolyte includes a third lithium salt, an organic solvent, and functional additives.

[0017] Optionally, it also includes: a cell housing for containing the first electrolyte and the bare cell, the bare cell including the positive electrode, the negative electrode and the separator assembled in a stacked or wound manner.

[0018] According to a second aspect of the present invention, a method for preparing a solid-liquid battery is provided, for preparing the above-mentioned solid-liquid battery, the method comprising: A positive electrode is prepared, the positive electrode comprising a first current collector, a first coating on the surface of the first current collector, and a first electrolyte network on the surface and within the pores of the first coating. A negative electrode is prepared, the negative electrode comprising a second current collector, a second coating on the surface of the second current collector, and a second electrolyte network on the surface and within the pores of the second coating, wherein the material of the second electrolyte network comprises a cross-linked polymer electrolyte. The positive electrode, the negative electrode, and the separator are assembled by stacking or winding to form a bare cell; A first electrolyte is injected into the bare battery cell.

[0019] Optionally, the preparation of the positive electrode sheet includes: preparing an initial positive electrode sheet, the initial positive electrode sheet including a first current collector and a first coating on the surface of the first current collector; preparing a first precursor solution, the first precursor solution including a polymer monomer, a first plasticizer, a first lithium salt, a high-boiling-point non-aqueous mixed solvent and a first initiator; applying the first precursor solution to the surface of the initial positive electrode sheet and performing in-situ curing treatment to form the positive electrode sheet; The preparation of the negative electrode sheet includes: preparing an initial negative electrode sheet, the initial negative electrode sheet including a second current collector and a second coating on the surface of the second current collector; preparing a second precursor solution, the second electrolyte network being formed by in-situ curing of the second precursor solution, the second precursor solution including a crosslinking center, a chain extender, a second plasticizer, a second initiator, and a second lithium salt; applying the second precursor solution to the surface of the initial negative electrode sheet and performing in-situ curing treatment to form the negative electrode sheet.

[0020] Optionally, the application method includes spraying, dipping, or roller coating.

[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: In the solid-liquid battery provided by the technical solution of this invention, firstly, since the first electrolyte network is only located on the surface and within the pores of the first coating, the formulation only needs to meet the electrochemical stability requirements at high potentials, and the electrochemical side reactions of the positive electrode can be significantly reduced. The first electrolyte network can encapsulate the positive electrode active particles within the first coating to suppress the dissolution of transition metal ions, and also has a certain inhibitory effect on the oxygen release of the positive electrode material at high temperatures. Secondly, since the second electrolyte network is only located on the surface and within the pores of the second coating, by selectively choosing a formulation with better stability for the negative electrode, the side reactions of the negative electrode can be significantly reduced. The polymer system with a cross-linked structure has a stronger binding force on small molecules, and a small amount of polymer can form a structurally stable gel, ensuring high ionic conductivity while preventing the migration of small molecules from the negative electrode to the positive electrode, thus preventing additional side reactions. On this basis, since the second electrolyte network encapsulates the negative electrode active particles, and the cross-linked structure has a certain rigidity, the second electrolyte network can alleviate the breathing effect of the negative electrode material during charging and discharging to a certain extent, thereby slowing down the electrolyte consumption caused by the continuous formation of new interfaces and enhancing the cycle performance of the cell. Furthermore, the cross-linked structure is microscopically more like a network, and the mesh can effectively immobilize small lithium-conducting molecules; a small amount of polymerization can create a gel electrolyte. From the above, it can be seen that different first and second electrolyte networks can meet the different requirements of the battery's positive and negative electrodes, thereby improving battery safety and cycle performance.

[0022] Furthermore, since the formation of the first electrolyte network and the second electrolyte network only requires two core processes after rolling and pressing—precursor solution wetting and polymerization initiation—and these two processes are independent of each other, it is easy to achieve large-scale production. Attached Figure Description

[0023] Figure 1 This is a flowchart of the solid-liquid battery preparation method provided in the embodiments of the present invention; Figure 2 This is a reaction pathway diagram within the second precursor solution provided in an embodiment of the present invention. Detailed Implementation

[0024] As described in the background section, the requirements for polymer electrolytes are different for the positive and negative electrodes of a battery.

[0025] In view of this, the present invention creatively proposes a solid-liquid battery, comprising: A positive electrode includes a first current collector and a first coating located on the surface of the first current collector; A first electrolyte network is located on the surface and within the pores of the first coating; The negative electrode includes a second current collector and a second coating located on the surface of the second current collector; A second electrolyte network is located on the surface and within the pores of the second coating, and the material of the second electrolyte network includes a cross-linked polymer electrolyte. A separator is located between the positive electrode and the negative electrode. The first electrolyte wets the positive electrode, the negative electrode, and the separator.

[0026] The first electrolyte network can suppress side reactions between the first electrolyte and the positive electrode active particles, and the second electrolyte network, through the elastic confinement of the three-dimensional cross-linked polymer network, can alleviate the huge volume effect of the negative electrode during charging and discharging, thereby improving the cycle performance of high-energy-density batteries. By using different first and second electrolyte networks, different requirements for the positive and negative electrodes of the battery can be met, thereby improving the battery's safety and cycle performance.

[0027] The embodiments of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. The terms "first," "second," "third," etc., in the specification, claims, and accompanying drawings are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the present invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0028] Please refer to Figure 1 This invention provides a method for preparing a solid-liquid battery, comprising: S1, Prepare a positive electrode sheet, the positive electrode sheet comprising a first current collector, a first coating on the surface of the first current collector, and a first electrolyte network on the surface and within the pores of the first coating; S2, Prepare a negative electrode sheet, which includes a second current collector, a second coating on the surface of the second current collector, and a second electrolyte network located on the surface and within the pores of the second coating. The material of the second electrolyte network includes a cross-linked polymer electrolyte. After the precursor is introduced into the electrode sheet, in-situ polymerization is performed by heating and maintaining a temperature of 45-85°C for 1-24 hours. S3, positive electrode, negative electrode and separator assembled by stacking or winding to form bare cell; S4, inject the first electrolyte into the bare cell.

[0029] The following provides a detailed explanation of each step in the preparation method of the solid-liquid battery described above.

[0030] In some embodiments, for S1, the method for preparing the positive electrode includes: S11, Prepare an initial positive electrode sheet, the initial positive electrode sheet including a first current collector and a first coating on the surface of the first current collector; S12, prepare a first precursor solution, the first precursor solution comprising a polymer monomer, a first plasticizer, a first lithium salt, a high-boiling-point non-aqueous mixed solvent, and a first initiator; S13, the first precursor solution is introduced onto the surface of the initial positive electrode sheet, and in-situ curing and die-cutting are performed sequentially to form the positive electrode sheet.

[0031] In some embodiments, S11, the method for preparing the initial positive electrode sheet includes: S111, the positive electrode active material, the first conductive agent and the first binder are added to the first solvent and uniformly dispersed to form the first slurry; S112, the first slurry is coated onto the first current collector and then dried and rolled in sequence to obtain the initial positive electrode sheet.

[0032] In other embodiments, the precursor solution may be introduced into the coating surface and pores before die cutting, polymerized in situ, and then die-cut into an electrode sheet. This invention does not limit this process.

[0033] In some embodiments, the positive electrode active material may be, for example, lithium nickel cobalt manganese oxide or lithium nickel cobalt aluminum oxide, including, high-nickel ternary active materials, etc.

[0034] In some embodiments, the first conductive agent may be at least one of superconducting carbon black, Ketjen black, carbon nanotubes, and graphene.

[0035] In some embodiments, the first adhesive may be, for example, polyvinylidene fluoride.

[0036] In some embodiments, the first solvent may be, for example, N,N-dimethylpyrrolidone solvent.

[0037] As an example, the first current collector could be an aluminum foil current collector.

[0038] In some embodiments, in S12, the first precursor solution contains a polymer monomer mass percentage of 1% to 50%, a first plasticizer mass percentage of 0% to 70%, a first lithium salt mass percentage of 10% to 35%, a high-boiling-point non-aqueous mixed solvent mass percentage of 0% to 50%, and a first initiator mass percentage of 0.1% to 3%.

[0039] In some embodiments, the polymer monomer includes at least one selected from vinylene carbonate (VC), vinyl ethylene carbonate (VEC), trimethylene carbonate (TMC), caprolactone (CL), cyanoacrylate (ECA), acrylonitrile (AN), isopropenyl dimethyl benzyl isocyanate (TMI), 4-vinylphenyl isocyanate (VPI), ethyl isocyanate methacrylate (MOI), and 4-cyanostyl styrene.

[0040] In some embodiments, the first plasticizer includes at least one of adiponitrile (ADN), succinate (SN), butyrolactone (GBL), propylene carbonate (PC), ethylene carbonate (EC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC).

[0041] In some embodiments, the first lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO4), lithium difluorooxalate borate (LiDFOB), lithium difluorophosphate (LiPO2F2), lithium bis(oxalate borate) (LiBOB), and lithium tetrafluoroborate (LiBF4).

[0042] As an example, the concentration range of the first lithium salt is 0.8M to 1.5M.

[0043] In some embodiments, the high-boiling-point non-aqueous mixed solvents include: Pyr14-FSI, PP13-TFSI, and EMIM-TFSI.

[0044] In some embodiments, the initiator includes at least one of a photoinitiator and a thermal initiator. Specifically, the photoinitiator includes 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO) or phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO); the thermal initiator includes 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylpentanonitrile), 1,1'-azobis(cyclohexane-1-carbamate), dimethyl 2,2'-azobisisobutyrate, benzoyl peroxide (BPO), diisopropyl peroxide dicarbonate (IPP), dilauroyl peroxide (LPO), or di-tert-butyl peroxide (DTBP).

[0045] In some embodiments, in S13, after the first precursor solution is introduced into the interior of the first coating, it is heated and kept at a constant temperature for in-situ polymerization. The holding temperature is 45°C - 85°C, and the time is 1 h - 24 h.

[0046] In some embodiments, for S2, the method for preparing the negative electrode sheet includes: S21, Prepare an initial negative electrode sheet, the initial negative electrode sheet including a second current collector and a second coating located on the surface of the second current collector; S22, prepare a second precursor solution, the second electrolyte network is formed by in-situ solidification of the second precursor solution, the second precursor solution includes a crosslinking center, a chain extender, a second plasticizer, a second initiator and a second lithium salt; S23, the second precursor solution is introduced onto the surface of the initial negative electrode sheet and in-situ solidification is performed to form the negative electrode sheet.

[0047] In some embodiments, in S21, the method for preparing the initial negative electrode sheet includes: S121, The negative electrode active material, the second conductive agent and the second binder are added to the second solvent and uniformly dispersed to form the second slurry; S122, the second slurry is applied to the second current collector and then dried and rolled in sequence to obtain the initial negative electrode roll, which is then die-cut to obtain the negative electrode sheet.

[0048] In other embodiments, the precursor solution may be introduced directly onto the coating surface in the electrode coil state and polymerized in situ; this invention does not limit this.

[0049] In some embodiments, the negative electrode active material comprises silicon with a content greater than 5%.

[0050] In some embodiments, the second conductive agent may include at least one of Super P, Ketjen Black (KB), and carbon nanotubes (CNT / SCNT).

[0051] In some embodiments, the second adhesive may include a mixture of sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), and styrene-butadiene rubber (SBR).

[0052] In some embodiments, the second solvent may include deionized water.

[0053] As an example, the second current collector includes a copper foil current collector.

[0054] In some embodiments, in S22, the mass percentage of the crosslinking center in the second precursor solution is 1% to 30%, the mass percentage of the chain extender is 0% to 30%, the mass percentage of the second plasticizer is 40% to 95%, the mass percentage of the second initiator is 0.1% to 5%, and the mass percentage of the second lithium salt is 10% to 35%.

[0055] In some embodiments, the crosslinking center includes: isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), 2,6-TDI, dicyclohexylmethane-4,4'-diisocyanate (4,4'-MDI), 1,5-naphthalene diisocyanate (NDI), hexamethylene diisocyanate (HDI), HDI trimer, dimer diisocyanate (DDI), lysine diisocyanate (LDI), triphenylmethane-4,4',4''-triisocyanate (TTI), trimethylolpropane triglycidyl ether (TMPTGE), pentaerythritol tetraglycidyl ether (PETGE), glycerol triglycidyl ether, dipentaerythritol hexaglycidyl ether (DPEPE), triglycidyl isocyanate (TGIC), 4,4'-methylenebis(N,N-diglycidylaniline) (TGDDM), or octaglycidyl ether silsesquioxane.

[0056] In some embodiments, the chain extender includes at least one of polypropylene glycol (PPG), polyethylene glycol (PEG, Mn<2000), polytetrahydrofuran glycol (PTMEG), polyglycerol, polycaprolactone diol (PCL), polyadipate polyester (PBA), polycarbonate diol (PCDL), polybutadiene diol (HTPB), dimer acid polyol, fluorinated polyol, silicon-containing polyol (such as polydimethylsiloxane diol), small molecule diol (such as 1,4-butanediol (BDO), 1,6-hexanediol (HDO), neopentyl glycol (NPG)), polyfunctional alcohol (such as trimethylolpropane (TMP), pentaerythritol, sorbitol), lithium 2-ethylhexyl alcohol, lithium isodecanol, lithium n-octyl alcohol, or lithium polyethylene glycol (PEG-Li).

[0057] Specifically, the crosslinking center includes 2 to 8 first active groups, and the chain extender includes at least two second active groups. The first and second active groups react under in-situ curing conditions to form a crosslinked polymer electrolyte. Please refer to [reference needed]. Figure 2 The left side of the arrow represents the reactants, where the wavy line structure represents a chain extender with two second active groups, and the dashed trident structure represents a crosslinking center with three first active groups. The right side of the arrow represents the reaction products, which represent a three-dimensional crosslinked polymer network.

[0058] The advantages of cross-linked structures are: 1. Cross-linked structures can absorb more small molecules. A small amount of polymerization can fix the lithium-conducting small molecules of the negative electrode in the cross-linked network to form a gel, thereby reducing the difference in ionic conductivity between the gel and the electrolyte; 2. Cross-linked structures are rigid. After wrapping the high-silicon negative electrode, they can suppress the expansion of silicon to a certain extent. At the same time, the active material is equivalent to being wrapped by an elastic giant net to prevent macroscopic peeling or pulverization of the active material and maintain the spatial integrity of the three-dimensional conductive / lithium-conducting network; 3. They are not prone to deformation under high temperature conditions.

[0059] As an example, the first active group includes an epoxy ether or an isocyanate group, and the second active group includes a hydroxyl group.

[0060] In some embodiments, the second plasticizer includes at least one of polyether-based and carbonate-based plasticizers. Specifically, polyether-based plasticizers include polyethylene glycol dialkyl ethers (including dimethyl ether (PEGDME), diethyl ether, dibutyl ether), polypropylene glycol dimethyl ether, or ethylene oxide / propylene oxide copolyether dimethyl ether; carbonate-based plasticizers include chain carbonates and cyclic carbonates, with chain carbonates including dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl ethyl carbonate (EMC); and cyclic carbonates including ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), and fluoroethylene carbonate (FEC).

[0061] In some embodiments, in addition to conventional photoinitiators and thermal initiators, the second initiator further includes a hydroxyl and NCO reaction catalyst; the hydroxyl and NCO reaction catalyst may include at least one of the following: bis(2-dimethylaminoethyl) ether, N,N,N'-trimethyl-N'-hydroxyethyl bisaminoethyl ether, dimethylaminopropylamine, N,N'-dimethylethanolamine, bis(3-dimethylaminopropyl)aminoisopropanol, tetramethyldipropylenetriamine, pentamethyldiethylenetriamine, triethylenediamine, 3,3'-iminobis(N,N-dimethylpropylamine), dibutyltin dilaurate, stannous octoate, di(2-ethylhexanoate), bismuth neodecanoate, bismuth octoate, zinc neodecanoate, zinc octoate, and zinc acetylacetonate.

[0062] In some embodiments, the second lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO4), lithium difluorooxalate borate (LiDFOB), lithium difluorophosphate (LiPO2F2), lithium bis(oxalate borate) (LiBOB), and lithium tetrafluoroborate (LiBF4).

[0063] In some embodiments, in S13 and S23, the introduction of the first precursor solution and the second precursor solution may include spraying, dipping, or roller coating. Furthermore, since the first coating has a porous structure, the first precursor solution can enter the internal pores of the first coating through capillary action, thus completely wetting the electrode. This allows the first electrolyte network subsequently formed through in-situ curing to fill the pores between the positive electrode active particles. Similarly, the second electrolyte network subsequently formed through in-situ curing can fill the pores between the negative electrode active particles.

[0064] In some embodiments, for S13 and S23, in the in-situ curing process, depending on the types of the first initiator and the second initiator, the initiation polymerization process can be photo-initiated first and then thermally initiated, thermally initiated first and then photo-initiated, or photo-initiated or thermally initiated separately.

[0065] Specifically, photoinitiation refers to irradiating the positive / negative electrode with ultraviolet light or visible light of a specific wavelength, causing the photoinitiator to generate active free radicals, which initiates the cross-linking and curing of the polymer monomers. Thermal initiation refers to heating and maintaining the positive / negative electrode to induce the thermal polymerization and curing of the polymer monomers.

[0066] The first electrolyte network includes a chain-structured electrolyte compatible with high potentials, which suppresses the dissolution of transition metal ions from the positive electrode active particles, improving both battery performance and safety. The second electrolyte network includes a cross-linked electrolyte compatible with low potentials and volume changes. The second electrolyte network, through its mechanical elasticity, alleviates the significant volume effect of the negative electrode during charging and discharging, solving the problem of macroscopic delamination of active material particles. Specifically, the three-dimensional cross-linked polymer electrolyte network exhibits high dimensional stability, including: First, through in-situ addition polymerization, the cross-linked polymer electrolyte uses strong covalent bonds to firmly bind countless polymer backbones together laterally and longitudinally, giving the three-dimensional network extremely high mechanical shear modulus and macroscopic deformation memory elasticity. It can rigidly confine silicon-based particles within in-situ porous channels like an 'elastic bandage' or a 'highly elastic rubber spring,' allowing the network to withstand enormous macroscopic tension without irreversible molecular chain misalignment or slippage when the battery is in a fully charged, expanded state. During the discharge contraction state, the network can utilize its spontaneously generated strong elastic recovery force to 'pull back' the negative electrode active material in situ and tightly clamp it, thereby maintaining the mechanical continuity and integrity of the electron transport channel during the long-term operation of the entire electrode sheet. Secondly, the three-dimensional cross-linking nodes can not only moderately absorb electrolyte solvent to construct nanoscale efficient lithium conduction channels, but also achieve 'insoluble and infusible' behavior under high polarity solvents and charge / discharge heating environments. This controlled gel network acts like a dense protective layer, forming a comprehensive, tight, and non-flowing confined coating of the negative electrode active particles deep within the electrode sheet.

[0067] In some embodiments, in S23, after the second precursor solution is introduced into the interior of the second coating, it is heated and kept at a constant temperature for in-situ polymerization. The holding temperature is 45°C - 85°C, and the time is 1 h - 24 h.

[0068] In other embodiments, the initial positive / negative electrode sheet can be cured in situ before being rolled.

[0069] In some embodiments, between S3 and S4, the preparation method further includes: S5, Die-cut the positive and negative electrode sheets according to the preset dimensions; S6, which assembles the positive electrode, negative electrode and separator by stacking or winding to form a bare cell; S7, Place the bare battery cell into the battery cell casing and dry it at high temperature; In some embodiments, in S4, the first electrolyte includes a third lithium salt, an organic solvent, and a functional additive. As an example, the third lithium salt may include at least one of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium tetrafluoroborate (LiBF4), and lithium bis(oxalate borate) (LiBOB); the organic solvent may include carbonate solvents; and the functional additive may include film-forming additives, etc.

[0070] Furthermore, after S4, processes such as settling, aging, degassing / second sealing, capacity testing, and shaping are required to obtain high-energy-density lithium-ion batteries.

[0071] This invention also provides a solid-liquid battery, obtained using the above-described preparation method. The solid-liquid battery includes: a positive electrode, a first electrolyte network, a negative electrode, a second electrolyte network, a separator, and a first electrolyte.

[0072] In some embodiments, the positive electrode includes a first current collector and a first coating on the surface of the first current collector, and a first electrolyte network located on the surface and within the pores of the first coating. The negative electrode includes a second current collector and a second coating on the surface of the second current collector, and a second electrolyte network located on the surface and within the pores of the second coating. The material of the second electrolyte network includes a cross-linked polymer electrolyte. A separator is located between the positive electrode and the negative electrode. A first electrolyte wets the positive electrode, the negative electrode, and the separator.

[0073] In some embodiments, the first electrolyte network is formed by in-situ curing of a first precursor solution, the first precursor solution comprising a polymer monomer, a first plasticizer, a first lithium salt, a high-boiling-point non-aqueous mixed solvent, and a first initiator.

[0074] In some embodiments, in the first precursor solution, the mass percentage of polymer monomer is 1% to 50%, the mass percentage of the first plasticizer is 0% to 70%, the mass percentage of the first lithium salt is 10% to 35%, the mass percentage of the high-boiling-point non-aqueous mixed solvent is 0% to 50%, and the mass percentage of the first initiator is 0.1% to 3%.

[0075] In some embodiments, the polymer monomer includes at least one selected from vinylene carbonate (VC), vinyl ethylene carbonate (VEC), trimethylene carbonate (TMC), caprolactone (CL), cyanoacrylate (ECA), acrylonitrile (AN), isopropenyl dimethyl benzyl isocyanate (TMI), 4-vinylphenyl isocyanate (VPI), ethyl isocyanate methacrylate (MOI), and 4-cyanostyl styrene.

[0076] In some embodiments, the first plasticizer includes at least one of adiponitrile (ADN), succinate (SN), butyrolactone (GBL), propylene carbonate (PC), ethylene carbonate (EC), vinylene carbonate (VEC), fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC).

[0077] In some embodiments, the first lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium perchlorate (LiClO4), lithium difluorooxalate borate (LiDFOB), lithium difluorophosphate (LiPO2F2), lithium bis(oxalate borate) (LiBOB), and lithium tetrafluoroborate (LiBF4).

[0078] In some embodiments, the high-boiling-point non-aqueous mixed solvents include: Pyr14-FSI, PP13-TFSI, and EMIM-TFSI.

[0079] In some embodiments, the first initiator includes at least one of a photoinitiator and a thermal initiator. Specifically, the photoinitiator includes 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO) or phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO); the thermal initiator includes 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylpentanonitrile), 1,1'-azobis(cyclohexane-1-carbamate), dimethyl 2,2'-azobisisobutyrate, benzoyl peroxide (BPO), diisopropyl peroxide dicarbonate (IPP), dilauroyl peroxide (LPO), or di-tert-butyl peroxide (DTBP).

[0080] In some embodiments, the second electrolyte network is formed by in-situ curing of a second precursor solution, the second precursor solution comprising a crosslinking center, a chain extender, a second plasticizer, a second initiator, and a second lithium salt.

[0081] In some embodiments, in the second precursor solution, the mass percentage of the crosslinking center is 1% to 30%, the mass percentage of the chain extender is 0% to 30%, the mass percentage of the second plasticizer is 40% to 95%, the mass percentage of the second initiator is 0.1% to 5%, and the mass percentage of the second lithium salt is 10% to 35%.

[0082] In some embodiments, the crosslinking center includes: isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), 2,6-TDI, dicyclohexylmethane-4,4'-diisocyanate (4,4'-MDI), 1,5-naphthalene diisocyanate (NDI), hexamethylene diisocyanate (HDI), HDI trimer, dimer diisocyanate (DDI), lysine diisocyanate (LDI), triphenylmethane-4,4',4''-triisocyanate (TTI), trimethylolpropane triglycidyl ether (TMPTGE), pentaerythritol tetraglycidyl ether (PETGE), glycerol triglycidyl ether, dipentaerythritol hexaglycidyl ether (DPEPE), triglycidyl isocyanate (TGIC), 4,4'-methylenebis(N,N-diglycidylaniline) (TGDDM), or octaglycidyl ether silsesquioxane.

[0083] In some embodiments, the chain extender includes at least one of polypropylene glycol (PPG), polyethylene glycol (PEG, Mn<2000), polytetrahydrofuran glycol (PTMEG), polyglycerol, polycaprolactone diol (PCL), polyadipate polyester (PBA), polycarbonate diol (PCDL), polybutadiene diol (HTPB), dimer acid polyol, fluorinated polyol, silicon-containing polyol (such as polydimethylsiloxane diol), small molecule diol (such as 1,4-butanediol (BDO), 1,6-hexanediol (HDO), neopentyl glycol (NPG)), polyfunctional alcohol (such as trimethylolpropane (TMP), pentaerythritol, sorbitol), lithium 2-ethylhexyl alcohol, lithium isodecanol, lithium n-octyl alcohol, or lithium polyethylene glycol (PEG-Li).

[0084] In some embodiments, the crosslinking center includes 2 to 8 first active groups, and the chain extender includes at least two second active groups. The first and second active groups are used to react under in-situ curing conditions to form a three-dimensional crosslinked polymer network.

[0085] As an example, the first active group includes an epoxy ether or an isocyanate group, and the second active group includes a hydroxyl group.

[0086] In some embodiments, the second plasticizer comprises at least one of polyether-based and carbonate-based plasticizers. The polyether-based plasticizers include polyethylene glycol dialkyl ethers (including dimethyl ether (PEGDME), diethyl ether, dibutyl ether), polypropylene glycol dimethyl ether, or ethylene oxide / propylene oxide copolyether dimethyl ether; the carbonate-based plasticizers include chain carbonates and cyclic carbonates. Chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC); cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), vinylene carbonate (VC), and fluoroethylene carbonate (FEC).

[0087] In some embodiments, the second initiator comprises a hydroxyl and NCO reaction catalyst; wherein the hydroxyl and NCO reaction catalyst comprises at least one of the following: bis(2-dimethylaminoethyl) ether, N,N,N'-trimethyl-N'-hydroxyethyl bis(aminoethyl) ether, dimethylaminopropylamine, N,N'-dimethylethanolamine, bis(3-dimethylaminopropyl)aminoisopropanol, tetramethyldipropylenetriamine, pentamethyldiethylenetriamine, triethylenediamine, 3,3'-iminobis(N,N-dimethylpropylamine), dibutyltin dilaurate, stannous octoate, di(2-ethylhexanoate)tin, bismuth neodecanoate, bismuth octoate, zinc neodecanoate, zinc octoate, and zinc acetylacetonate. The second photoinitiator catalyzes the nucleophilic addition reaction between isocyanate groups and hydroxyl groups, accelerating the formation of urethane bonds and achieving stepwise polymerization and curing of polyurethane.

[0088] In some embodiments, the second lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium bisfluorosulfonylimide, lithium perchlorate, lithium difluorooxalate borate, lithium difluorophosphate, lithium bisoxalate borate, and lithium tetrafluoroborate.

[0089] As an example, the concentration range of the second lithium salt is 0.8M to 1.5M.

[0090] In some embodiments, the diaphragm may be a polypropylene (PP), polyethylene (PE), or a composite layer material of polypropylene (PP) and polyethylene (PE) (PP / PE / PP).

[0091] In some embodiments, the solid-liquid battery further includes: a cell housing for containing a first electrolyte and a bare cell, the bare cell including a positive electrode, a negative electrode, and a separator assembled in a stacked or wound manner.

[0092] The battery cell housing can be, for example, a soft-pack housing, a square hard housing, or a cylindrical hard housing. Of course, any battery cell housing that can be used to accommodate the bare battery cell and the first electrolyte is within the scope of protection of this invention.

[0093] To enable those skilled in the art to more clearly understand the above-described implementation details and operations of the present invention, and to demonstrate the significant improvement in the performance of the positive electrode sheet and its preparation method in the embodiments of the present invention, the following examples illustrate the above implementation schemes.

[0094] Example 1

[0095] A method for preparing a solid-liquid battery is as follows: Step 1: The high-nickel positive electrode active material (N811), conductive agent (CNT / Super-P) and binder (PVDF) are fully and uniformly dispersed in NN-dimethylpyrrolidone solvent at a weight ratio of N811:CNT / Super-P:PVDF=97%:1.0% / 0.5%:1.5% to obtain the positive electrode slurry. Step 2: The positive electrode slurry is coated onto an aluminum foil current collector with a thickness of 12μm, and then dried, rolled, and die-cut in sequence to obtain the positive electrode sheet; Step 3: Prepare a first precursor solution, which includes VEC, SN, Pyr14-FSI, AIBN, and LiTFSI, wherein the mass percentage of VEC is 22.17%, the mass percentage of SN is 44.35%, the mass percentage of Pyr14-FSI is 7.39%, the mass percentage of LiTFSI is 25.45%, and the mass percentage of AIBN is 0.67%. Step 4: After the first precursor solution is rolled onto the surface of the positive electrode, wait for 20 seconds until the first precursor solution is immersed in the positive electrode and then perform a heating and heat preservation treatment (heating temperature is 60 degrees Celsius, heating time is 6 hours) to initiate the thermal polymerization and solidification of the monomers to form the first electrolyte network. Step 5: The negative electrode active material, conductive agent (acetylene black Super-P), and binder (sodium carboxymethyl cellulose CMC / polyacrylic acid PAA / styrene-butadiene rubber SBR) are fully and uniformly dispersed in deionized water according to the mass ratio of silicon-doped negative electrode: Super-P:CMC / PAA / SBR=96.0%:2.0%:1.5% / 0.5% / 1.5% to obtain the negative electrode slurry. Step 6: The negative electrode slurry is coated onto a copper foil current collector with a thickness of 8μm, and then dried, rolled, and die-cut in sequence to obtain the negative electrode sheet; Step 7: Prepare a second precursor solution, which includes PETGE, PEG-Li(300), diethylene glycol dimethyl ether, and LiTFSI, wherein PETGE accounts for 1.35% by mass, PEG-Li(300) accounts for 2.33% by mass, diethylene glycol dimethyl ether accounts for 69.92% by mass, and LiTFSI accounts for 26.40% by mass. Step 8: After introducing the second precursor solution onto the surface of the negative electrode, wait 20-30 seconds until the second precursor solution penetrates into the negative electrode. Then, perform a heating and heat preservation treatment (heating temperature is 60 degrees Celsius, heating time is 5 hours) to form the second electrolyte network. Step 9: The positive electrode, negative electrode and PE separator are assembled by Z-process stacking to obtain bare cell. Then the bare cell is placed in an aluminum-plastic film soft package that is punched according to the bare cell specifications and sealed and then dried at high temperature and vacuum. Step 11: Inject the first electrolyte into the dry bare cell, and then proceed through processes such as settling, aging, degassing / second sealing, capacity testing, and shaping to obtain a high-energy-density lithium-ion solid-liquid battery.

[0096] Example 2

[0097] The difference between Example 2 and Example 1 lies in the composition of the second precursor solution and the polymerization conditions. In Example 2, the second precursor solution includes HDI trimer, PEG (300), diethylene glycol dimethyl ether, dibutyltin dilaurate, and LiTFSI. The mass percentages of HDI trimer, PEG (300), and LiTFSI are as follows: 5.86%, 5.23%, 62.85%, 25.93%, and 0.18%. Furthermore, the heating temperature in steps 4 and 8 of Example 1 is changed to 70°C, and the heating time is changed to 18 hours.

[0098] Example 3

[0099] The difference between Example 3 and Example 1 is that the composition ratio of the second precursor solution is different. The composition ratio of the second precursor solution in Example 3 is as follows: PETGE 2.69% by mass, PEG-Li(300) 4.67% by mass, diethylene glycol dimethyl ether 66.24% by mass, and LiTFSI 26.40% by mass.

[0100] Example 4

[0101] The difference between Example 4 and Example 2 is that the composition ratio of the second precursor solution is different. The composition ratio of the second precursor solution in Example 4 is as follows: HDI trimer 11.70% by mass, PEG (300) 10.44% by mass, diethylene glycol dimethyl ether 51.66% by mass, LiTFSI 25.84% by mass, and dibutyltin dilaurate 0.35% by mass.

[0102] Comparative Example Comparative Example 1 uses a non-aqueous electrolyte suitable for high-nickel positive and silicon-containing negative electrode systems and a conventional liquid soft-pack battery cell production process. Neither the positive nor negative electrode sheets undergoes in-situ polymerization at the electrode layer level (corresponding to steps 3, 4, 7 and 8 in Example 1). The battery cell is directly injected with the non-aqueous electrolyte after assembly.

[0103] Based on Comparative Example 1, Comparative Example 2 uses the first precursor solution from Example 1 as the precursor electrolyte for the entire battery cell. That is, after the positive electrode, separator and negative electrode are assembled, the first precursor solution is injected into the battery cell and in-situ polymerization is carried out at the battery cell level.

[0104] Based on Comparative Example 1, Comparative Example 3 uses the second precursor solution of Example 1 as the precursor electrolyte for the entire battery cell. That is, after the positive electrode, separator and negative electrode are assembled, the second precursor solution is injected into the battery cell and in-situ polymerization is carried out at the battery cell level.

[0105] Based on Comparative Example 1, Comparative Example 4 uses the second precursor solution of Example 2 as the precursor electrolyte for the entire battery cell. That is, after the positive electrode, separator and negative electrode are assembled, the second precursor solution in Example 2 is injected into the battery cell and in-situ polymerization is carried out at the battery cell level.

[0106] Comparative Example 5 had the same treatment process and precursor solution composition as Example 1, but the composition ratio of the second precursor solution was changed as follows: 8.08% by mass of PETGE, 14.00% by mass of PEG-Li(300), 51.52% by mass of diethylene glycol dimethyl ether, and 26.40% by mass of LiTFSI.

[0107] Comparative Example 6 and Example 2 had the same treatment process and precursor solution composition, but the composition ratio of the second precursor solution was changed as follows: HDI trimer mass percentage 19.46%, PEG(300) mass percentage 17.36%, diethylene glycol dimethyl ether mass percentage 36.82%, LiTFSI mass percentage 25.78%, and dibutyltin dilaurate mass percentage 0.58%.

[0108] To illustrate the advancements of the solid-liquid batteries prepared in the embodiments of this application, the applicant conducted performance tests on the lithium-ion batteries in Examples 1-4 and Comparative Examples 1-6.

[0109] The formation capacity, first charge / discharge capacity, first charge / discharge efficiency, and cell internal resistance of the example and comparative cells were evaluated under the same test conditions. The test results are shown in Table 1.

[0110] Table 1. Cell performance test results

[0111] According to Table 1, comparing the test data of Examples 1-4 with Comparative Example 1, it can be seen that the cell internal resistance and first charge / discharge efficiency of the batteries prepared in Examples 1-4 are not significantly different from those of the batteries prepared in Comparative Example 1. Comparing the test data of Examples 1-4 with Comparative Examples 2-4, it can be seen that compared with the batteries prepared in Examples 1-4, the batteries formed by injecting the first precursor solution or the second precursor solution into the cell and then performing in-situ polymerization at the cell level exhibit increased cell internal resistance and decreased first charge / discharge efficiency, i.e., a significant decrease in performance. Comparing the test data of Examples 1-4 with Comparative Examples 5-6, it can be seen that when the mass ratio of polymer monomers in the first precursor solution or crosslinking centers in the second precursor solution is too high, it will lead to increased cell internal resistance and reduced capacity utilization of the battery.

[0112] Using the discharge capacity measured at a discharge rate of 0.33C for the batteries in Examples 1-4 and Comparative Examples 1-6 as a benchmark, discharge tests were conducted at discharge rates of 0.5C, 1.0C, and 2.0C, respectively. The test results are shown in Table 2.

[0113] Table 2. Performance Test Results by Rate Multiplier

[0114] According to Table 2, comparing the test results of Examples 1-4 with Comparative Example 1, it can be seen that the rate performance of the batteries prepared in Examples 1-4 is similar to that of the batteries prepared in Comparative Example 1. Comparing the test results of Examples 1-4 with Comparative Examples 5-6, it can be seen that when the mass proportion of polymer monomers in the first precursor solution or crosslinking centers in the second precursor solution is too high, the rate performance of the battery cell is significantly reduced. Comparing the test data of Examples 1-4 with Comparative Examples 2-4, it can be seen that compared with the batteries prepared in Examples 1-4, the rate performance of the batteries formed by injecting the first precursor solution or the second precursor solution into the battery cell and then performing in-situ polymerization at the battery cell level decreases.

[0115] The batteries in Examples 1-4 and Comparative Examples 1-6 were subjected to 200 charge-discharge cycles at a rate of 0.33C under normal temperature and pressure. The test results are shown in Table 2.

[0116] Table 3 Cyclic performance test results

[0117] According to Table 3, comparing the test results of Examples 1-4 with Comparative Example 1, it can be seen that the 200% full capacity retention rate of the batteries prepared in Examples 1-4 is higher than that of the batteries prepared in Comparative Example 1. Comparing the test results of Examples 1-4 with Comparative Examples 2-4, it can be seen that the cell cycle performance of the batteries formed by injecting the first precursor solution or the second precursor solution into the cell and then performing in-situ polymerization at the cell level is significantly reduced. Comparing the test results of Examples 1-4 with Comparative Examples 5-6, it can be seen that compared with the batteries in Examples 1-4, when the mass ratio of polymer monomers in the first precursor solution or crosslinking centers in the second precursor solution is too high, in-situ polymerization at the electrode level does not help improve the cell cycle performance.

[0118] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A solid-liquid battery, characterized in that, include: A positive electrode includes a first current collector and a first coating located on the surface of the first current collector; A first electrolyte network is located on the surface and within the pores of the first coating; The negative electrode includes a second current collector and a second coating located on the surface of the second current collector; A second electrolyte network is located on the surface and within the pores of the second coating, and the material of the second electrolyte network includes a cross-linked polymer electrolyte. A separator is located between the positive electrode and the negative electrode. The first electrolyte wets the positive electrode, the negative electrode, and the separator.

2. The solid-liquid battery according to claim 1, characterized in that, The first electrolyte network is formed by in-situ solidification of a first precursor solution, the first precursor solution comprising a polymer monomer, a first plasticizer, a first lithium salt, a high-boiling-point non-aqueous mixed solvent, and a first initiator.

3. The solid-liquid battery according to claim 2, characterized in that, In the first precursor solution, the polymer monomer accounts for 1% to 50% by mass, the first plasticizer accounts for 0% to 70% by mass, the first lithium salt accounts for 10% to 35% by mass, the high-boiling-point non-aqueous mixed solvent accounts for 0% to 50% by mass, and the first initiator accounts for 0.1% to 3% by mass.

4. The solid-liquid battery according to claim 2, characterized in that, The polymer monomers include at least one of vinylene carbonate, vinyl ethylene carbonate, trimethylene carbonate, caprolactone, cyanoacrylate, acrylonitrile, isopropylene dimethyl benzyl isocyanate, 4-vinylphenyl isocyanate, isocyanoethyl methacrylate, and 4-cyanostylstyrene. The first plasticizer includes at least one of adiponitrile, succinic anhydride, butyrolactone, propylene carbonate, ethylene carbonate, vinylene carbonate, fluoroethylene carbonate, dimethyl carbonate, and ethyl methyl carbonate. The first lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium bisfluorosulfonylimide, lithium perchlorate, lithium difluorooxalate borate, lithium difluorophosphate, lithium bisoxalate borate, and lithium tetrafluoroborate. The high-boiling-point non-aqueous mixed solvents include: Pyr14-FSI, PP13-TFSI, and EMIM-TFSI; The first initiator includes at least one of a photoinitiator and a thermal initiator.

5. The solid-liquid battery according to claim 4, characterized in that, The photoinitiator includes: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide; The thermal initiator includes: 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylpentanonitrile), 1,1'-azobis(cyclohexane-1-carbamate), dimethyl 2,2'-azobisisobutyrate, benzoyl peroxide, diisopropyl peroxide dicarbonate, dilauroyl peroxide, or di-tert-butyl peroxide.

6. The solid-liquid battery according to claim 1, characterized in that, The second electrolyte network is formed by in-situ solidification of a second precursor solution, the second precursor solution comprising a crosslinking center, a chain extender, a second plasticizer, a second initiator, and a second lithium salt.

7. The solid-liquid battery according to claim 6, characterized in that, In the second precursor solution, the mass percentage of the crosslinking center is 1% to 30%, the mass percentage of the chain extender is 0% to 30%, the mass percentage of the second plasticizer is 40% to 95%, the mass percentage of the second initiator is 0.1% to 5%, and the mass percentage of the second lithium salt is 10% to 35%.

8. The solid-liquid battery according to claim 6, characterized in that, The crosslinking center includes 2 to 8 first active groups, and the chain extender includes at least two second active groups. The first active groups and the second active groups are used to react under in-situ curing conditions to form the crosslinked polymer electrolyte.

9. The solid-liquid battery according to claim 8, characterized in that, The first active group includes an epoxy ether or an isocyanate group, and the second active group includes a hydroxyl group.

10. The solid-liquid battery according to claim 5, characterized in that, The crosslinking centers include: isophorone diisocyanate, toluene diisocyanate, 2,6-TDI, dicyclohexylmethane-4,4'-diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate (HDI), HDI trimer, dimer diisocyanate, lysine diisocyanate, triphenylmethane-4,4',4''-triisocyanate, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, glycerol triglycidyl ether, dipentaerythritol hexaglycidyl ether, triglycidyl isocyanate, 4,4'-methylenebis(N,N-diglycidylaniline or octaglycidyl ether silsesquioxane); The chain extender includes at least one of the following: polypropylene glycol, polyethylene glycol (PEG, Mn<2000), polytetrahydrofuran glycol, polyglycerol, polycaprolactone diol, polyadipate polyester, polycarbonate diol, polybutadiene diol, dimer acid polyol, fluorinated polyol, silicon-containing polyol, small molecule diol, polyfunctional alcohol, lithium 2-ethylhexyl alcohol, lithium isodecanol, lithium n-octanol, and lithium polyethylene glycol.

11. The solid-liquid battery according to claim 6, characterized in that, The second plasticizer includes at least one of polyether-based and carbonate-based plasticizers; The second initiator includes the first initiator, and also includes: a hydroxyl group and an NCO reaction catalyst; The second lithium salt includes at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium hexafluorophosphate, lithium bisfluorosulfonylimide, lithium perchlorate, lithium difluorooxalate borate, lithium difluorophosphate, lithium bisoxalate borate, and lithium tetrafluoroborate.

12. The solid-liquid battery according to claim 11, characterized in that, The polyether fully etherified types include: polyethylene glycol dialkyl ether, polypropylene glycol dimethyl ether, ethylene oxide or propylene oxide copolyether dimethyl ether; The carbonates include chain carbonates and cyclic carbonates; The chain carbonates include: dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate; The cyclic carbonates include: ethylene carbonate, propylene carbonate, vinylene carbonate, or fluoroethylene carbonate.

13. The solid-liquid battery according to claim 1, characterized in that, The first coating comprises a positive electrode active material, a first conductive agent, a first solvent, and a first binder; the second coating comprises a negative electrode active material, a second conductive agent, a second solvent, and a second binder. The first electrolyte includes a third lithium salt, an organic solvent, and functional additives.

14. The solid-liquid battery according to claim 1, characterized in that, Also includes: A cell housing for containing the first electrolyte and the bare cell, wherein the bare cell includes the positive electrode, the negative electrode, and the separator assembled in a stacked or wound manner.

15. A method for preparing a solid-liquid battery, characterized in that, A method for preparing a solid-liquid battery as described in any one of claims 1 to 14, comprising: A positive electrode is prepared, the positive electrode comprising a first current collector, a first coating on the surface of the first current collector, and a first electrolyte network on the surface and within the pores of the first coating. A negative electrode is prepared, the negative electrode comprising a second current collector, a second coating on the surface of the second current collector, and a second electrolyte network on the surface and within the pores of the second coating, wherein the material of the second electrolyte network comprises a cross-linked polymer electrolyte. The positive electrode, the negative electrode, and the separator are assembled by stacking or winding to form a bare cell; A first electrolyte is injected into the bare battery cell.

16. The method for preparing a solid-liquid battery according to claim 15, characterized in that, The preparation of the positive electrode sheet includes: preparing an initial positive electrode sheet, the initial positive electrode sheet including a first current collector and a first coating on the surface of the first current collector; preparing a first precursor solution, the first precursor solution including a polymer monomer, a first plasticizer, a first lithium salt, a high-boiling-point non-aqueous mixed solvent and a first initiator; introducing the first precursor solution onto the surface of the initial positive electrode sheet and performing in-situ curing treatment to form the positive electrode sheet; The preparation of the negative electrode sheet includes: preparing an initial negative electrode sheet, the initial negative electrode sheet including a second current collector and a second coating on the surface of the second current collector; preparing a second precursor solution, the second electrolyte network being formed by in-situ curing of the second precursor solution, the second precursor solution including a crosslinking center, a chain extender, a second plasticizer, a second initiator, and a second lithium salt; introducing the second precursor solution onto the surface of the initial negative electrode sheet and performing in-situ curing treatment to form the negative electrode sheet.

17. The method for preparing a solid-liquid battery according to claim 16, characterized in that, The methods for introducing the first precursor solution and the second precursor solution include spraying, dipping, or roller coating.