An electrolyte and a lithium-ion battery

By adding acid anhydride compounds and compounds containing sulfate ester structures to the electrolyte, the performance degradation problem caused by volume change at high temperatures in lithium cobalt oxide/silicon-carbon lithium-ion batteries was solved, and the high-temperature cycle performance and storage stability were improved.

CN123120868APending Publication Date: 2026-11-17KUNSHAN SYNERGY SCIENTECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611285838.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium cobalt oxide/silicon-carbon lithium-ion batteries suffer from capacity decay and shortened cycle life under high-temperature conditions due to the large volume change of the silicon-carbon anode. The SEI film formed by existing additives such as vinylene carbonate has high impedance and is difficult to meet the requirements for high-temperature stability.

Method used

An electrolyte without vinylene carbonate is used, and acid anhydride compounds and compounds containing sulfate ester structures are added, specifically succinic anhydride and mannitol carbonate sulfate, to synergistically improve the stability of the negative electrode interface, reduce the interface impedance, and inhibit the volume expansion of the silicon-carbon negative electrode and the shedding of active materials.

Benefits of technology

It significantly improves the cycle capacity retention and storage stability of lithium-ion batteries under high temperature conditions, avoids the high interface impedance problem caused by vinylene carbonate, and enhances the high temperature performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses an electrolyte and a lithium-ion battery. The electrolyte contains a non-aqueous solvent, a lithium salt, an acid anhydride compound, and a compound containing a sulfate ester structure. By adding an acid anhydride compound and a compound containing a sulfate ester structure to the electrolyte, the stability of the negative electrode interface is synergistically improved, high-temperature cycling volume expansion is suppressed, high-temperature cycling capacity retention and high-temperature storage stability are improved, and the high interfacial impedance problem caused by vinylene carbonate is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an electrolyte and a lithium-ion battery, belonging to the field of battery electrolyte technology. Background Technology

[0002] In lithium cobalt oxide / silicon-carbon lithium-ion batteries, the silicon-carbon anode undergoes significant volume changes during charge and discharge, leading to expansion of the anode active material. This expansion causes silicon particles to crack and pulverize, the SEI film to repeatedly rupture and regenerate, and the active material to detach, ultimately resulting in battery capacity decay and shortened cycle life. These problems are more pronounced at high temperatures, resulting in poor high-temperature cycle performance and high-temperature storage performance of lithium cobalt oxide / silicon-carbon batteries.

[0003] To address the aforementioned issues, vinylene carbonate is often added to the electrolyte as a film-forming additive. Vinylene carbonate can be reduced to form an SEI film on the negative electrode surface, improving high-temperature cycling and storage performance to some extent. However, the SEI film formed by vinylene carbonate has high impedance and its improvement effect on high-temperature cycling performance is limited, making it difficult to meet the high-temperature stability requirements of silicon-carbon negative electrode batteries. How to reduce the amount of vinylene carbonate used and further improve the high-temperature performance of lithium cobalt oxide / silicon-carbon batteries remains a problem that needs to be solved in this field. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide an electrolyte and lithium-ion battery that solves the problem of insufficient high-temperature cycle performance and high-temperature storage performance when using vinylene carbonate alone in existing lithium cobalt oxide / silicon-carbon system lithium-ion batteries.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0006] In a first aspect, the present invention provides an electrolyte comprising a non-aqueous solvent, a lithium salt, an acid anhydride compound, and a compound containing a sulfate ester structure, wherein the electrolyte does not contain vinylene carbonate.

[0007] In conjunction with the first aspect, further, the mass percentage of acid anhydride compounds in the electrolyte does not exceed 2.5%.

[0008] Furthermore, the anhydride compound is selected from at least one of succinic anhydride, 2-sulfobenzoic anhydride, butenoic anhydride, biphenyl anhydride, nadic anhydride, acrylic anhydride, and acetic propionic anhydride.

[0009] Furthermore, the acid anhydride compound is succinic anhydride.

[0010] Furthermore, the electrolyte contains no more than 5.5% by mass of compounds with a sulfate ester structure.

[0011] Furthermore, the compound containing the sulfate ester structure is selected from at least one of vinyl sulfate, sodium lauryl sulfate, erythritol disulfate, pentaerythritol disulfate, and mannitol carbonate sulfate.

[0012] Furthermore, the compound containing the sulfate ester structure is mannitol sulfate carbonate.

[0013] Furthermore, the electrolyte also contains fluoroethylene carbonate, with the fluoroethylene carbonate content being 10% to 15% by mass based on the total mass of the electrolyte.

[0014] In a second aspect, the present invention provides a lithium-ion battery comprising a positive electrode, a negative electrode, and an electrolyte as described in any one of the first aspects, wherein the positive electrode comprises lithium cobalt oxide; and the negative electrode comprises graphite and silicon-carbon materials, wherein the silicon-carbon materials account for 10% of the total mass of the graphite and silicon-carbon materials.

[0015] In conjunction with the second aspect, further, the anhydride compound in the electrolyte is succinic anhydride, and the compound containing a sulfate ester structure is mannitol carbonate sulfate; the expansion rate of the negative electrode plate in a fully charged state after 500 cycles at 45°C satisfies the following relationship: 1.1 < (15a + 1.6)b < 85, where a and b are the mass percentage values ​​of succinic anhydride and mannitol carbonate sulfate in the electrolyte, respectively.

[0016] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:

[0017] This invention provides an electrolyte and a lithium-ion battery. By adding a specific combination of acid anhydride compounds and compounds containing sulfate ester structures to the electrolyte, the stability of the negative electrode interface is synergistically improved, the interfacial impedance is reduced, and the volume expansion and active material shedding of the silicon-carbon negative electrode during high-temperature cycling are suppressed, thereby improving the high-temperature cycle capacity retention and high-temperature storage stability of the lithium-ion battery. At the same time, the electrolyte of this invention can achieve the above-mentioned high-temperature performance without adding vinylene carbonate, avoiding the high interfacial impedance problem caused by vinylene carbonate. Detailed Implementation

[0018] This invention provides an electrolyte and a lithium-ion battery. All raw materials used are commercially available, and their purity meets conventional standards in the field of lithium-ion battery electrolytes. The following examples are only used to more clearly illustrate the technical solution of this invention and should not be construed as limiting the scope of protection of this invention.

[0019] In all embodiments of the present invention, the preparation methods of the positive electrode, negative electrode, separator, and battery are the same, as detailed below:

[0020] Positive electrode preparation: Lithium cobalt oxide (positive electrode active material), carbon black (conductive agent), polyvinylidene fluoride (PVC) (binder), and carbon nanotubes were mixed in a mass ratio of 98:0.5:1.1:0.4 to obtain a mixture. This mixture was then added to N-methylpyrrolidone solvent, ensuring it comprised 30% of the total slurry mass (i.e., a solid content of 30%), and thoroughly stirred to form a uniform positive electrode slurry. The positive electrode slurry was coated onto a 10 μm thick aluminum foil current collector and dried. The double-sided density of the positive electrode was 30 mg / cm³. 2 The compacted density after roller pressing is 4.15 g / cm³. 3 This yields the positive electrode sheet.

[0021] Negative electrode preparation: The negative electrode active materials graphite, silicon carbide, binder styrene-butadiene rubber, polyacrylic acid, thickener lithium carboxymethyl cellulose, and carbon nanotubes were weighed out in a mass ratio of 86.85:9.65:1.5:1.5:0.25:0.25, respectively. These were added to an appropriate amount of deionized water and thoroughly mixed to form a uniform negative electrode slurry. The negative electrode slurry was coated onto an 8μm thick copper foil current collector and dried. The negative electrode areal density was 123.6 mg / cm³. 2 The compacted density after roller pressing is 1.60 g / cm³. 3 This yields the negative electrode.

[0022] Separator: A polyethylene separator with a thickness of 9μm is selected, and the surface coating contains aluminum oxide.

[0023] Battery preparation: The positive electrode, negative electrode and separator are wound and assembled into a cell. The bare cell is placed in the outer packaging shell, dried and injected with electrolyte. Then, vacuum sealing, standing, formation, shaping and capacity testing are carried out in sequence to obtain a soft-pack lithium-ion battery.

[0024] The electrolyte preparation methods of each embodiment and comparative example are as follows. In the embodiments, additive T1 is an acid anhydride compound, preferably succinic anhydride, and additive T2 is a compound containing a sulfate ester structure, preferably mannitol carbonate sulfate.

[0025] In this invention, additive T1 is not limited to succinic anhydride, but may also be selected from at least one of 2-sulfobenzoic anhydride, butenoic anhydride, biphenyl anhydride, nadic anhydride, acrylic anhydride, and acetic propionic anhydride; additive T2 is not limited to mannitol sulfate, but may also be selected from at least one of vinyl sulfate, sodium lauryl sulfate, erythritol disulfide, and pentaerythritol disulfide. The mass percentage of additive T1 does not exceed 2.5%, the mass percentage of additive T2 does not exceed 5.5%, and the mass percentage of fluorovinyl carbonate can be adjusted within the range of 10% to 15%.

[0026] The basic electrolyte is prepared as follows: In a glove box filled with argon gas and where the water and oxygen content are both below 0.01 ppm, ethylene carbonate, propylene carbonate, ethyl propionate, and propyl propionate are mixed in a mass ratio of 2:0.5:4.5:3, wherein ethyl propionate accounts for 60% of the total mass of carboxylic acid esters; lithium hexafluorophosphate with a mass percentage of 12.5% ​​and fluoroethylene carbonate with a mass percentage of 13% are added and mixed evenly to obtain the basic electrolyte.

[0027] In the following examples and comparative examples, unless otherwise stated, the amounts of each component are mass percentages based on the total mass of the final electrolyte.

[0028] Example 1:

[0029] Additive T1 (0.33% by mass) and additive T2 (0.33% by mass) were added to the above-mentioned basic electrolyte and mixed evenly to obtain an electrolyte. The above electrolyte was injected into a battery to obtain the lithium-ion battery of Example 1.

[0030] Example 2:

[0031] Additive T1 at a mass percentage of 0.5% and additive T2 at a mass percentage of 0.33% were added to the above-mentioned basic electrolyte, and the mixture was stirred evenly to obtain an electrolyte. The above electrolyte was injected into a battery to obtain the lithium-ion battery of Example 2.

[0032] Example 3:

[0033] Additive T1 (0.5% by mass) and additive T2 (0.5% by mass) were added to the above-mentioned basic electrolyte and mixed thoroughly to obtain an electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Example 3.

[0034] Example 4:

[0035] Additive T1 at a mass percentage of 0.8% and additive T2 at a mass percentage of 0.5% were added to the above-mentioned basic electrolyte, and the mixture was stirred evenly to obtain an electrolyte. The above electrolyte was injected into a battery to obtain the lithium-ion battery of Example 4.

[0036] Example 5:

[0037] Additive T1 (0.8% by mass) and additive T2 (0.8% by mass) were added to the above-mentioned basic electrolyte and mixed thoroughly to obtain an electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Example 5.

[0038] Example 6:

[0039] Additive T1 at a mass percentage of 1.2% and additive T2 at a mass percentage of 0.8% were added to the above-mentioned basic electrolyte, and the mixture was stirred evenly to obtain an electrolyte. The above electrolyte was injected into a battery to obtain the lithium-ion battery of Example 6.

[0040] Example 7:

[0041] Additive T1 (1.2% by mass) and additive T2 (1.2% by mass) were added to the above-mentioned basic electrolyte and mixed thoroughly to obtain an electrolyte. The above electrolyte was injected into a battery to obtain the lithium-ion battery of Example 7.

[0042] Example 8:

[0043] Additive T1 (1.5% by mass) and additive T2 (1.5% by mass) were added to the above-mentioned basic electrolyte and mixed thoroughly to obtain an electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Example 8.

[0044] Example 9:

[0045] Additive T1 (1.8% by mass) and additive T2 (1.8% by mass) were added to the above-mentioned basic electrolyte and mixed thoroughly to obtain an electrolyte. The above electrolyte was injected into a battery to obtain the lithium-ion battery of Example 9.

[0046] Example 10:

[0047] Additive T1 (2.0% by mass) and additive T2 (2.0% by mass) were added to the above-mentioned basic electrolyte and mixed thoroughly to obtain an electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Example 10.

[0048] Comparative Example 1:

[0049] In a glove box filled with argon and with water and oxygen content both below 0.01 ppm, ethylene carbonate, propylene carbonate, ethyl propionate, and propyl propionate were mixed in a mass ratio of ethylene carbonate:propylene carbonate:(ethyl propionate and propyl propionate) = 2:0.5:7.5, wherein ethyl propionate accounted for 60% of the total mass of carboxylic acid esters; lithium hexafluorophosphate (12.5% ​​by mass) and fluoroethylene carbonate (13% by mass) were added.

[0050] The above electrolyte raw materials were mixed without the addition of additives T1 and T2, and the mixture was stirred evenly to obtain an electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Comparative Example 1.

[0051] Comparative Example 2:

[0052] Additive T2 at a mass percentage of 0.33% was added to the above-mentioned basic electrolyte, while additive T1 was not added. The mixture was then thoroughly mixed to obtain the electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Comparative Example 2.

[0053] Comparative Example 3:

[0054] Additive T1 at a mass percentage of 0.33% was added to the above-mentioned basic electrolyte, while additive T2 was not added. The mixture was then thoroughly mixed to obtain the electrolyte. The electrolyte was then injected into a battery to obtain the lithium-ion battery of Comparative Example 3.

[0055] The lithium-ion batteries prepared in the above embodiments and comparative examples were subjected to the following performance tests:

[0056] High-temperature cycle performance test: Each battery was placed in a 45℃ constant temperature chamber and charged and discharged at a 3C rate and a 0.7C rate for charge-discharge cycle test. The voltage range was 3~4.55V. The capacity retention rate was recorded after 500 cycles.

[0057] High-temperature storage performance test: Each battery was stored at 85°C for 6 hours, and the change in battery thickness before and after storage was tested. A thickness change rate of ≤15% was considered acceptable.

[0058] Negative electrode expansion rate test: After the battery is fully charged after 500 cycles, the percentage increase in the thickness of the negative electrode relative to the initial thickness is measured, which is the negative electrode expansion rate.

[0059] The test results are shown in Table 1 below. In the table, a and b are the mass percentage values ​​of succinic anhydride and mannitol carbonate sulfate in the electrolyte, respectively.

[0060] Table 1:

[0061]

[0062] Based on the test results above, the batteries in Examples 1-10 are significantly superior to those in Comparative Examples 1-3 in terms of high-temperature cycle capacity retention, negative electrode expansion rate, and high-temperature storage performance. The synergistic use of anhydride compounds (succinic anhydride) and compounds containing sulfate ester structures (mannitol carbonate sulfate) can more effectively improve the high-temperature cycle performance and high-temperature storage stability of lithium-ion batteries in the lithium cobalt oxide / silicon-carbon system, without the use of vinylene carbonate. The overall battery performance is even better when the relationship 1.1 < (15a + 1.6)b < 85 is satisfied.

[0063] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. An electrolyte, characterized in that, The electrolyte contains non-aqueous solvents, lithium salts, acid anhydride compounds, and compounds containing sulfuric acid ester structures, but does not contain vinylene carbonate.

2. The electrolyte according to claim 1, characterized in that, The electrolyte contains anhydride compounds at a mass percentage not exceeding 2.5%.

3. The electrolyte according to claim 1, characterized in that, The anhydride compound is selected from at least one of succinic anhydride, 2-sulfobenzoic anhydride, butenoic anhydride, biphenyl anhydride, nadic anhydride, acrylic anhydride, and acetic propionic anhydride.

4. The electrolyte according to claim 3, characterized in that, The acid anhydride compound is succinic anhydride.

5. The electrolyte according to claim 1, characterized in that, The electrolyte contains compounds with a sulfate ester structure at a mass percentage not exceeding 5.5%.

6. The electrolyte according to claim 1, characterized in that, The compound containing a sulfate ester structure is selected from at least one of vinyl sulfate, sodium lauryl sulfate, erythritol disulfate, pentaerythritol disulfate, and mannitol carbonate sulfate.

7. The electrolyte according to claim 6, characterized in that, The compound containing the sulfate ester structure is mannitol sulfate carbonate.

8. The electrolyte according to claim 1, characterized in that, The electrolyte also contains fluoroethylene carbonate, wherein the fluoroethylene carbonate has a mass percentage of 10% to 15%.

9. A lithium-ion battery, characterized in that, The device includes a positive electrode, a negative electrode, and an electrolyte according to any one of claims 1-8, wherein the positive electrode comprises lithium cobalt oxide; and the negative electrode comprises graphite and silicon-carbon materials, wherein the silicon-carbon materials account for 10% of the total mass of the graphite and silicon-carbon materials.

10. The lithium-ion battery according to claim 9, characterized in that, The anhydride compound in the electrolyte is succinic anhydride, and the compound containing the sulfate ester structure is mannitol carbonate sulfate. The expansion rate of the negative electrode plate when it is fully charged after 500 cycles at 45°C satisfies the following relationship: 1.1 < (15a + 1.6)b < 85, where a and b are the mass percentage values ​​of succinic anhydride and mannitol carbonate sulfate, respectively.