An electrolyte and its application method, and a battery
By combining single-electrode and double-electrode solutions and controlling the mass content of cyclic sulfate compounds and vinylene carbonate, high-efficiency SEI and CEI films are formed, solving the problems of battery fast-charging performance and cycle life, and achieving an overall improvement in battery performance.
Patent Information
- Application Number
- CN202611425463.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, when vinylene carbonate is used in combination with cyclic sulfate compounds, antagonistic effects are easily generated, resulting in poor fast-charging performance and cycle life of the battery.
A combination of one-electrode and two-electrode solutions is adopted. The one-electrode solution contains cyclic sulfate ester compounds, and the two-electrode solution contains vinylene carbonate. By adjusting the mass content of each electrolyte, a high ionic conductivity and low impedance SEI membrane rich in inorganic sulfate compounds is formed, which also enhances the protective ability of the CEI membrane.
The battery achieves both good fast-charging performance and long cycle life. By optimizing the combination and ratio of electrolyte components, the overall performance of the battery has been improved.
Smart Images

Figure SMS_48 
Figure QLYQS_1 
Figure QLYQS_2
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, specifically to an electrolyte and its usage method, and a battery. Background Technology
[0002] Although the film-forming additive vinylene carbonate (VC) can form a solid electrolyte membrane (SEI membrane) on the negative electrode surface, it is difficult to effectively improve the battery's cycle performance and fast charging performance at the same time. Summary of the Invention
[0003] The purpose of this application is to overcome the shortcomings of the existing technology and provide an electrolyte and its usage method, as well as a battery. The electrolyte combines a primary electrolyte containing cyclic sulfate compounds with a secondary electrolyte containing vinylene carbonate, and regulates the mass content of cyclic sulfate compounds in the primary electrolyte and the mass content of vinylene carbonate in the secondary electrolyte, so that the battery has both good fast charging performance and long cycle life.
[0004] To achieve the above objectives, in a first aspect, this application provides an electrolyte, comprising a primary electrolyte and a secondary electrolyte; The electrolyte solution comprises cyclic sulfate compounds and vinylene carbonate, wherein the mass ratio of vinylene carbonate to cyclic sulfate compounds is ≤0.5; The mass content of cyclic sulfate compounds in the electrolyte is 0.2% to 5%; The second electrolyte solution includes vinylene carbonate; The mass content of vinylene carbonate in the second electrolyte is 5%~20%; The cyclic sulfate compounds include at least one of the compounds shown in Formula I; ; In Formula I, R1, R2, R3 and R4 are each independently selected from any one of the following groups as shown in Formula II: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group. ; In Formula II, R5 and R6 are each independently selected from any one of the following groups as shown in Formula III: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group. ; In Formula III, R7 and R8 are each independently selected from any one of the following: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group.
[0005] Secondly, this application provides a method for using the above-mentioned electrolyte, including the following steps: injecting the battery with a first injection of electrolyte, performing formation on the battery, injecting the battery with a second injection of electrolyte, aging the battery, and encapsulating it.
[0006] Thirdly, this application provides a battery including the electrolyte described above.
[0007] The beneficial effects of this application are as follows: This application provides an electrolyte that combines a primary electrolyte containing cyclic sulfate compounds with a secondary electrolyte containing vinylene carbonate, and regulates the mass content of the cyclic sulfate compounds in the primary electrolyte and the mass content of vinylene carbonate in the secondary electrolyte, so that the battery has both good fast charging performance and long cycle life. Detailed Implementation
[0008] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0009] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.
[0010] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.
[0011] The present application is further illustrated below with specific embodiments: This application provides an electrolyte, including a first electrolyte injection and a second electrolyte injection; The electrolyte solution comprises cyclic sulfate compounds and vinylene carbonate, wherein the mass ratio of vinylene carbonate to cyclic sulfate compounds is ≤0.5; The mass content of cyclic sulfate compounds in the electrolyte is 0.2% to 5%; The second electrolyte solution includes vinylene carbonate; The mass content of vinylene carbonate in the second electrolyte is 5%~20%; The cyclic sulfate compounds include at least one of the compounds shown in Formula I; ; In Formula I, R1, R2, R3 and R4 are each independently selected from any one of the following groups as shown in Formula II: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group. ; In Formula II, R5 and R6 are each independently selected from any one of the following groups as shown in Formula III: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group. ; In Formula III, R7 and R8 are each independently selected from any one of the following: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group.
[0012] During the application process, the inventors discovered that when vinylene carbonate and vinyl disulfate are used directly in combination, they produce an antagonistic effect. The impedance of the resulting SEI film is significantly greater than that of the SEI film formed when vinylene carbonate or vinyl disulfate is used alone, resulting in poor fast-charging performance and cycle life of the battery. This application combines a primary electrolyte containing cyclic sulfate compounds with a secondary electrolyte containing vinylene carbonate, and controls the mass content of cyclic sulfate compounds in the primary electrolyte and the mass content of vinylene carbonate in the secondary electrolyte, so that the battery has both good fast-charging performance and long cycle life.
[0013] Cyclic sulfate compounds in the first electrolyte are used to first form a high ionic conductivity and low impedance SEI film rich in inorganic sulfate compounds at the negative electrode. However, cyclic sulfate compounds have poor protective ability against the CEI film at the positive electrode. If vinylene carbonate in the second electrolyte is used to further enhance the protective ability of the CEI film, then the negative electrode has already formed an SEI film with good ionic conductivity. Vinylene carbonate basically does not participate or participates little in the formation of the SEI film and does not increase the impedance of the SEI film. Vinylene carbonate mainly participates in the formation of the CEI film, which can effectively inhibit the dissolution of transition metals at the positive electrode, thus enabling the battery to have both good fast charging performance and long cycle life.
[0014] In some embodiments, the mass content of the cyclic sulfate compound in the electrolyte is any one or any two of the following values: 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, and 5%.
[0015] More preferably, the mass content of cyclic sulfate compounds in the electrolyte is 0.5% to 1.5%.
[0016] It should be noted that, in this application, the mass content of cyclic sulfate compounds in the electrolyte solution can be confirmed by, but is not limited to, the following methods: The electrolyte solution of the sample to be tested was injected into an Agilent Intuvo 9000 gas chromatograph-mass spectrometer using a microsyringe to obtain GC-MS chromatograms. A standard solution of a certain concentration was prepared by dissolving cyclic sulfate compounds in EMC solvent, and the mass percentage of cyclic sulfate compounds in the standard solution was recorded as w%. The electrolyte solution to be tested and the standard solution were then injected into the Agilent Intuvo 9000 gas chromatograph-mass spectrometer to obtain standard GC-MS chromatograms. The GC-MS spectrum of the electrolyte to be tested was compared with the standard GC-MS spectrum to confirm whether the corresponding components were present (the matching degree between the standard curve and the electrolyte sample curve was ≥98%). The electrolyte sample to be tested and the standard solution were subjected to GC testing to obtain the peak area X1 of the cyclic sulfate ester compound in the GC test spectrum of the sample to be tested and the peak area X2 of the cyclic sulfate ester compound in the GC test spectrum of the standard solution. The mass content of the cyclic sulfate ester compound in one batch of electrolyte was calculated according to the following formula: S=(X1 / X2) ×w.
[0017] In some embodiments, the mass content of vinylene carbonate in the two electrolyte solutions is a range of any one or both of 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%.
[0018] More preferably, the mass content of vinylene carbonate in the second electrolyte is 10%~18%.
[0019] It should be noted that, in this application, the mass content of vinylene carbonate in the two electrolyte solutions can be confirmed by, but is not limited to, the following methods: The electrolyte solution of the sample to be tested was injected into an Agilent Intuvo 9000 gas chromatograph-mass spectrometer using a microsyringe to obtain a GC-MS chromatogram. A standard solution of a certain concentration was prepared by dissolving vinylene carbonate in EMC solvent, and the mass percentage of vinylene carbonate in the standard solution was recorded as m%. The electrolyte solution to be tested and the standard solution were then injected into the Agilent Intuvo 9000 gas chromatograph-mass spectrometer to obtain standard GC-MS chromatograms. The GC-MS spectrum of the electrolyte to be tested was compared with the standard GC-MS spectrum to confirm whether the corresponding component was present (the matching degree between the standard curve and the electrolyte sample curve was ≥98%). The electrolyte sample to be tested and the standard solution were subjected to GC testing to obtain the peak area Y1 of vinylene carbonate in the GC test spectrum of the sample to be tested and the peak area Y2 of vinylene carbonate in the GC test spectrum of the standard solution. The mass percentage of vinylene carbonate in the two electrolytes was calculated according to the following formula: S2=(Y1 / Y2)×m.
[0020] In some embodiments, Formula I contains 2 to 4 sulfate groups.
[0021] In some embodiments, Formula I contains two, three, or four sulfate groups.
[0022] In this application, the number of sulfate groups in Formula I is related to the film-forming performance of the negative electrode. The more sulfate groups there are, the greater the steric hindrance and the greater the impedance of the battery. When Formula I contains 2 to 4 sulfate groups, it can better balance the fast charging performance and cycle life of the battery.
[0023] In some embodiments, at least one of R1, R2, R3, and R4 is a hydrogen atom.
[0024] In this application, when at least one of R1, R2, R3, and R4 is a hydrogen atom, it is beneficial to reduce the steric hindrance of the compound shown in Formula I, thereby better promoting its participation in the formation of the protective film at the positive and negative electrode interface and alleviating the side reactions between the electrolyte and the positive and negative electrodes, thereby improving the cycle life of the battery.
[0025] In some implementations, R1 and R3 are the same.
[0026] In this application, when R1 and R3 are the same, it is beneficial to improve the structural symmetry of the compound shown in Formula I, so that the formed SEI film is more complete and further enhances the protection capability of the negative electrode.
[0027] In some embodiments, R1 and R3 are selected from any one of the following groups as shown in Formula II, hydrogen atoms, alkyl groups of 1 to 6 carbon atoms, halogen atoms, haloalkyl groups of 1 to 3 carbon atoms, alkoxy groups of 1 to 3 carbon atoms, haloalkoxy groups of 1 to 3 carbon atoms, alkenyl groups of 2 to 6 carbon atoms, alkynyl groups of 2 to 6 carbon atoms, aromatic groups, ester groups, cyano groups, and sulfonic acid groups.
[0028] In this application, when R1 and R3 are selected from the above-mentioned groups, it can better reduce the film-forming resistance while promoting the formation of a protective film at the positive and negative electrode interface, and can also alleviate the side reactions between the electrolyte and the positive and negative electrodes, thereby better improving the cycle life of the battery.
[0029] In some embodiments, the cyclic sulfate compound includes at least one of the following compounds: , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , , .
[0030] In some embodiments, the mass ratio of vinylene carbonate to cyclic sulfate compounds in the electrolyte is 0.01 to 0.5.
[0031] In some embodiments, the mass ratio of vinylene carbonate to cyclic sulfate compounds in the electrolyte is a range of any one or both of the following: 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.12, 0.14, 0.16, 0.18, 0.2, 0.22, 0.24, 0.26, 0.28, 0.3, 0.32, 0.34, 0.36, 0.38, 0.4, 0.42, 0.44, 0.46, 0.48, and 0.5.
[0032] In this application, when the mass ratio of vinylene carbonate to cyclic sulfate compounds in a single electrolyte is preferably within the above-mentioned range, the antagonistic effect of vinylene carbonate and cyclic sulfate compounds can be significantly alleviated, and the film-forming effect of both can be fully utilized, thereby improving the fast-charging performance and cycle life of the battery.
[0033] In some embodiments, the mass content of vinylene carbonate in the electrolyte is 0.01% to 0.5%.
[0034] In some embodiments, the mass content of vinylene carbonate in the electrolyte is within the range of any one or both of the following: 0.01%, 0.02%, 0.04%, 0.06%, 0.08%, 0.1%, 0.12%, 0.14%, 0.16%, 0.18%, 0.2%, 0.22%, 0.24%, 0.26%, 0.28%, 0.3%, 0.32%, 0.34%, 0.36%, 0.38%, 0.4%, 0.42%, 0.44%, 0.46%, 0.48%, and 0.5%.
[0035] In some embodiments, the mass ratio of the first electrolyte injection to the second electrolyte injection is 2.5:1 to 9:1.
[0036] In some embodiments, the mass ratio of the first electrolyte injection to the second electrolyte injection is any one or any two of the following: 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, and 9:1.
[0037] In this application, when the mass ratio of the first electrolyte to the second electrolyte is preferably within the above-mentioned range, it is more beneficial for the battery to achieve both good fast-charging performance and long cycle life.
[0038] In some embodiments, the first electrolyte injection includes solvent I, and the second electrolyte injection includes solvent II, wherein solvent I and solvent II are each independently selected from at least one of carboxylic acid ester solvents and carbonate solvents.
[0039] In some embodiments, the carboxylic acid ester solvent includes at least one selected from methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, methyl propionate, and propyl propionate.
[0040] In some embodiments, the carbonate solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethylene carbonate, vinylene carbonate, propylene carbonate, methyl ethyl carbonate, trimethylene carbonate, and butene carbonate.
[0041] In some embodiments, solvent I includes a carboxylic acid ester solvent and a carbonate solvent, wherein the mass ratio of the carboxylic acid ester solvent to the carbonate solvent is 0.1 to 2.5.
[0042] In some embodiments, the mass ratio of carboxylic acid ester solvent to carbonate solvent in solvent I is any one or any two of the following values: 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5.
[0043] In some embodiments, solvent II comprises a carboxylic acid ester solvent and a carbonate solvent, wherein the mass ratio of the carboxylic acid ester solvent to the carbonate solvent is 0.1 to 2.5.
[0044] In some embodiments, the mass ratio of carboxylic acid ester solvent to carbonate solvent in solvent II is a range of any one or both of the following: 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5.
[0045] In this application, when solvent I in one electrolyte injection or solvent II in two electrolyte injections includes a carboxylic acid ester solvent and a carbonate solvent, and the mass ratio of the two is preferably within the above range, the electrolyte can have a suitable viscosity to ensure the lithium ion transport performance and maintain the high ionic conductivity of the electrolyte; at the same time, it can also alleviate the side reactions between the electrolyte and the positive and negative electrodes, thereby better balancing the fast charging performance and cycle life of the battery.
[0046] It should be noted that, in this application, the mass ratio of carboxylic acid ester solvent to carbonate solvent in the electrolyte can be determined by, but is not limited to, the following methods: The electrolyte sample was injected into the Agilent Intuvo 9000 gas chromatograph-mass spectrometer using a micro-syringe for testing, and the GC-MS spectrum was obtained. Carboxylic acid esters were dissolved in methyl ethyl carbonate (EMC) solvent to prepare standard solutions of different concentrations, which were then injected into an Agilent Intuvo 9000 gas chromatograph-mass spectrometer to obtain standard GC-MS chromatograms. Standard solutions of different concentrations were prepared by dissolving carbonate in ethyl methyl carbonate (EMC) solvent, and injected into an Agilent Intuvo 9000 gas chromatograph-mass spectrometer to obtain standard GC-MS chromatograms. The GC-MS spectrum of the electrolyte was compared with the standard GC-MS spectrum. (1) It was confirmed whether the electrolyte contained the corresponding carboxylic acid ester. (2) The peak area X1 of the carboxylic acid ester in the GC-MS spectrum of the electrolyte and the peak area X2 of the carboxylic acid ester in the standard GC-MS spectrum were obtained. The mass content b1% of the carboxylic acid ester in the electrolyte was calculated. b1%=(X1 / X2)×m%, where m% is the mass content of the carboxylic acid ester compound in the standard solution. The GC-MS spectrum of the electrolyte was compared with the standard GC-MS spectrum. (1) It was confirmed whether the electrolyte contained the corresponding carbonate. (2) The peak area Y1 of the carbonate in the GC-MS spectrum of the electrolyte and the peak area Y2 of the carbonate in the standard GC-MS spectrum were obtained. The mass content b2% of the carbonate in the electrolyte was calculated. b2%=(Y1 / Y2)×n%, n% is the mass content of carbonate compound in the standard solution.
[0047] In some embodiments, the first electrolyte further includes lithium salt I, and the second electrolyte further includes lithium salt II, wherein lithium salt I and lithium salt II are each independently selected from at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, and lithium difluorooxalate borate.
[0048] In some embodiments, the mass content of lithium salt I in the electrolyte is 8% to 20%.
[0049] In some embodiments, the mass content of lithium salt I in the electrolyte is a range of any one or both of 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%.
[0050] In some embodiments, the mass content of lithium salt II in the secondary electrolyte is 8% to 20%.
[0051] In some embodiments, the mass content of lithium salt II in the two electrolyte solutions is any one or any two of the following values: 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%.
[0052] In this application, when the mass content of lithium salt in the electrolyte (single-cell electrolyte or double-cell electrolyte) is preferably within the above range, it is not only beneficial for the electrolyte to maintain low viscosity to maintain lithium ion transport performance, but also reduces the side reactions between the electrolyte and the positive and negative electrodes to reduce lithium salt consumption, thereby better improving the fast charging performance and cycle life of the battery at the same time.
[0053] It should be noted that, in this application, the mass content of lithium salt in the electrolyte can be confirmed by, but is not limited to, the following methods: After diluting the electrolyte sample with deionized water or organic solvent, filter it through a 0.22 μm filter membrane and inject it into an ion chromatogram (such as Thermo Scientific Dionex ICS-6000) for testing to obtain anion chromatograms; dissolve lithium salt in carbonate solvent to prepare standard solutions of different concentrations and inject them into an ion chromatogram to obtain standard anion chromatograms; compare the chromatogram of the electrolyte with the standard chromatograms to (1) confirm whether the electrolyte contains the corresponding lithium salt anion (such as PF6). ⁻ (2) Obtain the peak area A1 of the anion in the electrolyte chromatogram and the peak area A2 of the anion in the standard chromatogram. Calculate the mass content c% of the lithium salt in the electrolyte according to the following formula: c% = (A1 / A2) × c0% × n, where c0% is the mass content of the lithium salt in the standard solution and n is the dilution factor.
[0054] In some embodiments, the lithium salt I comprises lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, wherein the mass fraction of lithium bis(fluorosulfonyl)imide relative to lithium hexafluorophosphate is 1% to 10%.
[0055] In some embodiments, the mass fraction of lithium difluorosulfonylimide relative to lithium hexafluorophosphate in lithium salt I is any one or both of the following values: 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%.
[0056] In some embodiments, the lithium salt II comprises lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, wherein the mass fraction of lithium bis(fluorosulfonyl)imide relative to lithium hexafluorophosphate is 1% to 10%.
[0057] In some embodiments, the mass fraction of lithium difluorosulfonylimide relative to lithium hexafluorophosphate in lithium salt II is a range of any one or both of 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%.
[0058] In this application, the lithium salt in the electrolyte (single-cell electrolyte or double-cell electrolyte) includes lithium hexafluorophosphate and lithium difluorosulfonylimide, and when the mass ratio of the two is preferably within the above range, it can not only better shorten the fast charging time of the battery, but also help to extend its cycle life.
[0059] This application provides a method for using the above-mentioned electrolyte, including the following steps: The battery is first injected with one injection of electrolyte. After the battery has been formed, the battery is injected with a second injection of electrolyte. The battery is then aged and packaged.
[0060] This application provides a battery including the above-described electrolyte.
[0061] In this application, the battery is prepared using the following method: (1) Preparation of positive electrode sheet: According to the mass percentage of the positive electrode material layer, 94.5%~98.5% of positive electrode active material, 1.3%~2.2% of binder, 0.05%~1.5% of conductive agent and 0.05%~2% of dispersant are mixed evenly, and solvent is added to obtain positive electrode slurry. The positive electrode slurry is coated on at least one surface of the positive electrode current collector, dried, rolled and cut to obtain positive electrode sheet.
[0062] In the above-mentioned positive electrode sheet, the positive electrode active material is selected from lithium iron phosphate, lithium manganese iron phosphate, ternary materials, lithium nickel manganese oxide, etc.
[0063] In the above positive electrode, the conductive agent is selected from at least one of superconducting carbon (SP), acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, or carbon nanofibers.
[0064] In the above-mentioned positive electrode sheet, the binder is selected from at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene-propylene terpolymer, ethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, or fluorinated acrylate resin.
[0065] In the above-mentioned positive electrode sheet, the dispersant is selected from at least one of acrylic acid, acrylate, polyether ester, phosphate ester, small molecule alkanolamine, polyurethane, modified styrene / maleic anhydride, hydrogenated nitrile butadiene rubber (HNBR), polyvinylpyrrolidone (PVP) or polyethylene glycol (PEG).
[0066] In the above-mentioned positive electrode, the positive current collector can be a metal foil or a composite current collector.
[0067] Specifically, the metal foil can be aluminum or an aluminum alloy.
[0068] Specifically, the composite current collector includes an intermediate high-molecular layer and metal layers disposed on both sides of the polymer layer; wherein, the polymer layer includes polymer materials, including at least one of polyamide (PA), polyterephthalate, polyimide (PI), polyethylene (PE), polypropylene (PP), polystyrene (PS), polyvinyl chloride (PVC), aramid, acrylonitrile-butadiene-styrene copolymer (ABS), polybutylene terephthalate (PET), poly(p-phenylene terephthalamide) (PPTA), polypropylene (PPE), polyoxymethylene (POM), epoxy resin, phenolic resin, polytetrafluoroethylene (PTEE), polyvinylidene fluoride (PVDF), silicone rubber, polycarbonate (PC), polyvinyl alcohol (PVA), polyethylene glycol (PEG), cellulose, starch, protein, its derivatives, its crosslinks or copolymers; the metal layer includes at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver or silver alloy.
[0069] (2) Preparation of negative electrode sheet: The negative electrode active material, conductive agent, binder and dispersant are mixed and a solvent is added to obtain a negative electrode slurry, wherein the mass percentage of negative electrode active material: conductive agent: binder: dispersant is (90~98): (0~5): (1.5~5): (0.3~1.5). The negative electrode slurry is coated on at least one surface of the negative electrode current collector, dried, rolled and cut to obtain a negative electrode sheet.
[0070] In the above-mentioned negative electrode sheet, the negative electrode active material is selected as a silicon-based negative electrode material.
[0071] Specifically, the silicon-based anode material can be selected from one or more of silicon materials, silicon oxide materials, silicon carbon materials, and silicon alloy materials.
[0072] In the aforementioned negative electrode sheet, the conductive agent is selected from one or more of the following: superconducting carbon (SP), conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0073] In the aforementioned negative electrode sheet, the binder is selected from at least one of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, and water-based acrylic resins (e.g., polyacrylic acid (PAA), polymethacrylic acid (PMAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and sodium carboxymethyl methyl ester (CMC).
[0074] In the above-mentioned negative electrode sheet, the dispersant is selected from at least one of acrylic acid, acrylate, polyether ester, phosphate ester, small molecule alkanolamine, polyurethane, modified styrene / maleic anhydride, HNBR, and PVP.
[0075] In the aforementioned negative electrode, the current collector is selected from metal foil or composite current collector.
[0076] Specifically, the metal foil can be copper or a copper alloy.
[0077] Specifically, the composite current collector includes an intermediate high-molecular layer and metal layers disposed on both sides of the polymer layer. The polymer layer comprises polymeric materials, including at least one of polyamide (PA), polyterephthalate, polyimide (PI), polyethylene (PE), polypropylene (PP), polystyrene (PPE), polyvinyl chloride (PVC), aramid, acrylonitrile-butadiene-styrene copolymer (ABS), polybutylene terephthalate (PET), poly(p-phenylene terephthalamide) (PPTA), polypropylene (PPE), polyoxymethylene (POM), epoxy resin, phenolic resin, polytetrafluoroethylene (PTEE), polyvinylidene fluoride (PVDF), silicone rubber, polycarbonate (PC), polyvinyl alcohol (PVA), polyethylene glycol (PEG), cellulose, starch, protein, their derivatives, their crosslinks, and their copolymers. The metal layers are selected from at least one of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys.
[0078] (3) Separator: The separator is placed between the positive electrode and the negative electrode to separate the positive electrode and the negative electrode and prevent the positive electrode and the negative electrode from short-circuiting.
[0079] The material of the diaphragm is selected from at least one of glass fiber, nonwoven fabric, polyethylene (PE), polypropylene (PP) and / or polyvinylidene fluoride.
[0080] Specifically, a coating may also be provided on the surface of the diaphragm. The coating may be an inorganic coating and / or an organic coating. The inorganic coating material includes at least one of alumina, silicon oxide, titanium oxide, magnesium oxide, zirconium oxide or boehmite. The organic coating includes at least one of aramid coating or polyvinylidene fluoride (PVDF) coating.
[0081] (4) Stack the positive electrode, separator and negative electrode in sequence so that the separator is between the positive and negative electrode to play a role in isolation. Then wind them to obtain the bare cell. Place the bare cell in the outer packaging shell, dry it and inject the above electrolyte. After vacuum sealing, standing, formation and shaping, a lithium-ion battery is obtained.
[0082] The outer packaging includes aluminum-plastic film, metal shell, etc.; the metal shell can be aluminum, aluminum alloy (aluminum-magnesium alloy, aluminum-manganese alloy, etc.); steel, stainless steel, nickel-plated steel, carbon steel, etc.; titanium, titanium alloy, etc. Steps (1) to (4) are not in any particular order.
[0083] Example 1 A battery, the method for preparing the battery comprising the following steps: <Preparation of the positive electrode> The positive electrode active material (LiFePO4), conductive agent (acetylene black), binder (PVDF), and dispersant (polyvinylpyrrolidone) were mixed in a mass ratio of 96.5:1:1.7:0.8. NMP solvent was added, and the mixture was stirred under vacuum until homogeneous to obtain a positive electrode slurry. The positive electrode slurry was coated onto the upper and lower surfaces of a positive electrode current collector aluminum foil, air-dried at room temperature, and then transferred to an oven for further drying. After cold pressing and slitting, positive electrode sheets were obtained with an areal density of 360 g / cm³. 2 The compacted density is 2.5 g / cm³. 3 .
[0084] <Preparation of Negative Electrode> The negative electrode active material (graphite), conductive agent (Super P), binder (styrene-butadiene rubber), and dispersant (carboxymethyl cellulose) were dispersed in water at a mass ratio of 94:2.5:2.6:0.9. A slurry was prepared by vacuum stirring, and then coated onto both sides of the current collector copper foil. After drying, cold pressing, and slitting, the negative electrode sheet was obtained, with an areal density of 174 g / m³. 2 The compacted density is 1.55 g / cm³. 3 .
[0085] <Preparation of the diaphragm> Choose a commercially available polyethylene diaphragm with a thickness of 10μm (air permeability of 100s / 100mL).
[0086] <Preparation of Electrolyte> One-shot electrolyte: In a glove box (moisture content less than 10 ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 3:3:4 to obtain an organic solvent; then, dried lithium salt (composed of LiPF6 and LiFSI in a mass ratio of 100:5) is added to the organic solvent, followed by the addition of cyclic sulfate compound 1 and vinylene carbonate (if any), and mixed thoroughly to obtain one-shot electrolyte (where the mass content of the cyclic sulfate compound is 1%, the mass content of the organic solvent is 84%, and the mass content of the lithium salt is 15%).
[0087] The chemical structural formula of cyclic sulfate compound 1 is shown below: ; The above-mentioned cyclic sulfate compound 1 was prepared by the following method: Step 1: Add 2 mol of 1-methylpentanetetraol to a three-necked flask, start stirring, and add 4.4 mol of thionyl chloride dropwise to the three-necked flask. During the dropwise addition, control the temperature at about 15°C. After the dropwise addition is complete, keep the reaction at 45°C for 4 hours. A large amount of paste-like solid precipitates from the reaction solution. After cooling, slowly add 1 L of deionized water dropwise and quickly stir the reaction system to disperse it. The solid obtained by filtration is washed with deionized water several times until the pH is neutral. The filter cake is dried under reduced pressure at 60°C to obtain the intermediate product. Step 2: Add 0.8 mol of the intermediate product to a three-necked flask, add 1000 mL of acetonitrile, add 80 mg of ruthenium trichloride trihydrate catalyst, purge the system with nitrogen, cool the system to 20°C, start stirring, and add 2000 g of 20% sodium hypochlorite aqueous solution dropwise over 1 hour, controlling the reaction temperature at 10-20°C; after the addition is complete, stir at 10-20°C for 10 minutes, separate the layers, and quench the organic phase with sodium sulfite aqueous solution until the starch-potassium iodide test paper does not turn blue; separate the layers again, concentrate the organic layer, and crystallize the acetonitrile to obtain cyclic sulfate ester compound 1.
[0088] Secondary electrolyte: The operation is carried out in a glove box (moisture content less than 10 ppm). Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 3:3:4 to obtain an organic solvent. Then, dried lithium salt (composed of LiPF6 and LiFSI in a mass ratio of 100:5) is added to the organic solvent, followed by the addition of vinylene carbonate and mixed evenly to obtain a secondary electrolyte (where the mass content of vinylene carbonate is 15%, the mass content of the organic solvent is 70%, and the mass content of the lithium salt is 15%).
[0089] <Battery Manufacturing> The positive electrode, separator, and negative electrode are stacked in sequence, with the separator acting as a separator between the positive and negative electrodes. Then, they are wound to obtain a bare cell. The bare cell is placed in an outer packaging shell, dried, and then injected with one injection of electrolyte. After standing for 24 hours, it is formed at high temperature. After formation, it is stood for 12 hours and then injected with a second injection of electrolyte (the mass ratio of the first injection to the second injection of electrolyte is 5:1). After the second injection, it is stood for 12 hours before being packaged and volume-adjusted to obtain the battery.
[0090] Example 2 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 1.5%, the mass content of organic solvent is 83.5%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0091] Example 3 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 0.5%, the mass content of organic solvent is 84.5%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0092] Example 4 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 5%, the mass content of organic solvent is 80%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0093] Example 5 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 0.2%, the mass content of organic solvent is 84.8%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0094] Example 6 Except for the following: in the preparation of the electrolyte, the mass content of vinylene carbonate is 10%, the mass content of organic solvent is 75%, and the mass content of lithium salt is 15% in the second electrolyte, the rest is the same as in Example 1.
[0095] Example 7 Except for the following: in the preparation of the electrolyte, the mass content of vinylene carbonate is 18%, the mass content of organic solvent is 67%, and the mass content of lithium salt is 15% in the second electrolyte, the rest is the same as in Example 1.
[0096] Example 8 Except for the following: in the preparation of the electrolyte, the mass content of vinylene carbonate is 5%, the mass content of organic solvent is 80%, and the mass content of lithium salt is 15% in the second electrolyte, the rest is the same as in Example 1.
[0097] Example 9 Except for the preparation of the electrolyte, in the second electrolyte, the mass content of vinylene carbonate is 20%, the mass content of organic solvent is 65%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0098] Example 10 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 1%, the mass content of vinylene carbonate is 0.01%, the mass content of organic solvent is 83.99%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0099] Example 11 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 1%, the mass content of vinylene carbonate is 0.25%, the mass content of organic solvent is 83.75%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0100] Example 12 Except for the preparation of the electrolyte, in which the mass content of cyclic sulfate compounds is 1%, the mass content of vinylene carbonate is 0.5%, the mass content of organic solvent is 83.5%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0101] Example 13 Except for the mass ratio of the first electrolyte to the second electrolyte in the <Battery Preparation> section, which is 2.5:1, the rest is the same as in Example 1.
[0102] Example 14 Except for the mass ratio of the first electrolyte to the second electrolyte in the <Battery Preparation> section, which is 9:1, the rest is the same as in Example 1.
[0103] Example 15 Except for replacing cyclic sulfate compound 1 with cyclic sulfate compound 2 in one batch of electrolyte in <Preparation of Electrolyte>, the rest is the same as in Example 1.
[0104] The chemical structural formula of cyclic sulfate compound 2 is shown below: ; The above-mentioned cyclic sulfate compound 2 was prepared by the following method: Step 1: Add 2 mol of 4-[1,2-dihydroxy-2,2-bis(2-hydroxyethyl)ethyl]-5-(1,3-dihydroxypropyl)-1,3,2-dioxothiacyclopentane-2,2-dioxide to a three-necked flask, start stirring, and add 4.4 mol of thionyl chloride dropwise to the three-necked flask. During the dropwise addition, control the temperature at about 15°C. After the dropwise addition is complete, keep the reaction at 45°C for 4 hours. A large amount of paste-like solid precipitates from the reaction solution. After cooling, slowly add 1 L of deionized water. Quickly stir and disperse the reaction system. Filter the solid obtained and wash it with deionized water several times until the pH is neutral. Dry the filter cake under reduced pressure at 60°C to obtain the intermediate product. Step 2: Add 0.8 mol of the intermediate product to a three-necked flask, add 1000 mL of acetonitrile, add 80 mg of ruthenium trichloride trihydrate catalyst, purge the system with nitrogen, cool the system to 20°C, start stirring, and add 2000 g of 20% sodium hypochlorite aqueous solution dropwise over 1 hour, controlling the reaction temperature at 10-20°C; after the addition is complete, stir at 10-20°C for 10 minutes, separate the layers, and quench the organic phase with sodium sulfite aqueous solution until the starch-potassium iodide test paper does not turn blue; separate the layers again, concentrate the organic layer, and crystallize the acetonitrile to obtain cyclic sulfate ester compound 2.
[0105] Example 16 Except for replacing the cyclic sulfate compound 1 in the electrolyte in the <Preparation of Electrolyte> section with ethylene disulfate (BIDTD), the rest is the same as in Example 1.
[0106] Comparative Example 1 Except for the following: in the preparation of electrolyte, the mass content of cyclic sulfate compounds in the first electrolyte is 0.05%, the mass content of organic solvent is 84.95%, and the mass content of lithium salt is 15%, and the mass content of vinylene carbonate in the second electrolyte is 19%, the mass content of organic solvent is 66%, and the mass content of lithium salt is 15%, the rest are the same as in Example 1.
[0107] Comparative Example 2 Except for the following: in the preparation of electrolyte, the mass content of cyclic sulfate compounds in the first electrolyte is 7%, the mass content of organic solvent is 78%, and the mass content of lithium salt is 15%, and the mass content of vinylene carbonate in the second electrolyte is 6%, the mass content of organic solvent is 79%, and the mass content of lithium salt is 15%, the rest are the same as in Example 1.
[0108] Comparative Example 3 Except for the following: in the preparation of electrolyte, the mass content of cyclic sulfate compounds in the first electrolyte is 4.5%, the mass content of organic solvent is 80.5%, and the mass content of lithium salt is 15%, and the mass content of vinylene carbonate in the second electrolyte is 2%, the mass content of organic solvent is 83%, and the mass content of lithium salt is 15%, the rest are the same as in Example 1.
[0109] Comparative Example 4 Except for the following: in the preparation of electrolyte, the mass content of cyclic sulfate compounds in the first electrolyte is 0.3%, the mass content of organic solvent is 84.7%, and the mass content of lithium salt is 15%, and the mass content of vinylene carbonate in the second electrolyte is 25%, the mass content of organic solvent is 60%, and the mass content of lithium salt is 15%, the rest are the same as in Example 1.
[0110] Comparative Example 5 Except for the following: in the preparation of electrolyte, the mass content of cyclic sulfate compounds is 1%, the mass content of vinylene carbonate is 1%, the mass content of organic solvent is 83%, and the mass content of lithium salt is 15%, the rest is the same as in Example 1.
[0111] Example of effect The batteries obtained in each embodiment and comparative example were tested as follows, and the test results are shown in Table 1: (1) Fast charging time During battery assembly, a copper wire is added to the negative electrode side. After assembly, the battery is left to stand for 24 hours, then charged at 0.02C to 4.1V, followed by constant current charging at 0.33C to 3.65V, and then constant voltage charging to 0.05C. After standing for 10 minutes, it is discharged at 0.33C to 2.5V to complete formation. Subsequently, it is discharged and charged at 0.33C at a constant current rate to 3.65V, then charged at a constant voltage rate to 0.05C. After standing for 10 minutes, it is discharged at 0.33C at a constant current rate to 2.5V. This constitutes one cycle of capacity determination. After two cycles of capacity determination, the copper wire is first lithium-plated at 0.02C for 4 hours, and then charged at 0.33C to 10% of the capacity from the second cycle of capacity determination. Then, constant current charging is performed at a 4C rate until the negative parameter potential is 0 or the terminal voltage is 3.65V. Then, decremental charging is performed at a 0.2C gradient, with the cutoff condition remaining unchanged, until the charging rate drops to 0.33C or the capacity reaches 80%. Subsequently, constant current and constant voltage charging is performed at 0.33C to 3.65V. The test temperature is 25℃, and the device signal acquisition frequency is 100ms. After the test, the charging time t required for the battery to go from 10% to 80% SOC is calculated.
[0112] (2) Cycle life Capacity setting: Place the test object in a 25℃ temperature chamber and perform the following operations on the test object: charge at 0.33C to the upper limit voltage of 3.65V, then charge at constant voltage to the cutoff current of 0.05C; let stand for 30 minutes, then discharge at 0.33C to the lower limit voltage of 2.5V; repeat the above operation 3 times, and take the discharge capacity of the third cycle as the battery capacity setting. Then proceed with the following steps: 1) At 25℃, charge at a constant current rate of 1C to the upper limit voltage of 3.65V, and then charge at a constant voltage until the current drops to 0.05C; 2) Let it stand for 30 minutes; 3) Discharge at a 1C rate to the lower limit voltage of 2.5V; 4) Let it stand for 30 minutes; Perform cyclic testing according to steps 1)-4) until the battery capacity is less than 80% of the initial capacity, and record the number of cycles at this point.
[0113] Table 1 According to the data in Table 1, the cycle life of the batteries in Examples 1-16 is ≥880 cycles, and the fast charging time is ≤14 minutes, indicating that the electrolyte of this application can enable the battery to have both good fast charging performance and long cycle life. Meanwhile, according to Comparative Examples 1-4, when the mass content of cyclic sulfate compounds in one electrolyte is too low or too high, or the mass content of vinylene carbonate in two electrolytes is too low or too high, it is difficult to effectively improve the fast charging performance and cycle life of the battery. Furthermore, according to Comparative Example 5, when one electrolyte also contains vinylene carbonate, if the mass ratio of vinylene carbonate to cyclic sulfate compounds is too large, the cyclic sulfate compounds will have a significant antagonistic effect with vinylene carbonate, leading to a deterioration in the fast charging performance and cycle life of the battery.
Claims
1. An electrolyte, characterized in that, Includes one-cell and two-cell electrolyte solutions; The electrolyte solution comprises cyclic sulfate compounds and vinylene carbonate, wherein the mass ratio of vinylene carbonate to cyclic sulfate compounds is ≤0.5; The mass content of cyclic sulfate compounds in the electrolyte is 0.2% to 5%; The second electrolyte solution includes vinylene carbonate; The mass content of vinylene carbonate in the second electrolyte is 5%~20%; The cyclic sulfate compounds include at least one of the compounds shown in Formula I; ; In Formula I, R1, R2, R3 and R4 are each independently selected from any one of the following groups as shown in Formula II: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group. ; In Formula II, R5 and R6 are each independently selected from any one of the following groups as shown in Formula III: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group. ; In Formula III, R7 and R8 are each independently selected from any one of the following: hydrogen atom, alkyl group of 1 to 6 carbon atoms, halogen atom, haloalkyl group of 1 to 3 carbon atoms, alkoxy group of 1 to 3 carbon atoms, haloalkoxy group of 1 to 3 carbon atoms, alkenyl group of 2 to 6 carbon atoms, alkynyl group of 2 to 6 carbon atoms, aromatic group, ester group, cyano group, and sulfonic acid group.
2. The electrolyte as described in claim 1, characterized in that, The mass content of cyclic sulfate compounds in the electrolyte is 0.5%~1.5%; And / or, the mass content of vinylene carbonate in the two electrolyte solutions is 10%~18%.
3. The electrolyte as described in claim 1, characterized in that, Formula I contains 2 to 4 sulfate ester groups.
4. The electrolyte as described in claim 1, characterized in that, At least one of R1, R2, R3, and R4 is a hydrogen atom.
5. The electrolyte as described in claim 1, characterized in that, R1 and R3 are the same.
6. The electrolyte as described in claim 5, characterized in that, R1 and R3 are selected from any one of the following groups as shown in Formula II, hydrogen atoms, alkyl groups of 1 to 6 carbon atoms, halogen atoms, haloalkyl groups of 1 to 3 carbon atoms, alkoxy groups of 1 to 3 carbon atoms, haloalkoxy groups of 1 to 3 carbon atoms, alkenyl groups of 2 to 6 carbon atoms, alkynyl groups of 2 to 6 carbon atoms, aromatic groups, ester groups, cyano groups, and sulfonic acid groups.
7. The electrolyte as described in claim 1, characterized in that, The mass content of vinylene carbonate in the electrolyte is 0.01%~0.5%.
8. The electrolyte as described in claim 1, characterized in that, The mass ratio of the first electrolyte injection to the second electrolyte injection is 2.5:1 to 9:
1.
9. The electrolyte as described in claim 1, characterized in that, The first electrolyte injection includes solvent I, and the second electrolyte injection includes solvent II. Solvent I and solvent II are each independently selected from at least one of carboxylic acid ester solvents and carbonate solvents.
10. The electrolyte as described in claim 9, characterized in that, The carboxylic acid ester solvent includes at least one of methyl acetate, ethyl acetate, propyl acetate, ethyl propionate, methyl propionate, and propyl propionate. And / or, the carbonate solvent includes at least one of dimethyl carbonate, diethyl carbonate, ethylene carbonate, vinylene carbonate, propylene carbonate, methyl ethyl carbonate, trimethylene carbonate, and butene carbonate.
11. The electrolyte as described in claim 9, characterized in that, Solvent I includes a carboxylic acid ester solvent and a carbonate solvent, wherein the mass ratio of the carboxylic acid ester solvent to the carbonate solvent is 0.1 to 2.
5. And / or, the solvent II comprises a carboxylic acid ester solvent and a carbonate solvent, wherein the mass ratio of the carboxylic acid ester solvent to the carbonate solvent is 0.1 to 2.
5.
12. The electrolyte as described in claim 1, characterized in that, The first electrolyte also includes lithium salt I, and the second electrolyte also includes lithium salt II. Lithium salt I and lithium salt II are each independently selected from at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, and lithium difluorooxalate borate.
13. The electrolyte as described in claim 12, characterized in that, The mass content of lithium salt I in the electrolyte is 8%~20%; And / or, the mass content of lithium salt II in the two electrolyte solutions is 8%~20%.
14. The electrolyte as described in claim 12, characterized in that, The lithium salt I comprises lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide, wherein the mass fraction of lithium bis(fluorosulfonyl)imide relative to lithium hexafluorophosphate is 1% to 10%. And / or, the lithium salt II comprises lithium hexafluorophosphate and lithium bisfluorosulfonylimide, wherein the mass fraction of lithium bisfluorosulfonylimide relative to lithium hexafluorophosphate is 1% to 10%.
15. A method of using the electrolyte according to any one of claims 1 to 14, characterized in that, Includes the following steps: The battery is first injected with one injection of electrolyte. After the battery has been formed, the battery is injected with a second injection of electrolyte. The battery is then aged and packaged.
16. A battery, characterized in that, Includes the electrolyte as described in any one of claims 1 to 14.