An electrolyte and a lithium-ion battery including the electrolyte
By adding α-olefins and nano-metal particles to catalyze activated carbon particles in the electrolyte of lithium-ion batteries, the problem of battery performance degradation caused by the accumulation of acidic substances in the electrolyte is solved, and the battery cycle life and performance stability are improved. A low-cost and environmentally friendly method is used to inhibit acidic substance corrosion and gas generation.
Patent Information
- Application Number
- CN202611554259.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-09
- Publication Date
- 2026-11-17
AI Technical Summary
In existing lithium-ion batteries, the accumulation of acidic substances in the electrolyte during long-term charge-discharge cycles, especially during high-temperature cycles, can lead to a decline in battery performance, including damage to electrode interface stability, gas generation, and battery swelling. Existing additives are difficult to effectively remove acidic substances and avoid side reactions.
Adding α-olefins as additives to the electrolyte converts hydrogen ions into stable alkanes through an electrochemical reduction hydrogenation reaction, removes acidic substances, improves battery cycle life, and suppresses gas production. At the same time, nano-metal particles are used to catalyze activated carbon particles to enhance the efficiency of the hydrogenation reaction.
It effectively removes acidic substances, reduces erosion of the negative electrode SEI film, improves battery cycle life, suppresses gas generation, maintains battery performance stability, and improves long-term battery cycle performance through a low-cost, environmentally friendly method.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, specifically, it relates to an electrolyte and a lithium-ion battery including the electrolyte. Background Technology
[0002] During long-term charge-discharge cycles, especially high-temperature cycles, the accumulation of acidic substances in the electrolyte of lithium-ion batteries can adversely affect battery performance. Acidic substances can easily disrupt the stability of the electrode interface and generate gas, leading to a decrease in battery capacity retention, an increase in internal pressure, and in severe cases, battery swelling, thus limiting the long-term use of the battery.
[0003] To mitigate the adverse effects of acidic substances on battery performance, existing technologies typically involve adding functional additives to the electrolyte. For example, fluorinated cyclic carbonates, cyclophosphonitrile compounds, cyclic sulfates, and lithium fluorooxalate-borate salts can form stable CEI and SEI films on the positive and negative electrode surfaces to prevent acidic substances from corroding the electrode interfaces. Alternatively, isocyanates and silanes can react with or complex with acidic substances to reduce their content in the electrolyte. However, these additives generally suffer from complex molecular structures, long synthesis routes, and high material costs. Furthermore, the side reactions they may initiate can negatively impact the stability of the electrode interface films or increase the battery's internal resistance. In summary, existing additives currently struggle to simultaneously achieve effective removal of acidic substances from the electrolyte and stable maintenance of battery performance. Summary of the Invention
[0004] This invention provides an electrolyte and a lithium-ion battery including the electrolyte, which aims to effectively remove acidic substances from the lithium-ion battery electrolyte, suppress gas generation caused by the accumulation of acidic substances, and avoid battery side reactions induced by the introduction of additives, thereby maintaining good cycle performance of the lithium-ion battery.
[0005] According to a first aspect of the present invention, an electrolyte is provided, comprising an electrolyte additive, an organic solvent, and a lithium salt. The electrolyte additive comprises an α-olefin, wherein the α-olefin is a compound represented by CH2=CH-R, wherein R is a straight-chain or branched saturated alkyl group, and the general formula of R is C2. n H 2n+1The formula indicates that n is a positive integer selected from 5 to 9. This invention adds α-olefins as electrolyte additives, where "saturated alkyl" refers to a straight-chain or branched hydrocarbon group composed only of carbon and hydrogen atoms, without any unsaturated bonds (such as carbon-carbon double or triple bonds). Under the negative electrode voltage, the α-double bonds in the α-olefin can undergo an electrochemical reduction and hydrogenation reaction with hydrogen ions generated in the electrolyte due to solvent decomposition or the reaction of lithium salt with trace amounts of water. This converts corrosive hydrogen ions into stable, electrochemically inert saturated alkanes, thereby removing and reducing acidic substances in the electrolyte, reducing and inhibiting the erosion and damage of the negative electrode SEI film by acidic substances, reducing active lithium consumption, significantly improving battery cycle life, and suppressing gas production. Simultaneously, α-olefins and their hydrogenation product alkanes have high redox stability on the positive and negative electrode surfaces and do not participate in side reactions at the electrode interface, thus not negatively impacting the battery's cycle performance and ensuring performance stability during long-term cycling. Furthermore, the α-olefins used in this solution are widely available, inexpensive, and environmentally friendly.
[0006] Furthermore, the α-olefin includes at least one of 1-heptene, 1-octene, 1-nonene, 1-decene, and 1-undecene.
[0007] Furthermore, the α-olefin is 1-heptene.
[0008] Furthermore, the organic solvent includes ethylene carbonate, with a mass ratio of ethylene carbonate to α-olefin > 4.
[0009] Furthermore, the α-olefin accounts for 2% to 10% of the total mass of the electrolyte.
[0010] Furthermore, the electrolyte additives also include at least one of vinylene carbonate, fluorovinyl carbonate, and tris(trimethylsilyl)phosphite.
[0011] Furthermore, the organic solvent also includes at least one of propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethyl acetate (EC), and ethyl propionate.
[0012] Furthermore, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), and lithium bis(oxalato)borate (LiDFOB).
[0013] Furthermore, the lithium salt accounts for 10% to 15% of the mass of the electrolyte.
[0014] According to a second aspect of the present invention, a lithium-ion battery is provided, the lithium-ion battery comprising a positive electrode, a negative electrode and an electrolyte as described above.
[0015] Furthermore, the negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode functional additive, the negative electrode functional additive includes activated carbon particles loaded with nano-metal particles, and the nano-metal particles include at least one of nickel, iron, copper, and manganese.
[0016] Furthermore, the mass of the nano-metal particles accounts for 1% to 6% of the mass of the activated carbon particles, and the mass of the negative electrode functional additives accounts for 0.2% to 1.5% of the total mass of the negative electrode active material layer. Detailed Implementation
[0017] This invention discloses an electrolyte and a lithium-ion battery including the electrolyte. Those skilled in the art can refer to the content of this document and appropriately modify the process parameters to achieve the desired result. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in this application. The methods and applications of this application have been described through preferred embodiments, and those skilled in the art can obviously make modifications or appropriate changes and combinations to the methods and applications described herein without departing from the content, spirit, and scope of this application to realize and apply the technology of this application.
[0018] In the description of this application, the list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A and B are listed, then the phrase "at least one of A and B" means only A; only B; or A and B. In another instance, if items A, B, and C are listed, then the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may contain a single element or multiple elements. Item B may contain a single element or multiple elements. Item C may contain a single element or multiple elements.
[0019] The endpoints and any values of the ranges disclosed herein are not limited to the precise ranges or values, and should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges, or individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein. Unless otherwise stated, all embodiments and optional embodiments of this application can be combined with each other to form new technical solutions.
[0020] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0021] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0022] According to a first aspect of the present invention, an electrolyte is provided, comprising an electrolyte additive, an organic solvent, and a lithium salt. The electrolyte additive comprises an α-olefin, wherein the α-olefin is a compound represented by CH2=CH-R, wherein R is a straight-chain or branched saturated alkyl group, and the general formula of R is C2. n H 2n+1 The formula indicates that n is a positive integer selected from 5 to 9. This invention adds α-olefins as electrolyte additives, where "saturated alkyl" refers to a straight-chain or branched hydrocarbon group composed only of carbon and hydrogen atoms, without any unsaturated bonds (such as carbon-carbon double or triple bonds). Under the negative electrode voltage, the α-double bonds in the α-olefin can undergo an electrochemical reduction and hydrogenation reaction with hydrogen ions generated in the electrolyte due to solvent decomposition or the reaction of lithium salt with trace amounts of water. This converts corrosive hydrogen ions into stable, electrochemically inert saturated alkanes, thereby removing and reducing acidic substances in the electrolyte, reducing and inhibiting the erosion and damage of the negative electrode SEI film by acidic substances, reducing active lithium consumption, significantly improving battery cycle life, and suppressing gas production. Simultaneously, α-olefins and their hydrogenation product alkanes have high redox stability on the positive and negative electrode surfaces and do not participate in side reactions at the electrode interface, thus not negatively impacting the battery's cycle performance and ensuring performance stability during long-term cycling. Furthermore, the α-olefins used in this solution are widely available, inexpensive, and environmentally friendly.
[0023] In one embodiment of the present invention, the α-olefin includes at least one selected from 1-heptene, 1-octene, 1-nonene, 1-decene, and 1-undecene. These olefins have moderate boiling points and maintain low viscosity at battery operating temperatures. The moderate boiling point ensures stable internal gas pressure during high-temperature cycling, while the low viscosity helps maintain the overall fluidity of the electrolyte, ensuring rapid migration of lithium ions within the electrolyte.
[0024] In one embodiment of the present invention, the α-olefin is 1-heptene. By using 1-heptene as the electrolyte additive of the present invention, the cycle life of the battery can be further improved and gas production can be suppressed.
[0025] In one embodiment of the present invention, the organic solvent includes ethylene carbonate, and the mass ratio of ethylene carbonate to α-olefin is greater than 4. α-olefins are nonpolar hydrocarbons, and their introduction reduces the overall dielectric constant of the electrolyte system, thereby affecting the dissociation and conductivity of the lithium salt. Ethylene carbonate (EC) has a high dielectric constant of 89.6 and a strong ability to dissociate lithium salts. This solution compensates for the reduction in the dielectric constant of the system due to the addition of α-olefins by introducing EC into the electrolyte. Based on the amount of α-olefin used, the mass ratio of EC to α-olefins is controlled to be greater than 4 to regulate the EC content in the electrolyte, thereby avoiding the adverse effects of the introduction of α-olefins on lithium salt dissociation and electrolyte conductivity. Exemplarily, the mass ratio of ethylene carbonate to α-olefins can be 4.2, 4.3, 4.4, 4.5, 5, 5.2, 5.4, 5.6, 5.8, 6, 8, 10, etc., but is not limited to the listed values; other unlisted values within this range are also applicable.
[0026] In one embodiment of the present invention, the mass of α-olefin accounts for 2% to 10% of the total mass of the electrolyte. Exemplarily, the mass of α-olefin in the total mass of the electrolyte can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0027] In one embodiment of the present invention, the electrolyte additive further includes at least one selected from vinylene carbonate, fluoroethylene carbonate, and tris(trimethylsilyl)phosphite. Introducing vinylene carbonate (VC), fluoroethylene carbonate (FEC), and tris(trimethylsilyl)phosphite (TMSP) into the electrolyte provided by this solution is beneficial for improving the density and stability of the SEI film and CEI film, thereby further preventing acidic substances from corroding the electrodes.
[0028] In one embodiment of the present invention, the organic solvent further includes at least one of propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), ethyl acetate (EC), and ethyl propionate.
[0029] In one embodiment of the present invention, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium bisfluorosulfonylimide (LiFSI), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), and lithium bis(oxalate-borate) (LiDFOB).
[0030] In one embodiment of the present invention, the lithium salt accounts for 10% to 15% of the mass of the electrolyte. Exemplarily, the mass percentage of the lithium salt in the electrolyte may be 10%, 11%, 12%, 13%, 14%, 15%, etc., but is not limited to the listed values, and other unlisted values within this range are also applicable.
[0031] According to a second aspect of the present invention, a lithium-ion battery is provided, the lithium-ion battery comprising a positive electrode, a negative electrode and an electrolyte as described above.
[0032] In one embodiment of the present invention, the negative electrode includes a negative electrode active material layer, which includes a negative electrode functional additive. The negative electrode functional additive includes activated carbon particles loaded with nano-metal particles, wherein the nano-metal particles include at least one of nickel, iron, copper, and manganese. Activated carbon has a porous structure and a high specific surface area, enabling it to effectively adsorb and enrich α-olefins in the electrolyte, which is beneficial for the reductive hydrogenation reaction. The nano-metal particles loaded in the activated carbon are highly efficient catalysts for the electrochemical hydrogenation reaction, reducing the activation energy of the α-olefin reductive hydrogenation reaction, thus improving the hydrogen ion removal efficiency of α-olefins and further enhancing the electrolyte's gas generation suppression capability, thereby improving the battery's cycle performance.
[0033] In one embodiment of the present invention, the mass of the nano-metal particles accounts for 1% to 6% of the mass of the activated carbon particles, and the mass of the negative electrode functional additive accounts for 0.2% to 1.5% of the total mass of the negative electrode active material layer. The pore structure of the activated carbon simultaneously serves to enrich α-olefins and support nano-metal particles. Based on this, this solution controls the loading of nano-metal ions in the activated carbon particles to ensure effective enrichment of α-olefins while providing sufficient catalytic active sites for the hydrogenation reduction reaction of α-olefins. Furthermore, by controlling the amount of negative electrode functional additive, the efficiency of the catalytic hydrogenation reduction reaction of α-olefins can be effectively improved, while avoiding a significant decrease in the stability of the negative electrode slurry due to the introduction of the negative electrode functional additive, thus helping to ensure the uniformity of the negative electrode active material layer. For example, the mass ratio of nano-metal particles to the activated carbon particles can be 1%, 2%, 3%, 4%, 5%, 6%, etc., but is not limited to the listed values; other unlisted values within this range are also applicable. For example, the mass of the negative electrode functional additive as a percentage of the total mass of the negative electrode active material layer can be 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, etc., but is not limited to the listed values. Other unlisted values within this range are also applicable.
[0034] In the following examples and comparative examples, the α-olefins referred to are compounds represented by CH2=CH-R, where R is a straight-chain or branched saturated alkyl group, and the general formula of R is C2. n H2n+1 express.
[0035] Example 1 This embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. 1. Prepare the electrolyte The electrolyte provided in this embodiment includes electrolyte additives, organic solvents, and lithium salts. The electrolyte additives include α-olefins, vinylene carbonate (VC), fluoroethylene carbonate (FEC), and tris(trimethylsilyl)phosphite (TMSP). In this embodiment, the α-olefin is specifically 1-heptene. The organic solvents include ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). The lithium salt is lithium hexafluorophosphate (LiPF6). Based on the total mass of the electrolyte, the following specific formulation is used for preparation: α-olefin 6%, VC 3%, FEC 0.5%, TMSP 0.5%, EC 27%, EMC 20%, DMC 30%, and LiPF6 13%. In the above formulation, the mass ratio of EC to α-olefin is 27:6, or 4.5.
[0036] After the preparation of materials is completed, the components in the electrolyte formula are mixed evenly to obtain the electrolyte of this embodiment.
[0037] 2. Preparation of negative electrode sheet (1) Preparation of negative electrode functional additives loaded with nano-metal particles Activated carbon is pulverized and ground into D 50 The powder is approximately 15 μm in size. 1.7 g of nickel nitrate hexahydrate (Ni(NO3)2·6H2O) was dissolved in 50 mL of deionized water to obtain a metal ion solution. 10 g of finely ground activated carbon powder was added to the metal ion solution and stirred until homogeneous. The sample was then impregnated under vacuum for 12 hours to allow the activated carbon to fully absorb Ni(NO3)2·6H2O. The impregnated sample was dried in an oven at 120°C for 12 hours. The dried sample was then subjected to a carbothermic reduction reaction in a tube furnace under a nitrogen atmosphere. The carbothermic reduction reaction temperature was 600°C, and the reaction time was 4 hours. The sample was then cooled to room temperature under a nitrogen atmosphere to obtain a negative electrode functional additive loaded with nano-metal particles. In this embodiment, the nano-metal ions originated from Ni(NO3)2·6H2O in the raw material; therefore, the negative electrode functional additive obtained in this embodiment is activated carbon loaded with nano-nickel particles.
[0038] (2) Preparation of negative electrode active material layer The raw materials used to prepare the negative electrode active material layer include negative electrode active material, negative electrode binder, thickener, negative electrode conductive agent, and negative electrode functional additive. In this embodiment, graphite is used as the negative electrode active material, styrene-butadiene rubber (SBR) as the negative electrode binder, sodium carboxymethyl cellulose (CMC) as the thickener, and conductive carbon black (SP) as the negative electrode conductive agent. The negative electrode functional additive used is the activated carbon loaded with nano-nickel particles obtained in this embodiment. The above materials are mixed in a mass ratio of negative electrode active material: negative electrode binder: thickener: negative electrode conductive agent: negative electrode functional additive = 95.6:1.8:1.2:0.6:0.8 and dispersed in deionized water to prepare a negative electrode slurry. The negative electrode slurry is coated onto a current collector copper foil, and then baked, rolled, and slit to obtain the negative electrode sheet of this embodiment. The negative electrode functional additive accounts for 0.8% of the mass of the negative electrode active material layer.
[0039] 3. Preparation of positive electrode sheet The raw materials used to prepare the positive electrode active material layer include positive electrode active material, positive electrode binder, and positive electrode conductive agent. In this embodiment, lithium iron phosphate is used as the positive electrode active material, polyvinylidene fluoride (PVDF) is used as the positive electrode binder, and conductive carbon black (SP) is used as the positive electrode conductive agent. The above materials are mixed at a mass ratio of positive electrode active material: positive electrode binder: positive electrode conductive agent = 97:2:1 and dispersed in the solvent N-methylpyrrolidone (NMP) to prepare a positive electrode slurry. The positive electrode slurry is coated on the current collector aluminum foil, and then baked, rolled, and slit to obtain the positive electrode sheet of this embodiment.
[0040] 4. Assemble lithium-ion batteries A commercial PE separator was used as the separator for assembling the lithium-ion battery in this embodiment. The positive electrode, negative electrode, and separator prepared in this embodiment were assembled into a battery, injected with the electrolyte prepared in this embodiment, and encapsulated to obtain a lithium-ion battery.
[0041] Example 2 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery comprising the same. The only difference between this embodiment and Example 1 is that 1-undecene is used in place of 1-heptene in Example 1 as an α-olefin in the electrolyte additive. Apart from the above difference, the raw materials and their proportions used in preparing the electrolyte, as well as the corresponding operating steps, are consistent with those in Example 1.
[0042] Subsequently, the electrolyte prepared in this embodiment was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0043] Example 3 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the same. The only difference between this embodiment and Example 1 is that the α-olefin in the electrolyte additive is replaced by 1-nonene instead of 1-heptene; that is, in this embodiment, 1-nonene is used as the aforementioned α-olefin. Apart from the above difference, the raw materials and their proportions used in preparing the electrolyte, as well as the corresponding operating steps, are consistent with those in Example 1.
[0044] Subsequently, the electrolyte prepared in this embodiment was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0045] Example 4 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that, based on the total mass of the electrolyte, the amounts of EC and α-olefin are adjusted so that the mass percentages of EC and α-olefin in the electrolyte are 31% and 2%, respectively. The sum of the mass percentages of EC and α-olefin in the electrolyte of this embodiment is equal to the sum of the mass percentages of EC and α-olefin in the electrolyte of Example 1. That is, the electrolyte formulation (calculated by mass percentage) used in this embodiment is: α-olefin 2%, VC 3%, FEC 0.5%, TMSP 0.5%, EC 31%, EMC 20%, DMC 30%, LiPF6 13%. Among them, the α-olefin used in this embodiment is still 1-heptene. The mass ratio of EC to α-olefin is 31:2, i.e., 15.5. Apart from the above differences, the raw materials and their proportions used in preparing the electrolyte in this embodiment, as well as the corresponding operating steps, are consistent with those in Example 1.
[0046] Subsequently, the electrolyte prepared in this embodiment was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0047] Example 5 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that, based on the total mass of the electrolyte, the amounts of EC and α-olefin are adjusted so that the mass percentages of EC and α-olefin in the electrolyte are 28% and 5%, respectively. The sum of the mass percentages of EC and α-olefin in the electrolyte of this embodiment is equal to the sum of the mass percentages of EC and α-olefin in the electrolyte of Example 1. That is, the electrolyte formulation (calculated by mass percentage) used in this embodiment is: α-olefin 5%, VC 3.0%, FEC 0.5%, TMSP 0.5%, EC 28%, EMC 20%, DMC 30%, LiPF6 13%. Among them, the α-olefin used in this embodiment is still 1-heptene. The mass ratio of EC to α-olefin is 28:5, i.e., 5.6. Apart from the above differences, the raw materials and their proportions used in preparing the electrolyte in this embodiment, as well as the corresponding operating steps, are consistent with those in Example 1.
[0048] Subsequently, the electrolyte prepared in this embodiment was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0049] Example 6 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that, based on the total mass of the electrolyte, the amounts of EC and α-olefin are adjusted so that the mass percentages of EC and α-olefin in the electrolyte are 25% and 8%, respectively. The sum of the mass percentages of EC and α-olefin in the electrolyte of this embodiment is equal to the sum of the mass percentages of EC and α-olefin in the electrolyte of Example 1. That is, the electrolyte formulation (calculated by mass percentage) used in this embodiment is: α-olefin 8%, VC 3%, FEC 0.5%, TMSP 0.5%, EC 25%, EMC 20%, DMC 30%, LiPF6 13%. Among them, the α-olefin used in this embodiment is still 1-heptene. The mass ratio of EC to α-olefin is 25:8, i.e., 3.125. Apart from the above differences, the raw materials and their proportions used in preparing the electrolyte in this embodiment, as well as the corresponding operating steps, are consistent with those in Example 1.
[0050] Subsequently, the electrolyte prepared in this embodiment was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0051] Example 7 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that, based on the total mass of the electrolyte, the amounts and types of EC, EMC, DMC, and lithium salt are adjusted to EC 22%, EMC 19%, DMC 34%, and lithium salt 16%, and the lithium salt is replaced by lithium hexafluorophosphate (LiPF6) with lithium bisfluorosulfonylimide (LiFSI). That is, the electrolyte formulation used in this embodiment (calculated by mass percentage) is: α-olefin 5%, VC 3%, FEC 0.5%, TMSP 0.5%, EC 22%, EMC 19%, DMC 34%, and LiFSI 16%. Among them, the α-olefin used in this embodiment is still 1-heptene. The mass ratio of EC to α-olefin is 22:5, i.e., 4.4. Apart from the above differences, the raw materials and their proportions used in preparing the electrolyte in this embodiment, as well as the corresponding operating steps, are consistent with those in Example 1.
[0052] Subsequently, the electrolyte prepared in this embodiment was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0053] Example 8 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that the nano-metal particles in the negative electrode functional additive are replaced with copper instead of nickel. That is, the negative electrode functional additive used in this embodiment is activated carbon particles loaded with nano-copper particles. Correspondingly, in the preparation process of the negative electrode functional additive, nickel nitrate hexahydrate used in Example 1 is replaced with copper nitrate trihydrate. Specifically, the operation for preparing the negative electrode functional additive loaded with nano-metal particles in this embodiment is as follows: Activated carbon is pulverized and ground into D 50The powder is approximately 15 μm in size. 1.3 g of copper nitrate trihydrate (Cu(NO3)2·3H2O) was dissolved in 50 mL of deionized water to obtain a metal ion solution. 10 g of finely ground activated carbon powder was added to the metal ion solution and stirred until homogeneous. The sample was then impregnated under vacuum for 12 hours to allow the activated carbon to fully absorb Cu(NO3)2·3H2O. The impregnated sample was dried in an oven at 120°C for 12 hours. The dried sample underwent a carbothermic reduction reaction in a tube furnace under a nitrogen atmosphere. The reaction temperature was 600°C, and the reaction time was 4 hours. The sample was then cooled to room temperature under a nitrogen atmosphere to obtain a negative electrode functional additive loaded with nano-metal particles. In this embodiment, the nano-metal particles originated from Cu(NO3)2·3H2O in the raw material; therefore, the negative electrode functional additive obtained in this embodiment is activated carbon loaded with nano-copper particles. In the preparation of the negative electrode sheet, the specific operations of Example 1 are followed, with the activated carbon loaded with nano-copper particles prepared in this example replacing the activated carbon loaded with nano-nickel particles in Example 1 by an equal mass as a negative electrode functional additive. Except for the differences mentioned above, the raw materials, their proportions, and corresponding operating steps used in preparing the negative electrode sheet in this example are consistent with those in Example 1.
[0054] Subsequently, the negative electrode sheet prepared in this embodiment was used to replace the negative electrode sheet used in Example 1, and the same electrolyte, positive electrode sheet, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations of Example 1 regarding the assembly of lithium-ion batteries.
[0055] Example 9 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that no negative electrode functional additive is added to the negative electrode active material layer of the negative electrode sheet. Specifically, in preparing the negative electrode active material layer, activated carbon particles loaded with nano-metal particles are not used; only graphite, styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), and conductive carbon black (SP) are used as the negative electrode active material. The above four components are mixed according to the mass ratio in Example 1 except for the negative electrode functional additive, i.e., graphite:SBR:CMC:SP=95.6:1.8:1.2:0.6. Apart from the above differences, the raw materials and their proportions used in preparing the negative electrode sheet, the corresponding operation steps, and the electrolyte, positive electrode sheet, separator, and lithium-ion battery assembly operations used in this embodiment are the same as in Example 1.
[0056] Subsequently, the negative electrode sheet prepared in this embodiment was used to replace the negative electrode sheet used in Example 1, and the same electrolyte, positive electrode sheet, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations of Example 1 regarding the assembly of lithium-ion batteries.
[0057] Example 10 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that the mass percentage of the negative electrode functional additive in the negative electrode active material layer is adjusted to 0.2%. Specifically, the negative electrode functional additive used in this embodiment is the same as that in Example 1, which is activated carbon particles loaded with nano-nickel particles. Based on the total mass of the negative electrode active material layer, the mass of the negative electrode functional additive accounts for 0.2% of the total mass of the negative electrode active material layer in this embodiment. The other components in the negative electrode active material layer, excluding the negative electrode functional additive, namely the negative electrode active material graphite, the negative electrode binder styrene-butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC), and the negative electrode conductive agent conductive carbon black (SP), maintain the same mass ratio as in Example 1, namely graphite:SBR:CMC:SP=95.6:1.8:1.2:0.6, and the amount of each component is adjusted accordingly so that the total mass of the above materials accounts for 99.8% of the total mass of the negative electrode active material layer. Apart from the differences mentioned above, the raw materials and their proportions used in preparing the negative electrode sheet in this embodiment, as well as the corresponding operating steps, are consistent with those in Example 1. The electrolyte, positive electrode sheet, separator, and assembly operation of the lithium-ion battery are also the same as those in Example 1.
[0058] Subsequently, the negative electrode sheet prepared in this embodiment was used to replace the negative electrode sheet used in Example 1, and the same electrolyte, positive electrode sheet, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations of Example 1 regarding the assembly of lithium-ion batteries.
[0059] Example 11 Referring to Example 1, this embodiment provides an electrolyte and a lithium-ion battery including the electrolyte. The only difference between this embodiment and Example 1 is that the mass ratio of the negative electrode functional additive in the negative electrode active material layer is adjusted to 1.5%. Specifically, the negative electrode functional additive used in this embodiment is the same as that in Example 1, which is activated carbon particles loaded with nano-nickel particles. Based on the total mass of the negative electrode active material layer, the mass of the negative electrode functional additive accounts for 1.5% of the total mass of the negative electrode active material layer in this embodiment. The other components in the negative electrode active material layer, excluding the negative electrode functional additive, namely the negative electrode active material graphite, the negative electrode binder styrene-butadiene rubber (SBR), the thickener sodium carboxymethyl cellulose (CMC), and the negative electrode conductive agent conductive carbon black (SP), maintain the same mass ratio as in Example 1, namely graphite:SBR:CMC:SP=95.6:1.8:1.2:0.6, and the amount of each component is adjusted accordingly so that the total mass of the above materials accounts for 98.5% of the total mass of the negative electrode active material layer. Apart from the differences mentioned above, the raw materials and their proportions used in preparing the negative electrode sheet in this embodiment, as well as the corresponding operating steps, are consistent with those in Example 1. The electrolyte, positive electrode sheet, separator, and assembly operation of the lithium-ion battery are also the same as those in Example 1.
[0060] Subsequently, the negative electrode sheet prepared in this embodiment was used to replace the negative electrode sheet used in Example 1, and the same electrolyte, positive electrode sheet, and separator as in Example 1 were used to assemble the lithium-ion battery of this embodiment according to the relevant operations of Example 1 regarding the assembly of lithium-ion batteries.
[0061] Comparative Example 1 Referring to Example 1, this comparative example provides an electrolyte and a lithium-ion battery comprising the same. The only difference between this comparative example and Example 1 is that the electrolyte does not contain α-olefins. Apart from the absence of α-olefins, the types of raw materials used to prepare the electrolyte in this comparative example are the same as in Example 1. When preparing the electrolyte, each raw material is prepared in exactly the same mass ratio as the corresponding material in Example 1. Apart from the above differences, the raw materials used and their proportions, as well as the corresponding operating steps, in preparing the electrolyte in this comparative example are consistent with those in Example 1.
[0062] Subsequently, the electrolyte prepared in this comparative example was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this comparative example according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0063] Comparative Example 2 Referring to Example 1, this comparative example provides an electrolyte and a lithium-ion battery comprising the same. The only difference between this comparative example and Example 1 is that this comparative example does not use α-olefins in the electrolyte preparation; instead, 1-fluoro-1-heptene is used in an equal mass fraction to replace 1-heptene used in Example 1. In other words, the electrolyte in this comparative example does not contain α-olefins. Apart from the above differences, the raw materials and their proportions used in preparing the electrolyte in this comparative example, as well as the corresponding operating steps, are consistent with those in Example 1.
[0064] Subsequently, the electrolyte prepared in this comparative example was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this comparative example according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0065] Comparative Example 3 Referring to Example 1, this comparative example provides an electrolyte and a lithium-ion battery comprising the same. The only difference between this comparative example and Example 1 is that this comparative example does not use α-olefins in the electrolyte preparation; instead, it uses heptane in equal mass to replace 1-heptene used in Example 1. In other words, the electrolyte in this comparative example does not contain α-olefins. Apart from the above differences, the raw materials and their proportions used in preparing the electrolyte, as well as the corresponding operating steps, are consistent with those in Example 1.
[0066] Subsequently, the electrolyte prepared in this comparative example was used instead of the electrolyte used in Example 1, and the same negative electrode, positive electrode, and separator as in Example 1 were used to assemble the lithium-ion battery of this comparative example according to the relevant operations for assembling lithium-ion batteries in Example 1.
[0067] Test case 1. Test subjects and test items This test example uses the lithium-ion batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 3 as test objects, and conducts high-temperature cycle life test and cycle gas generation pressure test on each test object.
[0068] (1) The method for high-temperature cycle life testing is as follows: The test object is clamped with a metal clamp and then placed in a constant temperature environment of 45℃. It is charged at a constant current and constant voltage of 0.5 C to 3.65 V, with a cutoff current of 0.05 C. Then, the test object is discharged at 0.5 C to 2.5 V, and the discharge capacity of the test object in the first cycle is recorded. The above charging and discharging steps are continued until 1000 cycles are completed. The discharge capacity of the 1000th cycle is recorded, and the capacity retention rate is calculated according to the following formula: Capacity retention rate = (Discharge capacity at 1000th cycle / Discharge capacity at the first cycle) × 100%.
[0069] (2) The method of cyclic gas pressure test is as follows: a gas needle is reserved on the shell of the test object, the gas needle is connected to the pressure sensor, and after the above high temperature cycle life test is completed, the pressure value of the pressure sensor is read, which is the internal gas pressure of the test object after the cycle.
[0070] 2. Test Results The test results for this test example are shown in Table 1. As can be seen from Table 1, in the high-temperature cycling test set in this test example, the capacity retention rate of the lithium-ion batteries in Examples 1-11 was generally higher than that of the lithium-ion batteries in Comparative Examples 1-3. After high-temperature cycling, the internal gas pressure of the lithium-ion batteries in Examples 1-11 was generally lower than that of the lithium-ion batteries in Comparative Examples 1-3. The electrolytes used in Examples 1-11 all contained α-olefins as electrolyte additives. These α-olefins are pure hydrocarbons without halogen substitution. Their terminal α-double bonds can, under negative electrode voltage, gain electrons with hydrogen ions generated in the electrolyte due to solvent decomposition or the reaction of lithium salt with trace amounts of water, undergoing an electrochemical reduction and hydrogenation reaction. This converts corrosive hydrogen ions into electrochemically inert saturated alkanes, thereby reducing acidic substances in the electrolyte at the source, inhibiting the erosion and damage of the negative electrode SEI film by acidic substances, reducing the irreversible consumption of active lithium, and suppressing gas generation caused by the accumulation of acidic substances. Meanwhile, α-olefins and their hydrogenation products, alkanes, exhibit high redox stability on the positive and negative electrode surfaces and do not participate in side reactions at the electrode interface. Therefore, they can maintain stable battery cycle performance while removing acidic substances.
[0071] Unlike Examples 1-11, the electrolytes used in Comparative Examples 1-3 did not contain α-olefins. The following comparisons will use Example 1 as a control to analyze the reasons for the aforementioned performance differences.
[0072] Example 1 was compared with Comparative Example 1, the difference being that Comparative Example 1 did not introduce α-olefins as electrolyte additives. The test results show that the lithium-ion battery of Comparative Example 1 had a relatively low capacity retention rate and a relatively high internal gas pressure after cycling. This indicates that in the absence of α-olefins in the electrolyte, acidic substances generated by solvent decomposition or the reaction of lithium salts with trace amounts of moisture cannot be effectively removed. This leads to increased erosion of the negative electrode interface by acidic substances, increased consumption of active lithium, and gas accumulation, ultimately resulting in decreased cycle performance and increased internal pressure.
[0073] In Comparative Example 2, 1-fluoro-1-heptene was used instead of the 1-heptene used in Example 1 in the electrolyte formulation. The group connecting the carbon-carbon double bond in the 1-fluoro-1-heptene molecule is a fluoroalkyl group, which does not meet the structural requirement that R in α-olefins must be a straight-chain or branched saturated alkyl group; therefore, this compound does not belong to α-olefins. Compared with the lithium-ion battery of Example 1, the lithium-ion battery of Comparative Example 2 showed lower capacity retention and higher internal gas pressure after high-temperature cycling. This indicates that fluorinated olefins are difficult to achieve acid removal effects comparable to α-olefins, and fluorinated olefins may undergo side reactions with the negative electrode, which is detrimental to the improvement of battery cycle performance and gas generation suppression.
[0074] Comparative Example 3 replaced 1-heptene with heptane in Example 1. Heptane is a saturated alkane and does not contain carbon-carbon double bonds, thus it cannot undergo an electrochemical reduction hydrogenation reaction on the negative electrode surface. Compared to the lithium-ion battery of Example 1, the lithium-ion battery of Comparative Example 3 showed lower capacity retention and higher internal gas pressure after high-temperature cycling. This indicates that if only a saturated alkane with a structure similar to the hydrogenation product of α-olefins is added to the electrolyte, without introducing α-olefins with α-double bonds, the hydrogen ions in the electrolyte cannot be consumed through an electrochemical reduction hydrogenation reaction. Acidic substances will continue to corrode the negative electrode interface and cause active lithium consumption and gas generation, thus limiting the improvement of cycle performance.
[0075] Overall, the lithium-ion batteries of Examples 1-11 are superior to the lithium-ion batteries of Comparative Examples 1-3 in terms of capacity retention and internal gas pressure after cycling. This indicates that introducing α-olefins as electrolyte additives can effectively remove acidic substances in the electrolyte, suppress gas generation caused by the accumulation of acidic substances, and avoid battery side reactions induced by the introduction of additives, thus maintaining good cycle performance of lithium-ion batteries.
[0076] Examples 1, 2, and 3 used 1-heptene, 1-undecene, and 1-nonene as α-olefins in the electrolyte, respectively. As mentioned above, compared to the lithium-ion batteries in Comparative Examples 1-3, the lithium-ion batteries in Examples 1-3 all achieved higher high-temperature cycle capacity retention and lower internal gas pressure after high-temperature cycling, indicating that the aforementioned α-olefins can effectively suppress the gas generation of acidic substances in the electrolyte. Furthermore, compared to Example 2 using 1-undecene and Example 3 using 1-nonene, the lithium-ion battery prepared in Example 1 using 1-heptene showed relatively higher capacity retention and lower internal gas pressure after cycling, indicating that selecting 1-heptene as the α-olefin in the electrolyte formulation can further improve the cycle life of the lithium-ion battery and suppress gas generation.
[0077] The main difference between Examples 1, 4, 5, 6, and 7 lies in the different mass ratios of EC to α-olefins in the electrolyte. In Example 4, the mass of α-olefin accounted for 2% of the total mass of the electrolyte, EC accounted for 31%, and the mass ratio of EC to α-olefin was 15.5. In Example 5, the α-olefin accounted for 5% of the total mass of the electrolyte, EC accounted for 28%, and the mass ratio of EC to α-olefin was 5.6. In Example 1, the mass of α-olefin accounted for 6% of the total mass of the electrolyte, EC accounted for 27%, and the mass ratio of EC to α-olefin was 4.5. In Example 6, the mass of α-olefin accounted for 8% of the total mass of the electrolyte, EC accounted for 25%, and the mass ratio of EC to α-olefin was 3.125. In Example 7, the α-olefin accounted for 5% of the total mass of the electrolyte, EC accounted for 22%, the mass ratio of EC to α-olefin was 4.4, and the lithium salt was replaced by lithium bis(fluorosulfonyl)imide instead of lithium hexafluorophosphate.
[0078] A comparison of the test results from Examples 1, 4, 5, 6, and 7 shows that as the mass percentage of α-olefins in the electrolyte increases, the electrolyte's ability to remove acidic substances is correspondingly enhanced, and the internal pressure generally decreases after cycling. Among the lithium-ion batteries provided in the above examples, the lithium-ion battery in Example 4 has the lowest α-olefin content in the electrolyte, resulting in a relatively limited removal effect on acidic substances. Therefore, the lithium-ion battery in Example 4 has the highest internal pressure after cycling, and its cycle performance is inferior to that of the lithium-ion batteries in the other examples. As the α-olefin content in the electrolyte gradually increases, the effect of suppressing gas generation caused by the accumulation of acidic substances gradually strengthens, and the internal pressure decreases accordingly after cycling. However, at the same time, α-olefins are non-polar hydrocarbons, and their introduction reduces the overall dielectric constant of the electrolyte system, thereby affecting the dissociation and conductivity of lithium salts. When the mass ratio of EC to α-olefin is greater than 4, as in the electrolytes prepared in Examples 1, 5, and 7, EC can effectively compensate for the decrease in dielectric constant of the electrolyte system due to the addition of α-olefin, maintaining good dissociation of lithium salt and electrolyte conductivity. Therefore, the lithium-ion batteries in these examples can maintain high capacity retention after high-temperature cycling. However, when the mass ratio of EC to α-olefin in the electrolyte is not higher than 4, as in the electrolyte prepared in Example 6, the relatively insufficient EC content and the introduction of α-olefin cause a significant decrease in the dielectric constant of the electrolyte system, affecting the electrolyte conductivity and reducing the kinetic transport efficiency of lithium ions in the electrolyte. Therefore, compared to the lithium-ion batteries of Examples 1, 5, and 7, the measured capacity retention of the lithium-ion battery in Example 6 is lower. In summary, by controlling the mass ratio of EC to α-olefins in the electrolyte to be above 4, it is possible to effectively remove acidic substances and suppress gas production using α-olefins, while also taking into account the dissociation and conductivity of lithium salts in the electrolyte, thereby enabling lithium-ion batteries to achieve better high-temperature cycle performance.
[0079] Comparing Examples 1, 8, and 9, the differences are as follows: the negative electrode active material layer prepared in Example 9 does not contain any negative electrode functional additives; the negative electrode active material layer prepared in Example 1 contains activated carbon particles loaded with nano-nickel particles; and the negative electrode active material layer prepared in Example 8 contains activated carbon particles loaded with nano-copper particles. The test results show that, compared with the lithium-ion battery of Example 9, the lithium-ion batteries of Examples 1 and 8 maintain higher capacity retention and achieve lower internal pressure after high-temperature cycling tests. This is because in Examples 1 and 8, a negative electrode functional additive was used to participate in the construction of the negative electrode active material layer. The activated carbon in the negative electrode functional additive has a porous structure and a high specific surface area, which can effectively adsorb and enrich α-olefins in the electrolyte, thereby increasing the concentration of α-olefins near the negative electrode interface, which is conducive to the occurrence of reduction hydrogenation reaction. Meanwhile, the nano-metal particles supported in the activated carbon act as a highly efficient catalyst for electrochemical hydrogenation reaction, which can reduce the activation energy of α-olefin reduction hydrogenation reaction, improve the α-olefin removal efficiency of hydrogen ions, enhance the ability to suppress gas production caused by the accumulation of acidic substances, and thus improve the high-temperature cycle capacity retention rate of lithium-ion battery and reduce the internal gas pressure after cycling.
[0080] The main difference between Examples 1, 10, and 11 lies in the different mass percentages of the negative electrode functional additive in the negative electrode active material layer. Specifically, the mass percentages of the negative electrode functional additive in the negative electrode active material layer in Examples 10, 1, and 11 are 0.2%, 0.8%, and 1.5%, respectively. Compared to Example 9, which did not add any negative electrode functional additive to the negative electrode active material layer, the lithium-ion batteries of Examples 1, 10, and 11 all maintained high capacity retention and low post-cycle internal pressure after high-temperature cycling tests.
[0081] Table 1. Statistics of test results for this test case
[0082] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention, but such modifications or substitutions are all within the scope of protection of the present invention.
Claims
1. An electrolyte, characterized in that, The electrolyte comprises an electrolyte additive, an organic solvent, and a lithium salt. The electrolyte additive includes an α-olefin, which is a compound represented by CH2=CH-R, wherein R is a straight-chain or branched saturated alkyl group, and the general formula of R is C2. n H 2n+1 The expression indicates that n is a positive integer selected from 5 to 9.
2. The electrolyte according to claim 1, characterized in that, The α-olefin includes at least one of 1-heptene, 1-octene, 1-nonene, 1-decene, and 1-undecene.
3. The electrolyte according to claim 2, characterized in that, The α-olefin is 1-heptene.
4. The electrolyte according to claim 1, characterized in that, The organic solvent includes ethylene carbonate, and the mass ratio of ethylene carbonate to the α-olefin is greater than 4.
5. The electrolyte according to claim 1, characterized in that, The α-olefin accounts for 2% to 10% of the total mass of the electrolyte.
6. The electrolyte according to claim 1, characterized in that, The electrolyte additive also includes at least one of vinylene carbonate, fluoroethylene carbonate, and tris(trimethylsilyl)phosphite.
7. The electrolyte according to claim 1, characterized in that, The electrolyte satisfies at least one of the following a and b: a. The organic solvent further includes at least one of propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethyl acetate, and ethyl propionate; b. The lithium salt includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium perchlorate, and lithium bis(oxalato)borate.
8. A lithium-ion battery, characterized in that, The lithium-ion battery includes a positive electrode, a negative electrode, and an electrolyte according to any one of claims 1 to 7.
9. The lithium-ion battery according to claim 8, characterized in that, The negative electrode includes a negative electrode active material layer, the negative electrode active material layer includes a negative electrode functional additive, the negative electrode functional additive includes activated carbon particles loaded with nano-metal particles, and the nano-metal particles include at least one of nickel, iron, copper, and manganese.
10. The lithium-ion battery according to claim 9, characterized in that, The mass of the nano-metal particles accounts for 1% to 6% of the mass of the activated carbon particles, and the mass of the negative electrode functional additive accounts for 0.2% to 1.5% of the total mass of the negative electrode active material layer.