A tetrasubstituted urea-based high-voltage electrolyte, its preparation method and application
By constructing a deep eutectic system of tetrasubstituted urea-based high-voltage electrolyte, the problem of oxidation decomposition of anode-less sodium-ion batteries under high voltage and high temperature conditions was solved, thereby improving the high-voltage cycle life and thermal safety of the battery.
Patent Information
- Application Number
- CN202611613381.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-19
- Publication Date
- 2026-11-17
Smart Images

Figure QLYQS_1
Abstract
Description
Technical Field
[0001] This application belongs to the field of sodium-ion battery technology, and particularly relates to a tetrasubstituted urea-based high-voltage electrolyte, its preparation method and application. Background Technology
[0002] Electrodeless sodium-ion batteries eliminate the traditional negative electrode active material, relying on in-situ deposition of metallic sodium on the current collector surface to achieve the negative electrode function. They possess significant advantages such as simplified cell structure, reduced manufacturing costs, and significantly improved energy density, making them promising for large-scale and portable energy storage applications. However, because the electrodeless system lacks a buffer layer of negative electrode active material, metallic sodium directly nucleates and grows on the current collector surface. This sodium deposition behavior is highly sensitive to electrolyte composition, easily leading to problems such as repeated rupture and regeneration of the interfacial film, sodium dendrite growth, and a continuous increase in interfacial impedance. Therefore, electrodeless sodium-ion batteries place stringent requirements on the electrolyte: it must possess excellent high-temperature thermal stability to construct a stable interfacial passivation film on both the positive and negative electrodes, suppressing solvent decomposition and gas generation at high temperatures and the degradation of the positive electrode active material; simultaneously, it must ensure good sodium salt dissociation and ion conduction capabilities to meet the requirements of long-cycle operation over a wide temperature range.
[0003] Ether solvents, with their low viscosity and high ionic conductivity, exhibit good intrinsic compatibility with metallic sodium, making them the mainstream research focus for sodium-ion battery electrolytes. However, conventional chain-like ether electrolytes have significant drawbacks: firstly, the lone pair electrons of ether molecules are prone to oxidative decomposition at high temperatures and pressures on the positive electrode side, resulting in insufficient thermal stability, exacerbated side reactions, and severe gas generation in the cell under high-temperature conditions; secondly, the solvation sheath layer of traditional ether electrolytes is dominated by a large number of free ether molecules, with limited sodium salt dissociation, making it difficult to induce the formation of a dense and stable interfacial film on the electrode surface. During high-temperature cycling, the CEI and SEI films are easily damaged and detached, failing to effectively suppress transition metal dissolution and sodium dendrite growth, thus limiting the high-temperature cycle life and thermal safety performance of anode-less sodium-ion batteries.
[0004] Given that conventional ether electrolytes have limited oxidation resistance, they are prone to oxidation and decomposition on the surface of layered oxide cathodes under high-voltage conditions, generating gas and inducing lattice instability in the cathode. This makes it difficult to meet the high-voltage cycling and thermal safety requirements of anode-less sodium batteries. This application aims to provide a solution to the above problems. Summary of the Invention
[0005] The first objective of this application is to provide a tetrasubstituted urea-based high-voltage electrolyte to solve the problem of oxidative decomposition of ether electrolytes under high-voltage conditions, thereby improving the high-voltage cycle life and thermal safety performance of a cathodeless sodium battery.
[0006] To achieve the above-mentioned objectives, this application adopts the following technical solution: A tetrasubstituted urea-based high-voltage electrolyte comprises a solvent and a sodium salt. The solvent includes tetrasubstituted urea solvents and chain ether solvents, wherein the tetrasubstituted urea solvent conforms to the following general formula: ; In the formula: R1, R2, R3 and R4 are each independently selected from straight-chain or branched alkyl groups having 1-6 carbon atoms; The sodium salt comprises at least one electron-rich sodium salt.
[0007] Further settings are as follows: The tetrasubstituted urea solvent is selected from at least one of tetramethylurea, 1,1,3,3-tetraethylurea, and 1,1,3,3-tetra-n-butylurea.
[0008] The chain ether solvent is selected from at least two of dimethyl acetal, propylene glycol dimethyl ether, 1,2-diethoxypropane, diethoxymethane, dimethyl alcohol acetal, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol diethyl ether, and ethylene glycol dibutyl ether, and contains at least one of dimethyl acetal, propylene glycol dimethyl ether, and 1,2-diethoxypropane.
[0009] The mass ratio of the tetrasubstituted urea solvent to the chain ether solvent is 1:4 to 1:1.
[0010] The sodium salt is selected from at least one of NaPF6, NaClO4, NaBF4, NaAsF6, NaODFB, NaOTF, NaFSI, and NaTFSI, and includes at least one of the electron-rich sodium salts NaClO4, NaFSI, and NaTFSI.
[0011] The concentration of the sodium salt is 0.9–3.5 mol / L, preferably 1.2–2.5 mol / L.
[0012] The mechanism of action of this application is as follows: This application constructs a synergistic urea-based deep eutectic electrolyte system consisting of a tetrasubstituted urea solvent, a high-voltage resistant branched ether, and an electron-rich sodium salt, wherein: (1) Tetrasubstituted urea solvents contain a strongly polar urea carbonyl group. The carbonyl oxygen acts as a Lewis base and can react with Na. + Coordination occurs; the anions contained in the electron-rich NaTFSI, NaFSI, and NaClO4 have strong dipole interactions with the tetrasubstituted urea solvents, which can significantly enhance the dissociation degree of sodium salts and promote the formation of a room-temperature stable ionic deep eutectic electrolyte between the solvent and sodium salts, ensuring the system's excellent ion conductivity; the eutectic structure can effectively suppress the negative electrode reduction side reaction caused by the strong polarity of urea solvents, while the deep eutectic effect can significantly reduce the melting point of the system and broaden the working range of the electrolyte in liquid state.
[0013] (2) The tetrasubstituted urea solvent used in this application has a urea bond -N-CO-N- molecular skeleton, which does not have α-H sites that are easily attacked by thermal reduction intermediates, resulting in higher intrinsic thermal stability. At the same time, the strong solvation complexation between the tetrasubstituted urea and sodium ions can bind free solvent molecules, reduce direct contact between the solvent and metallic sodium, effectively suppress the exothermic side reaction between the solvent and sodium metal, and improve the overall thermal safety level of the electrolyte. Meanwhile, the introduction of methyl-substituted branched ether solvents into the system can significantly reduce the bulk viscosity of the tetrasubstituted urea electrolyte and improve ion migration ability. On the other hand, these branched ethers have excellent oxidation resistance and work synergistically with the deep eutectic system to jointly improve the high-voltage withstand capability of the electrolyte.
[0014] On the positive electrode side, the tetrasubstituted urea-branched ether eutectic system can construct a stable passivation interface film on the surface of the high-voltage layered oxide positive electrode, preventing direct contact between the electrolyte and the positive electrode material, inhibiting solvent oxidation and decomposition, transition metal dissolution, and positive electrode lattice destruction under high voltage, and alleviating gas generation problems. On the side without sodium metal in the negative electrode, this deep eutectic system reconstructs the sodium ion solvation sheath, regulates the sodium ion desolvation behavior, induces the formation of a stable negative electrode interface film, inhibits repeated rupture and regeneration of the interface film, alleviates sodium dendrite growth, and avoids continuous accumulation of interface impedance.
[0015] (3) This application solves the problems of high-voltage interface oxidation decomposition and insufficient thermal safety of electrodeless sodium-ion batteries by means of the deep eutectic synergistic effect of tetrasubstituted urea solvents, high-voltage resistant branched ethers and electron-rich sodium salts, from multiple dimensions such as sodium salt dissociation regulation, elimination of weak sites of α-H thermal decomposition, reduction of system viscosity, widening of liquid window, and high voltage protection of positive and negative electrode dual interfaces, significantly improving the high voltage cycle life and thermal safety performance of electrodeless sodium batteries.
[0016] The second aspect of this application is to provide a method for preparing a tetrasubstituted urea-based high-voltage electrolyte, comprising the following steps: in an argon atmosphere glove box with a water content of <10ppm, dissolving sodium salt in a mixed solvent of a tetrasubstituted urea solvent and a chain ether solvent, stirring until completely dissolved, to obtain a tetrasubstituted urea-based high-voltage electrolyte.
[0017] The third objective of this application is to provide an application of a tetrasubstituted urea-based high-voltage electrolyte in a negative electrode-free sodium-ion battery.
[0018] The negative electrode-free sodium-ion battery includes a positive electrode, a negative electrode current collector, an electrolyte, and a separator.
[0019] The cathode material is selected from layered oxide cathode materials and polyanionic cathode materials.
[0020] The layered oxide cathode material is selected from any one of the following compounds: NaCoO2, NaMnO2, NaNiO2, NaCrO2, NaNi0.5 Mn 0.5 O2, NaNi 0.5 Ti 0.5 O2, NaFe 0.5 Mn 0.5 O2, NaCu 0.5 Fe 0.5 O2, NaNi 0.33 Fe 0.33 Mn 0.33 O2, NaNi 0.33 Co 0.33 Mn 0.33 O2; preferably NaNi 0.33 Fe 0.33 Mn 0.33 O2.
[0021] The polyanionic cathode material is selected from any one of the following compounds: Na2FeP2O7, Na2MnP2O7, Na4Fe3(PO4)2P2O7; Na2Fe2(SO4)3, Na2Fe2(PO4)(SO4)2, Na4Fe3(PO4)2P2O7.
[0022] The diaphragm is selected from any one of polyethylene monolayer membrane (PE), polypropylene monolayer membrane (PP), multilayer microporous membrane composed of PP and PE, cellulose nonwoven fabric, polyvinylidene fluoride porous membrane, polyimide electrospun porous membrane, and glass fiber diaphragm, preferably glass fiber diaphragm.
[0023] The negative electrode current collector is made of aluminum foil or copper foil, and a conductive coating is coated on the surface of the negative electrode current collector. The conductive coating is at least one of graphene, carbon nanotubes or hard carbon, and the coating thickness is 1 to 5 μm.
[0024] Compared with existing technical solutions, this application has the following advantages: (1) This application provides a tetrasubstituted urea-based high-voltage electrolyte, which adopts a deep eutectic synergistic system of "tetrasubstituted urea solvent - high-voltage resistant branched ether - electron-rich sodium salt", breaking through the technical bottleneck of easy oxidation and decomposition of traditional ether electrolytes under high pressure. This application selects a tetrasubstituted urea solvent that does not contain α-H sites in the molecule. Relying on the Lewis base effect of urea carbonyl oxygen to generate a strong dipole interaction with the electron-rich sodium salt anion, it significantly improves the dissociation ability of sodium salt and constructs an ionic deep eutectic electrolyte that can exist stably at room temperature. The deep eutectic interaction inhibits the sodium metal anode reduction side reaction caused by the strong polarity of urea solvent on the one hand, and significantly reduces the melting point of the system on the other hand, widening the liquid working temperature range of the electrolyte. At the same time, the system is compounded with high-voltage resistant branched ether, which can not only greatly reduce the high bulk viscosity of the tetrasubstituted urea system and improve ion migration efficiency, but also synergistically regulate the sodium ion solvation sheath, optimize the sodium ion desolvation energy barrier, and reduce the interfacial charge transfer impedance.
[0025] The tetrasubstituted urea-based high-voltage electrolyte of this application achieves long-term stability at both the positive and negative electrode interfaces under high-voltage conditions: a deep eutectic synergistic system of "tetrasubstituted urea solvent - high-voltage resistant branched ether - electron-rich sodium salt" can construct dense and stable passivation interface films on both the high-voltage positive electrode surface and the sodium metal deposition side. On the positive electrode side, the passivation film effectively prevents direct contact between the electrolyte and the high-voltage layered oxide positive electrode active material, inhibiting solvent oxidation and decomposition, transition metal dissolution, positive electrode lattice destruction, and cell gas generation under high-voltage conditions, maintaining the structural integrity of the positive electrode during high-voltage cycling. On the side without sodium metal in the negative electrode, the reconstructed solvation structure induces the formation of a stable negative electrode interface film, inhibiting repeated rupture and regeneration of the interface film, alleviating sodium dendrite growth, reducing the continuous accumulation of interface impedance, and significantly improving the high-voltage cycling stability and thermal safety performance of the battery.
[0026] (2) The electrolyte of this application, when applied to a negative electrode-free sodium-ion battery, exhibits excellent high-voltage, long-cycle electrochemical performance: The electrolyte is combined with layered oxides (NaNi) 0.33 Fe 0.33 Mn 0.33 An O2-based sodium-ion battery with no negative electrode exhibits a capacity retention of >80% after 500 cycles at 25°C with a cutoff voltage of 4.1V. Under even higher voltage conditions (4.2V cutoff voltage), the capacity retention remains >80% after 300 cycles at 25°C. This electrolyte effectively suppresses problems such as continuous oxidative decomposition, interfacial film failure and detachment, and positive electrode structure collapse under high voltage. It overcomes the shortcomings of traditional ether-based electrolytes, such as rapid capacity decay and large fluctuations in coulombic efficiency after increasing the cutoff voltage, ensuring the electrochemical reversibility of the battery under high voltage conditions. Furthermore, this electrolyte demonstrates good compatibility with polyanionic cathode materials, meeting the cycling requirements of different cathode systems.
[0027] (3) The electrolyte formulation of this application is simple and controllable, the raw materials are highly versatile, and it has good industrial adaptability: The solvent is obtained by compounding a tetrasubstituted urea solvent with a commercially available chain ether. The sodium salt is selected from commercially available sodium salts, requiring only that the system contains at least one electron-rich sodium salt, without the need for a large number of functional additives. This solution addresses the issue of high viscosity in urea solvents while maintaining good ionic conductivity and membrane wetting ability of the electrolyte. This electrolyte exhibits good compatibility with layered oxides, mainstream sodium-ion battery cathode materials, various membranes, and anode current collectors with carbon-based conductive coatings. The preparation process only requires dissolving the sodium salt in the mixed solvent and stirring in an inert glove box with low water content. The process is simple, compatible with existing battery cell mass production systems, has low implementation costs, and possesses good engineering and industrialization promotion value. Detailed Implementation
[0028] The technical solutions of this application will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of this application, and should not be construed as limiting the scope of protection of this application. All technologies implemented based on the above content of this application are covered within the scope of protection intended by this application.
[0029] Unless otherwise stated, the raw materials and reagents used in the following examples are commercially available products or can be prepared by known methods.
[0030] The following tetrasubstituted urea solvents were used in the examples: Solvent A: Tetramethylurea (TMU, CAS: 632-22-4); Solvent B: 1,1,3,3-Tetraethylurea (TEU, CAS: 1187-03-7); Solvent C: 1,1,3,3-Tetra-n-butylurea (TBU, CAS: 4559-86-8).
[0031] Example 1
[0032] A tetrasubstituted urea-based high-voltage electrolyte comprising a sodium salt and a mixed solvent.
[0033] Mixed solvent: composed of solvent A (tetramethylurea) and chain ether, with a mass ratio of solvent A to chain ether of 1:2; the chain ether is composed of propylene glycol dimethyl ether and diethylene glycol dimethyl ether; the mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether is 1:1.
[0034] Sodium salt: The common sodium salt NaPF6 and the electron-rich sodium salt NaTFSI are compounded. The total concentration of sodium salt is 2.0 mol / L, of which NaPF6 is 1.4 mol / L and NaTFSI is 0.6 mol / L.
[0035] Preparation method: In an argon glove box with a water content of <10ppm, fully dried NaPF6 and NaTFSI are added sequentially to the above mixed solvent, and the mixture is continuously magnetically stirred for 4-8 hours until the solid is completely dissolved and the system is homogeneous and transparent, thus obtaining a tetrasubstituted urea-based high-voltage electrolyte.
[0036] To investigate the effects of different sodium salt combinations on electrolyte performance, Examples 2-6 were set up.
[0037] Example 2
[0038] The preparation method is the same as in Example 1, except that the electron-rich sodium salt is replaced with NaClO4, and the total concentration of sodium salt is maintained at 2.0 mol / L, of which: NaPF6 1.4 mol / L + NaClO4 0.6 mol / L.
[0039] Example 3
[0040] The preparation method is the same as in Example 1, except that the electron-rich sodium salt is replaced with NaFSI, and the total sodium salt concentration is maintained at 2.0 mol / L, of which: NaPF6 1.4 mol / L + NaFSI 0.6 mol / L.
[0041] Example 4
[0042] The preparation method is the same as in Example 1, except that a single electron-rich sodium salt system is used, and the total sodium salt concentration is maintained at 2.0 mol / L, i.e., NaTFSI 2.0 mol / L.
[0043] Example 5
[0044] The preparation method is the same as in Example 1, except that the common sodium salt component is replaced with NaBF4, and the total sodium salt concentration is maintained at 2.0 mol / L, of which: NaBF4 1.4 mol / L + NaTFSI 0.6 mol / L.
[0045] Example 6
[0046] The preparation method is the same as in Example 1, except that the ordinary sodium salt component is replaced with NaOTF, and the total sodium salt concentration is maintained at 2.0 mol / L, of which: NaOTF 1.4 mol / L + NaClO4 0.6 mol / L.
[0047] To investigate the effects of different solvent systems on electrolyte performance, Examples 7-10 were set up.
[0048] Example 7
[0049] The preparation method is the same as in Example 1, except that the tetrasubstituted urea solvent is replaced with solvent B (1,1,3,3-tetraethylurea TEU).
[0050] Mixed solvent: The mass ratio of solvent B to the chain ether is 1:2; In the chain ether: the mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether is 1:1.
[0051] Example 8
[0052] The preparation method is the same as in Example 1, except that the tetrasubstituted urea solvent is replaced with solvent C (1,1,3,3-tetrabutylurea TBU).
[0053] Mixed solvent: The mass ratio of solvent C to chain ether is 1:2; In the chain ether: the mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether is 1:1.
[0054] Example 9
[0055] The preparation method is the same as in Example 1, except that the chain ether is replaced with propylene glycol dimethyl ether + ethylene glycol diethyl ether.
[0056] Mixed solvent: The mass ratio of solvent A to the chain ether is 1:2, and the chain ether is propylene glycol dimethyl ether + ethylene glycol diethyl ether, with a mass ratio of propylene glycol dimethyl ether + ethylene glycol diethyl ether of 1:1.
[0057] Example 10 The preparation method is the same as in Example 1, except that the mass ratio of solvent A to the chain ether is adjusted.
[0058] Mixed solvent: The mass ratio of solvent A to the chain ether is 1:4, the chain ether is propylene glycol dimethyl ether + diethylene glycol dimethyl ether, and the mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether is 1:1.
[0059] To investigate the effect of sodium salt concentration on electrolyte performance, Examples 11 and 12 were set up.
[0060] Example 11 The preparation method is the same as in Example 1, except that the total concentration of sodium salt is adjusted to 1.2 mol / L, wherein: NaPF6 0.84 mol / L + NaTFSI 0.36 mol / L.
[0061] Example 12 The preparation method is the same as in Example 1, except that the total concentration of sodium salt is adjusted to 2.5 mol / L, wherein: NaPF6 1.75 mol / L + NaTFSI 0.75 mol / L.
[0062] Comparative Example 1 The preparation method is the same as in Example 1, except that no tetrasubstituted urea solvent is added to the mixed solvent, and only propylene glycol dimethyl ether + diethylene glycol dimethyl ether is used.
[0063] The electrolyte composition is as follows: Mixed solvents: propylene glycol dimethyl ether + diethylene glycol dimethyl ether, with a mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether of 1:1.
[0064] Sodium salt: NaPF6 1.4mol / L + NaTFSI 0.6mol / L, total concentration 2.0mol / L.
[0065] Comparative Example 2 The preparation method is the same as in Example 1, except that the electrolyte does not contain electron-rich sodium salt; only ordinary sodium salt NaPF6 is used.
[0066] The electrolyte composition is as follows: Mixed solvent: composed of solvent A (tetramethylurea) and chain ether, with a mass ratio of solvent A to chain ether of 1:2; the chain ether is composed of propylene glycol dimethyl ether and diethylene glycol dimethyl ether; the mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether is 1:1.
[0067] Sodium salt: NaPF6 2.0mol / L.
[0068] Comparative Example 3 The preparation method is the same as in Example 1, except that the proportion of branched ether propylene glycol dimethyl ether in the chain ether is adjusted.
[0069] The electrolyte composition is as follows: Mixed solvent: Solvent A + chain ether, with a mass ratio of solvent A to chain ether of 1:2; the chain ether is composed of propylene glycol dimethyl ether + diethylene glycol dimethyl ether, with a mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether of 1:5.
[0070] Sodium salt: NaPF6 1.4mol / L + NaTFSI 0.6mol / L, total concentration 2.0mol / L.
[0071] Comparative Example 4 The preparation method is the same as in Example 1, except that the ratio of tetrasubstituted urea solvent to chain ether is adjusted.
[0072] The electrolyte composition is as follows: Mixed solvent: Solvent A + chain ether; the mass ratio of solvent A to chain ether is 1:5; in the chain ether: the mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether is 1:1.
[0073] Sodium salt: NaPF6 1.4mol / L + NaTFSI 0.6mol / L, total concentration 2.0mol / L.
[0074] Comparative Example 5 The preparation method is the same as in Example 1, except that no tetrasubstituted urea solvent is added to the mixed solvent, and no electron-rich sodium salt is added.
[0075] The electrolyte composition is as follows: Mixed solvents: propylene glycol dimethyl ether + diethylene glycol dimethyl ether, with a mass ratio of propylene glycol dimethyl ether to diethylene glycol dimethyl ether of 1:1.
[0076] Sodium salt: NaPF6 2.0mol / L.
[0077] Application Examples
[0078] The electrolytes prepared in the aforementioned examples and comparative examples were applied to sodium-ion batteries without negative electrodes to test their electrochemical performance.
[0079] A negative electrode-free sodium-ion battery includes a positive electrode, a negative electrode current collector, a separator, and an electrolyte.
[0080] Positive electrode preparation: The positive electrode active material is selected from NFM (NaNi) 1 / 3 Fe 1 / 3 Mn 1 / 3 O2), positive electrode active material, conductive carbon black (SP), and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 92:5:3, and N-methylpyrrolidone (NMP) is added and stirred thoroughly until the slurry is uniform; the mixed slurry is uniformly coated on the surface of aluminum foil current collector, and then dried, rolled and compacted, and cut into sheets to obtain NFM positive electrode sheets.
[0081] Negative electrode current collector: Copper foil with a 2μm carbon-based conductive layer on its surface is used as the negative electrode current collector.
[0082] Separator: Glass fiber diaphragm is selected.
[0083] Electrolyte: The electrolyte prepared in the aforementioned examples and comparative examples is used.
[0084] Battery assembly: The positive electrode, separator, and negative electrode current collector are stacked and aligned in sequence to obtain a bare cell; the bare cell is packaged in an aluminum-plastic film bag to complete the dry cell preparation, and then the electrolyte is injected into the dry cell to complete the heat sealing; after going through the electrolyte full wetting, small current activation formation, and cell shaping processes in sequence, a negative electrode-free sodium-ion battery is finally obtained.
[0085] Performance testing: The Blue Battery testing system was used, and the test environment temperature was set to 25℃ according to the experimental requirements. The NFM battery voltage range was 2.0V-4.1V and 2.0V-4.2V.
[0086] NFM Battery Cycling Performance Test At 25℃, the NFM system sodium-ion battery without a negative electrode was charged to 4.1V / 4.2V with a constant current of 0.1C, and then discharged to 2.0V with a constant current of 0.1C. This charge-discharge cycle was repeated twice to complete the cell activation. After activation, the battery was continuously cycled for 500 cycles (4.1V) and 300 cycles (4.2V) using a charge-discharge regime of 1C constant current to 4.1V / 4.2V and 1C constant current to 2.0V. The discharge capacity during the cycle was recorded, and the battery capacity retention rate after the cycle was calculated.
[0087] The formula for calculating battery capacity retention rate is as follows: Capacity retention rate = discharge capacity for the corresponding number of cycles / discharge capacity for the first stable cycle after activation × 100%.
[0088] (2) Battery internal resistance test DC pulse internal resistance was tested on NFM sodium-ion batteries at 25℃ and 50% SOC. The batteries were allowed to stand until the open-circuit voltage stabilized, and a 1C constant current discharge pulse was applied for 10 seconds. The open-circuit voltage before the pulse and the terminal voltage at the end of the pulse were collected. The DC internal resistance was calculated based on the voltage difference and the pulse current.
[0089] (3) Thermal safety performance test ARC adiabatic accelerated calorimetry test: A fully charged battery is placed in an adiabatic accelerated calorimeter and heated from room temperature to 300°C at a rate of 5°C / min. The thermal runaway trigger temperature of the battery cell is recorded.
[0090] The test results are shown in Table 1.
[0091] Table 1 .
[0092] The test results in the table above show that: (1) The urea-based deep eutectic electrolyte system prepared by Examples 1-12 of this application, which is constructed from "tetrasubstituted urea solvent-high voltage resistant branched ether-electron-rich sodium salt", has higher capacity retention, lower battery internal resistance and higher thermal runaway temperature under high voltage conditions of 4.1V and 4.2V. Its electrochemical and safety performance is significantly better than that of the comparative examples. All examples meet the requirements of capacity retention > 80% after 500 cycles at 25℃-4.1V and capacity retention > 80% after 300 cycles at 25℃-4.2V.
[0093] Comparative Example 1 used only a chain-like mixed ether solvent without adding a tetrasubstituted urea solvent. Lacking the strong complexation between the urea carbonyl group and sodium ions, a stable deep eutectic solvation structure could not be constructed. Under high pressure, the ether solvent was prone to oxidative decomposition, leading to the failure of the positive electrode passivation film. After 500 cycles at 25℃-4.1V, the capacity retention was only 62.3%, and after 300 cycles at 25℃-4.2V, the capacity retention was only 51.7%. The internal resistance increased significantly, and the thermal runaway temperature decreased significantly, proving that the tetrasubstituted urea solvent is a necessary component for constructing the deep eutectic system of this invention.
[0094] Comparative Example 2 used a mixed solvent of tetrasubstituted urea and chain ether, but only used ordinary sodium salt NaPF6, which did not contain electron-rich sodium salt. This resulted in a lack of strong dipole interaction between the anion and the urea carbonyl group, insufficient sodium salt dissociation, and difficulty in forming the target deep eutectic. Consequently, the high-voltage interface protection capability was significantly weakened; the capacity retention rate after 500 cycles at 25℃-4.1V was only 67.5%, and after 300 cycles at 25℃-4.2V, it was only 58.2%. This indicates that electron-rich sodium salt is a core condition for achieving a stable high-voltage interface within the system.
[0095] The proportion of branched ether in Comparative Example 3 was too low, resulting in insufficient high-voltage resistant branched ether components, decreased antioxidant capacity of the system, and significant deterioration of high-voltage cycling performance. This verifies that the amount of branched ether added has a significant impact on the high-voltage tolerance of the electrolyte.
[0096] In Comparative Example 4, the proportion of tetrasubstituted urea solvent in the solvent system was too low, resulting in insufficient deep eutectic effect, failure of solvation sheath layer regulation, and rapid capacity decay under high pressure.
[0097] Comparative Example 5 is a double-deficient control group, which has neither tetrasubstituted urea solvents nor electron-rich sodium salts. It completely loses the deep eutectic synergistic protection effect. The electrolyte undergoes severe oxidative decomposition on the high-voltage positive electrode side, and its performance is the worst among all groups. This directly proves the necessity of the synergistic effect of "tetrasubstituted urea solvents - high-voltage resistant branched ethers - electron-rich sodium salts".
[0098] (2) By adjusting the combination of electron-rich sodium salts, the types of tetrasubstituted urea solvents, the composition of chain ether solvents, the urea-ether ratio, and the total concentration of sodium salts, the dissociation of sodium salts in the electrolyte, the solvation structure, the interfacial film formation, and the high-pressure cycling performance can be controlled.
[0099] As can be seen from Examples 1-6, under the condition of a total salt concentration of 2.0 mol / L, NaTFSI, NaClO4, and NaFSI can all be used as electron-rich sodium salts. They can form stable urea-based deep eutectic when combined with ordinary sodium salts or used alone. Among them, the single NaTFSI system (Example 4) has the best overall performance. The increased proportion of electron-rich anions is beneficial to strengthening the dipole interaction and interface protection.
[0100] As can be seen from the comparison with Examples 1 and 7-8, different tetrasubstituted urea solvents can be adapted to this system; with the increase of alkyl carbon chain, the electrolyte viscosity increases, the battery internal resistance increases, and the high voltage performance decreases slightly. Tetramethylurea TMU has the best overall performance.
[0101] As can be seen from Examples 1, 9-10, the electrolyte can still achieve the performance indicators with different types of chain ethers and urea-ether ratios, demonstrating the good universality of the formulation system.
[0102] As can be seen from Examples 1 and 11-12, a stable deep eutectic can be formed in the sodium salt concentration range of 1.2-2.5 mol / L. When the concentration is too low, there are insufficient ion carriers, the internal resistance increases, and the performance decreases slightly. Increasing the concentration is beneficial to improving the interface and thermal safety, but excessively high viscosity will also lead to increased ion transport resistance.
[0103] Summarize: This application provides a tetrasubstituted urea-based high-voltage electrolyte that leverages the deep eutectic synergistic effect of a tetrasubstituted urea solvent, a high-voltage resistant branched ether, and an electron-rich sodium salt. It utilizes the intrinsic molecular advantage of the absence of α-H in the urea bond to enhance thermal safety, relies on the strong dipole interaction between the carbonyl group and the anion to improve sodium salt dissociation, and simultaneously uses the branched ether to improve viscosity and enhance high-voltage resistance. A stable interface is constructed on both sides of the high-voltage positive electrode and the non-anode sodium metal, addressing the pain points of traditional ether-based electrolytes, such as easy oxidation under high voltage and insufficient thermal safety. Applied to a non-anode sodium-ion battery, it achieves a capacity retention of 86.4% after 500 cycles at 25℃-4.1V and 83.9% after 300 cycles at 25℃-4.2V, with a battery internal resistance as low as 71mΩ and a thermal runaway temperature reaching 166℃. High-voltage long-cycle operation and thermal safety are simultaneously improved. The raw materials are readily available, the process is simple, and it is compatible with existing cell manufacturing processes, possessing significant engineering application value.
Claims
1. A tetrasubstituted urea-based high-voltage electrolyte, characterized in that: Includes solvents and sodium salts, with solvents including tetrasubstituted urea solvents and chain ether solvents, wherein the tetrasubstituted urea solvents conform to the following general formula: ; In the formula: R1, R2, R3 and R4 are each independently selected from straight-chain or branched alkyl groups having 1-6 carbon atoms; The sodium salt comprises at least one electron-rich sodium salt, which is selected from one of NaClO4, NaFSI, and NaTFSI. The chain ether solvent is selected from at least two of dimethyl acetal, propylene glycol dimethyl ether, 1,2-diethoxypropane, diethoxymethane, dimethyl alcohol acetal, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol diethyl ether, and ethylene glycol dibutyl ether, and contains at least one of dimethyl acetal, propylene glycol dimethyl ether, and 1,2-diethoxypropane.
2. The tetrasubstituted urea-based high-voltage electrolyte according to claim 1, characterized in that: The tetrasubstituted urea solvent is selected from at least one of tetramethylurea, 1,1,3,3-tetraethylurea, and 1,1,3,3-tetra-n-butylurea.
3. The tetrasubstituted urea-based high-voltage electrolyte according to claim 1, characterized in that: The chain-like ether solvent is selected from at least two of propylene glycol dimethyl ether, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether, and contains at least propylene glycol dimethyl ether.
4. The tetrasubstituted urea-based high-voltage electrolyte according to claim 1, characterized in that: The mass ratio of the tetrasubstituted urea solvent to the chain ether solvent is 1:4 to 1:
1.
5. The tetrasubstituted urea-based high-voltage electrolyte according to claim 1, characterized in that: The sodium salt is selected from at least one of NaPF6, NaClO4, NaBF4, NaAsF6, NaODFB, NaOTF, NaFSI, and NaTFSI.
6. The tetrasubstituted urea-based high-voltage electrolyte according to claim 1, characterized in that: The concentration of the sodium salt is 0.9–3.5 mol / L.
7. The tetrasubstituted urea-based high-voltage electrolyte according to claim 6, characterized in that: The concentration of the sodium salt is 1.2–2.5 mol / L.
8. A method for preparing the tetrasubstituted urea-based high-voltage electrolyte according to claim 1, characterized in that: In an argon atmosphere glove box with a water content of <10ppm, sodium salt is dissolved in a mixed solvent of tetrasubstituted urea solvents and chain ether solvents, and stirred until completely dissolved to obtain a tetrasubstituted urea high-voltage electrolyte.
9. The application of the tetrasubstituted urea-based high-voltage electrolyte of claim 1 in a negative electrode-less sodium-ion battery.
10. The application of the tetrasubstituted urea-based high-voltage electrolyte according to claim 9 in a negative electrode-free sodium-ion battery, characterized in that: The negative electrode-free sodium-ion battery includes a positive electrode, a negative electrode current collector, an electrolyte, and a separator; The cathode material is selected from one of layered oxide cathode materials and polyanionic cathode materials. The layered oxide cathode material is selected from any one of the following compounds: NaCoO2, NaMnO2, NaNiO2, NaCrO2, NaNi 0.5 Mn 0.5 O2, NaNi 0.5 Ti 0.5 O2, NaFe 0.5 Mn 0.5 O2, NaCu 0.5 Fe 0.5 O2, NaNi 0.33 Fe 0.33 Mn 0.33 O2, NaNi 0.33 Co 0.33 Mn 0.33 O2; The polyanionic cathode material is selected from any one of the following compounds: Na2FeP2O7, Na2MnP2O7, Na4Fe3(PO4)2P2O7, Na2Fe2(SO4)3, Na2Fe2(PO4)(SO4)2, and Na4Fe3(PO4)2P2O7. The diaphragm is selected from any one of polyethylene monolayer membrane, polypropylene monolayer membrane, multilayer microporous membrane composed of PP and PE, cellulose nonwoven fabric, polyvinylidene fluoride porous membrane, polyimide electrospun porous membrane, and glass fiber diaphragm. The negative electrode current collector is made of aluminum foil or copper foil, and a conductive coating is coated on the surface of the negative electrode current collector. The conductive coating is at least one of graphene, carbon nanotubes or hard carbon, and the coating thickness is 1 to 5 μm.