Battery cells, battery packs, electrical devices
By using a specific ratio of first and second additives in battery cells to generate an SEI film rich in inorganic components, the problems of insufficient storage performance and cycle performance of battery cells are solved, and the stability and lifespan of the battery are improved.
Patent Information
- Application Number
- CN202510623726.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
Smart Images

Figure CN123120877A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and more specifically, to a battery cell, a battery device, and an electrical device. Background Technology
[0002] The new energy industry is attracting increasing attention. Within this industry, battery technology is a crucial factor in its development.
[0003] The development of battery technology requires consideration of various design factors, such as energy density, cycle life, storage performance, charge / discharge rate, and reliability. Electrolyte design is crucial to the performance of individual battery cells, directly affecting their storage and cycle performance. Therefore, improving the storage and cycle performance of individual battery cells is a pressing technical challenge. Summary of the Invention
[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery cell, battery device, and power supply device that can improve the storage performance and cycle performance of the battery cell.
[0005] In a first aspect, a battery cell is provided, comprising an electrolyte, the electrolyte comprising a solvent, a first additive, and a second additive; wherein the first additive comprises at least one compound of formula (I):
[0006]
[0007] R1 includes at least one of alkyl, cycloalkyl, and halogen elements having 1-6 carbon atoms;
[0008] The second additive includes at least one of the compounds represented by formula (II):
[0009]
[0010] Wherein, R2 includes at least one of tert-butyl, isopropyl, phenyl, and naphthyl; R3 includes at least one of alkyl and cycloalkyl groups having 1-6 carbon atoms;
[0011] Based on the total mass of the electrolyte, the mass content of the first additive is greater than or equal to the mass content of the second additive.
[0012] In the embodiments of this application, the first additive shown in formula (I) and the second additive shown in formula (II) have higher reduction potentials and are preferentially reduced by solvent molecules. The thio groups in the first and second additives participate in the formation of the SEI film, which is beneficial to generating an SEI film rich in inorganic components. This is beneficial to improving the stability and density of the SEI film, reducing the risk of repeated breakage and reconstruction of the SEI film, and reducing lithium-ion consumption, thereby improving the storage performance and cycle performance of the battery cell. The SEI film rich in inorganic components is denser than the SEI film rich in organic components, which can reduce the risk of organic solvents in the electrolyte penetrating the SEI film and contacting the negative electrode active material. This can further reduce the risk of generating an SEI film rich in organic components and is more conducive to generating an SEI film rich in inorganic components. The SEI film rich in inorganic components has better thermal stability and mechanical properties than the SEI film rich in organic components. It is not easy to break during the charge and discharge cycle of the battery cell, which can reduce the active lithium consumed by repeated breakage and reconstruction of the SEI film, and is beneficial to improving the storage performance and cycle performance of the battery cell.
[0013] By setting the mass content of the first additive to be greater than or equal to the mass content of the second additive, the first additive can play a dominant role in the formation of inorganic components in the SEI film. The first additive has an unsaturated structure and a high reduction potential. In the electrolyte, it preferentially reacts with the solvent over the second additive to generate a polymer with a high molecular weight. This polymer covers the surface of the negative electrode active material, reducing the contact between the negative electrode active material and the organic solvent in the electrolyte, reducing the occurrence of side reactions and the risk of organic components forming in the SEI film, which is beneficial to improving the storage performance of the battery cell.
[0014] The second additive shown in formula (II) preferentially decomposes before the solvent and can participate in the formation of the SEI film, thereby generating an SEI film rich in inorganic components at the negative electrode, which is beneficial to increasing the inorganic component in the SEI film. After the second additive decomposes, the side chain groups include active free radicals, which easily contact solvent molecules to generate chain-like organic matter, leading to an increase in the organic component in the SEI film. The R2 group in the second additive has a large steric hindrance, which can reduce the contact between the solvent and the active free radicals of the decomposed second additive, reduce the generation of chain-like organic matter, and help increase the proportion of inorganic matter in the SEI film, thereby improving the storage performance and cycle performance of the battery cell. After the unsaturated structure in the first additive decomposes, it provides active sites, inducing the second additive to aggregate on the surface of the negative electrode active material, which is further beneficial to generating an SEI film rich in inorganic components, improving the stability and density of the SEI film, and having a good effect on improving the storage performance and cycle performance of the battery cell. Therefore, the technical solution of the embodiments of this application can improve the storage performance and cycle performance of the battery cell.
[0015] In some embodiments, based on the total mass of the electrolyte, the mass ratio of the first additive to the second additive satisfies 1:1 to 4:1.
[0016] In the above technical solution, the first additive and the second additive have a suitable mass ratio, which can increase the proportion of inorganic matter in the SEI film, thus improving the storage and cycle performance of the battery cell. When the mass ratio of the first additive and the second additive is greater than or equal to 1:1, it helps to reduce the possibility that the mass content of the first additive is low, and the decomposed second additive will react with the solvent to form chain-like organic matter, increasing the organic component in the SEI film. When the mass ratio of the first additive and the second additive is less than or equal to 4:1, it prevents the mass ratio of the first additive to the second additive from being too high, which can reduce the risk of the first additive undergoing side reactions within the battery cell due to excessive content, thereby reducing the adverse effects of side reactions on the storage performance of the battery cell.
[0017] In some embodiments, based on the total mass of the electrolyte, the mass content A of the first additive satisfies: 0.001% ≤ A ≤ 2%.
[0018] In the above technical solution, when the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the storage performance of the battery cell; when the mass content of the first additive is less than or equal to 2% based on the total mass of the electrolyte, it can reduce the risk of the first additive undergoing side reactions in the battery cell due to excessive content of the first additive, thereby reducing the adverse effects of side reactions on the storage performance of the battery cell.
[0019] In some embodiments, based on the total mass of the electrolyte, the mass content A of the first additive satisfies: 0.5% ≤ A ≤ 2%. This results in a battery cell with good storage performance.
[0020] In some embodiments, based on the total mass of the electrolyte, the mass content A of the first additive satisfies: 0.001% ≤ A ≤ 0.5%.
[0021] In the above technical solution, when the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the storage performance of the battery cell; when the mass content of the first additive is less than or equal to 0.5% based on the total mass of the electrolyte, the risk of the first additive undergoing side reactions in the battery cell due to excessive content of the first additive can be reduced, thereby reducing the adverse effects of side reactions on the storage performance of the battery cell.
[0022] In some embodiments, based on the total mass of the electrolyte, the mass content B of the second additive satisfies: 0.1% ≤ B ≤ 2%.
[0023] When the mass content of the second additive is greater than or equal to 0.1% based on the total mass of the electrolyte, it helps to reduce the risk of excessive organic components in the SEI film due to excessively low mass content of the second additive, which would lead to repeated rupture and reconstruction of the SEI film and consumption of active lithium, thus improving the cycle performance of the battery cell. When the mass content of the second additive is less than or equal to 2% based on the total mass of the electrolyte, it helps to reduce the risk of side reactions of the second additive in the battery cell due to excessive content, thus reducing the adverse effects of side reactions on the cycle performance of the battery cell.
[0024] In some embodiments, the battery cell includes a negative electrode sheet, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes graphite.
[0025] In the above technical solution, the first additive will preferentially decompose and cover the surface of graphite, providing more active sites and inducing the second additive to aggregate on the surface of the graphite negative electrode active material. This is beneficial to improve the SEI film with a high proportion of inorganic matter, improve the stability and density of the SEI film, and improve the storage performance and cycle performance of the battery cell.
[0026] In some embodiments, the graphite includes at least one of artificial graphite and natural graphite.
[0027] In this technical solution, graphite may include natural graphite, artificial graphite, or a mixture of natural and artificial graphite.
[0028] In some embodiments, the second additive includes at least one selected from dicyclohexyl sulfate, cyclohexylmethylthioacetic acid, 2-cyclohexyltoluene-4-ethyl sulfate, 3,5-dimethylcyclohexyl sulfate, dicyclohexyl dithiophosphate, 4-butyl ethylene sulfite, and 4-propyl ethylene sulfite.
[0029] In the above technical solution, the steric hindrance effect of the side chain groups of the second additive is relatively large, which can reduce the contact between the solvent and the active free radicals of the decomposed second additive, reduce the generation of chain organic matter, and help increase the proportion of inorganic matter in the SEI film.
[0030] In some embodiments, the solvent includes at least one of linear ester solvents and cyclic carbonate solvents.
[0031] In the above technical solutions, carbonate solvents are beneficial for forming a polymer coating film on the surface of the negative electrode active material, which can buffer the volume expansion of the battery cell during the charging and discharging process, and also help repair the damaged sites of the SEI film during long-term charge and discharge cycles, thereby improving the life of the battery cell; linear ester solvents are beneficial for improving the ionic conductivity of the electrolyte and improving the ion transport efficiency, thereby meeting the fast charging performance of the battery cell.
[0032] In some embodiments, the battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material includes a lithium phosphate. Thus, the lithium phosphate exhibits high structural stability, and battery cells containing lithium phosphate have a long cycle life.
[0033] In a second aspect, a battery device is provided, comprising a battery cell as described in the first aspect and any possible implementation thereof.
[0034] Thirdly, an electrical device is provided, comprising a battery cell as in the first aspect and any possible implementation thereof; and / or, according to the second aspect and any possible implementation thereof, the battery cell or battery device is used to store or provide electrical energy. Attached Figure Description
[0035] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0036] Figure 1 This is a schematic diagram of the X-ray photoelectron spectrum of sulfur in the negative electrode sheet according to an embodiment of this application.
[0037] Figure 2 A schematic diagram of the X-ray photoelectron spectroscopy of sulfur in the negative electrode of a battery cell without the first additive, provided as an embodiment of this application.
[0038] Figure 3 This is a schematic diagram of the structure of a battery cell according to an embodiment of this application;
[0039] Figure 4 This is a schematic diagram of the structure of a battery device according to an embodiment of this application;
[0040] Figure 5 This is a schematic diagram of an electrical device according to an embodiment of this application;
[0041] Figure 6This is a schematic diagram of an electrical device according to another embodiment of this application.
[0042] Reference numerals: 1: Vehicle; 2: Energy storage device; 10: Battery device; 4: Controller; 5: Motor; 11: Housing; 111: First housing section; 112: Second housing section; 3: Battery cell; 30: Outer casing; 31: Housing; 32: Cover plate assembly; 33: Electrode assembly; 34: Current collector; 331: Tab; 322: Electrode terminal; Pressure relief mechanism: 313. Detailed Implementation
[0043] The technical solutions in the embodiments of this application will now be described with reference to the accompanying drawings.
[0044] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0045] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0046] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used in the description of this application is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms "comprising" and "having," and any variations thereof, in the description, claims, and accompanying drawings of this application are intended to cover non-exclusive inclusion. The terms "first," "second," etc., in the description, claims, or accompanying drawings of this application are used to distinguish different objects, not to describe a specific order or hierarchy.
[0047] In the embodiments of this application, the "intercalation" process refers to the process in which lithium ions are intercalated into the positive electrode active material and the negative electrode active material due to an electrochemical reaction, while the "extraction" and "deintercalation" processes mentioned in this application refer to the process in which lithium ions are extracted from the positive electrode active material and the negative electrode active material due to an electrochemical reaction.
[0048] In this application, the reference to "embodiment" means that a specific feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a mutually exclusive, independent, or alternative embodiment. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described in this application can be combined with other embodiments.
[0049] In the description of this application, it should be noted that, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "attachment" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal communication between two components. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0050] In this application, the term "and / or" is merely a description of the relationship between related objects, indicating that there can be three relationships. For example, A and / or B can represent three situations: A exists alone, A and B exist simultaneously, and B exists alone.
[0051] Typically, a battery cell includes a positive electrode, a negative electrode, an electrolyte, and a separator. During charging and discharging, active ions shuttle between the positive and negative electrodes, inserting and extracting. The electrolyte acts as a conductor between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing active ions to pass through. During charging, lithium ions are extracted from the positive electrode active material, move, and insert into the negative electrode active material; conversely, during discharging, lithium ions are extracted from the negative electrode active material, move, and insert into the positive electrode active material.
[0052] In the embodiments of this application, if mentioned, the SEI film is a passivation film layer formed by the reaction between the active material and the electrolyte at the solid-liquid interface during the first charge and discharge process of the battery cell, covering the surface of the active material. The active material includes the negative electrode active material.
[0053] In this embodiment, formation can be understood as the initialization of a battery cell, a process that activates the active materials within the cell; it can also be understood as a charging process for the battery cell, with formation contributing to the formation of the SEI film within the cell. In this embodiment, formation is a process performed before the battery cell leaves the factory.
[0054] The development of battery technology must consider multiple design factors simultaneously, such as energy density, cycle life, capacity retention, charge / discharge rate, and reliability. As a crucial component of lithium-ion batteries, the electrolyte plays a vital role in conducting ions, and its composition and properties directly affect the storage and cycle performance of individual battery cells.
[0055] Specifically, solvents are added to the electrolyte of battery cells to optimize electrolyte performance, such as improving ion transport efficiency and thus enhancing the performance of the battery cell. Common solvents, such as ethylene carbonate (EC), readily undergo irreversible reduction during the first charge, forming a solid electrolyte interphase (SEI) film. However, excessive reduction by solvents like EC can lead to the formation of large amounts of organic compounds, resulting in a high proportion of organic components in the SEI film and reducing its stability and mechanical strength. In some treatment methods, cyclic sulfate compounds are used. These cyclic sulfates preferentially decompose, forming an SEI film containing Li₂SO₄ and ROSO₂Li (R being an alkyl group) on the negative electrode surface. Li₂SO₄ is an electrochemically inert inorganic salt with high chemical stability, effectively covering the negative electrode active sites and preventing contact between the electrolyte and the negative electrode active material. ROSO₂Li is an organic-inorganic hybrid component, with the -SO₄ group in its molecule... 2- The group is polar and can adsorb Li +This forms a localized conductive network, accelerating Li+ transport, thereby reducing the discharge coefficient (DCR) of individual cells, improving their low-temperature discharge performance and high-temperature stability, and enhancing their cycle performance. However, after the decomposition of cyclic sulfate compounds, they react with solvent molecules to generate organic substances. These organic substances in the SEI film are easily stripped or dissolved during cell cycling, leading to unstable interfacial structures and reducing the cell's storage and cycle performance.
[0056] In view of this, embodiments of this application provide a battery cell including an electrolyte, the electrolyte comprising a solvent, a first additive, and a second additive; wherein the first additive comprises at least one of the compounds shown in formula (I):
[0057]
[0058] R1 includes at least one of alkyl, cycloalkyl, and halogen elements having 1-6 carbon atoms;
[0059] The second additive includes at least one of the compounds represented by formula (II):
[0060]
[0061] Wherein, R2 includes at least one of tert-butyl, isopropyl, phenyl, and naphthyl; R3 includes at least one of alkyl and cycloalkyl groups having 1-6 carbon atoms;
[0062] Based on the total mass of the electrolyte, the mass content of the first additive is greater than or equal to the mass content of the second additive.
[0063] The first additive shown in formula (I) and the second additive shown in formula (II) have high reduction potentials and are preferentially reduced by solvent molecules. The thio groups in the first and second additives participate in the formation of the SEI film, which is beneficial to the generation of an SEI film rich in inorganic components. This is beneficial to improving the stability and density of the SEI film, reducing the risk of repeated breakage and reconstruction of the SEI film, and reducing lithium-ion consumption, thereby improving the storage performance and cycle performance of the battery cell. The SEI film rich in inorganic components is denser than the SEI film rich in organic components, which can reduce the risk of organic solvents in the electrolyte penetrating the SEI film and contacting the negative electrode active material. This can further reduce the risk of generating an SEI film rich in organic components and is more conducive to generating an SEI film rich in inorganic components. The SEI film rich in inorganic components has better thermal stability and mechanical properties than the SEI film rich in organic components. It is not easy to break during the charge and discharge cycle of the battery cell, which can reduce the active lithium consumed by repeated breakage and reconstruction of the SEI film and help improve the life of the battery cell.
[0064] By setting the mass content of the first additive to be greater than or equal to the mass content of the second additive, the first additive can play a dominant role in the formation of inorganic components in the SEI film. The first additive has an unsaturated structure and a high reduction potential. In the electrolyte, it preferentially reacts with the solvent over the second additive to generate a polymer with a high molecular weight. This polymer covers the surface of the negative electrode active material, reducing the contact between the negative electrode active material and the organic solvent in the electrolyte, reducing the occurrence of side reactions and the risk of organic components forming in the SEI film, which is beneficial to improving the storage performance of the battery cell.
[0065] The second additive shown in formula (II) preferentially decomposes before the solvent and can participate in the formation of the SEI film, thereby generating an SEI film rich in inorganic components at the negative electrode, which is beneficial to increasing the inorganic component in the SEI film. After the second additive decomposes, the side chain groups include active free radicals, which easily contact solvent molecules to generate chain-like organic matter, leading to an increase in the organic component in the SEI film. The R2 group in the second additive has a large steric hindrance, which can reduce the contact between the solvent and the active free radicals of the decomposed second additive, reduce the generation of chain-like organic matter, and help increase the proportion of inorganic matter in the SEI film, thereby improving the storage performance and cycle performance of the battery cell. After the unsaturated structure in the first additive decomposes, it provides active sites, inducing the second additive to aggregate on the surface of the negative electrode active material, which is further beneficial to generating an SEI film rich in inorganic components, improving the stability and density of the SEI film, and having a good effect on improving the storage performance and cycle performance of the battery cell. Therefore, the technical solution of the embodiments of this application can improve the storage performance and cycle performance of the battery cell.
[0066] [Battery cell]
[0067] This application provides a battery cell including an electrolyte, which comprises a solvent, a first additive, and a second additive; wherein the first additive comprises at least one compound of formula (I):
[0068]
[0069] R1 includes at least one of alkyl, cycloalkyl, and halogen elements having 1-6 carbon atoms;
[0070] The second additive includes at least one of the compounds shown in formula (II):
[0071]
[0072] Wherein, R2 includes at least one of tert-butyl, isopropyl, phenyl, and naphthyl; R3 includes at least one of alkyl and cycloalkyl groups having 1-6 carbon atoms;
[0073] Based on the total mass of the electrolyte, the mass content of the first additive is greater than or equal to the mass content of the second additive.
[0074] R1 and R3 can be the same group or different groups.
[0075] In the embodiments of this application, the substituents such as tert-butyl, isopropyl, phenyl, and naphthyl have a large volume in three-dimensional space. Due to the large volume of the substituents in the molecule of the second additive, the steric hindrance effect makes it difficult for other groups or reactants to approach the active free radical sites of the second additive, thereby reducing the possibility of organic solvent molecules combining with the decomposed second additive to generate chain-like organic compounds.
[0076] In this embodiment, the first additive shown in formula (I) and the second additive shown in formula (II) have high reduction potentials and are preferentially reduced by solvent molecules. The thio groups in the first and second additives participate in the formation of the SEI film, which is beneficial for generating an SEI film rich in inorganic components. This is beneficial for improving the stability and density of the SEI film, reducing the risk of repeated breakage and reconstruction of the SEI film, and reducing lithium-ion consumption, thereby improving the storage performance and cycle performance of the battery cell. The SEI film rich in inorganic components is denser than the SEI film rich in organic components, which can reduce the risk of organic solvents in the electrolyte penetrating the SEI film and contacting the negative electrode active material. This can further reduce the risk of generating an SEI film rich in organic components and is more conducive to generating an SEI film rich in inorganic components. The SEI film rich in inorganic components has better thermal stability and mechanical properties than the SEI film rich in organic components. It is not easy to break during the charge and discharge cycle of the battery cell, which can reduce the active lithium consumed by repeated breakage and reconstruction of the SEI film and improve the life of the battery cell.
[0077] By setting the mass content of the first additive to be greater than or equal to the mass content of the second additive, the first additive can play a dominant role in the formation of inorganic components in the SEI film. The first additive has an unsaturated structure and a high reduction potential. In the electrolyte, it preferentially reacts with the solvent over the second additive to generate a polymer with a high molecular weight. This polymer covers the surface of the negative electrode active material, reducing the contact between the negative electrode active material and the organic solvent in the electrolyte, reducing the occurrence of side reactions and the risk of organic components forming in the SEI film, which is beneficial to improving the storage performance of the battery cell.
[0078] The second additive shown in formula (II) preferentially decomposes before the solvent and can participate in the formation of the SEI film, thereby generating an SEI film rich in inorganic components at the negative electrode, which is beneficial to increasing the inorganic component in the SEI film. After the second additive decomposes, the side chain groups include active free radicals, which easily contact solvent molecules to generate chain-like organic matter, leading to an increase in the organic component in the SEI film. The R2 group in the second additive has a large steric hindrance, which can reduce the contact between the solvent and the active free radicals of the decomposed second additive, reduce the generation of chain-like organic matter, and is beneficial to increasing the proportion of inorganic matter in the SEI film, thereby improving the storage performance and cycle performance of the battery cell. After the unsaturated structure in the first additive decomposes, it provides active sites, inducing the second additive to aggregate on the surface of the negative electrode active material, which is further beneficial to generating an SEI film rich in inorganic components, improving the stability and density of the SEI film, and having a good effect on improving the storage performance and cycle performance of the battery cell. Therefore, the technical solution of the embodiments of this application can improve the storage performance and cycle performance of the battery cell. It should be understood that during the formation process of the battery cell, the first additive and the second additive decompose at least partially. After the battery cell is formed, the first additive plays a leading role in the formation of the SEI film. The first additive may be completely consumed or remain.
[0079] It should be noted that "the first additive is completely consumed" here can refer to a situation where the first additive cannot be detected due to exceeding the instrument's detection accuracy. As an example, if the mass content of the first additive is 0.001% based on the total mass of the electrolyte, it can be considered that the first additive is completely consumed.
[0080] In some embodiments, based on the total mass of the electrolyte, the mass ratio of the first additive and the second additive satisfies: 1:1 to 4:1.
[0081] Specifically, the mass ratio of the first additive to the second additive can be 1:1, 2:1, 3:1, 4:1, or any value within the above range. It should be understood that the mass ratio of the first additive to the second additive can refer to a normalized ratio, which can be calculated from the actual mass content of the first additive and the mass content of the second additive used.
[0082] In the above technical solution, the first additive and the second additive have a suitable mass ratio, which can increase the proportion of inorganic matter in the SEI film, thus improving the storage and cycle performance of the battery cell. When the mass ratio of the first additive and the second additive is greater than or equal to 1:1, it helps to reduce the possibility that the mass content of the first additive is low, and the decomposed second additive will react with the solvent to form chain-like organic matter, increasing the organic component in the SEI film. When the mass ratio of the first additive and the second additive is less than or equal to 4:1, it prevents the mass ratio of the first additive to the second additive from being too high, which can reduce the risk of the first additive undergoing side reactions within the battery cell due to excessive content, thereby reducing the adverse effects of side reactions on the storage performance of the battery cell.
[0083] The mass ratio of the first additive and the second additive mentioned above can be the ratio of the mass content of the first additive and the second additive before the battery cell is formed.
[0084] During the charge-discharge cycle of the formed battery cell and throughout its entire lifespan, the first and second additives are consumed, and their mass ratio changes.
[0085] In some embodiments, based on the total mass of the electrolyte, the mass content A of the first additive satisfies: 0.001% ≤ A ≤ 2%.
[0086] Specifically, based on the total mass of the electrolyte, the mass content A of the first additive can be 0.001%, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, or any value within the above range.
[0087] The aforementioned mass content of the first additive includes both the mass content during the battery cell preparation process and the mass content after the battery cell has been formed. For example, after the battery cell has been formed, the mass content of the first additive may be 0.001% based on the total mass of the electrolyte. As another example, during the battery cell preparation process, the mass content of the first additive may be 2% based on the total mass of the electrolyte.
[0088] As an example, if the mass content of the first additive is greater than or equal to 1% based on the total mass of the electrolyte before the battery cell is formed, there will be some of the first additive remaining after formation.
[0089] Furthermore, as an example, if a battery cell is stored at room temperature (e.g., 25°C) for a short period (e.g., 3 months) after formation, the mass content of the first additive within the battery cell is essentially the same as that in a freshly formed battery cell. As another example, if a battery cell is stored at a higher temperature (e.g., 45°C) for a short period (e.g., within 5 days) after formation, the mass content of the first additive within the battery cell is essentially the same as that in a freshly formed battery cell. As yet another example, if a battery cell is stored at a higher temperature (e.g., 45°C) for a longer period (e.g., more than 15 days) after formation, the first additive can be completely consumed. In this embodiment of the application, when the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the storage performance of the battery cell; when the mass content of the first additive is less than or equal to 2% based on the total mass of the electrolyte, the risk of the first additive undergoing side reactions in the battery cell due to excessive content of the first additive can be reduced, thereby reducing the adverse effects of side reactions on the storage performance of the battery cell.
[0090] In some embodiments, based on the total mass of the electrolyte, the mass content A of the first additive satisfies: 0.5% ≤ A ≤ 2%.
[0091] The mass content of the first additive mentioned above refers to the mass content of the battery cell before formation, or it can refer to the mass content of the first additive during the preparation of the battery cell.
[0092] Before the battery cell is formed, based on the total mass of the electrolyte, the mass content of the first additive can be 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.5%, 1.8%, 2% or any value within the above range.
[0093] In this embodiment, when the mass content of the first additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it has a good effect on improving the storage performance of the battery cell; when the mass content of the first additive is less than or equal to 2% based on the total mass of the electrolyte, the risk of the first additive undergoing side reactions in the battery cell due to excessive content of the first additive can be reduced, thereby reducing the adverse effects of side reactions on the storage performance of the battery cell.
[0094] In some embodiments, after the battery cell is formed, the mass content A of the first additive satisfies: 0.001% ≤ A ≤ 0.55%.
[0095] The mass content of the first additive mentioned above refers to the mass content of the battery cell after formation. Here, "formed battery cell" refers to, for example, a battery cell that has just been manufactured and is not yet in use in a vehicle, or a battery cell that has just been removed from the storage compartment and is not yet installed in a vehicle.
[0096] After the battery cell is formed, based on the total mass of the electrolyte, the mass content of the first additive can be 0.001%, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.55%, or any value within the above range.
[0097] In some embodiments, based on the total mass of the electrolyte, the mass content B of the second additive satisfies: 0.1% ≤ B ≤ 2%.
[0098] The mass content of the second additive mentioned above includes both the mass content during the preparation process of the battery cell and the mass content after the battery cell has been formed. For example, after the battery cell has been formed, the mass content of the second additive may be 0.1% based on the total mass of the electrolyte. As another example, during the preparation process of the battery cell, the mass content of the second additive may be 2% based on the total mass of the electrolyte.
[0099] Specifically, the mass content B of the second additive can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, or any value within the above range.
[0100] During the formation of the battery cell, the second additive undergoes at least partial decomposition. After battery cell formation, the second additive will generally remain. For example, the type and content of the second additive can be determined by NMR spectroscopy. In the embodiments of this application, when the mass content of the second additive is greater than or equal to 0.1% based on the total mass of the electrolyte, it is beneficial to reduce the risk of excessively low mass content of the second additive leading to a higher proportion of organic components in the SEI film, resulting in repeated rupture and reconstruction of the SEI film and consumption of active lithium, thus improving the cycle performance of the battery cell. When the mass content of the second additive is less than or equal to 2% based on the total mass of the electrolyte, it is beneficial to reduce the risk of side reactions of the second additive within the battery cell due to excessive content, thereby reducing the adverse effects of side reactions on the cycle performance of the battery cell.
[0101] In some embodiments, the mass content B of the second additive satisfies: 0.5% ≤ B ≤ 2%. Thus, before the battery cell is formed, if the mass content of the second additive meets the above range based on the total mass of the electrolyte, the battery cell has better cycle performance.
[0102] The mass content of the second additive mentioned above refers to the mass content of the battery cell before formation, or it can refer to the mass content of the second additive during the preparation of the battery cell.
[0103] Before the battery cell is formed, based on the total mass of the electrolyte, the mass content of the second additive can be 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.5%, 1.8%, 2% or any value within the above range.
[0104] In some embodiments, the mass content B of the second additive satisfies: 0.1% ≤ B ≤ 0.6%.
[0105] The mass content of the second additive mentioned above refers to the mass content of the battery cell after formation. Here, "formed battery cell" refers to, for example, a battery cell that has just been manufactured and is not yet in use in a vehicle, or a battery cell that has just been removed from the storage compartment and is not yet installed in a vehicle.
[0106] After the battery cells are formed, the mass content of the second additive can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, or any value within the above range, based on the total mass of the electrolyte. If the first and second additives are not completely consumed, their mass content and the methods used can be determined by gas chromatography, gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), or inductively coupled plasma optical emission spectrometry (ICP-OES).
[0107] As an example, at 25°C, a single battery cell was charged to 3.8V at a constant current of 0.33C and discharged to 2.0V at a constant current of 0.33C. The battery cell was then disassembled, and the electrolyte was extracted (if the electrolyte in the battery cell was small, the positive and negative electrode plates could be centrifuged to obtain the electrolyte from them). Next, 500 μl of deuterated reagent was added to an NMR tube in an argon-filled glove box, and 100 μl of electrolyte sample was added to the NMR tube. The NMR tube was shaken to dissolve the non-aqueous electrolyte in the deuterated reagent. The composition and mass of the first and second additives in the electrolyte were tested using an Oxford Instruments X-Pulse benchtop NMR spectrometer. The mass content of the first additive in the electrolyte was calculated by dividing the mass of the first additive by the mass of the entire electrolyte, and the mass content of the second additive in the electrolyte was calculated by dividing the mass of the second additive by the mass of the entire electrolyte.
[0108] When the first additive is depleted, it can be determined whether the first additive was added during the electrolyte preparation process by testing the cyclic sulfate ester structure in the electrolyte and the content of inorganic sulfur-containing compounds in the solid electrolyte interphase (SEI) film on the surface of the negative electrode active material layer. For example, if the first additive cannot be detected by nuclear magnetic resonance spectroscopy, but the electrolyte contains a cyclic sulfate ester structure and the X-ray photoelectron spectrum of sulfur in the negative electrode shows a large peak area and high characteristic peak intensity at 165±0.2 eV, then it can be inferred that the first additive was included in the electrolyte during the preparation of the battery cell.
[0109] The content of inorganic sulfur compounds in the solid electrolyte interphase (SEI) film on the surface of the negative electrode active material layer can be determined as follows: At 25°C, the battery cell is charged to 3.8V at a constant current of 0.33C, and then the battery cell is disassembled to obtain the negative electrode sheet. The inorganic sulfur compounds in the SEI film on the surface of the negative electrode active material layer can be detected by X-ray photoelectron spectroscopy (XPS). Using the negative electrode sheet as the sample and an Al target as the X-ray source at a power of 300W, X-rays are used to bombard the surface of the negative electrode active material layer, exciting the inner-shell electrons or valence electrons of atoms or molecules. The C1s peak (284.8 eV) is used as the XPS reference peak position to analyze surface elements (e.g., sulfur) and functional groups. As an example, the X-ray photoelectron spectroscopy (XPS) of sulfur in the negative electrode was tested, and the peak areas at 169±0.2 eV and 165±0.2 eV were measured and recorded. The peak at 169±0.2 eV represents organic sulfur-containing compounds, and the peak at 165±0.2 eV represents inorganic sulfur-containing compounds. Adding a first additive and a second additive facilitates the formation of a higher content of inorganic sulfur-containing compounds at the negative electrode (i.e., a higher inorganic component in the SEI film). A larger peak area and higher characteristic peak intensity at 165±0.2 eV indicate a greater amount of inorganic sulfur-containing compounds in the SEI film.
[0110] Figure 1 This is a schematic diagram of the X-ray photoelectron spectrum of sulfur in the negative electrode sheet according to an embodiment of this application. Figure 2 This is a schematic diagram of the X-ray photoelectron spectroscopy (XPS) of sulfur in the negative electrode of a battery cell excluding the first additive, provided as an embodiment of this application. Figure 1 The image shows the positions of the peaks in the electrolyte, including the first additive and the second additive. Figure 2 The image shows the positions of the peaks in the electrolyte excluding the first additive. (Combined with...) Figure 1 and Figure 2As shown, when the electrolyte includes the first additive, in the X-ray photoelectron spectroscopy of sulfur in the negative electrode, the peak area at 169±0.2 eV is small, and the characteristic peak intensity is low. This peak represents the organic sulfur-containing components RSO4 / RSO3. The peak area at 165 eV±0.2 eV is large, and the characteristic peak intensity is high, indicating a higher content of inorganic sulfur-containing compounds such as Li2SO4, Li2SO3, and Li2S. By adding the first and second additives, it is beneficial to generate a higher content of inorganic sulfur-containing compounds at the negative electrode (i.e., a higher inorganic component in the SEI film). The SEI film is more dense and stable, and the risk of repeated SEI film breakage and reconstruction is lower, which helps to reduce lithium-ion consumption and thus improves the storage performance and cycle performance of the battery cell.
[0111] In some embodiments, the battery cell includes a negative electrode sheet, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes graphite.
[0112] In this embodiment, the first additive preferentially decomposes and covers the surface of artificial graphite, providing more active sites and inducing the second additive to aggregate on the surface of the negative electrode active material of artificial graphite. This is beneficial to improve the SEI film with a high proportion of inorganic matter, improve the stability and density of the SEI film, and improve the storage performance and cycle performance of the battery cell.
[0113] In some embodiments, at least a portion of the graphite surface has an amorphous carbon coating. This carbon coating facilitates the rapid insertion and extraction of lithium ions into the graphite, resulting in better fast-charging performance for the battery cell.
[0114] In some embodiments, the carbon coating layer comprises amorphous carbon.
[0115] Amorphous carbon has good isotropy, allowing lithium ions to embed into graphite from all directions, which is beneficial for improving the fast-charging performance of battery cells. In addition, the SEI film on the graphite surface has good density and stability through the addition of the first additive, which can reduce the risk of side reactions between amorphous carbon and electrolytes that consume lithium ions and reduce the adverse impact on the lifespan of battery cells.
[0116] As an example, a thin slice of about 100 nm thickness can be cut from the middle of the negative electrode active material particles using focused ion beam (FIB), and then TEM testing can be performed on the slice. It can be observed that the surface region includes a coating layer. The lattice fringes in the coating layer exhibit long-range disorder and short-range order, and the electron diffraction pattern shows a halo-like appearance, indicating that the coating layer includes amorphous carbon.
[0117] In this embodiment, graphite can be obtained by disassembling a battery cell. As an example, the battery cell is discharged at a constant current of 0.33C to 2.0V at 25°C to obtain a battery cell with 0% SOC. Then, the negative electrode sheet is removed from the battery cell, and the negative electrode film layer is scraped off to obtain the powder of the negative electrode film layer. Then, water is added to the powder of the negative electrode film layer and stirred. After filtration and drying, graphite is obtained.
[0118] In some embodiments, graphite includes at least one of natural graphite and artificial graphite.
[0119] In this embodiment, graphite may include natural graphite, artificial graphite, or a mixture of natural and artificial graphite. For example, in some embodiments, graphite includes artificial graphite.
[0120] In some embodiments, the first additive includes at least one of 1,3-propenyl-sulfonyl lactone and 3-fluoro-1,3-propanesulfonyl lactone.
[0121] In this embodiment, the first additive is preferentially decomposed in the electrolyte compared to the second additive and solvent, which helps to increase the proportion of inorganic matter in the SEI film, improves the stability and density of the SEI film, and thus enhances the storage performance of the battery cell. Furthermore, different first additives can be selected according to actual usage requirements.
[0122] In some embodiments, the second additive includes at least one selected from dicyclohexyl sulfate, cyclohexylmethylthioacetic acid, 2-cyclohexyltoluene-4-ethyl sulfate, 3,5-dimethylcyclohexyl sulfate, dicyclohexyl dithiophosphate, 4-butyl ethylene sulfite, and 4-propyl ethylene sulfite.
[0123] In some embodiments, the second additive has the following structural formula:
[0124]
[0125] In this embodiment, the steric hindrance effect of the side chain groups of the second additive is significant, which can reduce the contact between the solvent and the active free radicals of the decomposed second additive, reduce the formation of chain-like organic matter, and help increase the proportion of inorganic matter in the SEI film. Meanwhile, different first additives can be selected according to actual application needs.
[0126] In some embodiments, the solvent includes at least one of linear ester solvents and cyclic carbonate solvents.
[0127] Cyclic carbonate solvents are a class of organic carbonate compounds with cyclic structures, containing cyclic structures formed by carbonate groups (-O-CO-O-). As an example, cyclic carbonate solvents include at least one of ethylene carbonate and propylene carbonate.
[0128] In this embodiment, carbonate solvents are beneficial for forming a polymer coating film on the surface of the negative electrode active material, which can buffer the volume expansion of the battery cell during charging and discharging, and also help repair the damaged sites of the SEI film during long-term charge and discharge cycles, thereby improving the lifespan of the battery cell; linear ester solvents are beneficial for improving the ionic conductivity of the electrolyte and improving the lithium ion transport efficiency, thereby meeting the fast charging performance of the battery cell.
[0129] In some embodiments, cyclic carbonate solvents include at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
[0130] The aforementioned cyclic carbonate solvents have high dielectric constants and good solvation capabilities, which are beneficial for the dissociation of lithium ions in the electrolyte salt, thereby increasing the lithium ion transference number in the electrolyte. As a result, the battery cells have lower resistance, which is beneficial for improving the lifespan of the battery cells.
[0131] In some embodiments, the sum of the mass contents of linear ester solvents and cyclic carbonate solvents, based on the total mass of the electrolyte, satisfies 80% to 90%.
[0132] Based on the total mass of the electrolyte, the sum of the mass contents of linear ester solvents and cyclic carbonate solvents can be 80%, 85%, 90%, or any value within the above range.
[0133] When the total mass content of linear ester solvents and cyclic carbonate solvents is greater than or equal to 80% based on the total mass of the electrolyte, the battery cell exhibits good storage performance. When the total mass content of linear ester solvents and cyclic carbonate solvents is less than or equal to 90% based on the total mass of the electrolyte, it is beneficial to reduce the risk of more severe side reactions within the battery cell caused by a higher solvent content, and can reduce the adverse effects of side reactions on the storage performance of the battery cell.
[0134] As an example, the test methods for cyclic carbonates and linear ester solvents can refer to the standard GB / T9722-2006, which uses organic gas chromatography to quantitatively analyze the content of cyclic carbonates and linear ester solvents in the electrolyte.
[0135] In some embodiments, the battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive active material, and the positive active material includes a lithium phosphate.
[0136] Lithium-containing phosphates refer to phosphates with an olivine structure, such as lithium iron phosphate, lithium manganese iron phosphate, and lithium manganese phosphate. Lithium-containing phosphates include transition metals, such as iron and manganese. Lithium-containing phosphates can also be modified by doping or surface coating to improve their performance. For example, the surface of lithium-containing phosphates can be coated with carbon materials, thereby improving the conductivity of the positive electrode active material.
[0137] In this embodiment, the positive electrode active material includes lithium-containing phosphates. Lithium iron phosphates and other lithium-containing phosphates have high structural stability, which is beneficial to improving the cycle performance of battery cells.
[0138] In some embodiments, the lithium phosphate-containing cathode active material includes at least one of LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4. The above-mentioned lithium phosphate-containing cathode active materials exhibit high structural stability, which helps to improve the cycle performance of battery cells.
[0139] In some embodiments, the elements in the positive electrode active material and the content of each element can be determined using an argon ion cross-section polisher (model JEOL IB-19530CP) and a scanning electron microscope (model Zeiss Sigma 300) (configured with an X-ray energy dispersive spectrometer (EDS, model Oxford X-Max-50mm2).
[0140] As an example, at 25°C, the battery cell was charged to 3.8V at a constant current of 0.33C and discharged to 2.0V at a constant current of 0.33C to obtain a battery cell with 0% SOC. Then, the positive electrode was removed from the battery cell, and the longitudinal cross-section of the positive electrode film was obtained using an ion section polisher. The cross-section of the positive electrode active material particles was scanned using a scanning electron microscope to test the elements and their content.
[0141] During the charging and discharging process, lithium (Li) undergoes insertion / extraction and consumption within a single battery cell. The molar content of Li in the positive electrode active material varies depending on the discharge state of the cell. In the examples of positive electrode active materials in this application, the molar content of Li refers to the initial state of the material, i.e., the state before feeding. After charge-discharge cycles, the molar content of Li changes when the positive electrode active material is applied to the battery system. Similarly, the molar content of O in the examples of positive electrode active materials in this application is only an ideal value. Oxygen release from the crystal lattice causes changes in the molar content of O, resulting in fluctuations in the actual molar content of O.
[0142] The embodiments of this application do not impose any particular restrictions on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. Figure 3 This is a schematic diagram of the structure of a battery cell according to an embodiment of this application. For example, as shown... Figure 3As shown, the battery cell 3 is a square battery cell. The battery cell 3 includes a housing 30 and an electrode assembly 33 disposed within the housing 30. The housing 30 includes a shell 31 and a cover plate 32. The shell 31 may include side plates connected to a base plate, and the base plate and side plates together form a receiving cavity. The shell 31 has an opening communicating with the receiving cavity, and the cover plate 32 can cover the opening to close the receiving cavity. The positive electrode, negative electrode, and separator can be formed into the electrode assembly 33 through a winding process or a stacking process. The electrode assembly 33 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 33. The battery cell 5 can contain one or more electrode assemblies 33, which can be selected by those skilled in the art according to specific practical needs.
[0143] The electrode assembly 33 can be manufactured from a positive electrode, a negative electrode, and a separator through a winding or stacking process. The electrode assembly 33 may include tabs 331.
[0144] Cover plate 32 includes electrode terminals 322, such as Figure 3 As shown, the cover plate 32 includes two electrode terminals 322, one of which is a positive electrode terminal and the other is a negative electrode terminal.
[0145] The battery cell 3 also includes a connecting member 34 for connecting the tab 331 and the electrode terminal 322 of the electrode assembly 33. For example, one connecting member 34 is used to connect the tab of the positive electrode and the positive electrode terminal, and another connecting member 34 is used to connect the tab of the negative electrode and the negative electrode terminal.
[0146] In some embodiments, the battery cell 3 includes a pressure relief mechanism 313 for releasing substances inside the battery cell 3 when thermal runaway occurs, thereby reducing the risk caused by the failure to release the emissions from the battery cell 3 in a timely manner.
[0147] In some embodiments, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be one or more, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.
[0148] In some embodiments, the battery cell may include a housing. The housing is used to encapsulate components such as electrode assemblies and electrolytes. The housing may be made of steel, aluminum, plastic (such as polypropylene), composite metal (such as copper-aluminum composite), or aluminum-plastic film, etc. The housing includes a shell and a cover plate.
[0149] [Negative electrode plate]
[0150] The negative electrode sheet includes a negative current collector and a negative active material layer disposed on the negative current collector, the negative active material layer including a negative active material. The negative active material layer can be disposed on one side surface of the negative current collector or on both sides of the negative current collector.
[0151] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0152] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0153] In some embodiments, the negative electrode active material layer may optionally include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0154] As described above, in some embodiments, the negative electrode active material layer may optionally include conductive carbon. The conductive carbon may be selected from at least one of superconducting carbon, acetylene black, conductive carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0155] In some embodiments, the negative electrode active material layer may also optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0156] In some embodiments, the negative electrode sheet can be prepared by dispersing the above-mentioned components for preparing the negative electrode sheet, such as negative electrode active material, conductive carbon, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto a negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0157] [Positive electrode plate]
[0158] The positive electrode sheet includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, the positive active material layer including a positive active material.
[0159] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive active material layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0160] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0161] In some embodiments, the positive electrode active material in the positive electrode active material layer includes a lithium phosphate with an olivine structure. Examples of lithium phosphate with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.
[0162] The positive electrode active material layer may optionally include at least one of the positive electrode active materials known in the art for batteries: lithium transition metal oxides and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM) 333 LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM) 523 LiNi 0.5 Co 0.25Mn 0.25 O2 (also known as NCM) 211 LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM) 622 LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM) 811 ), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.15 Al 0.05 At least one of O2 and its modified compounds.
[0163] In some embodiments, the positive electrode active material layer may optionally include a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0164] In some embodiments, the positive electrode active material layer may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0165] In one embodiment, the positive electrode sheet can be prepared by forming a positive electrode slurry using the components described above. For example, the positive electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., N-methylpyrrolidone) to form the positive electrode slurry. The positive electrode slurry is then coated onto a positive electrode current collector, and after drying, cold pressing, and other processes, the positive electrode sheet is obtained.
[0166] [Electrolytes]
[0167] In some embodiments, the electrolyte is an electrolyte solution, which may include the additives and solvents in any of the above embodiments, or the additives and solvents in any of the above embodiments.
[0168] In some embodiments, the electrolyte includes an electrolyte salt and a solvent.
[0169] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate, and lithium tetrafluorooxalate phosphate.
[0170] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0171] In some embodiments, the electrolyte may optionally include additives. For example, additives may include the first and second additives described above, and may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0172] This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. The electrolyte can be liquid, semi-solid, or solid.
[0173] [Isolation membrane]
[0174] In some embodiments, the battery cell also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0175] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0176] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0177] In some embodiments, the battery cell may include an outer packaging. This outer packaging can be used to encapsulate the electrode assembly and electrolyte described above.
[0178] In some embodiments, the outer packaging of the battery cell can be a rigid shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the battery cell can also be a flexible package, such as a pouch. The material of the flexible package can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0179] This application does not impose any particular restrictions on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape.
[0180] [Battery Device]
[0181] In some embodiments, the battery device includes one or more battery cells.
[0182] Figure 4 This is a schematic diagram of a battery device according to an embodiment of this application. For example, such as... Figure 4 As shown, the battery device 10 is a battery pack. The battery pack may include a housing and multiple individual battery cells housed within the housing. These individual battery cells are connected in series, parallel, or a combination of both. The individual battery cells can directly assemble into a battery pack, or they can first be assembled into battery modules, and then multiple battery modules can be combined to form a battery pack.
[0183] The battery device 10 may further include a housing 11, which has a hollow interior and houses multiple battery cells 3. For example, multiple battery cells 3 may be connected in parallel, series, or a combination thereof and then placed inside the housing 11. The housing 11 may include a first housing portion 111 and a second housing portion 112, which are fitted together to form the housing 11. The shapes of the first housing portion 111 and the second housing portion 112 may be determined by the shape of the components housed within, for example, by the shape of the combination of multiple battery cells 3 housed within. At least one of the first housing portion 111 and the second housing portion 112 may have an opening. For example, as... Figure 4 As shown, the first housing portion 111 and the second housing portion 112 can both be hollow cuboids with one open side each. The openings of the first housing portion 111 and the second housing portion 112 are opposite to each other, and the first housing portion 111 and the second housing portion 112 are interlocked to form a housing 11 with a closed chamber, which can be used to accommodate multiple battery cells 3. The multiple battery cells 3 are connected in parallel, series, or mixed and placed inside the housing 11 formed by the interlocking of the first housing portion 111 and the second housing portion 112.
[0184] For example, unlike Figure 4 As shown, either the first housing portion 111 or the second housing portion 112 may have only one hollow cuboid with an opening, while the other is plate-shaped to cover the opening. Taking the second housing portion 112 as a hollow cuboid with one opening and the first housing portion 111 as a plate-shaped example, then the first housing portion 111 covers the opening of the second housing portion 112 to form a housing 11 with a closed chamber, which can be used to accommodate multiple battery cells 3.
[0185] In some embodiments, the battery device 10 may further include other components. For example, the battery device 10 may further include a busbar component, which can be used to realize electrical connections between multiple battery cells 3, such as in parallel, series, or mixed connections. Specifically, the busbar component can realize electrical connections between battery cells 3 by connecting to the electrode terminals of the battery cells 3; or, the busbar component can also realize electrical connections between battery cells 3 by connecting to other components of the battery cells 3. The busbar component can be fixed to corresponding components of the battery cells 3 by welding, for example, by welding to electrode terminals, sealing structures, or housings, etc., and the embodiments of this application are not limited thereto.
[0186] The battery cells 3 can be directly assembled into the battery device 10, or they can be first assembled into battery modules, and then multiple battery modules can be assembled into the battery device 10.
[0187] In some embodiments, the battery device 10 may be located in an energy storage device. The energy storage device includes an energy storage container, an energy storage cabinet, etc.
[0188] [Electrical appliances]
[0189] This includes at least one of the battery cells, battery modules, or battery packs provided in this application. The battery cells, battery modules, or battery packs can be used as the power source for an electrical device or as the energy storage unit of an electrical device. Electrical devices can include, but are not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0190] As an electrical device, you can choose individual battery cells, battery modules, or battery packs according to your usage requirements.
[0191] Electrical devices can include vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and power tools, etc. Vehicles can be gasoline-powered cars, natural gas-powered cars, or new energy vehicles; new energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. Spacecraft include airplanes, rockets, space shuttles, and spacecraft, etc. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc. This application does not impose any special limitations on the above-mentioned electrical devices.
[0192] Figure 5This is a schematic diagram of an electrical device according to an embodiment of this application. Figure 5 As shown, this application provides an electrical device, which can be a vehicle 1, and includes the lithium-ion secondary battery in the above embodiment.
[0193] Vehicle 1 can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A motor 5, a controller 4, and a battery device 10 can be installed inside vehicle 1. The controller 4 controls the battery device 10 to supply power to the motor 5. For example, the battery device 10 can be installed under, at the front, or at the rear of vehicle 1. The battery device 10 can be used to power vehicle 1; for example, it can serve as the operating power source for the vehicle 1's electrical system, such as meeting the power requirements for starting, navigation, and operation. In another embodiment of this application, the battery device 10 can not only serve as the operating power source for vehicle 1 but also as the driving power source, replacing or partially replacing gasoline or natural gas to provide driving power to vehicle 1.
[0194] Another example device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a lithium-ion rechargeable battery as their power source.
[0195] Figure 6 This is a schematic diagram of an electrical device according to another embodiment of this application. Figure 6 As shown, this application provides an electrical device, which is an energy storage device 2, and the energy storage device 2 may include multiple battery devices 10. The energy storage device 2 can be applied to a power storage station to store and release electrical energy.
[0196] Alternatively, the electrical device may also be an energy storage device, a lighting device, a spacecraft, etc., as is the case in the embodiments of this application.
[0197] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0198] [Examples and Comparative Examples]
[0199] Example 1
[0200] (1) Preparation of positive electrode sheet
[0201] Lithium iron phosphate, a positive electrode active material, carbon black (Super P), a conductive agent, and polyvinylidene fluoride (PVDF) a binder are mixed evenly in a mass ratio of 97:0.7:2.3 and dissolved in N-methylpyrrolidone (NMP) solvent. After thorough mixing, a positive electrode slurry is prepared. The positive electrode slurry is then uniformly coated on two opposite surfaces of a positive electrode current collector aluminum foil. After drying, cold pressing, and slitting, a positive electrode sheet is obtained.
[0202] (2) Preparation of negative electrode sheet
[0203] Artificial graphite (negative electrode active material), conductive carbon black (Super P), styrene-butadiene rubber (SBR) (binder), and sodium carboxymethyl cellulose (thickener) were dissolved in deionized water at a mass ratio of 96.5:0.5:1.8:1.2. After thorough mixing, a negative electrode slurry was prepared. This slurry was then coated onto both surfaces of a copper foil current collector. After drying, the foil underwent cold pressing, edge trimming, cutting, and slitting to obtain the negative electrode sheet. The graphite active material had a particle size Dv50 of 9.6 μm and a specific surface area of 1.65 m². 2 / g.
[0204] (3) Separating membrane
[0205] The separator includes a base film, which is a polyethylene (PE) film with a thickness of 7 μm. An inorganic coating with a thickness of 2 μm is disposed on the side of the base film facing the negative electrode. The inorganic coating includes alumina ceramic particles.
[0206] (4) Preparation of electrolyte
[0207] The electrolyte was prepared in an argon atmosphere glove box with a water content of less than 10 ppm and an oxygen content of less than 1 ppm. The specific process was as follows: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed evenly at a volume ratio of 30:70. Then, lithium hexafluorophosphate (LiPF6) was added and stirred thoroughly until completely dissolved. Next, the first additive, the second additive, and vinylene carbonate (VC) were added and stirred thoroughly until completely dissolved. The chemical structural formula of the first additive is:
[0208] (Acryloyl-1,3-sulfonyl lactone);
[0209] The chemical structural formula of the second additive is:
[0210]
[0211] Based on the total mass of the electrolyte, the mass content of the first additive is 1%, the mass content of the second additive is 0.5%, the mass content of vinylene carbonate (VC) is 4%, the mass content of the electrolyte salt LiPF6 is 12.5%, the mass content of EC is 27%, and the mass content of DEC is 55%.
[0212] (5) Preparation of battery cells
[0213] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to isolate them. The electrode assembly is then wound to form an electrode assembly. The tabs of the electrode assembly are connected to the cover plate (e.g., by welding the tabs to the cover plate using connecting components). The electrode assembly is placed in an aluminum casing and dried at 85°C for 6 hours. Electrolyte is then injected at an injection rate of 3.0 g / Ah. After vacuum sealing, settling, formation, and shaping, a battery cell is obtained. The formation process involves charging the battery cell to 30% state of charge (SOC) at 0.04C.
[0214] Examples 2-4
[0215] Compared to Example 1, based on the total mass of the electrolyte, the mass ratio of the first additive and the second additive is different, and the mass content of the first additive is greater than or equal to the mass content of the second additive. Specific parameters are detailed in Table 1.
[0216] Examples 5-6
[0217] Compared to Example 1, the mass content of the first additive differs based on the total mass of the electrolyte. Specific parameters are detailed in Table 1.
[0218] Examples 7-9
[0219] Compared to Example 1, the mass content of the second additive differs based on the total mass of the electrolyte. Specific parameters are detailed in Table 1.
[0220] Example 10
[0221] Compared to Example 1, the first additive is different in type, and its chemical structural formula is as follows:
[0222]
[0223] Examples 11-12
[0224] The second additive is different from that in Example 10. The chemical structural formula of the second additive in Example 10 is as follows:
[0225]
[0226] The chemical structural formula of the second additive in Example 11 is as follows:
[0227]
[0228] Comparative Example 1
[0229] The difference between Comparative Example 1 and Example 1 is that the mass content of the first additive in the electrolyte is less than the mass content of the second additive, and the mass contents of the first additive and the second additive are both greater than 2%.
[0230] Comparative Example 2
[0231] The difference between Comparative Example 2 and Example 1 is that the electrolyte includes a first additive but does not include a second additive.
[0232] Comparative Example 3
[0233] The difference between Comparative Example 3 and Example 1 is that the electrolyte does not contain the first additive, but includes the second additive.
[0234] The specific parameters in the examples and comparative examples are shown in Table 1.
[0235] In Table 1, A represents the mass content of the first additive; B represents the mass content of the first additive; the remaining mass content represents the mass content of the first and second additives after the battery cell is formed; in Table 2, cycles represents the number of cycles of the battery cell.
[0236] Table 1. Specific parameters and test results for the examples and comparative examples.
[0237]
[0238]
[0239]
[0240] Table 2 Test results of the examples and comparative examples
[0241] Serial Number Number of cycles to 80% SOH Storage time at 45℃ to 80% SOH / years Example 1 2000 1.95 Example 2 1950 1.90 Example 3 1940 1.92 Example 4 1980 1.89 Example 5 1900 1.92 Example 6 1890 1.86 Example 7 1980 1.91 Example 8 1960 1.86 Example 9 1920 1.86 Example 10 1925 1.89 Example 11 1950 1.93 Example 12 2050 1.97 Comparative Example 1 1840 1.80 Comparative Example 2 1870 1.85 Comparative Example 3 1880 1.84
[0242] It should be noted that in Comparative Example 3, since the first additive was not added, the type of the first additive, its mass content before and after formation are indicated by " / " in Table 1. In Examples 5-12, the focus is mainly on the first and second additives, and the effects of their respective mass content changes and types on storage and cycling performance. Because the cycle life in Examples 5-11 is slightly shorter than that in Example 1, and because the second additive used in Example 12 provides more active free radical sites, the storage and cycling performance are slightly higher than in Example 1. Therefore, the mass content of the first additive after formation in Examples 5-12 was not tested. The mass content of the first additive after formation in Examples 5-12 is indicated by " / " in Table 1.
[0243] In the actual use of a battery cell, the improvement effect on storage performance and cycle performance may not be linear as the mass content of the first and second additives changes. However, these are all reasonable changes under the technical solution of this application and fall within the protection scope of this solution.
[0244] In this embodiment, cycle performance is reflected by the number of cycles a battery cell completes to 80% SOH (State of Health). The more cycles a battery cell completes, the better its cycle performance. Storage performance is reflected by the number of days a battery cell is stored at 45°C to 80% SOH. The more storage days a battery cell is stored, the longer its storage performance.
[0245] Examples 1-12 and Comparative Examples 1-3 and their test results are explained below:
[0246] Based on Examples 1-4 and Comparative Examples 1-3, the storage times of the battery cells in Examples 1-4 were 1.95 years, 1.90 years, 1.92 years, and 1.89 years, respectively, and the number of cycles were 2000 cycles, 1950 cycles, 1940 cycles, and 1980 cycles, respectively, all higher than those in Comparative Examples 1-3. By incorporating the first and second additives, their reduction potentials are higher, preferentially reducing the solvent molecules. The thio groups in the first and second additives participate in the formation of the SEI film, which is beneficial for generating an SEI film rich in inorganic components. This improves the stability and density of the SEI film, reduces the risk of repeated SEI film breakage and reconstruction, and reduces lithium-ion consumption, thereby improving the storage and cycle performance of the battery cells. The first additive plays a dominant role in the formation of inorganic components in the SEI film. Having an unsaturated structure and a high reduction potential, it preferentially reacts with the solvent in the electrolyte, over the second additive, to generate a high-molecular-weight polymer that coats the surface of the negative electrode active material. This reduces the contact between the negative electrode active material and the organic solvent in the electrolyte, minimizing side reactions and the risk of organic component formation in the SEI film, thus improving the storage performance of the battery cell. The second additive decomposes preferentially over the solvent and participates in the formation of the SEI film, resulting in an inorganic-rich SEI film at the negative electrode, further increasing the inorganic content of the SEI film. After decomposition, the side chain groups of the second additive, including active free radicals, readily contact solvent molecules, generating chain-like organic compounds, leading to an increase in the organic content of the SEI film. The steric hindrance of the R2 group in the second additive reduces the contact between the solvent and the active free radicals of the decomposed second additive, reducing the formation of chain-like organic compounds and increasing the proportion of inorganic matter in the SEI film, thereby improving the storage and cycle performance of the battery cell. The unsaturated structure in the first additive decomposes, providing active sites and inducing the aggregation of the second additive on the surface of the negative electrode active material. This further facilitates the formation of an SEI film rich in inorganic components, improving the stability and density of the SEI film and significantly enhancing the storage and cycle performance of the battery cell. In Comparative Example 1, the storage time and cycle count of the battery cell were 1.80 years and 1840 cycles, respectively. On the one hand, the excessively high mass content of both the first and second additives made them prone to side reactions in the electrolyte, reducing the storage and cycle performance of the battery cell. On the other hand, the higher mass content of the second additive compared to the first made it easier for the decomposed second additive to contact solvent molecules, generating chain-like organic compounds. This increased the organic component in the SEI film, reduced its stability, and consequently decreased the storage and cycle performance of the battery cell.
[0247] As shown in Examples 1-12 and Comparative Examples 1-3, the first additive and the second additive have a suitable mass ratio, which can increase the proportion of inorganic matter in the SEI film, which is beneficial to improving the storage performance and cycle performance of the battery cell.
[0248] Based on Examples 5-6 and Comparative Examples 1 and 3, the storage times of the battery cells in Examples 5-6 were 1.92 years and 1.86 years, respectively, and the number of cycles were 1900 cycles and 1890 cycles, respectively, which are higher than those in Comparative Examples 1 and 3. By setting the mass content A of the first additive to satisfy 0.5% ≤ A ≤ 2%, it is beneficial to improve the SEI film with a higher proportion of inorganic matter, thereby improving the stability and density of the SEI film and having a better effect on improving the storage performance and cycle performance of the battery cells.
[0249] Referring to Examples 7-9 and Comparative Examples 1 and 2, the storage times of the battery cells in Examples 5-6 were 1.91 years, 1.86 years, and 1.86 years, respectively, and the number of cycles were 1980 cycles, 1960 cycles, and 1920 cycles, respectively, which are higher than those in Comparative Examples 1 and 2. By setting the mass content B of the second additive to meet the condition of 0.5% ≤ B ≤ 2%, it is beneficial to reduce solvent decomposition and the generation of chain-like organic matter after decomposition of the second additive. This reduces the amount of organic matter in the SEI film, decreases the stability of the SEI film, and causes repeated rupture and reconstruction of the SEI film, consuming active lithium and resulting in a decrease in the storage and cycle performance of the battery cells.
[0250] As shown in Examples 10-12, different types of first and second additives can be selected according to actual usage needs.
[0251] [Testing methods for individual battery cell parameters]
[0252] (1) Cyclic performance testing
[0253] At 25°C, charge the battery cell to 3.8V at a charging rate of 0.5C, then charge it to 0.05C at a constant voltage of 3.8V, let it stand for 10 minutes, and then discharge it to the discharge cutoff voltage (e.g., 2.0V) at a discharging rate of 0.33C, and let it stand for 10 minutes. One charge-discharge cycle is one cycle. The test is stopped when the capacity of the battery cell decays to 80% of the discharge capacity of the first cycle. This number is recorded as the number of cycles at 80% SOH. The more cycles, the better the cycle performance.
[0254] (2) Storage performance testing
[0255] At 25℃, the battery cells are charged at a constant current rate of 0.5C to 3.8V, then charged at a constant voltage of 3.8V to 0.05C, left to stand for 10 minutes, and then discharged at a constant current rate of 0.33C to 2.0V, left to stand for 10 minutes. The resulting discharge capacity is recorded as the initial capacity D0. The battery cells are then charged at a constant current rate of 0.33C to 100% state of charge (SOC) and stored at 45℃. The above steps are repeated every 30 days, and the discharge capacity Dn of the battery after n (n = 30, 60, 90, 120…) days of storage is recorded. The battery capacity retention rate after n days of storage is Qn = Dn / D0 * 100%. When Qn ≤ 80%, the test is stopped, and the number of storage days is recorded.
[0256] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A battery cell, characterized in that, include: An electrolyte, the electrolyte comprising a solvent, a first additive, and a second additive; The first additive includes at least one of the compounds represented by formula (I): R1 includes at least one of alkyl, cycloalkyl, and halogen elements having 1-6 carbon atoms; The second additive includes at least one of the compounds represented by formula (II): Wherein, R2 includes at least one of tert-butyl, isopropyl, phenyl, and naphthyl; R3 includes at least one of alkyl and cycloalkyl groups having 1-6 carbon atoms; Based on the total mass of the electrolyte, the mass content of the first additive is greater than or equal to the mass content of the second additive.
2. The battery cell according to claim 1, characterized in that, The mass ratio of the first additive to the second additive satisfies the condition: 1:1 to 4:
1.
3. The battery cell according to claim 1 or 2, characterized in that, Based on the total mass of the electrolyte, the mass content A of the first additive satisfies: 0.001% ≤ A ≤ 2%.
4. The battery cell according to any one of claims 1-3, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive satisfies: 0.5% ≤ A ≤ 2%.
5. The battery cell according to any one of claims 1-4, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive satisfies: 0.001% ≤ A ≤ 0.55%.
6. The battery cell according to any one of claims 1-5, characterized in that, Based on the total mass of the electrolyte, the mass content B of the second additive satisfies: 0.1% ≤ B ≤ 2%.
7. The battery cell according to any one of claims 1-6, characterized in that, The battery cell includes a negative electrode sheet, the negative electrode sheet includes a negative electrode active material, and the negative electrode active material includes graphite.
8. The battery cell according to any one of claims 1-7, characterized in that, The graphite includes at least one of artificial graphite and natural graphite.
9. The battery cell according to any one of claims 1-8, characterized in that, The second additive includes at least one of dicyclohexyl sulfate, cyclohexylmethylthioacetic acid, 2-cyclohexyltoluene-4-ethyl sulfate, 3,5-dimethylcyclohexyl sulfate, dicyclohexyl dithiophosphate, 4-butyl ethylene sulfite, and 4-propyl ethylene sulfite.
10. The battery cell according to any one of claims 1-9, characterized in that, The solvent includes at least one of linear ester solvents and cyclic carbonate solvents.
11. The battery cell according to any one of claims 1-10, characterized in that, The battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive electrode active material, and the positive electrode active material includes lithium phosphate.
12. A battery device, characterized in that, Includes the battery cell as described in any one of claims 1-11.