Battery cells, battery devices, electrical equipment
By controlling the content of cyclic carbonate solvents and adding specific additives in the battery cells, the formation of the SEI film is optimized, solving the problems of insufficient battery cell life and fast charging performance, and achieving battery performance with longer life and lower internal resistance.
Patent Information
- Application Number
- CN202510624666.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
How to provide a battery cell with a long lifespan to address the shortcomings of existing battery technologies in terms of energy density, cycle life, service life, capacity, and fast charging performance.
By using cyclic carbonate solvents with a content of less than 8% in the battery cell and adding first and second additives with specific structures, including fluorosulfonyl imide salts, the formation of the SEI film is optimized, its stability and density are improved, the lithium-ion transference number is enhanced, the internal resistance is reduced, and the lithium-ion consumption is reduced.
It improves the lifespan and cycle life of individual battery cells, reduces internal resistance, enhances fast charging performance, and improves the overall performance of the battery.
Smart Images

Figure CN123120879A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and more specifically, to a battery cell, a battery device, and an electrical appliance. Background Technology
[0002] The new energy industry is attracting increasing attention. Within this industry, battery technology is a crucial factor in its development.
[0003] The development of battery technology requires consideration of various design factors, such as energy density, cycle life, lifespan, capacity, fast charging performance, and reliability. How to provide a battery cell with a long lifespan is a pressing technical problem that needs to be solved. Summary of the Invention
[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide a battery cell with a long life.
[0005] To achieve the above objectives, this application provides a battery cell, a battery device, and an electrical appliance.
[0006] In a first aspect, a battery cell is provided, comprising: a negative electrode sheet, the negative electrode sheet comprising a negative electrode active material, the negative electrode active material comprising graphite; an electrolyte, the electrolyte comprising a solvent, a first additive, and a second additive; wherein the solvent comprises a cyclic carbonate solvent, and the mass content of the cyclic carbonate solvent is less than or equal to 8% based on the total mass of the electrolyte; the first additive comprises a compound represented by formula (I):
[0007]
[0008] Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano; the second additive includes a fluorosulfonylimide salt.
[0009] This application provides a battery cell in which the cyclic carbonate solvent has a low mass content, which reduces the instability of the cyclic carbonate solvent formation and the risk of a loose SEI film, thereby reducing the consumption of active lithium. In addition, the electrolyte includes a first additive, which competes with the cyclic carbonate for SEI film formation. By reducing the mass content of the cyclic carbonate, its competitive advantage is reduced, allowing the first additive to fully participate in SEI film formation. Furthermore, the first additive includes a compound of formula (I), where R in the compound of formula (I) includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (e.g., hexafluorophosphate ions) in the electrolyte, thereby generating an SEI film rich in inorganic components. This improves the stability and density of the SEI film, reduces the risk of repeated SEI film breakage and reconstruction, reduces lithium ion consumption, and thus improves the battery cell's lifespan. Furthermore, the first additive includes a compound of formula (I). The benzene ring in the compound and the graphite have a π-π interaction, allowing the compound shown in formula (I) to preferentially adsorb onto the graphite surface and enter the inner Helmholtz layer of the electrode / electrolyte interface. This facilitates the enrichment of more anions on the graphite surface anode, thus promoting the formation of an SEI film rich in inorganic components and resulting in a longer battery cell lifespan. Furthermore, the electrolyte includes a second additive, specifically a fluorosulfonyl imide salt. Since the anions in the fluorosulfonyl imide salt have larger radii, lithium ions dissociate more easily, increasing the lithium ion transference number in the electrolyte. This compensates for the insufficient lithium ion transference number caused by the reduced mass content of cyclic carbonate solvents, resulting in a lower internal resistance in the battery cell and improved cycle life. Therefore, the battery cells in this embodiment have a longer lifespan.
[0010] In some embodiments, R comprises one of boron or phosphine, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each component independently includes at least one of the following: hydrogen, chlorine, bromine, fluorine, nitro, sulfonic acid, cyano, trifluoromethyl, trichloromethyl, tribromomethyl, methyl, ethyl, methoxy, and ethoxy. This facilitates the formation of an SEI film rich in inorganic components, thereby reducing lithium ion consumption.
[0011] In some embodiments, the X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It consists of at least two different atoms and includes different heteroatoms.
[0012] In the above technical solution, the substituents on the benzene ring have at least two different groups and include different heteroatoms, which is beneficial for generating an SEI film rich in inorganic components containing different components, thereby facilitating the diffusion of lithium ions and reducing the impedance of the battery cell.
[0013] In some embodiments, the X 12 X 13 X 14 X 15 X 22 X 23 X 24 X 25 X 32 X 33 X 34 X 35 For hydrogen, X 11 X 21 X 31 Each independently includes at least one of fluorine, chlorine, bromine, nitro, sulfonic acid, cyano, methyl, ethyl, methoxy, ethoxy, trifluoromethyl, trichloromethyl, and tribromomethyl. Thus, R and X in the compound shown in formula (I) 11 X 21 X 31 The combination of functional groups is beneficial to the separation of the positive and negative charge centers of the compound molecules shown in formula (I) to form a dipole moment, thereby inducing the accumulation of anions at the negative electrode interface to generate an SEI film rich in inorganic components. The first additive has a better effect and is beneficial to improving the life of the battery cell.
[0014] In some embodiments, the X 11 X 12 X 13 X 14 X 15 X 21 X 22 X23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 The number of hydrogen atoms in the compound ranges from 0 to 3. This results in a higher number of substituent groups on the benzene ring, a lower LUMO energy level and a higher reduction potential for the first additive, making it more likely to decompose preferentially relative to the solvent in the electrolyte. This reduces the risk of poor SEI film quality due to solvent decomposition, thus helping to reduce lithium-ion consumption and improve the lifespan of the battery cell.
[0015] In some embodiments, the first additive includes at least one of 2,4,6-tris(4-fluorophenyl)cycloboroxane, tris(4-fluorophenyl)phosphine, tris(pentafluorophenyl)phosphine, tris(4-chlorophenyl)phosphine, triphenylphosphine, triphenylborane, tris(pentafluorophenyl)borane, and triphenylphosphine oxide.
[0016] The aforementioned first additive has a good effect and is beneficial to improving the lifespan of battery cells.
[0017] In some embodiments, the mass content of the first additive is 0.001% to 5% based on the total mass of the electrolyte.
[0018] The aforementioned mass content of the first additive includes both the mass content during the battery cell preparation process and the mass content after the battery cell has been formed. When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the battery cell lifespan. When the mass content of the first additive is less than or equal to 5% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the first additive within the battery cell due to excessive content, thereby reducing the adverse impact of side reactions on the battery cell lifespan. Furthermore, since the cyclic carbonate solvents in the electrolyte have a low mass content, using a smaller mass content of the first additive is beneficial for improving the battery cell lifespan.
[0019] In some embodiments, the mass content of the first additive is 0.5% to 5% based on the total mass of the electrolyte.
[0020] The mass content of the first additive mentioned above refers to the mass content of the battery cell before formation. When the mass content of the first additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it has a good effect on improving the lifespan of the battery cell. When the mass content of the first additive is less than or equal to 5% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the first additive within the battery cell due to excessive content, thereby reducing the adverse impact of side reactions on the lifespan of the battery cell.
[0021] In some embodiments, the mass content of the first additive is 1.2% to 3.5% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0022] In some embodiments, the mass content of the first additive is 0.001% to 1.7% based on the total mass of the electrolyte.
[0023] The mass content of the first additive mentioned above refers to the mass content of the battery cell after formation. When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the lifespan of the battery cell. When the mass content of the first additive is less than or equal to 1.7% based on the total mass of the electrolyte, it can reduce the risk of excessive residual first additive after formation, which could lead to side reactions within the battery cell, thereby reducing the adverse impact of side reactions on the lifespan of the battery cell.
[0024] In some embodiments, the mass content of the first additive is 0.3% to 0.8% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0025] In some embodiments, in the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area of the peak at 53.8 ± 0.2 eV accounts for less than 40%.
[0026] The peak at 53.8 ± 0.2 eV corresponds to organic matter in the SEI film. The proportion of the peak area at 53.8 ± 0.2 eV reflects the content of organic matter in the SEI film. The smaller the proportion of the peak area at 53.8 ± 0.2 eV, the lower the content of organic matter in the SEI film, the higher the content of inorganic components, and the denser and more stable the SEI film. In the embodiments of this application, the proportion of the peak area at 53.8 ± 0.2 eV is less than 40%, indicating a higher content of inorganic components in the SEI film. This makes the SEI film denser and more stable, which helps reduce the risk of repeated breakage and reconstruction of the SEI film, reduces lithium-ion consumption, and thus helps improve the lifespan of the battery cells.
[0027] In some embodiments, in the X-ray photoelectron spectroscopy of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for 10% to 32%. This results in a denser and more stable SEI film, reducing the risk of repeated breakage and reconstruction, which helps reduce lithium-ion consumption and thus improves the lifespan of the battery cell.
[0028] In some embodiments, the mass content of the second additive is 0.001% to 3% based on the total mass of the electrolyte.
[0029] When the mass content of the second additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it helps to compensate for the insufficient lithium-ion transference number caused by the low mass content of cyclic carbonate solvents. This results in a more suitable lithium-ion transference number in the electrolyte, lower internal resistance in the battery cell, and consequently, a longer battery cell lifespan. When the mass content of the second additive is less than or equal to 3% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the second additive, thereby reducing the risk of lithium-ion consumption and resulting in a longer battery cell lifespan.
[0030] In some embodiments, the mass content of the second additive is 0.5% to 3% based on the total mass of the electrolyte.
[0031] The mass content of the second additive mentioned above refers to the mass content of the battery cell before formation. When the mass content of the second additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it helps to compensate for the insufficient lithium-ion transference number caused by the low mass content of cyclic carbonate solvents, resulting in a more suitable lithium-ion transference number in the electrolyte, lower internal resistance in the battery cell, and consequently, a longer battery cell lifespan. When the mass content of the second additive is less than or equal to 3% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the second additive, thereby reducing the risk of lithium-ion consumption and resulting in a longer battery cell lifespan.
[0032] In some embodiments, the mass content of the second additive is 1.5% to 2% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0033] In some embodiments, the mass content of the second additive is 0.2% to 2.0% based on the total mass of the electrolyte.
[0034] The mass content of the second additive mentioned above refers to the mass content of the battery cell after formation. When the mass content of the second additive is greater than or equal to 0.2% based on the total mass of the electrolyte, it helps to compensate for the insufficient lithium-ion transference number caused by the low mass content of cyclic carbonate solvents, resulting in a more suitable lithium-ion transference number in the electrolyte, lower internal resistance in the battery cell, and consequently, a longer battery cell lifespan. When the mass content of the second additive is less than or equal to 2.0% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the second additive, thereby reducing the risk of lithium-ion consumption and resulting in a longer battery cell lifespan.
[0035] In some embodiments, the mass content of the second additive is 1.2% to 1.4% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0036] In some embodiments, the second additive includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonate)imide.
[0037] The aforementioned second additive has a larger anionic radius, making it easier to dissociate. This helps to increase the lithium-ion migration number in the electrolyte, reduce the internal resistance of the battery cell, and thus improve the lifespan of the battery cell.
[0038] In some embodiments, the cyclic carbonate solvent has a mass content of 2% to 6% based on the total mass of the electrolyte.
[0039] When the mass content of cyclic carbonate solvent is greater than or equal to 2% based on the total mass of the electrolyte, the electrolyte has a suitable lithium-ion transference number, the battery cell has a low internal resistance, and thus the battery cell has a long lifespan. When the mass content of cyclic carbonate solvent is less than or equal to 6% based on the total mass of the electrolyte, it is beneficial to reduce the risk of unstable SEI film rich in organic components formed by cyclic carbonate solvent at the negative electrode, which in turn is beneficial to reduce the risk of repeated SEI film rupture and reconstruction consuming active lithium, and the battery cell has a long lifespan.
[0040] In some embodiments, the cyclic carbonate solvent includes at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
[0041] The aforementioned cyclic carbonate solvents have high dielectric constants and good solvation capabilities, which are beneficial for the dissociation of lithium ions in the electrolyte salt, thereby increasing the lithium ion transference number in the electrolyte. As a result, the battery cells have lower resistance, which is beneficial for improving the lifespan of the battery cells.
[0042] In some embodiments, the electrolyte further includes at least one of a third additive and a fourth additive, wherein the third additive includes a carbonate additive and the fourth additive includes a sulfur-containing additive.
[0043] Carbonate additives facilitate the formation of polymer coatings on graphite surfaces, which can buffer the volume expansion of battery cells during charge and discharge processes. They also help repair damaged sites in the SEI film during long-term charge and discharge cycles, thereby improving the lifespan of battery cells.
[0044] The film formed on the graphite surface by sulfur-containing additives has good ion-conducting ability, which helps reduce the increase of DC resistance in the battery cell and thus improves the kinetic isoelectric performance of the battery cell. Furthermore, the combined use of carbonate and sulfur-containing additives helps to balance the battery cell's lifespan and kinetic performance.
[0045] In some embodiments, the carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate. These additives have a good effect on improving the lifespan of individual battery cells.
[0046] In some embodiments, the sulfur-containing additive includes at least one selected from vinyl sulfate, vinyl disulfate, butenyl sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate. These additives have a good effect on improving the kinetic performance of battery cells.
[0047] In some embodiments, the sum of the mass contents of the third additive and the fourth additive is 0.5% to 10% based on the total mass of the electrolyte.
[0048] When the mass content of the third and fourth additives is greater than or equal to 0.5% based on the total mass of the electrolyte, the battery cell has a longer lifespan. When the mass content of the third and fourth additives is less than or equal to 10% based on the total mass of the electrolyte, it is beneficial to reduce the risk of more severe side reactions in the battery cell caused by the higher content of the third and fourth additives, and can reduce the adverse effects of side reactions on the lifespan of the battery cell.
[0049] In some embodiments, the combined mass content of the third and fourth additives is 2% to 8% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0050] In some embodiments, the electrolyte comprises an electrolyte salt, including lithium hexafluorophosphate. Lithium hexafluorophosphate is readily dissociable and reasonably priced, making it suitable as a primary electrolyte salt in electrolytes.
[0051] In some embodiments, the electrolyte satisfies at least one of the following conditions:
[0052] The electrolyte has a conductivity of 8 mS / cm to 20 mS / cm at 20°C to 30°C.
[0053] The viscosity of the electrolyte at 20°C to 30°C is 2.0 mPa·s to 3.5 mPa·s.
[0054] The electrolyte has a density of 1.05 g / mL to 1.35 g / mL at 20°C to 30°C.
[0055] When the conductivity of the electrolyte meets the above-mentioned range, the electrolyte has high conductivity, which is conducive to the migration of lithium ions, thereby helping to reduce the ohmic resistance of the battery cell and the kinetic lithium consumption caused by polarization, and thus helping to improve the life of the battery cell.
[0056] When the viscosity of the electrolyte meets the above-mentioned range, the electrolyte has a lower viscosity, which is conducive to the migration of lithium ions, thereby reducing the ohmic resistance of the battery cell and the kinetic lithium consumption caused by polarization, and thus helping to improve the life of the battery cell.
[0057] When the electrolyte density meets the above-mentioned range, it is beneficial for the electrolyte to have higher conductivity and lower viscosity, which is conducive to the migration of lithium ions. This helps to reduce the ohmic resistance of the battery cell and the kinetic lithium consumption caused by polarization, thereby improving the life of the battery cell.
[0058] In some embodiments, the graphite satisfies at least one of the following conditions:
[0059] The volume average particle size Dv50 of the graphite is 8 μm to 14 μm;
[0060] The specific surface area of the graphite is 0.8 m². 2 / g to 1.7m 2 / g.
[0061] When the volume average particle size Dv50 of graphite is greater than or equal to 8 μm, there is a suitable pore size between graphite particles, which facilitates the wetting of electrolyte and thus the transport of lithium ions, which is beneficial to improving the fast charging performance of the battery cell. When the volume average particle size Dv50 of graphite is less than or equal to 14 μm, lithium ions have a suitable diffusion path, which facilitates the diffusion of lithium ions and is beneficial to improving the fast charging performance of the battery cell.
[0062] When the specific surface area of graphite is greater than or equal to 0.8 m² 2At a specific surface area of 1.7 m² / g, this facilitates the insertion and extraction of lithium ions into graphite, thus improving the fast-charging performance of individual battery cells; 2 At a rate of / g, it is beneficial to reduce the degree of side reactions between graphite and electrolyte due to the large number of active sites in graphite, which can reduce the consumption of lithium ions caused by side reactions, thereby improving the lifespan of battery cells.
[0063] In some embodiments, the graphite satisfies at least one of the following conditions:
[0064] The volume average particle size Dv50 of the graphite is 10 μm to 13 μm;
[0065] The specific surface area of the graphite is 1.0 m². 2 / g to 1.4m 2 / g.
[0066] With a graphite volume average particle size (Dv50) of 10 μm to 13 μm, the battery cell exhibits good fast-charging performance; and with a graphite specific surface area of 1.0 m², the battery cell demonstrates good fast-charging performance. 2 / g to 1.4m 2 At a rate of / g, the battery cells exhibit good fast-charging performance and a long lifespan.
[0067] In some embodiments, at least a portion of the surface of the graphite has a carbon coating layer, the graphitization degree of the carbon coating layer being 0.85 to 0.9. This facilitates the rapid insertion and extraction of lithium ions into the graphite, resulting in better fast-charging performance of the battery cell.
[0068] In some embodiments, the graphite includes at least one of artificial graphite or natural graphite.
[0069] In this embodiment, graphite may include natural graphite, artificial graphite, or a mixture of natural and artificial graphite.
[0070] In some embodiments, the graphite comprises at least one of primary particles and secondary particles.
[0071] In this embodiment, graphite may include primary particles, secondary particles, or a mixture of primary and secondary particles.
[0072] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including the negative electrode active material, and the negative electrode sheet satisfies at least one of the following conditions:
[0073] The compaction density of the negative electrode film is 1.50 g / cm³. 3Up to 1.70 g / cm 3 ;
[0074] The porosity of the negative electrode sheet is 25% to 60%;
[0075] The one-sided density of the negative electrode film is 7 mg / cm³. 2 Up to 10.5 mg / cm 2 .
[0076] The compaction density of the negative electrode film layer is greater than or equal to 1.50 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the negative electrode film is less than or equal to 1.70 g / cm³, it is beneficial to improve the energy density of individual battery cells. 3 In this case, it is beneficial to reduce the risk of particle breakage of negative electrode active material due to the high compaction density of the negative electrode film layer. It can reduce the side reactions between broken particles and electrolyte, reduce lithium ion consumption, and thus help reduce the adverse impact on the life of battery cells.
[0077] When the porosity of the negative electrode sheet is greater than or equal to 25%, it facilitates the transport and diffusion of lithium ions, which is beneficial to improving the fast charging performance of the battery cell. When the porosity of the negative electrode sheet is less than or equal to 60%, the negative electrode sheet has a suitable strength, which can reduce the risk of cracking of the negative electrode sheet and is beneficial to improving the life of the battery cell.
[0078] The density on one side of the negative electrode film layer is greater than or equal to 7 mg / cm³. 2 Under these conditions, it is beneficial to improve the energy density of the battery cell; when the density on one side of the negative electrode film is less than or equal to 10.5 mg / cm³, it is beneficial to improve the energy density of the battery cell. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial for improving the fast-charging performance of individual battery cells. Furthermore, the combination of the first additive with the areal density and compaction density of the negative electrode film within the aforementioned range also contributes to a longer battery cell lifespan.
[0079] In some embodiments, the negative electrode sheet satisfies at least one of the following conditions:
[0080] The compaction density of the negative electrode film is 1.52 g / cm³. 3 Up to 1.60 g / cm 3 ;
[0081] The porosity of the negative electrode sheet is 25% to 35%;
[0082] The single-sided density of the negative electrode film is 7.8 mg / cm³. 2 Up to 9.8 mg / cm 2 .
[0083] The compaction density of the negative electrode film layer is 1.52 g / cm³. 3 Up to 1.60 g / cm 3 Under these conditions, the battery cell exhibits high energy density and long lifespan; with a negative electrode porosity of 25% to 35%, the battery cell demonstrates good fast-charging performance and long lifespan; and with a single-sided density of 7.8 mg / cm³ in the negative electrode film layer... 2 Up to 9.8 mg / cm 2 Under these conditions, the battery cells have high energy density and good fast charging performance.
[0084] In some embodiments, the battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side surface of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium phosphate.
[0085] Lithium phosphates have high structural stability, and lithium phosphate battery cells have long cycle life.
[0086] In some embodiments, at least a portion of the surface of the lithium phosphate has a coating layer comprising carbon. This helps improve the conductivity of the lithium phosphate, facilitating the utilization of the battery cell's capacity and extending its lifespan.
[0087] In some embodiments, the lithium-containing phosphate includes a component having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.1.
[0088] In some embodiments, the specific capacity of the positive electrode active material is between 135 mAh / g and 150 mAh / g. This results in a suitable specific capacity for the positive electrode active material and a suitable energy density for the battery cell.
[0089] In some embodiments, the positive electrode film layer satisfies at least one of the following conditions:
[0090] The compaction density of the positive electrode film is 2.52 g / cm³. 3 Up to 2.78 g / cm 3 ;
[0091] The areal density of one side of the positive electrode film is 12 mg / cm³. 2 Up to 19 mg / cm 2 .
[0092] The compaction density of the positive electrode film layer is greater than or equal to 2.52 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the positive electrode film is less than or equal to 2.78 g / cm³. 3 Under these conditions, it is beneficial for the transport of lithium ions, thereby improving the fast charging performance of individual battery cells.
[0093] The density on one side of the positive electrode film is greater than or equal to 12 mg / cm³. 2 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the density on one side of the positive electrode film is less than or equal to 19 mg / cm³, it is beneficial to improve the energy density of individual battery cells. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial for improving the fast-charging performance of individual battery cells. Furthermore, the combination of the first additive with the areal density and compaction density of the positive electrode film within the aforementioned range also contributes to a longer battery cell lifespan.
[0094] In a second aspect, a battery device is provided, comprising the battery cell of the first aspect and any of the embodiments thereof.
[0095] Thirdly, an electrical device is provided, comprising a battery cell of the first aspect and any of the embodiments thereof, or a battery device of the second aspect, wherein the battery cell or battery device is used to store or provide electrical energy. Attached Figure Description
[0096] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0097] Figure 1 This is a schematic diagram of a vehicle according to an embodiment of this application;
[0098] Figure 2 This is a schematic diagram of a battery device according to an embodiment of this application;
[0099] Figure 3 This is a schematic diagram of the negative electrode sheet according to an embodiment of this application;
[0100] Figure 4 This is a schematic diagram of the positive electrode sheet according to an embodiment of this application;
[0101] Figure 5This is a schematic diagram of a battery cell according to an embodiment of this application. Detailed Implementation
[0102] Embodiments of the battery cell, battery device, and electrical appliance of this application have been described in detail with appropriate reference to the accompanying drawings; however, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0103] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0104] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0105] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0106] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0107] This application aims to develop a battery cell with a long lifespan. The battery cell includes: a negative electrode sheet comprising a negative electrode active material, the negative electrode active material comprising graphite; an electrolyte comprising a solvent, a first additive, and a second additive; wherein the solvent comprises a cyclic carbonate solvent, and the mass content of the cyclic carbonate solvent is less than or equal to 8% based on the total mass of the electrolyte; the first additive comprises a compound represented by formula (I):
[0108]
[0109] Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano; the second additive includes a fluorosulfonylimide salt.
[0110] Cyclic carbonate solvents can effectively dissociate lithium salts in the electrolyte, which is beneficial for increasing the lithium ion transference number in the electrolyte. However, cyclic carbonate solvents participate in the formation of the SEI film at the negative electrode, and the generated SEI film is mostly composed of organic components such as lithium ethylene dicarbonate (LEDC). This SEI film has a relatively loose structure and poor stability, and is at high risk of repeated breakage and reconstruction during the charge-discharge cycle of the battery cell, resulting in a large consumption of active lithium and hindering the improvement of the cycle life of the battery cell.
[0111] This application provides a battery cell in which the cyclic carbonate has a low mass content, which reduces the risk of the cyclic carbonate participating in the formation of a loose SEI film, thereby reducing the consumption of active lithium. Furthermore, the electrolyte includes a first additive, which competes with the cyclic carbonate for SEI film formation. By reducing the mass content of the cyclic carbonate, its competitive advantage is reduced, allowing the first additive to fully participate in SEI film formation. In addition, the first additive includes a compound of formula (I), where R in the compound of formula (I) includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (e.g., hexafluorophosphate ions) in the electrolyte, thereby generating an SEI film rich in inorganic components. This improves the stability and density of the SEI film, reduces the risk of repeated SEI film breakage and reconstruction, reduces lithium ion consumption, and thus improves the battery cell's lifespan. Furthermore, formula (I)... The compound shown exhibits a π-π interaction between the benzene ring and graphite, allowing the compound of formula (I) to preferentially adsorb onto the graphite surface and enter the inner Helmholtz layer of the electrode / electrolyte interface. This facilitates the induction of more anions to accumulate on the graphite surface anode, thus promoting the formation of an SEI film rich in inorganic components and resulting in a longer battery cell lifespan. Furthermore, the electrolyte includes a second additive, which comprises a fluorosulfonyl imide salt. Since the anions in the fluorosulfonyl imide salt have larger radii, lithium ions dissociate more easily, increasing the lithium ion transference number in the electrolyte. This compensates for the insufficient lithium ion transference number caused by the reduced mass content of cyclic carbonate solvents, resulting in a lower internal resistance in the battery cell and improved cycle life. Therefore, the battery cells of this embodiment have a longer lifespan.
[0112] The technical solutions described in the embodiments of this application are applicable to various electrical devices that use battery devices.
[0113] Electrical equipment can include vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and power tools, etc. Vehicles can be gasoline-powered cars, natural gas-powered cars, or new energy vehicles; new energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. Spacecraft include airplanes, rockets, space shuttles, and spacecraft, etc. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc. This application does not impose any special limitations on the above-mentioned electrical equipment.
[0114] For ease of explanation, the following embodiments use a vehicle as an example of electrical equipment.
[0115] For example, such as Figure 1 The diagram shown is a structural schematic of a vehicle 1 according to one embodiment of this application. Vehicle 1 can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A motor 40, a controller 30, and a battery device 10 can be installed inside vehicle 1. The controller 30 controls the battery device 10 to supply power to the motor 40. For example, the battery device 10 can be installed at the bottom, front, or rear of vehicle 1. The battery device 10 can be used to power vehicle 1. For example, the battery device 10 can serve as the operating power source for vehicle 1, for example, to meet the electrical system requirements of vehicle 1, such as for starting, navigation, and operation. In another embodiment of this application, the battery device 10 can not only serve as the operating power source for vehicle 1, but also as the driving power source for vehicle 1, replacing or partially replacing gasoline or natural gas to provide driving power for vehicle 1.
[0116] Figure 2 A partial structural schematic diagram of the battery device 10 according to an embodiment of this application is shown. For example, as... Figure 2 As shown, the battery device 10 of this application embodiment may include a plurality of battery cells 3 to meet different power usage requirements. The shape of the battery cell 3 in this application embodiment can be set according to actual application. For example, the battery cell 3 can be cylindrical, or it can be cuboid or other shapes, and this application embodiment is not limited to this.
[0117] It should be understood that, such as Figure 2 As shown, the battery device 10 of this embodiment may further include a housing 11, which can be used to accommodate multiple battery cells 3. The housing 11 of this embodiment has a hollow interior, and the multiple battery cells 3 are accommodated within the housing 11. The housing 11 may include two parts, referred to herein as a first housing portion 111 and a second housing portion 112, which are fastened together. The shapes of the first housing portion 111 and the second housing portion 112 can be determined according to the shape of the components housed inside, for example, according to the shape of the combination of the multiple battery cells 3 housed inside. At least one of the first housing portion 111 and the second housing portion 112 has an opening. For example, as... Figure 2As shown, the first housing portion 111 and the second housing portion 112 can both be hollow cuboids with one open side each. The openings of the first housing portion 111 and the second housing portion 112 are opposite to each other, and the first housing portion 111 and the second housing portion 112 are interlocked to form a housing 11 with a closed chamber, which can be used to accommodate multiple battery cells 3. The multiple battery cells 3 are connected in parallel, series, or mixed and placed inside the housing 11 formed by the interlocking of the first housing portion 111 and the second housing portion 112.
[0118] For example, unlike Figure 2 As shown, either the first housing portion 111 or the second housing portion 112 may have only one hollow cuboid with an opening, while the other is plate-shaped to cover the opening. Taking the second housing portion 112 as a hollow cuboid with one opening and the first housing portion 111 as a plate-shaped example, then the first housing portion 111 covers the opening of the second housing portion 112 to form a housing 11 with a closed chamber, which can be used to accommodate multiple battery cells 3.
[0119] In this embodiment of the application, the battery cell can be a secondary battery, which refers to a battery cell that can be recharged to activate the active materials and continue to be used after the battery cell has been discharged.
[0120] The battery cell can be a lithium-ion battery.
[0121] During the charging process of a single battery cell, lithium ions are released from the positive electrode active material, move and embed into the negative electrode; while during the discharging process, lithium ions are released from the negative electrode, move and embed into the positive electrode active material.
[0122] It should be understood that the “intercalation” process described in this application refers to the process by which lithium ions are intercalated in the positive electrode active material or the negative electrode due to an electrochemical reaction, and the “extraction” process described in this application refers to the process by which lithium ions are extracted from the positive electrode active material or the negative electrode due to an electrochemical reaction.
[0123] Typically, a battery cell includes a positive electrode, a negative electrode, an electrolyte, and a separator. The following section describes the battery cell and its components provided in this application.
[0124] [Battery cell]
[0125] This application provides a battery cell, including an electrolyte and a negative electrode.
[0126] The negative electrode sheet includes a negative electrode active material, which includes graphite. The graphite may include at least one of natural graphite or artificial graphite.
[0127] The electrolyte includes a solvent, a first additive, and a second additive.
[0128] The solvents include cyclic carbonate solvents, and the mass content of cyclic carbonate solvents is less than or equal to 8% based on the total mass of the electrolyte.
[0129] Cyclic carbonate solvents are a class of organic carbonate compounds with cyclic structures, containing cyclic structures formed by carbonate groups (-O-CO-O-). As an example, cyclic carbonate solvents include at least one of ethylene carbonate and propylene carbonate.
[0130] Based on the total mass of the electrolyte, the mass content of the cyclic carbonate solvent can be 8%, 7.5%, 7%, 6.5%, 6%, 5.5%, 5%, 4.5%, 4%, 3.5%, 3%, 2.5%, 2%, or any value within the above range.
[0131] When the mass content of cyclic carbonate solvent is less than or equal to 8% based on the total mass of the electrolyte, the cyclic carbonate solvent in the battery cell has a low mass content. This can reduce the instability of cyclic carbonate solvent formation and the risk of loose SEI film, thereby reducing the consumption of active lithium and improving the life of the battery cell.
[0132] The first additive includes the compound shown in formula (I):
[0133]
[0134] Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano.
[0135] As an example, the halogen element includes at least one of fluorine, chlorine, and bromine; the C1-C3 alkyl group includes at least one of methyl, ethyl, and propyl; the halogen-substituted C1-C3 alkyl group includes at least one of fluorine, chlorine, or bromine-substituted C1-C3 alkyl group; and the C1-C3 alkoxy group includes at least one of methoxy, ethoxy, and propoxy.
[0136] X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Any two groups can be the same group or different groups.
[0137] In X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When all components are hydrogen, the first additive can have the following structure:
[0138]
[0139] In X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35When each of the following groups independently includes at least one of halogen elements (e.g., fluorine, chlorine, bromine), nitro, sulfonic acid group, cyano, C1-C3 alkoxy (e.g., methoxy, ethoxy), or halogen-substituted C1-C3 alkyl (e.g., trifluoromethyl, trichloromethyl, tribromomethyl), the above groups (hereinafter collectively referred to as X groups) are electron-withdrawing groups and can form X-electron-rich centers. When X groups are combined with R, the positive and negative charge centers of the compound molecule shown in formula (I) are separated to form a dipole moment. Through ionic dipole interaction, anion enrichment is induced, and anion decomposition is promoted to form a relatively stable SEI film rich in inorganic components.
[0140] In the compound shown in formula (I), R includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (such as hexafluorophosphate ions) in the electrolyte. The decomposition of the anions participates in the formation of the SEI film, thereby generating an anion-derived SEI film rich in inorganic components at the negative electrode. The inorganic-rich SEI film is denser than the organic-rich SEI film, which reduces the risk of organic solvents in the electrolyte penetrating the SEI film and contacting the graphite of the negative electrode, thus reducing the risk of forming an organic-rich SEI film and making it more favorable for forming an inorganic-rich SEI film. The inorganic-rich SEI film has better thermal stability and mechanical properties than the organic-rich SEI film, and is less prone to breakage during the charge-discharge cycle of the battery cell. This reduces the consumption of active lithium caused by repeated breakage and reconstruction of the SEI film, which is beneficial to improving the lifespan of the battery cell.
[0141] The benzene ring in the compound shown in formula (I) has a π-π interaction with the graphite, allowing the compound to enter the inner Helmholtz layer of the electrical double layer at the graphite / electrolyte interface. Since the electrical double layer is closer to the graphite surface than the electrolyte phase, and the SEI film is a solid electrolyte membrane at the graphite / electrolyte interface, the entry of the compound in formula (I) into the electrical double layer facilitates its preferential adsorption on the graphite surface, inducing more anions to accumulate on the graphite surface anode. This, in turn, is more conducive to the formation of anion-derived, inorganic-rich SEI film, thereby improving the lifespan of the battery cell.
[0142] Furthermore, the compound shown in formula (I) is a molecular compound, which is not easily dissociated in the electrolyte and is more conducive to adsorption on the surface of graphite. This allows for the formation of a higher quality SEI film on the graphite surface, which helps reduce the lithium ions consumed by repeated rupture and reconstruction of the SEI film, resulting in a longer battery cell lifespan.
[0143] The second additive includes fluorosulfonyl imide salts.
[0144] Fluorosulfonyl imide salts are a class of anionic fluorine-containing sulfonyl imide compounds. Their structure consists of a sulfonyl imide group (-SO2-N-SO2-) in which a hydrogen atom or a fluorine-containing group is substituted, and the salt is formed by combining with a cation (such as lithium). As an example, fluorosulfonyl imide salts include at least one of bis(fluorosulfonyl) imide salts and trifluoromethanesulfonyl imide salts.
[0145] Because the anions in fluorosulfonyl imide salts have larger radii, lithium ions are more easily dissociated, which helps to increase the lithium ion migration number in the electrolyte. This can compensate for the insufficient lithium ion migration number caused by the reduced mass content of cyclic carbonate solvents, resulting in lower internal resistance in the battery cell. This can reduce the adverse effects of increased internal resistance on the battery cell's lifespan and help improve the cycle life of the battery cell.
[0146] In this embodiment, the cyclic carbonate solvent in the battery cell has a low mass content, which reduces the instability of the cyclic carbonate solvent formation and the risk of a loose SEI film, thereby reducing the consumption of active lithium. Furthermore, the electrolyte includes a first additive, which competes with the cyclic carbonate for SEI film formation. By reducing the mass content of the cyclic carbonate, its competitive advantage is reduced, allowing the first additive to fully participate in SEI film formation. The first additive includes a compound of formula (I), where R in the compound includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (e.g., hexafluorophosphate ions) in the electrolyte, thereby generating an SEI film rich in inorganic components. This improves the stability and density of the SEI film, reduces the risk of repeated SEI film breakage and reconstruction, reduces lithium ion consumption, and thus improves the battery cell's lifespan. In addition, the compound of formula (I)... The compound shown exhibits a π-π interaction between the benzene ring and graphite, allowing the compound of formula (I) to preferentially adsorb onto the graphite surface and enter the inner Helmholtz layer of the electrode / electrolyte interface. This facilitates the induction of more anions to accumulate on the graphite surface at the negative electrode, thus promoting the formation of an SEI film rich in inorganic components and resulting in a longer battery cell lifespan. Furthermore, the electrolyte includes a second additive, specifically a fluorosulfonyl imide salt. Since the anions in the fluorosulfonyl imide salt have larger radii, lithium ions dissociate more easily, increasing the lithium ion transference number in the electrolyte. This compensates for the insufficient lithium ion transference number caused by the reduced mass content of cyclic carbonate solvents, resulting in a lower internal resistance and improved cycle life. Therefore, the battery cells of this embodiment have a longer lifespan.
[0147] In some embodiments, R includes one of boron or phosphine, X 11 X 12X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each component independently includes at least one of the following: hydrogen, fluorine, chlorine, bromine, nitro, sulfonic acid, cyano, methyl, ethyl, methoxy, ethoxy, trifluoromethyl, trichloromethyl, and tribromomethyl. This facilitates the formation of an SEI film rich in inorganic components, thereby reducing lithium ion consumption.
[0148] In some embodiments, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It consists of at least two different atoms and includes different heteroatoms.
[0149] Heteroatoms are atoms other than carbon and hydrogen. For example, heteroatoms include at least one of O, N, F, Cl, and Br.
[0150] In the above technical solution, the substituents on the benzene ring have at least two different groups and include different heteroatoms, which is beneficial for generating an SEI film rich in inorganic components containing different components, thereby facilitating the diffusion of lithium ions and reducing the impedance of the battery cell.
[0151] As an example, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35The generated SEI film, rich in inorganic components, can contain at least two different heteroatoms, including LiF, Li₂O, Li₂CO₃, Li₃N, Li₂SO₃, and Li₂SO₄. These diverse components contribute to grain boundary diversification, allowing lithium ions to conduct and diffuse through these boundaries. This diversification facilitates lithium ion diffusion, thereby reducing the impedance of the battery cell. Furthermore, reduced impedance also helps lower the temperature rise of the battery cell, thus mitigating the exacerbation of side reactions within the cell at higher temperatures and ultimately extending the battery cell's lifespan.
[0152] In some embodiments, X 12 X 13 X 14 X 15 X 22 X 23 X 24 X 25 X 32 X 33 X 34 X 35 For hydrogen, X 11 X 21 X 31 Each independently includes at least one of fluorine, chlorine, bromine, nitro, sulfonic acid, cyano, methyl, ethyl, methoxy, ethoxy, trifluoromethyl, trichloromethyl, and tribromomethyl. Thus, R and X in the compound shown in formula (I) 11 X 21 X 31 The combination of functional groups is beneficial to the separation of the positive and negative charge centers of the compound molecules shown in formula (I) to form a dipole moment, thereby inducing the accumulation of anions at the negative electrode interface to generate an SEI film rich in inorganic components. The first additive has a better effect and is beneficial to improving the life of the battery cell.
[0153] As an example, the compound shown in formula (I) has the following structure:
[0154]
[0155] As an example, X11, X21, and X31 each independently include at least one of fluorine, chlorine, bromine, trifluoromethyl, trichloromethyl, and tribromomethyl.
[0156] As a predictable mechanism, the first additive has a strong adsorption effect on anions, which is more conducive to the formation of an SEI film rich in inorganic components, reducing the risk of repeated rupture and reconstruction of the SEI film, reducing the consumption of lithium ions, and thus helping to improve the life of the battery cell.
[0157] In the above embodiments, the first additive has a better effect and is beneficial to improving the lifespan of the battery cell.
[0158] In some embodiments, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It contains 0 to 3 hydrogen atoms.
[0159] X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 The number of hydrogen atoms can be 0, 1, 2, or 3.
[0160] In X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When the number of hydrogen atoms is 0, all positions on the benzene ring have substituents.
[0161] The more substituents on the benzene ring, the lower the LUMO energy level of the first additive becomes. The first additive has a higher reduction potential, which in turn makes the difference between the reduction potential of the first additive and the organic solvent in the electrolyte larger. This makes it easier for the first additive to decompose preferentially relative to the organic solvent in the electrolyte, thereby reducing the risk of poor SEI film quality caused by solvent decomposition.
[0162] In this embodiment, the benzene ring has a large number of substituent groups, the first additive has a lower LUMO energy level and a higher reduction potential, and is more likely to decompose preferentially relative to the solvent in the electrolyte. This can reduce the risk of poor SEI film quality caused by solvent decomposition, which is beneficial to reduce lithium ion consumption and improve the life of the battery cell.
[0163] As an example, in X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When fluorine is included, the number of fluorine substitutions on each benzene ring is less than 5. If the number of fluorine substitutions on each benzene ring is too high (e.g., 5), defluorination may generate more HF, increasing the risk of metal ion dissolution in the positive electrode active material. The dissolved metal ions are then reduced to elemental metals on the negative electrode side, increasing the risk of damaging the SEI film. Compared to cases with fewer fluorine substitutions (e.g., 4 fluorine substitutions per benzene ring), this is detrimental to further improving cycle life.
[0164] In some embodiments, the first additive includes at least one of 2,4,6-tris(4-fluorophenyl)cycloboroxane, tris(4-fluorophenyl)phosphine, tris(pentafluorophenyl)phosphine, tris(4-chlorophenyl)phosphine, triphenylphosphine, 2, triphenylborane, tris(pentafluorophenyl)borane, and triphenylphosphine oxide.
[0165] The aforementioned first additive has a good effect and is beneficial to improving the lifespan of battery cells.
[0166] In some embodiments, the mass content of the first additive is 0.001% to 5% based on the total mass of the electrolyte.
[0167] The aforementioned mass content of the first additive includes both the mass content during the battery cell preparation process and the mass content after the battery cell has been formed. For example, after the battery cell has been formed, the mass content of the first additive may be 0.001% based on the total mass of the electrolyte. As another example, during the battery cell preparation process, the mass content of the first additive may be 5% based on the total mass of the electrolyte.
[0168] During the formation of a battery cell, the first additive undergoes at least partial decomposition. After the battery cell is formed, the first additive may be completely consumed or remain partially. It should be noted that "complete consumption of the first additive" here can refer to a situation where the first additive cannot be detected due to exceeding the instrument's detection precision. As an example, if the mass content of the first additive is 0.001% based on the total mass of the electrolyte, it can be considered that the first additive has been completely consumed.
[0169] As an example, if the mass content of the first additive is greater than or equal to 0.6% based on the total mass of the electrolyte before the formation of the battery cell, there will be some of the first additive remaining after formation.
[0170] Furthermore, as an example, if a battery cell is stored at room temperature (e.g., 25°C) for a short period (e.g., 2 months) after formation, the mass content of the first additive within the battery cell is essentially the same as that in a freshly formed battery cell. As another example, if a battery cell is stored at a higher temperature (e.g., 45°C) for a short period (e.g., within 30 days) after formation, the mass content of the first additive within the battery cell is essentially the same as that in a freshly formed battery cell. As yet another example, if a battery cell is stored at a higher temperature (e.g., 45°C) for a longer period (e.g., more than 180 days) after formation, the first additive can be completely consumed.
[0171] If the first additive is not completely consumed, its mass content can be determined by gas chromatography, gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), or inductively coupled plasma optical emission spectrometry (ICP-OES). As an example, the battery cell is discharged at a constant current of 0.33C to 2.0V at 25°C. The battery cell is then disassembled, and the electrolyte is extracted (if the electrolyte content in the battery cell is low, the positive and negative electrode plates can be centrifuged to obtain the electrolyte from them). Next, 500 μl of deuterated reagent was added to the NMR tube in an argon-filled glove box. Then, 100 μl of the electrolyte sample was added to the NMR tube. The NMR tube was shaken to dissolve the non-aqueous electrolyte in the deuterated reagent. The composition and mass of the first additive in the electrolyte were tested using an Oxford Instruments X-Pulse benchtop NMR spectrometer. The mass content of the first additive in the electrolyte was calculated by dividing the mass of the first additive by the mass of the entire electrolyte.
[0172] When the first additive is depleted, it can be determined whether the first additive was added during the electrolyte preparation process by testing the benzene ring structure in the electrolyte and the content of inorganic lithium compounds in the solid electrolyte interphase (SEI) film on the surface of the negative electrode. For example, if the first additive cannot be detected by nuclear magnetic resonance spectroscopy, but the benzene ring structure in the electrolyte is detected and the peak area of the lithium element in the negative electrode at 53.8 ± 0.2 eV accounts for less than 40%, then it can be inferred that the first additive was included in the electrolyte during the preparation of the battery cell.
[0173] The content of inorganic lithium compounds in the solid electrolyte interphase (SEI) film on the surface of the negative electrode layer can be determined as follows: At 25°C, the battery cell is discharged at a constant current of 0.33C to 2.0V, and then the battery cell is disassembled to obtain the negative electrode. The inorganic lithium compounds in the SEI film on the surface of the negative electrode layer can be detected by X-ray photoelectron spectroscopy (XPS). Using the negative electrode as a sample and an Al target as the X-ray source at a power of 300W, X-rays are used to bombard the surface of the negative electrode layer, exciting the inner-shell electrons or valence electrons of atoms or molecules. The C1s peak (284.8 eV) is used as the XPS reference peak position to analyze surface elements (e.g., lithium) and functional groups. As an example, the X-ray photoelectron spectrum of lithium in the negative electrode is tested, and the peak area at 53.8 ± 0.2 eV is measured and recorded. This peak represents the organic component lithium ethylene dicarbonate (LEDC). Adding the first additive is beneficial for generating a higher content of inorganic lithium compounds at the negative electrode (i.e., the inorganic component in the SEI film becomes higher). The lower the proportion of the peak area at 53.8±0.2eV, the more inorganic lithium compounds are in the SEI film.
[0174] Based on the total mass of the electrolyte, the mass content of the first additive is 0.001%, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, or any value within the above range.
[0175] When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the life of the battery cell. When the mass content of the first additive is less than or equal to 5% based on the total mass of the electrolyte, the risk of side reactions of the first additive within the battery cell due to excessive content can be reduced, thereby mitigating the adverse effects of side reactions on the battery cell's lifespan. Furthermore, since the cyclic carbonate solvents in the electrolyte have a low mass content, using a smaller mass content of the first additive is beneficial for improving the lifespan of the battery cell.
[0176] In some embodiments, the mass content of the first additive is 0.5% to 5% based on the total mass of the electrolyte.
[0177] The mass content of the first additive mentioned above refers to the mass content of the battery cell before formation, or it can refer to the mass content of the first additive during the preparation of the battery cell.
[0178] Before the formation of the battery cell, based on the total mass of the electrolyte, the mass content of the first additive can be 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, or any value within the above range.
[0179] Before the formation of battery cells, if the mass content of the first additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it has a good effect on improving the life of the battery cells. If the mass content of the first additive is less than or equal to 5% based on the total mass of the electrolyte, it can reduce the risk of the first additive causing side reactions in the battery cells due to excessive content, thereby reducing the adverse effects of side reactions on the life of the battery cells.
[0180] In some embodiments, the mass content of the first additive is 1.2% to 3.5% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0181] In some embodiments, the mass content of the first additive is 0.001% to 1.7% based on the total mass of the electrolyte.
[0182] The mass content of the first additive mentioned above refers to the mass content of the battery cell after formation. Here, "formed battery cell" refers to, for example, a battery cell that has just been manufactured and is not yet in use in a vehicle, or a battery cell that has just been removed from the storage compartment and is not yet installed in a vehicle.
[0183] After the battery cell is formed, based on the total mass of the electrolyte, the mass content of the first additive can be 0.001%, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, or any value within the above range.
[0184] When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the life of the battery cell. When the mass content of the first additive is less than or equal to 1.7% based on the total mass of the electrolyte, it can reduce the risk of the first additive causing side reactions in the battery cell due to excessive residual first additive after formation, thereby reducing the adverse effect of side reactions on the life of the battery cell.
[0185] In some embodiments, the mass content of the first additive is 0.3% to 0.8% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0186] In some embodiments, in the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for less than 40%.
[0187] In the X-ray photoelectron spectrum of lithium in the negative electrode, the percentage of the peak area at 53.8 ± 0.2 eV can be 40%, 38%, 35%, 33%, 30%, 28%, 25%, 22%, 20%, 18%, 16%, 14%, 12%, 10%, 8%, or any value within the above range.
[0188] The peak position at 53.8±0.2 eV corresponds to organic matter in the SEI membrane. The proportion of the peak area at 53.8±0.2 eV can reflect the content of organic matter in the SEI membrane. The smaller the proportion of the peak area at 53.8±0.2 eV, the less organic matter in the SEI membrane, the more inorganic components in the SEI membrane, and the denser and more stable the SEI membrane.
[0189] As an example, before the formation of the battery cell, based on the total mass of the electrolyte, when the mass content of the first additive is 0.5%, the peak area at the peak position of 53.8±0.2 eV accounts for approximately 31.5%; without the addition of the first additive, the peak area at the peak position of 53.8±0.2 eV accounts for approximately 49.3%.
[0190] In the embodiments of this application, the peak area of the peak at 53.8±0.2eV accounts for less than 40%, the content of inorganic components in the SEI film is relatively high, the SEI film is more dense and stable, which helps to reduce the risk of repeated breakage and reconstruction of the SEI film, reduce the consumption of lithium ions, and thus help to improve the life of the battery cell.
[0191] In some embodiments, in the X-ray photoelectron spectroscopy of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for 10% to 32%. This results in a denser and more stable SEI film, with a lower risk of repeated breakage and reconstruction, which helps reduce lithium-ion consumption and thus improves the lifespan of the battery cell.
[0192] In some embodiments, the mass content of the second additive is 0.001% to 3% based on the total mass of the electrolyte.
[0193] Based on the total mass of the electrolyte, the mass content of the second additive is 0.001%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.5%, 0.8%, 0.9%, 1%, 1.5%, 2%, 2.5%, 3%, or any value within the above range.
[0194] When the mass content of the second additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it helps to compensate for the insufficient lithium-ion transference number caused by the low mass content of cyclic carbonate solvents, thereby resulting in a more suitable lithium-ion transference number in the electrolyte, lower internal resistance of the battery cell, and thus a longer battery cell life. When the mass content of the second additive is less than or equal to 3% based on the total mass of the electrolyte, the battery cell life can be improved with less second additive, and it is also beneficial to have a higher content of electrolyte salts in the electrolyte.
[0195] In some embodiments, the mass content of the second additive is 0.5% to 3% based on the total mass of the electrolyte.
[0196] The mass content of the second additive mentioned above refers to the mass content of the battery cell before formation, or it can refer to the mass content of the second additive during the preparation of the battery cell.
[0197] Before the battery cell is formed, based on the total mass of the electrolyte, the mass content of the second additive can be 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, or any value within the above range.
[0198] During the formation of a battery cell, the second additive undergoes at least partial decomposition. After the battery cell is formed, the second additive will generally remain. For example, the type and content of the second additive can be determined using nuclear magnetic resonance (NMR) testing.
[0199] When the mass content of the second additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it helps to compensate for the insufficient lithium-ion transference number caused by the low mass content of cyclic carbonate solvents. This results in a more suitable lithium-ion transference number in the electrolyte, lower internal resistance in the battery cell, and consequently, a longer battery cell lifespan. When the mass content of the second additive is less than or equal to 3% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the second additive, thereby reducing the risk of lithium-ion consumption and resulting in a longer battery cell lifespan.
[0200] In some embodiments, the mass content of the second additive is 1.5% to 2% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0201] In some embodiments, the mass content of the second additive is 0.2% to 2.0% based on the total mass of the electrolyte.
[0202] The mass content of the second additive mentioned above is the mass content after the battery cell has been formed.
[0203] After the battery cell is formed, based on the total mass of the electrolyte, the mass content of the second additive can be 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, or any value within the above range.
[0204] After the battery cell is formed, if the mass content of the second additive is greater than or equal to 0.2% based on the total mass of the electrolyte, it helps to compensate for the problem of insufficient lithium-ion transference number caused by the low mass content of cyclic carbonate solvents. This results in a more suitable lithium-ion transference number in the electrolyte, lower internal resistance in the battery cell, and thus a longer battery cell lifespan. If the mass content of the second additive is less than or equal to 2.0% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the second additive, thereby reducing the risk of lithium-ion consumption and resulting in a longer battery cell lifespan.
[0205] In some embodiments, the mass content of the second additive is 1.2% to 1.4% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0206] In some embodiments, the second additive includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonate)imide.
[0207] The aforementioned second additive has a larger anionic radius, making it easier to dissociate. This helps to increase the lithium-ion migration number in the electrolyte, reduce the internal resistance of the battery cell, and thus improve the lifespan of the battery cell.
[0208] The second additive and its mass content can be determined by the following method. For example, after disassembling a battery cell to obtain the electrolyte, 500 μl of deuterated reagent is added to an NMR tube in an argon-filled glove box. 100 μl of non-aqueous electrolyte sample is then added to the NMR tube. The NMR tube is shaken to dissolve the non-aqueous electrolyte in the deuterated reagent. The composition and mass of the electrolyte are then tested using an Oxford Instruments X-Pulse benchtop NMR spectrometer to determine whether the second additive is included and its mass content.
[0209] In some embodiments, the mass content of the cyclic carbonate solvent is 2% to 6% based on the total mass of the electrolyte.
[0210] Based on the total mass of the electrolyte, the mass content of the cyclic carbonate solvent can be 2%, 2.2%, 2.4%, 2.6%, 2.8%, 3%, 3.1%, 3.3%, 3.5%, 3.7%, 3.9%, 4%, 4.1%, 4.3%, 4.5%, 4.7%, 4.9%, 5%, 6%, or any value within the above range.
[0211] When the mass content of cyclic carbonate solvent is greater than or equal to 2% based on the total mass of the electrolyte, the electrolyte has a suitable lithium-ion transference number, the battery cell has a low internal resistance, and thus the battery cell has a long lifespan. When the mass content of cyclic carbonate solvent is less than or equal to 6% based on the total mass of the electrolyte, it is beneficial to reduce the risk of unstable SEI film rich in organic components formed by cyclic carbonate solvent at the negative electrode, which in turn is beneficial to reduce the risk of repeated SEI film rupture and reconstruction consuming active lithium, and the battery cell has a long lifespan.
[0212] In some embodiments, cyclic carbonate solvents include at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
[0213] The aforementioned cyclic carbonate solvents have high dielectric constants and good solvation capabilities, which are beneficial for the dissociation of lithium ions in the electrolyte salt, thereby increasing the lithium ion transference number in the electrolyte. As a result, the battery cells have lower resistance, which is beneficial for improving the lifespan of the battery cells.
[0214] As an example, the content of cyclic carbonates in electrolytes can be quantitatively analyzed by organic gas chromatography, referring to the standard GB / T9722-2006.
[0215] In some embodiments, the electrolyte further includes at least one of a third additive and a fourth additive, wherein the third additive includes a carbonate additive and the fourth additive includes a sulfur-containing additive.
[0216] Carbonate additives facilitate the formation of polymer coatings on graphite surfaces, which can buffer the volume expansion of battery cells during charge and discharge processes. They also help repair damaged sites in the SEI film during long-term charge and discharge cycles, thereby improving the lifespan of battery cells.
[0217] The film formed on the graphite surface by sulfur-containing additives has good ion-conducting ability, which helps reduce the increase of DC resistance in the battery cell and thus improves the kinetic isoelectric performance of the battery cell. Furthermore, the combined use of carbonate and sulfur-containing additives helps to balance the battery cell's lifespan and kinetic performance.
[0218] In some embodiments, the carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate. These additives have a good effect on improving the lifespan of individual battery cells.
[0219] In some embodiments, the carbonate additive includes vinylene carbonate (VC), and the mass content of vinylene carbonate is 0.5% to 5% based on the total mass of the electrolyte, for example, it can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or any value within the range above.
[0220] In some embodiments, the carbonate additive includes fluoroethylene carbonate (FEC), and the mass content of fluoroethylene carbonate is 0.1% to 3% based on the total mass of the electrolyte, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3% or any value within the above range.
[0221] In some embodiments, the sulfur-containing additive includes at least one selected from vinyl sulfate, vinyl disulfate, butenyl sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate. These additives have a good effect on improving the kinetic performance of the battery cell.
[0222] In some embodiments, the sum of the mass contents of the third and fourth additives is 0.5% to 10% based on the total mass of the electrolyte.
[0223] The sum of the mass contents of the third and fourth additives mentioned above can be the sum of the mass contents of the third and fourth additives after the battery cell has been formed.
[0224] As an example, the third and fourth additives are consumed during the charge-discharge cycles of the formed battery cell and throughout the entire life cycle of the battery cell.
[0225] Based on the total mass of the electrolyte, the mass content of the third and fourth additives can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, or any value within the above range.
[0226] When the mass content of the third and fourth additives is greater than or equal to 0.5% based on the total mass of the electrolyte, the battery cell has a longer lifespan. When the mass content of the third and fourth additives is less than or equal to 10% based on the total mass of the electrolyte, it is beneficial to reduce the risk of more severe side reactions in the battery cell caused by the higher content of the third and fourth additives, and can reduce the adverse effects of side reactions on the lifespan of the battery cell.
[0227] In some embodiments, the combined mass content of the third and fourth additives is 2% to 8% based on the total mass of the electrolyte. This results in a longer battery cell lifespan.
[0228] The third and fourth additives can be tested by nuclear magnetic resonance spectroscopy. The specific procedure is as follows: 500 μl of deuterated reagent is added to the NMR tube in an argon-filled glove box. 100 μl of non-aqueous electrolyte sample is added to the NMR tube. The NMR tube is shaken to dissolve the non-aqueous electrolyte into the deuterated reagent. The composition and quality of the electrolyte are tested using an Oxford Instruments X-Pulse benchtop NMR spectrometer.
[0229] In some embodiments, the electrolyte comprises an electrolyte salt, including lithium hexafluorophosphate. Lithium hexafluorophosphate is readily dissociable and reasonably priced, making it suitable as the primary electrolyte salt in electrolytes.
[0230] In some embodiments, the molar concentration of lithium hexafluorophosphate (LiPF6) is from 0.5 mol / L to 1.2 mol / L, for example, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, or any value within the above range.
[0231] In some embodiments, the molar concentration of lithium hexafluorophosphate (LiPF6) is from 0.8 mol / L to 1.0 mol / L.
[0232] In some embodiments, the electrolyte satisfies at least one of the following conditions:
[0233] The electrolyte conductivity at 20℃ to 30℃ is 8 mS / cm to 20 mS / cm.
[0234] The viscosity of the electrolyte at 20°C to 30°C is 2.0 mPa·s to 3.5 mPa·s.
[0235] The electrolyte density at 20°C to 30°C is 1.05 g / mL to 1.35 g / mL.
[0236] The conductivity of the electrolyte at 20℃ to 30℃ can be 8ms / cm, 9ms / cm, 10ms / cm, 11ms / cm, 12ms / cm, 13ms / cm, 14ms / cm, 15ms / cm, 16ms / cm, 17ms / cm, 18ms / cm, 19ms / cm, 20ms / cm or any value within the above range.
[0237] The viscosity of the electrolyte at 20°C to 30°C can be 2.0 mPa·s, 2.1 mPa·s, 2.2 mPa·s, 2.3 mPa·s, 2.4 mPa·s, 2.5 mPa·s, 2.6 mPa·s, 2.7 mPa·s, 2.8 mPa·s, 2.9 mPa·s, 3.0 mPa·s, 3.1 mPa·s, 3.2 mPa·s, 3.3 mPa·s, 3.4 mPa·s, 3.5 mPa·s, or any value within the above range.
[0238] The electrolyte density at 20°C to 30°C is 1.05 g / mL, 1.08 g / mL, 1.10 g / mL, 1.12 g / mL, 1.15 g / mL, 1.18 g / mL, 1.20 g / mL, 1.22 g / mL, 1.25 g / mL, 1.28 g / mL, 1.30 g / mL, 1.32 g / mL, 1.33 g / mL, 1.35 g / mL, or any value within the above range.
[0239] In the embodiments of the application, the conductivity, viscosity or density of the electrolyte meets the above-mentioned range by combining the carbonate solvent, the first additive and the second additive in the above-mentioned mass content.
[0240] When the conductivity of the electrolyte meets the above-mentioned range, the electrolyte has high conductivity, which is conducive to the migration of lithium ions, thereby helping to reduce the ohmic resistance of the battery cell and the kinetic lithium consumption caused by polarization, and thus helping to improve the life of the battery cell.
[0241] When the viscosity of the electrolyte meets the above-mentioned range, the electrolyte has a lower viscosity, which is conducive to the migration of lithium ions, thereby reducing the ohmic resistance of the battery cell and the kinetic lithium consumption caused by polarization, and thus helping to improve the life of the battery cell.
[0242] When the electrolyte density meets the above-mentioned range, it is beneficial for the electrolyte to have higher conductivity and lower viscosity, which is conducive to the migration of lithium ions. This helps to reduce the ohmic resistance of the battery cell and the kinetic lithium consumption caused by polarization, thereby improving the life of the battery cell.
[0243] In this embodiment, the electrolyte can be obtained by disassembling the battery cell, and then tested using the following method. The method for obtaining the electrolyte is described above and will not be repeated here.
[0244] For example, according to HG / T 4067-2015, the ionic conductivity of the electrolyte to be tested is measured using a conductivity meter: Take about 100 ml of the sample to be tested in a dry, clean, corrosion-resistant sample bottle, seal it and place it in a constant temperature water bath at 25±0.5℃. When the temperature of the sample to be tested is constant, replace the cap of the sample bottle with a rubber stopper with an electrode inserted. When the temperature is within the range of 25±0.5℃, read the data, which is the ionic conductivity of the sample to be tested.
[0245] For example, the viscosity of an electrolyte can be determined using instruments and methods known in the art. For non-Newtonian fluids, the rotational viscometer method provided in the national standard GB / T22235-2008 "Determination of Viscosity of Liquids" can be used. Specifically, a certain mass of electrolyte sample is placed in a sample container and tested using a Brookfield DV2TLV rotational viscometer. At a certain temperature, the shear force experienced by the rotor rotating continuously at a constant speed within the sample causes the spring to generate torque. The torque is proportional to the viscosity, yielding the viscosity value. The testing equipment meets the following environmental conditions: 1. External environment: temperature 15–28℃, humidity RH < 80%; 2. Internal environment: 2 / 3 of the sample container is immersed in a water bath, the medium being water, which is used to maintain the temperature of the sample.
[0246] The density of the electrolyte can be tested using an Anton Paar DMA35 V4 EX densitometer, in accordance with standard GB / T2013-2010.
[0247] In some embodiments, the electrolyte further includes a linear carbonate solvent, which includes at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate.
[0248] Linear carbonate solvents have lower viscosity, which can compensate for the shortcomings of cyclic carbonate solvents, such as high viscosity, poor flowability and wettability. By using linear carbonate solvents in combination with cyclic carbonate solvents, the electrolyte can achieve a balance between suitable viscosity and suitable ionic conductivity, which is beneficial for lithium-ion transport and facilitates the improvement of the fast-charging performance of battery cells.
[0249] In some embodiments, the electrolyte further includes linear carboxylic acid ester solvents.
[0250] Linear carboxylic acid ester solvents may include one or more of ethyl acetate, methyl acetate, methyl butyrate, ethyl propionate, ethyl butyrate, butyl acetate, methyl propionate, and propyl butyrate.
[0251] Linear carboxylic acid ester solvents have lower viscosity than linear carbonate solvents, which is beneficial for lithium ion migration. Combining cyclic carbonate solvents and linear carboxylic acid ester solvents can help improve the fast charging performance of battery cells.
[0252] In some embodiments, the mass content of the linear carboxylic acid ester solvent is 10% to 70% based on the total mass of the solvent, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, or any value within the range above.
[0253] In some embodiments, the mass content of the linear carboxylic acid ester solvent is 10% to 40% based on the total mass of the solvent.
[0254] As an example, the test method for linear carbonate and linear carboxylic acid ester solvents can refer to the standard GB / T9722-2006, which uses organic gas chromatography to quantitatively analyze the content of cyclic carbonates and linear carboxylic acid esters in the electrolyte.
[0255] In some embodiments, graphite satisfies at least one of the following conditions:
[0256] The volume average particle size Dv50 of graphite ranges from 8 μm to 14 μm;
[0257] The specific surface area of graphite is 0.8 m². 2 / g to 1.7m 2 / g.
[0258] For example, at 25°C, a single battery cell is discharged at a constant current of 0.33C to 2.0V to obtain a battery cell with 0% SOC. The negative electrode is then removed from the battery cell, and the negative electrode film is scraped off to obtain negative electrode film powder. Water is added to the negative electrode film powder, which is then stirred, filtered, and dried to obtain graphite. The volume average particle size (Dv50) of graphite represents the particle size corresponding to a cumulative volume distribution percentage of 50%, and can be determined using instruments and methods known in the art. For example, it can be conveniently determined using a laser particle size analyzer, referring to GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method. The testing instrument can be the Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0259] The specific surface area of graphite is measured using the nitrogen adsorption method. First, the graphite sample is placed in a storage tube, an instrument commonly known as a Quantachrome physisorption analyzer. Nitrogen gas is passed through the storage tube and brought into contact with the graphite sample at a specific temperature: 77 K (-196 degrees Celsius). When the nitrogen gas passes through the graphite sample, physisorption occurs, meaning nitrogen molecules adhere to the graphite surface. After the adsorption process is complete, the storage tube is immediately removed from the analyzer and quickly sealed to prevent the nitrogen molecules adsorbed on the graphite surface from escaping. Finally, the storage tube is placed back into the analyzer, and high-purity helium gas is introduced. Because helium has a smaller molecular weight than nitrogen, it can penetrate the pores of the graphite, displacing the nitrogen molecules adsorbed on the graphite surface. By measuring the time and pressure required for the helium gas to pass through the storage tube, the specific surface area of the graphite material can be calculated.
[0260] The formula for calculating specific surface area using nitrogen adsorption mainly relies on the BET formula. The BET formula is based on the Ideal Adsorption Solution Theory (IAST), which assumes that the adsorbate interacts with only a single molecule on the solid surface during adsorption. The expression for the BET formula is:
[0261] Specific surface area (m²) 2 / g)=((P / P0)ln(P / P0)-1) / (RBET*(ΔP / P0));
[0262] Where P is the nitrogen pressure adsorbed on the solid surface, P0 is the nitrogen pressure before adsorption, RBET is the BET specific surface area, and ΔP is the pressure change during adsorption and desorption.
[0263] The volume average particle size Dv50 of graphite can be 8μm, 8.5μm, 9μm, 9.5μm, 10μm, 10.5μm, 11μm, 11.5μm, 12μm, 12.5μm, 13μm, 13.5μm, 14μm or any value within the above range.
[0264] The specific surface area of graphite is the BET adsorption specific surface area, which can be obtained by measuring the Quantachrome physical adsorption analyzer.
[0265] The specific surface area of graphite can be 0.8 m². 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m2 / g or any value within the above range.
[0266] When the volume average particle size Dv50 of graphite is greater than or equal to 8 μm, there is a suitable pore size between graphite particles, which facilitates the wetting of electrolyte and thus the transport of lithium ions, which is beneficial to improving the fast charging performance of the battery cell. When the volume average particle size Dv50 of graphite is less than or equal to 14 μm, lithium ions have a suitable diffusion path, which facilitates the diffusion of lithium ions and is beneficial to improving the fast charging performance of the battery cell.
[0267] When the specific surface area of graphite is greater than or equal to 0.8 m² 2 At a specific surface area of 1.7 m² / g, this facilitates the insertion and extraction of lithium ions into graphite, thus improving the fast-charging performance of individual battery cells; 2 At a rate of / g, it is beneficial to reduce the degree of side reactions between graphite and electrolyte due to the large number of active sites in graphite, which can reduce the consumption of lithium ions caused by side reactions, thereby improving the lifespan of battery cells.
[0268] In some embodiments, graphite satisfies at least one of the following conditions:
[0269] The volume average particle size Dv50 of graphite is 10 μm to 13 μm;
[0270] The specific surface area of graphite is 1.0 m². 2 / g to 1.4m 2 / g.
[0271] With a graphite volume average particle size (Dv50) of 10 μm to 13 μm, the battery cell exhibits good fast-charging performance; and with a graphite specific surface area of 1.0 m², the battery cell demonstrates good fast-charging performance. 2 / g to 1.4m 2 At a rate of / g, the battery cells exhibit good fast-charging performance and a long lifespan.
[0272] In some embodiments, at least a portion of the surface of the graphite has a carbon coating layer, the degree of graphitization of the carbon coating layer being 0.85 to 0.9.
[0273] The degree of graphitization of the carbon coating can be 0.86, 0.87, 0.88, 0.89, 0.9 or any value within the above range.
[0274] As an example, after disassembling the battery cell, the negative electrode active material in the negative electrode film layer is obtained. The coating layer on the graphite surface is peeled off (e.g., by focused ion beam (FIB) cutting). The peeled powder is then tested according to the following method to obtain the graphitization degree of the coating layer.
[0275] The degree of graphitization of graphite (or its coating) was determined by X-ray diffraction. Silicon (at a C:Si mass ratio of 5:1) was added to the graphite powder during sample preparation for peak alignment. A Cu target was used for testing. The wavelength was Kα = 0.1541874 nm, the voltage was 40 kV, the current was 40 mA, the scanning range was 52°–58°, and the scanning speed was 1° / min. This method was employed to obtain the interlayer spacing d of the graphite (002) crystal plane. 002 Based on the interlayer spacing d of the graphite (002) crystal plane. 002 The degree of graphitization (G) is calculated using the Mering-Maire formula (Franklin's formula): G = (0.3440 - d) / (2π) d ... 002 ) / (0.3440-0.3354); where 0.3440nm is the interlayer spacing of non-graphitized carbon and 0.3354nm is the interlayer spacing of ideal graphite.
[0276] As an example, the carbon coating layer includes amorphous carbon. For instance, by using a focused ion beam (FIB) to cut a thin slice approximately 100 nm thick from the middle of the negative electrode active material particles, and then performing TEM testing on the slice, it can be observed that the surface region includes a coating layer. The lattice fringes in the coating layer exhibit long-range disorder and short-range order, and the electron diffraction pattern shows a halo-like appearance, indicating that the coating layer includes amorphous carbon.
[0277] When at least a portion of the graphite surface has a carbon coating, it facilitates the rapid insertion and extraction of lithium ions within the graphite, resulting in better fast-charging performance for the battery cell. When the graphitization degree of the carbon coating is between 0.85 and 0.9, the graphite exhibits good isotropy, which is beneficial for lithium ion insertion from various directions, leading to better kinetic performance and fast-charging performance for the battery cell. Furthermore, the superior kinetic performance of the aforementioned graphite can compensate for the increased concentration polarization caused by the low content of cyclic carbonates, thus resulting in better overall kinetic performance for the battery cell, thereby meeting the power and fast-charging requirements of electrical devices.
[0278] In some embodiments, graphite includes at least one of artificial graphite or natural graphite.
[0279] In this embodiment, graphite may include natural graphite, artificial graphite, or a mixture of natural and artificial graphite.
[0280] In some embodiments, graphite includes at least one of primary particles and secondary particles.
[0281] In this embodiment, graphite may include primary particles, secondary particles, or a mixture of primary and secondary particles.
[0282] Figure 3This is a schematic diagram of the negative electrode sheet according to an embodiment of this application. In some embodiments, such as Figure 3 As shown, the negative electrode sheet 6 includes a negative electrode current collector 60 and a negative electrode film layer 61 disposed on at least one side surface of the negative electrode current collector 60. The negative electrode film layer 61 includes a negative electrode active material, and the negative electrode sheet satisfies at least one of the following conditions:
[0283] The compaction density of the negative electrode film is 1.50 g / cm³. 3 Up to 1.70 g / cm 3 ;
[0284] The porosity of the negative electrode sheet is 25% to 60%;
[0285] The single-sided density of the negative electrode film is 7 mg / cm³. 2 Up to 10.5 mg / cm 2 .
[0286] The negative electrode current collector 60 has two opposing surfaces along its own thickness direction. The negative electrode film layer 61 can be disposed on one side surface of the negative electrode current collector 60 or on both sides surface of the negative electrode current collector 60.
[0287] The aforementioned compaction density of the negative electrode film can be considered as the compaction density of the negative electrode film when the battery cell is in a fully discharged state. Here, "fully discharged state" refers to the state of charge (SOC) of the battery cell being 0%. Specifically, at 25°C, a battery cell is discharged at a constant current of 0.33C to 2.0V; at this point, the battery cell has a 0% SOC.
[0288] The compaction density of the negative electrode film can be 1.5 g / cm³. 3 1.52g / cm 3 1.55g / cm 3 1.58g / cm 3 1.6g / cm 3 1.62g / cm 3 1.65g / cm 3 1.68g / cm 3 1.7g / cm 3 Or any value within the above range, the unilateral density of the negative electrode film can be 7 mg / cm³. 2 7.2 mg / cm 2 7.5 mg / cm 2 7.8 mg / cm 2 8mg / cm 2 8.5 mg / cm 2 8.8 mg / cm 2 9mg / cm 29.2 mg / cm 2 9.5 mg / cm 2 9.8 mg / cm 2 10mg / cm 2 10.5 mg / cm 2 The porosity of the negative electrode sheet can be 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, or any value within the above range.
[0289] The compaction density of the negative electrode film layer is greater than or equal to 1.50 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the negative electrode film is less than or equal to 1.70 g / cm³, it is beneficial to improve the energy density of individual battery cells. 3 In this case, it is beneficial to reduce the risk of particle breakage of negative electrode active material due to the high compaction density of the negative electrode film layer. It can reduce the side reactions between broken particles and electrolyte, reduce lithium ion consumption, and thus help reduce the adverse impact on the life of battery cells.
[0290] When the porosity of the negative electrode sheet is greater than or equal to 25%, it facilitates the transport and diffusion of lithium ions, which is beneficial to improving the fast charging performance of the battery cell. When the porosity of the negative electrode sheet is less than or equal to 60%, the negative electrode sheet has a suitable strength, which can reduce the risk of cracking of the negative electrode sheet and is beneficial to improving the life of the battery cell.
[0291] The density on one side of the negative electrode film layer is greater than or equal to 7 mg / cm³. 2 Under these conditions, it is beneficial to improve the energy density of the battery cell; when the density on one side of the negative electrode film is less than or equal to 10.5 mg / cm³, it is beneficial to improve the energy density of the battery cell. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial for improving the fast-charging performance of individual battery cells. Furthermore, the combination of the first additive with the areal density and compaction density of the negative electrode film within the aforementioned range also contributes to a longer battery cell lifespan.
[0292] The areal density and compaction density of the negative and positive electrode films can be measured as follows: At 25°C, the battery cell is discharged at a constant current of 0.33C to 2.0V to obtain a battery cell with 0% SOC. Then, the positive and negative electrode sheets are removed from the battery cell, and the thickness of the electrode sheet and the current collector are measured respectively. The electrode sheet is then cut into small circular pieces with an area of S1 (if it is a double-sided coated electrode sheet, the film layer on one side can be wiped off first), and its weight is recorded as M1. Then, the film layer of the weighed electrode sheet is wiped off, and the weight of the current collector is recorded as M0. The areal density of one side = (M1 - M0) / S1. The compaction density = areal density / (electrode thickness - current collector thickness).
[0293] The porosity of the negative and positive electrode sheets can be determined according to the standard procedure GB / T 24586-2009. The specific test procedure is as follows: Select more than 20 round sheets with good appearance and no powder falling off the edges using tweezers and place them into a sample cup. Record the number of sheets and calculate the apparent volume V1. Then, place the sample cup containing the sample into a true density tester AccuPycⅡ1340, seal the test system, and introduce helium gas according to the procedure. By detecting the gas pressure in the sample chamber and expansion chamber, and then calculating the true volume V2 according to Bohr's Law (PV=nRT), the porosity of the sample to be tested is obtained as P=(V1-V2) / V1×100%.
[0294] In some embodiments, the negative electrode sheet satisfies at least one of the following conditions:
[0295] The compaction density of the negative electrode film is 1.52 g / cm³. 3 Up to 1.60 g / cm 3 ;
[0296] The porosity of the negative electrode sheet is 25% to 35%;
[0297] The density of the negative electrode film on one side is 7.8 mg / cm³. 2 Up to 9.8 mg / cm 2 .
[0298] The compaction density of the negative electrode film layer is 1.52 g / cm³. 3 Up to 1.60 g / cm 3 Under these conditions, the battery cell exhibits high energy density and long lifespan; with a negative electrode porosity of 25% to 35%, the battery cell demonstrates good fast-charging performance and long lifespan; and with a single-sided density of 7.8 mg / cm³ in the negative electrode film layer... 2 Up to 9.8 mg / cm 2 Under these conditions, the battery cells have high energy density and good fast charging performance.
[0299] Figure 4 This is a schematic diagram of a positive electrode sheet according to an embodiment of this application. In some embodiments, such as Figure 4 As shown, the battery cell includes a positive electrode 5, the positive electrode 5 includes a positive current collector 50 and a positive electrode film 51 disposed on at least one side surface of the positive current collector 50, the positive electrode film 51 includes a positive electrode active material, the positive electrode active material includes lithium phosphate.
[0300] The positive electrode current collector 50 has two opposing surfaces along its own thickness direction. The positive electrode film layer 51 can be disposed on one side surface of the positive electrode current collector 50 or on both sides surface of the positive electrode current collector 50.
[0301] Lithium-containing phosphates can refer to lithium-containing transition metal phosphates with an olivine structure, such as lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, and their modified forms. The modification can be either doping or surface modification. For example, in doping modification, elements such as titanium can be doped into lithium iron phosphate; in surface modification, a coating layer can be applied to the surface of lithium iron phosphate.
[0302] Lithium phosphates have high structural stability, and lithium phosphate battery cells have long cycle life.
[0303] In some embodiments, at least a portion of the surface of the lithium phosphate contains a coating layer comprising carbon. This helps improve the conductivity of the lithium phosphate, facilitating the utilization of the battery cell's capacity and extending its lifespan.
[0304] In some embodiments, the positive electrode film layer includes a conductive agent and a positive electrode active material, wherein the mass content of the conductive agent is 0% to 1.5% based on the total mass of the positive electrode film layer.
[0305] Based on the total mass of the positive electrode film, the mass content of the conductive agent can be 0%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, or any value within the above range.
[0306] When the lithium phosphate surface has a carbon coating layer, the mass content of the conductive agent in the positive electrode film can be 0%. When the mass content of the conductive agent is greater than 0% based on the total mass of the positive electrode film, the positive electrode film has good conductivity, which facilitates the utilization of the battery cell's capacity and helps to improve the battery cell's lifespan. When the mass content of the conductive agent is less than or equal to 1.5% based on the total mass of the positive electrode film, the positive electrode active material in the positive electrode film has a high content, which helps to improve the energy density of the battery cell.
[0307] In some embodiments, lithium phosphates include components having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.1.
[0308] In the above general formula, m can be 0.8, 0.82, 0.85, 0.88, 0.9, 0.92, 0.95, 0.98, 1, 1.0, 1.15 or any value within the above range; x can be 0.9, 0.92, 0.95, 0.98, 1 or any value within the above range; y can be 0.95, 0.96, 0.97, 0.98, 0.99, 1 or any value within the above range; j can be 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value within the above range; and q can be 0.01, 0.02, 0.04, 0.05, 0.06, 0.08, 0.09, 0.1 or any value within the above range.
[0309] During the charging and discharging process of a single battery cell, the molar content of lithium, oxygen, and other elements in the lithium phosphate cathode active material changes within a certain range.
[0310] The elements and their contents in the positive electrode active material can be determined using an argon ion cross-section polisher (model JEOLIB-19530CP) and a scanning electron microscope (model Zeiss Sigma 300) (equipped with an X-ray energy dispersive spectrometer (EDS, model Oxford X-Max-50mm2)).
[0311] As an example, the battery cell was discharged at a constant current of 0.33C to 2.0V at 25°C to obtain a battery cell with 0% SOC. Then, the positive electrode was removed from the battery cell, and a longitudinal cross-section of the positive electrode film was obtained using an ion section polisher. The cross-section of the positive electrode active material particles was then scanned using a scanning electron microscope to test the elements and their content.
[0312] In some embodiments, the lithium phosphate-containing cathode active material includes at least one of LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4. The aforementioned lithium phosphate-containing cathode active materials exhibit high structural stability, which helps to improve the cycle life of individual battery cells.
[0313] During the charging and discharging process, lithium (Li) undergoes insertion / extraction and consumption within a single battery cell. The molar content of Li in the positive electrode active material varies depending on the discharge state of the cell. In the examples of positive electrode active materials in this application, the molar content of Li refers to the initial state of the material, i.e., the state before feeding. After charge-discharge cycles, the molar content of Li changes when the positive electrode active material is applied to the battery system. Similarly, the molar content of O in the examples of positive electrode active materials in this application is only an ideal value. Oxygen release from the crystal lattice causes changes in the molar content of O, resulting in fluctuations in the actual molar content of O.
[0314] In some embodiments, the specific capacity of the positive electrode active material is from 135 mAh / g to 150 mAh / g.
[0315] The specific capacity of the positive electrode active material can be measured as follows: A positive electrode slurry is prepared by mixing the positive electrode active material, conductive agent, binder, and solvent. This slurry is then coated onto aluminum foil to obtain the positive electrode sheet. The positive electrode sheet is then assembled with a lithium foil to form a coin cell. The coin cell is charged at a constant current rate of 0.1C to 3.8V, and then discharged at a constant current rate to 2.0V. The discharge capacity of the coin cell is then measured. The specific capacity of the positive electrode active material is calculated as: discharge capacity / mass of the positive electrode active material.
[0316] As an example, the positive electrode active material is obtained by disassembling a battery cell. At 25°C, the battery cell is discharged at a constant current of 0.33C to 2.0V to obtain a battery cell with 0% SOC. The positive electrode sheet is then disassembled, and the positive electrode film layer is scraped off. The powder of the positive electrode film layer is added to the solvent NMP, and then filtered and dried to obtain the positive electrode active material.
[0317] The specific capacity of the positive electrode active material can be 135mAh / g, 138mAh / g, 140mAh / g, 142mAh / g, 145mAh / g, 146mAh / g, 148mAh / g, 150mAh / g or any value within the above range.
[0318] In this embodiment, the positive electrode active material has a suitable specific capacity, and the battery cell has a suitable energy density.
[0319] In some embodiments, the positive electrode film layer satisfies at least one of the following conditions:
[0320] The compaction density of the positive electrode film is 2.52 g / cm³. 3 Up to 2.78 g / cm 3 ;
[0321] The areal density of one side of the positive electrode film is 12 mg / cm³. 2 Up to 19 mg / cm 2 .
[0322] The compaction density of the positive electrode film mentioned above can be the compaction density of the positive electrode film when the battery cell is in a fully discharged state, where the fully discharged state refers to the state of charge (SOC) of the battery cell being 0%.
[0323] The compaction density of the positive electrode film can be 2.52 g / cm³. 3 2.55g / cm 3 2.57g / cm 3 2.59g / cm 32.6g / cm 3 2.62 g / cm 3 2.65g / cm 3 2.68g / cm 3 2.7g / cm 3 2.72 g / cm 3 2.75g / cm 3 2.78g / cm 3 Or any value within the above range, the unilateral density of the positive electrode film can be 12 mg / cm³. 2 13mg / cm 2 14mg / cm 2 15mg / cm 2 16mg / cm 2 17mg / cm 2 18mg / cm 2 19mg / cm 2 Or any value within the above range.
[0324] The compaction density of the positive electrode film layer is greater than or equal to 2.52 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the positive electrode film is less than or equal to 2.78 g / cm³. 3 Under these conditions, it is beneficial for the transport of lithium ions, thereby improving the fast charging performance of individual battery cells.
[0325] The density on one side of the positive electrode film is greater than or equal to 12 mg / cm³. 2 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the density on one side of the positive electrode film is less than or equal to 19 mg / cm³, it is beneficial to improve the energy density of individual battery cells. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial for improving the fast-charging performance of individual battery cells. Furthermore, the combination of the first additive with the areal density and compaction density of the positive electrode film within the aforementioned range also contributes to a longer battery cell lifespan.
[0326] Figure 5 This is a schematic diagram of the structure of a battery cell according to an embodiment of this application. In one embodiment of this application, for example, referring to... Figure 5 As shown, the battery cell 3 includes a housing 31, an end cap assembly 32, and an electrode assembly 33. The housing 31 has an opening for accommodating the electrode assembly 33, and the end cap assembly 32 is used to close the opening. The electrode assembly 33 may include a positive electrode, a negative electrode, and a separator located between the positive electrode and the negative electrode.
[0327] The electrode assembly 33 can be prepared by a winding or stacking process from a positive electrode sheet, a negative electrode sheet, and an insulating element. As an example, the electrode assembly 33 is prepared by a winding process from a positive electrode sheet, a negative electrode sheet, and an insulating element.
[0328] In some embodiments, the end cap assembly 32 includes electrode terminals 322, such as Figure 5 As shown, the end cap assembly 32 includes two electrode terminals 322, one of which is a positive electrode terminal and the other is a negative electrode terminal.
[0329] The battery cell 3 also includes a connecting member 34 for connecting the tab 331 and the electrode terminal 322 of the electrode assembly 33. For example, one connecting member 34 is used to connect the tab of the positive electrode and the positive electrode terminal, and another connecting member 34 is used to connect the tab of the negative electrode and the negative electrode terminal.
[0330] [Positive electrode plate]
[0331] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0332] In some embodiments, the positive electrode film layer further includes a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0333] In some embodiments, the positive electrode film layer further includes a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0334] In one embodiment, the positive electrode sheet can be prepared by forming a positive electrode slurry using the components described above. For example, the positive electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., N-methylpyrrolidone) to form the positive electrode slurry. The positive electrode slurry is then coated onto a positive electrode current collector, and after drying, cold pressing, and other processes, the positive electrode sheet is obtained.
[0335] [Negative electrode plate]
[0336] In some embodiments, the negative electrode current collector can be a metal foil or a composite negative electrode current collector. The negative electrode current collector can be a copper foil. The composite negative electrode current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0337] The negative electrode film layer includes a negative electrode active material. The negative electrode active material can be any negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material includes graphite, and may also include at least one of the following materials: soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0338] The negative electrode film layer may also optionally include a binder. As an example, the binder may include at least one of styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), water-soluble unsaturated resin SR-1B, waterborne acrylic resins (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0339] The negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0340] In one embodiment, the negative electrode sheet can be prepared by forming a negative electrode slurry using the components described above. For example, the negative electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., deionized water) to form the negative electrode slurry. The negative electrode slurry is then coated onto a negative electrode current collector, and after drying, cold pressing, and other processes, the negative electrode sheet is obtained.
[0341] [Isolation Component]
[0342] The separator is used to separate the positive electrode and the negative electrode. This application does not impose any particular restrictions on the type of separator; for example, any known porous membrane with good chemical and mechanical stability can be selected.
[0343] In one embodiment, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer may be the same or different, without particular limitation.
[0344] This application provides a battery device, including the battery cell in any of the above embodiments.
[0345] This application provides an electrical device including a battery cell or battery device as described in any of the above embodiments, wherein the battery cell or battery device is used to store or provide electrical energy.
[0346] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0347] [Example]
[0348] Example 1
[0349] (1) Preparation of negative electrode sheet
[0350] Artificial graphite (anode active material), carbon black (conductive agent), styrene-butadiene rubber (SBR) (binder), and sodium carboxymethyl cellulose (CMC-Na) (thickener) were thoroughly stirred in a deionized water solvent system at a mass ratio of 96.5:0.5:1.8:1.2 to obtain a negative electrode slurry. The negative electrode slurry was then uniformly coated onto copper foil (negative electrode current collector), followed by drying, cold pressing, and slitting to obtain the negative electrode sheet. The artificial graphite had a volume average particle size (Dv50) of 9.6 μm, a coating layer with a graphitization degree of 0.87, and a specific surface area of 1.65 m². 2 / g, with the battery cell at 0% SOC, the compaction density of the negative electrode film is 1.58 g / cm³. 3 The single-sided density of the negative electrode film is 8.9 mg / cm³. 2 .
[0351] (2) Preparation of positive electrode sheet
[0352] Lithium iron phosphate (LiFePO4), carbon black (CNY), and polyvinylidene fluoride (PVDF) (PVDF) binder were mixed thoroughly in an N-methylpyrrolidone (NMP) solvent system at a mass ratio of 97:0.7:2.3 to obtain a positive electrode slurry. This slurry was then uniformly coated onto an aluminum foil current collector, followed by drying, cold pressing, and slitting to obtain the positive electrode sheet. With the battery cell at 0% SOC, the compaction density of the positive electrode film was 2.55 g / cm³. 3 The single-sided density of the positive electrode film is 17.5 mg / cm³. 2 .
[0353] (3) Preparation of electrolyte
[0354] In an argon-atmospheric glove box (H2O content <10ppm, O2 content <1ppm), the electrolyte salt lithium hexafluorophosphate (LiPF6) was dissolved in a mixture of the organic solvents ethylene carbonate (EC) and diethyl carbonate (DEC) and stirred until homogeneous. Then, a first additive, a second additive, and a third additive were added, wherein the first additive comprises tris(4-fluorophenyl)phosphine, the second additive comprises lithium bis(fluorosulfonyl)imide (LiFSI), and the third additive comprises ethylene carbonate (VC).
[0355] Based on the total mass of the electrolyte, the mass content of cyclic carbonate EC is 6%.
[0356] Based on the total mass of the electrolyte, the mass content of the first additive is 1.2%, the mass content of the second additive is 1.5%, and the mass content of the third additive is 5%. It should be noted that the mass contents of the first, second, and third additives mentioned here refer to the mass contents during the preparation process (before the battery cell formation).
[0357] Based on the total mass of the electrolyte, the mass content of DEC is 73.8%, and the mass content of the electrolyte salt LiPF6 is 12.5%.
[0358] (4) Separating membrane
[0359] The separator includes a base film, which is a polyethylene (PE) film with a thickness of 7 μm. An inorganic coating with a thickness of 2 μm is disposed on the side of the base film facing the negative electrode. The inorganic coating includes alumina ceramic particles.
[0360] (5) Preparation of battery cells
[0361] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to isolate them. This is then wound to form an electrode assembly. The tabs of the electrode assembly are connected to the end caps (e.g., by welding the tabs to the end caps using connecting components). The electrode assembly is placed in an aluminum casing and dried at 85°C for 6 hours. Electrolyte is then injected at an injection rate of 3.0 g / Ah. After vacuum sealing, settling, formation, and shaping, a battery cell is obtained. The formation process involves charging the battery cell to 30% State of Charge (SOC) at 0.04C.
[0362] Examples 2-4
[0363] The difference between Examples 2-4 and Example 1 is that the mass content of the first additive is different based on the total mass of the electrolyte.
[0364] Examples 5-10
[0365] The difference between Examples 5-10 and Example 1 is that the type of the first additive is different.
[0366] In Example 5, the first additive included tris(pentafluorophenyl)phosphine; in Example 6, the first additive included tris(pentafluorophenyl)borane; in Example 7, the first additive included triphenylborane; in Example 8, the first additive included tris(pentafluorophenyl)phosphine and tris(4-fluorophenyl)phosphine; in Example 9, the first additive included triphenylphosphine; and in Example 10, the first additive included bis(2-trifluorophenyl)(3-sulfonylphenyl)phosphine.
[0367] Examples 11-13
[0368] The difference between Examples 11-13 and Example 1 is that the mass content of cyclic carbonate EC is different based on the total mass of the electrolyte.
[0369] Examples 14-16
[0370] The difference between Examples 14-16 and Example 1 is that the mass content of the second additive is different based on the total mass of the electrolyte.
[0371] Example 17
[0372] The difference between Example 17 and Example 1 is that the type of the second additive is different. In Example 17, the second additive is lithium trifluoromethanesulfonylimide (LiTFSI).
[0373] Comparative Example 1
[0374] The difference between Comparative Example 1 and Example 1 is that the electrolyte does not contain the first additive and the second additive.
[0375] Comparative Example 2
[0376] The difference between Comparative Example 2 and Example 2 is that the electrolyte includes a first additive but does not include a second additive.
[0377] Comparative Example 3
[0378] The difference between Comparative Example 3 and Example 1 is that the electrolyte includes a second additive but does not include the first additive.
[0379] Comparative Example 4
[0380] The difference between Comparative Example 4 and Example 1 is that, based on the total mass of the electrolyte, the mass content of cyclic carbonate is greater than 8%, and the electrolyte does not contain the first additive or the second additive.
[0381] Comparative Example 5
[0382] The difference between Comparative Example 5 and Example 1 is that the mass content of cyclic carbonate is greater than 8% based on the total mass of the electrolyte.
[0383] Table 1. Data from Examples and Comparative Cases
[0384]
[0385]
[0386] It should be noted that in Comparative Example 1, since neither the first nor the second additive was added, the types of the first and second additives, their mass content before and after formation are indicated by " / " in Table 1. Similarly, in Comparative Example 2, since no second additive was added, the types of the second additive, their mass content before and after formation are indicated by " / " in Table 1. Furthermore, Comparative Example 2 primarily focuses on the effect of the second additive; therefore, the mass content of the first additive after formation was not tested in Table 1, and the mass content of the first additive after formation is indicated by " / ". The following information is provided in Comparative Example 3: Since no first additive was added, the types of the first additive, its mass content before and after formation are shown in Table 1 using " / ". Furthermore, since Comparative Example 3 primarily focuses on the effect of the first additive, the mass content of the second additive after formation was not tested in Table 1, and its mass content after formation is shown in Table 1 using " / ". Similarly, in Comparative Example 4, since neither the first nor the second additive was added, the types of the first and second additives, their mass content before and after formation are shown in Table 1 using " / ". In Examples 2-4, the focus was primarily on the effect of the mass content of the first additive on the lifetime; therefore, the mass content of the second additive after formation was not tested. The mass content of the second additive after formation is indicated by " / " in Table 1. In Examples 5-10, the type of the first additive differed from that in Example 1. Since the cycle life in Examples 5-10 was slightly shorter than that in Example 1, the mass content of the first additive after formation in Examples 5-10 was not tested. The mass content of the first additive after formation in Examples 5-10 is indicated by " / " in Table 1. In Examples 14-17, the focus was primarily on the effect of the mass content and type of the second additive on the lifetime; therefore, the mass content of the first additive after formation was not tested. The mass content of the first additive after formation is indicated by " / " in Table 1.
[0387] In this embodiment, the lifespan of a single battery cell can be represented by cycle life and storage life. Cycle life is represented by the number of cycles a single battery cell completes to 90% SOH (State of Health); the more cycles, the longer the cycle life. Storage life is represented by the number of days the battery cell is stored at 45°C to 80% SOH; the more storage days, the longer the storage life.
[0388] As shown in Example 1 and Comparative Example 1, the addition of the first additive and the second additive is beneficial to improving the lifespan of the battery cell; as shown in Example 2 and Comparative Example 2, the addition of the second additive is beneficial to improving the lifespan of the battery cell; as shown in Example 1 and Comparative Example 3, the addition of the first additive is beneficial to improving the lifespan of the battery cell; as shown in Example 1 and Comparative Examples 4-5, based on the total mass of the electrolyte, a cyclic carbonate content of less than or equal to 8% is beneficial to improving the lifespan of the battery cell.
[0389] As shown in Examples 1-17, the battery cell exhibits a good lifespan through the combination of the first additive, the second additive, and a cyclic carbonate solvent with a mass content of less than or equal to 8% based on the total mass of the electrolyte.
[0390] As shown in Examples 1-4, during the preparation of battery cells (before battery cell formation), when the mass content of the first additive is 0.5% to 5% based on the total mass of the electrolyte, the battery cells have a longer lifespan; during the preparation of battery cells (before battery cell formation), when the mass content of the first additive is 1.2% to 3.5% based on the total mass of the electrolyte, the battery cells have an even longer lifespan.
[0391] As shown in Examples 1-4, after the battery cell is formed, the battery cell has a longer lifespan when the mass content of the first additive is 0.001% to 1.7% based on the total mass of the electrolyte; and the battery cell has an even longer lifespan when the mass content of the first additive is 0.3% to 0.8% based on the total mass of the electrolyte.
[0392] As shown in Examples 1 and 5-10, the first additive comprising one or more components is beneficial for improving the lifespan of the battery cell; as shown in Examples 5-10, R in the first additive comprising boron or phosphine has a good effect on improving lifespan; as shown in Examples 5-6 and 9, setting a substituent (e.g., fluorine) on the benzene ring of the first additive is beneficial for further improving the lifespan of the battery cell; as shown in Examples 1 and 8, when the electrolyte includes LiFSI, the number of fluorine substituents in the first additive being less than 5 is beneficial for further improving the lifespan of the battery cell.
[0393] As shown in Examples 11-13, based on the total mass of the electrolyte, the battery cells exhibit a longer lifespan when the cyclic carbonate content is between 2% and 8%. Furthermore, when the cyclic carbonate content is between 6% and 8%, the increased cyclic carbonate content provides a competitive advantage over lower cyclic carbonate content in the process of competing with the first additive to form the SEI film, resulting in an increase in the organic components in the generated SEI film and a decrease in the improvement in cycle life. When the cyclic carbonate content is between 2% and 6%, the increased cyclic carbonate content leads to an increase in lithium-ion transference number, reducing the polarization of the battery cells and also contributing to improved cycle life.
[0394] As shown in Examples 14-16, during the preparation of battery cells (before battery cell formation), when the mass content of the second additive is 0.5% to 3% based on the total mass of the electrolyte, the battery cells have a longer lifespan; during the preparation of battery cells (before battery cell formation), when the mass content of the second additive is 1.5% to 2% based on the total mass of the electrolyte, the battery cells have an even longer lifespan.
[0395] As shown in Examples 14-16, after the battery cell is formed, the battery cell has a longer lifespan when the mass content of the second additive is 0.3% to 2.5% based on the total mass of the electrolyte; and when the battery cell has an even longer lifespan when the mass content of the second additive is 1.2% to 1.4% based on the total mass of the electrolyte.
[0396] As shown in Example 17, the combination of various second and first additives with low mass content of cyclic carbonate solvents has a good effect on improving the lifespan of battery cells.
[0397] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
[0398] The following is a brief description of the testing methods for the physicochemical and performance parameters involved in the embodiments of this application. It should be understood that the following testing methods are only examples, and other testing methods known in the art can also be used for testing.
[0399] 1. Cycle life testing
[0400] At 25°C, charge the battery cell to 3.8V at a charging rate of 0.5C, then charge it to 0.05C at a constant voltage of 3.8V, let it stand for 10 minutes, and then discharge it to the discharge cutoff voltage (e.g., 2.0V) at a discharge rate of 0.33C, and let it stand for 10 minutes. One charge-discharge cycle is one cycle. The test is stopped when the capacity of the battery cell decays to 90% of the discharge capacity of the first cycle. This number is recorded as the number of cycles at 90% SOH. The more cycles, the longer the cycle life and the better the cycle performance.
[0401] 2. Storage lifespan testing
[0402] At 25℃, the battery cells are charged at a constant current rate of 0.5C to 3.8V, then charged at a constant voltage of 3.8V to 0.05C, left to stand for 10 minutes, and then discharged at a constant current rate of 0.33C to 2.0V, left to stand for 10 minutes. The resulting discharge capacity is recorded as the initial capacity D0. The battery cells are then charged at a constant current rate of 0.33C to 100% state of charge (SOC) and stored at 45℃. The above steps are repeated every 30 days, and the discharge capacity Dn of the battery after n (n = 30, 60, 90, 120…) days of storage is recorded. The battery capacity retention rate after n days of storage is Qn = Dn / D0 * 100%. When Qn ≤ 80%, the test is stopped, and the number of storage days is recorded.
Claims
1. A battery cell, characterized in that, include: A negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material comprises graphite; An electrolyte, the electrolyte comprising a solvent, a first additive, and a second additive; in, The solvent includes cyclic carbonate solvents, and the mass content of the cyclic carbonate solvent is less than or equal to 8% based on the total mass of the electrolyte; The first additive comprises the compound shown in formula (I): Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano. The second additive includes a fluorosulfonyl imide salt.
2. The battery cell according to claim 1, characterized in that, The R includes one of boron or phosphine, and the X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of these groups independently includes at least one of hydrogen, chlorine, fluorine, bromine, nitro, sulfonic acid, cyano, trifluoromethyl, trichloromethyl, tribromomethyl, methyl, ethyl, methoxy, and ethoxy.
3. The battery cell according to claim 1 or 2, characterized in that, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It consists of at least two different atoms and includes different heteroatoms.
4. The battery cell according to any one of claims 1-3, characterized in that, X 12 X 13 X 14 X 15 X 22 X 23 X 24 X 25 X 32 X 33 X 34 X 35 For hydrogen, X 11 X 21 X 31 Each of these groups independently includes at least one of chlorine, fluorine, bromine, nitro, sulfonic acid, cyano, trifluoromethyl, trichloromethyl, tribromomethyl, methyl, ethyl, methoxy, and ethoxy.
5. The battery cell according to any one of claims 1-3, characterized in that, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It contains 0 to 3 hydrogen atoms.
6. The battery cell according to any one of claims 1-3, characterized in that, The first additive includes at least one of 2,4,6-tris(4-fluorophenyl)cycloboroxane, tris(4-fluorophenyl)phosphine, tris(pentafluorophenyl)phosphine, tris(4-chlorophenyl)phosphine, triphenylphosphine, triphenylborane, tris(pentafluorophenyl)borane, and triphenylphosphine oxide.
7. The battery cell according to any one of claims 1-6, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 0.001% to 5%.
8. The battery cell according to claim 7, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 0.5% to 5%.
9. The battery cell according to claim 8, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 1.2% to 3.5%.
10. The battery cell according to claim 7, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is from 0.001% to 1.7%.
11. The battery cell according to claim 10, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 0.3% to 0.8%.
12. The battery cell according to any one of claims 1-7, characterized in that, In the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for less than 40%.
13. The battery cell according to claim 12, characterized in that, In the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area of the peak at 53.8±0.2 eV accounts for 10% to 32%.
14. The battery cell according to any one of claims 1-13, characterized in that, Based on the total mass of the electrolyte, the mass content of the second additive is 0.001% to 3%.
15. The battery cell according to claim 14, characterized in that, Based on the total mass of the electrolyte, the mass content of the second additive is 0.5% to 3%.
16. The battery cell according to claim 15, characterized in that, Based on the total mass of the electrolyte, the mass content of the second additive is 1.5% to 2%.
17. The battery cell according to claim 14, characterized in that, Based on the total mass of the electrolyte, the mass content of the second additive is 0.3% to 2.5%.
18. The battery cell according to claim 17, characterized in that, Based on the total mass of the electrolyte, the mass content of the second additive is 1.2% to 1.4%.
19. The battery cell according to any one of claims 1-18, characterized in that, The second additive includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonate)imide.
20. The battery cell according to any one of claims 1-19, characterized in that, Based on the total mass of the electrolyte, the mass content of the cyclic carbonate solvent is 2% to 6%.
21. The battery cell according to any one of claims 1-20, characterized in that, The cyclic carbonate solvents include at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
22. The battery cell according to any one of claims 1-21, characterized in that, The electrolyte further includes at least one of a third additive and a fourth additive, wherein the third additive includes a carbonate additive and the fourth additive includes a sulfur-containing additive.
23. The battery cell according to claim 22, characterized in that, The carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate.
24. The battery cell according to claim 22 or 23, characterized in that, The sulfur-containing additive includes at least one of vinyl sulfate, vinyl disulfate, butene sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate.
25. The battery cell according to any one of claims 22-24, characterized in that, Based on the total mass of the electrolyte, the sum of the mass contents of the third additive and the fourth additive is 0.5% to 10%.
26. The battery cell according to claim 25, characterized in that, Based on the total mass of the electrolyte, the sum of the mass contents of the third additive and the fourth additive is 2% to 8%.
27. The battery cell according to any one of claims 1-26, characterized in that, The electrolyte includes an electrolyte salt, which includes lithium hexafluorophosphate.
28. The battery cell according to any one of claims 1-27, characterized in that, The electrolyte satisfies at least one of the following conditions: The electrolyte has a conductivity of 8 mS / cm to 20 mS / cm at 20°C to 30°C. The viscosity of the electrolyte at 20°C to 30°C is 2.0 mPa·s to 3.5 mPa·s. The electrolyte has a density of 1.05 g / mL to 1.35 g / mL at 20°C to 30°C.
29. The battery cell according to any one of claims 1-28, characterized in that, The graphite satisfies at least one of the following conditions: The volume average particle size Dv50 of the graphite is 8 μm to 14 μm; The specific surface area of the graphite is 0.8 m². 2 / g to 1.7m 2 / g.
30. The battery cell according to claim 29, characterized in that, The graphite satisfies at least one of the following conditions: The volume average particle size Dv50 of the graphite is 10 μm to 13 μm; The specific surface area of the graphite is 1.0 m². 2 / g to 1.4m 2 / g.
31. The battery cell according to any one of claims 1-30, characterized in that, At least a portion of the surface of the graphite has a carbon coating layer, the degree of graphitization of the carbon coating layer being 0.85 to 0.
9.
32. The battery cell according to any one of claims 1-31, characterized in that, The graphite includes at least one of natural graphite and artificial graphite.
33. The battery cell according to any one of claims 1-32, characterized in that, The graphite includes at least one of primary particles and secondary particles.
34. The battery cell according to any one of claims 1-33, characterized in that, The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including the negative electrode active material, and the negative electrode sheet satisfies at least one of the following conditions: The compaction density of the negative electrode film is 1.50 g / cm³. 3 Up to 1.70 g / cm 3 ; The porosity of the negative electrode sheet is 25% to 60%; The one-sided density of the negative electrode film is 7 mg / cm³. 2 Up to 10.5 mg / cm 2 .
35. The battery cell according to claim 34, characterized in that, The negative electrode sheet satisfies at least one of the following conditions: The compaction density of the negative electrode film is 1.52 g / cm³. 3 Up to 1.60 g / cm 3 ; The porosity of the negative electrode sheet is 25% to 35%; The density of the negative electrode film layer on one side is 7.8 mg / cm³. 2 Up to 9.8 mg / cm 2 .
36. The battery cell according to any one of claims 1-35, characterized in that, The battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side surface of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium phosphate.
37. The battery cell according to claim 36, characterized in that, At least a portion of the surface of the lithium phosphate has a coating layer comprising carbon.
38. The battery cell according to claim 36 or 37, characterized in that, The lithium-containing phosphate includes components having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes at least one of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.
1.
39. The battery cell according to any one of claims 36-38, characterized in that, The specific capacity of the positive electrode active material is from 135 mAh / g to 150 mAh / g.
40. The battery cell according to any one of claims 36-39, characterized in that, The positive electrode film layer satisfies at least one of the following conditions: The compaction density of the positive electrode film is 2.52 g / cm³. 3 Up to 2.78 g / cm 3 ; The one-sided density of the positive electrode film is 12 mg / cm³. 2 Up to 19 mg / cm 2 .
41. A battery device, characterized in that, include: Multiple battery cells according to any one of claims 1-40.
42. An electrical appliance, characterized in that, include: A plurality of battery cells according to any one of claims 1-40, or a battery device according to claim 41, wherein the battery cells or battery device are used to store or provide electrical energy.