Battery cells, battery devices, electrical equipment
By using high-specific-capacity graphite and specific additives to generate an inorganic SEI film in battery cells, the problem of balancing energy density and cycle life in battery cells is solved, achieving battery performance with high energy density and long cycle life.
Patent Information
- Application Number
- CN202510624935.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-15
- Publication Date
- 2026-11-17
AI Technical Summary
How to provide a battery cell with high energy density and long cycle life, solving the problem that it is difficult to balance the energy density and cycle performance of a battery cell in the existing technology.
Graphite is used as the negative electrode active material, and a first additive with a specific structure, including the compound shown in formula (I), is added to the electrolyte. Through π-π interaction and empty electron orbitals, anions are attracted to generate a stable SEI film rich in inorganic components, thereby reducing lithium ion consumption and improving the cycle life of the battery cell.
High energy density and long cycle life of battery cells were achieved. By generating a dense inorganic SEI film, the risk of repeated breakage and reconstruction of the SEI film was reduced, lithium-ion consumption was reduced, and the overall performance of the battery was improved.
Smart Images

Figure CN123120881A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and more specifically, to a battery cell, a battery device, and an electrical appliance. Background Technology
[0002] The new energy industry is attracting increasing attention. Within this industry, battery technology is a crucial factor in its development.
[0003] The development of battery technology requires consideration of various design factors, such as energy density, cycle life, lifespan, capacity, fast charging performance, and reliability. How to provide a battery cell with high energy density and long cycle life is a pressing technical problem that needs to be solved. Summary of the Invention
[0004] This application is made in view of the above-mentioned issues, and its purpose is to provide a battery cell with high energy density and long cycle life.
[0005] To achieve the above objectives, this application provides a battery cell, a battery device, and an electrical appliance.
[0006] In a first aspect, a battery cell is provided, comprising: a negative electrode sheet, the negative electrode sheet comprising a negative electrode active material, the negative electrode active material comprising graphite, the specific capacity of the graphite being 360 mAh / g to 370 mAh / g; and an electrolyte comprising a first additive, the first additive comprising a compound represented by formula (I):
[0007]
[0008] Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano.
[0009] This application provides a battery cell whose negative electrode active material includes graphite with a specific capacity of 360 mAh / g to 370 mAh / g, giving the battery cell a high energy density. The electrolyte of the battery cell includes a first additive, which comprises a compound of formula (I). In the compound of formula (I), R includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (e.g., hexafluorophosphate ions) in the electrolyte, thereby generating an SEI film rich in inorganic components, which is beneficial for improving the stability and cohesiveness of the SEI film. The high density of the graphite reduces the risk of repeated SEI film rupture and reconstruction caused by the large stress exerted on the SEI film by the high-capacity graphite, thus reducing lithium-ion consumption and improving the cycle life of the battery cell. Furthermore, the π-π interaction between the benzene ring in the compound shown in formula (I) and the graphite allows the compound to preferentially adsorb onto the graphite surface and enter the inner Helmholtz layer of the electrode / electrolyte interface. This facilitates the enrichment of more anions on the graphite surface anode, further promoting the formation of an SEI film rich in inorganic components, resulting in a longer cycle life for the battery cell. Therefore, the battery cell of this embodiment has a long cycle life.
[0010] In some embodiments, R comprises one of boron or phosphine, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each component independently includes at least one of the following: hydrogen, chlorine, bromine, fluorine, nitro, sulfonic acid, cyano, trifluoromethyl, trichloromethyl, tribromomethyl, methyl, ethyl, methoxy, and ethoxy. This facilitates the formation of an SEI film rich in inorganic components, thereby reducing lithium ion consumption.
[0011] In some embodiments, the X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X33 X 34 X 35 It consists of at least two different atoms and includes different heteroatoms.
[0012] In the above technical solution, the substituents on the benzene ring have at least two different groups and include different heteroatoms, which is beneficial for generating an SEI film rich in inorganic components containing different components, thereby facilitating the diffusion of lithium ions and reducing the impedance of the battery cell.
[0013] In some embodiments, the X 12 X 13 X 14 X 15 X 22 X 23 X 24 X 25 X 32 X 33 X 34 X 35 For hydrogen, X 11 X 21 X 31 Each independently includes at least one of fluorine, chlorine, bromine, nitro, sulfonic acid, cyano, methyl, ethyl, methoxy, ethoxy, trifluoromethyl, trichloromethyl, and tribromomethyl. Thus, R and X in the compound shown in formula (I) 11 X 21 X 31 The combination of functional groups is beneficial to the separation of the positive and negative charge centers of the compound molecules shown in formula (I) to form a dipole moment, thereby inducing the accumulation of anions at the negative electrode interface to generate an SEI film rich in inorganic components. The first additive has a better effect and is beneficial to improving the cycle life of the battery cell.
[0014] In some embodiments, the X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35The number of hydrogen atoms in the compound ranges from 0 to 3. This results in a higher number of substituent groups on the benzene ring, a lower LUMO energy level and a higher reduction potential for the first additive, making it more likely to decompose preferentially relative to the solvent in the electrolyte. This reduces the risk of poor SEI film quality due to solvent decomposition, which helps reduce lithium-ion consumption and improve the cycle life of the battery cell.
[0015] In some embodiments, the first additive includes at least one of 2,4,6-tris(4-fluorophenyl)cycloboroxane, tris(4-fluorophenyl)phosphine, tris(pentafluorophenyl)phosphine, tris(4-chlorophenyl)phosphine, triphenylphosphine, triphenylborane, tris(pentafluorophenyl)borane, and triphenylphosphine oxide.
[0016] The aforementioned first additive has a good effect and is beneficial to improving the cycle life of battery cells.
[0017] In some embodiments, the mass content of the first additive is 0.001% to 8% based on the total mass of the electrolyte.
[0018] The aforementioned mass content of the first additive includes both the mass content during the battery cell preparation process and the mass content after the battery cell has been formed. When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the cycle life of the battery cell. When the mass content of the first additive is less than or equal to 8% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the first additive within the battery cell due to excessive content, thereby reducing the adverse impact of side reactions on the cycle life of the battery cell.
[0019] In some embodiments, the mass content of the first additive is 0.5% to 8% based on the total mass of the electrolyte.
[0020] The mass content of the first additive mentioned above refers to the mass content of the battery cell before formation. When the mass content of the first additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it has a good effect on improving the cycle life of the battery cell. When the mass content of the first additive is less than or equal to 8% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the first additive within the battery cell due to excessive content, thereby reducing the adverse impact of side reactions on the cycle life of the battery cell.
[0021] In some embodiments, the mass content of the first additive is 1.5% to 6% based on the total mass of the electrolyte. This results in a longer cycle life for the battery cell.
[0022] In some embodiments, the mass content of the first additive is from 0.001% to 3.6% based on the total mass of the electrolyte.
[0023] The mass content of the first additive mentioned above refers to the mass content of the battery cell after formation. When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the cycle life of the battery cell. When the mass content of the first additive is less than or equal to 3.6% based on the total mass of the electrolyte, it can reduce the risk of excessive residual first additive after formation, which could lead to side reactions within the battery cell, thereby reducing the adverse impact of side reactions on the cycle life of the battery cell.
[0024] In some embodiments, the mass content of the first additive is 0.2% to 1.8% based on the total mass of the electrolyte. This results in a longer cycle life for the battery cell.
[0025] In some embodiments, in the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for less than 45%.
[0026] The peak at 53.8 ± 0.2 eV corresponds to organic matter in the SEI film. The proportion of the peak area at 53.8 ± 0.2 eV reflects the content of organic matter in the SEI film. The smaller the proportion of the peak area at 53.8 ± 0.2 eV, the lower the content of organic matter in the SEI film, the higher the content of inorganic components, and the denser and more stable the SEI film. In the embodiments of this application, the proportion of the peak area at 53.8 ± 0.2 eV is less than 45%, indicating a higher content of inorganic components in the SEI film. This makes the SEI film denser and more stable, which helps reduce the risk of repeated breakage and reconstruction of the SEI film, reduces lithium-ion consumption, and thus helps improve the cycle life of the battery cells.
[0027] In some embodiments, in the X-ray photoelectron spectroscopy of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for 10% to 40%. This results in a denser and more stable SEI film, reducing the risk of repeated breakage and reconstruction, which helps reduce lithium-ion consumption and thus improves the cycle life of the battery cell.
[0028] In some embodiments, the graphite has a graphitization degree greater than or equal to 94%. This allows the graphite to have a higher specific capacity and a higher powder compaction density, which is beneficial for improving the energy density of individual battery cells.
[0029] In some embodiments, the graphite has a graphitization degree of 94% to 96%. This allows the graphite to have a higher specific capacity and a higher powder compaction density, which is beneficial for improving the energy density of the battery cell.
[0030] In some embodiments, the volume average particle size Dv50 of the graphite is 14 μm to 18 μm.
[0031] When the volume average particle size (Dv50) of graphite is between 14 μm and 18 μm, graphite exhibits high powder compaction density and specific capacity, which is beneficial for improving the energy density of individual battery cells. Furthermore, when the volume average particle size (Dv50) of graphite is less than or equal to 18 μm, lithium ions have a suitable diffusion path length, facilitating lithium ion diffusion and improving the fast-charging performance of individual battery cells.
[0032] In some embodiments, the volumetric particle size distribution (Dv90-Dv10) / Dv50 of the graphite is 0.9 to 1.25.
[0033] In the above embodiments, the volume particle size distribution of graphite meets the above range, which is beneficial to improving the compaction density of the negative electrode film layer, thereby giving the battery cell a higher energy density. In addition, it is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, which is beneficial to improving the transport performance of active ions and electrons in the negative electrode film layer, and thus beneficial to improving the dynamic performance of the battery cell.
[0034] In some embodiments, the graphite comprises secondary particles. This helps reduce the orientation of the graphite structure and helps buffer the volume changes of the graphite during the cycling process of the battery cell, thereby giving the graphite and the negative electrode film layer better structural stability and improving the cycle life of the battery cell.
[0035] In some embodiments, the graphite includes at least one of artificial graphite or natural graphite.
[0036] In this embodiment, graphite may include natural graphite, artificial graphite, or a mixture of natural and artificial graphite.
[0037] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including the negative electrode active material, and the negative electrode sheet satisfies at least one of the following conditions:
[0038] The compaction density of the negative electrode film is 1.62 g / cm³. 3 Up to 1.77 g / cm 3 ;
[0039] The porosity of the negative electrode sheet is 25% to 60%;
[0040] The one-sided density of the negative electrode film is 7 mg / cm³. 2 Up to 12 mg / cm 2 .
[0041] The compaction density of the negative electrode film layer is greater than or equal to 1.62 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the negative electrode film is less than or equal to 1.77 g / cm³, it is beneficial to improve the energy density of individual battery cells. 3 In this case, it is beneficial to reduce the risk of particle breakage of negative electrode active material due to the high compaction density of the negative electrode film layer. It can reduce the side reactions between broken particles and electrolyte, reduce lithium ion consumption, and thus help reduce the adverse impact on the cycle life of battery cells.
[0042] When the porosity of the negative electrode sheet is greater than or equal to 25%, it facilitates the transport and diffusion of lithium ions, which is beneficial to improving the fast charging performance of the battery cell. When the porosity of the negative electrode sheet is less than or equal to 60%, the negative electrode sheet has a more suitable strength, which can reduce the risk of cracking of the negative electrode sheet and is beneficial to improving the cycle life of the battery cell.
[0043] The density on one side of the negative electrode film layer is greater than or equal to 7 mg / cm³. 2 Under certain conditions, this is beneficial for improving the energy density of individual battery cells; when the density on one side of the negative electrode film is less than or equal to 12 mg / cm³, it is conducive to improving the energy density of individual battery cells. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial to improving the fast-charging performance of the battery cell. In addition, the combination of the first additive with the areal density and compaction density of the negative electrode film within the above-mentioned range is also beneficial to giving the battery cell a longer cycle life.
[0044] In some embodiments, the negative electrode sheet satisfies at least one of the following conditions:
[0045] The compaction density of the negative electrode film is 1.62 g / cm³. 3 Up to 1.68 g / cm 3 ;
[0046] The porosity of the negative electrode sheet is 25% to 35%;
[0047] The single-sided density of the negative electrode film is 8 mg / cm³. 2 Up to 10 mg / cm 2 .
[0048] The compaction density of the negative electrode film layer is 1.62 g / cm³. 3 Up to 1.68 g / cm 3Under these conditions, the battery cell exhibits high energy density and long cycle life; with a negative electrode porosity of 25% to 35%, the battery cell demonstrates good fast-charging performance and long cycle life; and with a single-sided surface density of 8 mg / cm³ for the negative electrode film... 2 Up to 10 mg / cm 2 Under these conditions, the battery cells have high energy density and good fast charging performance.
[0049] In some embodiments, the battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side surface of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium phosphate.
[0050] Lithium phosphates have high structural stability, and lithium phosphate-containing battery cells have long cycle life.
[0051] In some embodiments, at least a portion of the surface of the lithium phosphate has a coating layer comprising carbon. This helps improve the conductivity of the lithium phosphate, facilitating the utilization of the battery cell's capacity and improving its cycle life.
[0052] In some embodiments, the lithium-containing phosphate includes a component having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.1.
[0053] In some embodiments, the specific capacity of the positive electrode active material is between 135 mAh / g and 150 mAh / g. This results in a suitable specific capacity for the positive electrode active material and a suitable energy density for the battery cell.
[0054] In some embodiments, the positive electrode film layer satisfies at least one of the following conditions:
[0055] The compaction density of the positive electrode film is 2.52 g / cm³. 3 Up to 2.78 g / cm 3 ;
[0056] The areal density of one side of the positive electrode film is 12 mg / cm³. 2 Up to 22 mg / cm 2.
[0057] The compaction density of the positive electrode film layer is greater than or equal to 2.52 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the positive electrode film is less than or equal to 2.78 g / cm³. 3 Under these conditions, it is beneficial for the transport of lithium ions, thereby improving the fast charging performance of individual battery cells.
[0058] The density on one side of the positive electrode film is greater than or equal to 12 mg / cm³. 2 Under certain conditions, this is beneficial for improving the energy density of individual battery cells; when the density on one side of the positive electrode film is less than or equal to 22 mg / cm³, it is advantageous for improving the energy density of individual battery cells. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial for improving the fast-charging performance of individual battery cells. Furthermore, the combination of the first additive with the areal density and compaction density of the positive electrode film within the aforementioned range also helps to give the individual battery cells a longer cycle life.
[0059] In some embodiments, the electrolyte further includes at least one of a second additive and a third additive, wherein the second additive includes a carbonate additive and the third additive includes a sulfur-containing additive.
[0060] Carbonate additives facilitate the formation of polymer coatings on graphite surfaces, which can buffer the volume expansion of battery cells during charge and discharge processes. They also help repair damaged sites in the SEI film during long-term charge and discharge cycles, thereby improving the cycle life of battery cells.
[0061] The film formed on the graphite surface by sulfur-containing additives has good ion-conducting ability, which helps to reduce the increase of DC resistance in the battery cell and thus improves the kinetic isoelectric performance of the battery cell. In addition, the combined use of carbonate additives and sulfur-containing additives helps to balance the cycle life and kinetic performance of the battery cell.
[0062] In some embodiments, the carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate. These additives have a good effect on improving the cycle life of battery cells.
[0063] In some embodiments, the sulfur-containing additive includes at least one selected from vinyl sulfate, vinyl disulfate, butenyl sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate. These additives have a good effect on improving the kinetic performance of battery cells.
[0064] In some embodiments, the mass content of the second additive and the third additive is 0.5% to 10% based on the total mass of the electrolyte.
[0065] When the mass content of the second and third additives is greater than or equal to 0.5% based on the total mass of the electrolyte, the battery cell has a longer cycle life. When the mass content of the second and third additives is less than or equal to 10% based on the total mass of the electrolyte, it is beneficial to reduce the risk of more severe side reactions in the battery cell caused by the higher content of the second and third additives, and can reduce the adverse effects of side reactions on the cycle life of the battery cell.
[0066] In some embodiments, the mass content of the second additive and the third additive is 2% to 8% based on the total mass of the electrolyte. This results in a longer cycle life for the battery cell.
[0067] In some embodiments, the electrolyte further includes a fourth additive, which includes a lithium salt additive, and the lithium salt additive includes at least one of lithium difluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium dioxalate borate.
[0068] The aforementioned additives facilitate the formation of an SEI film at the negative electrode, which can reduce the risk of lithium-ion consumption due to SEI film rupture and improve the cycle life of individual battery cells.
[0069] In some embodiments, the electrolyte comprises an organic solvent, which includes cyclic carbonate solvents, and the cyclic carbonate solvents include at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
[0070] Cyclic carbonate solvents have high dielectric constants and mainly play a role in dissociating lithium salts. This helps to increase the transport number of lithium ions, reduce the internal resistance of battery cells, and thus reduce the risk of increased lithium ion consumption due to higher battery cell temperatures, thereby improving the cycle life of battery cells.
[0071] In some embodiments, the cyclic carbonate solvent comprises 20% to 40% by mass, based on the total mass of the organic solvent. This results in a suitable electrolyte with appropriate ionic conductivity, thereby providing the battery cell with suitable fast-charging performance.
[0072] In some embodiments, the electrolyte comprises an organic solvent, which comprises a linear carboxylic acid ester solvent, and the linear carboxylic acid ester solvent comprises at least one of methyl formate, methyl acetate, ethyl acetate, methyl butyrate, ethyl propionate, ethyl butyrate, butyl acetate, methyl propionate, and propyl butyrate.
[0073] The aforementioned linear carboxylic acid ester solvents have low viscosity and high ionic conductivity, which is beneficial for improving the fast charging performance of battery cells.
[0074] In some embodiments, the linear carboxylic acid ester solvent has a mass content of 10% to 70% based on the total mass of the organic solvent.
[0075] When the mass content of linear carboxylic acid ester solvent is greater than or equal to 10% based on the total mass of organic solvents, the electrolyte has lower viscosity and higher ionic conductivity, thus giving the battery cell better fast-charging performance. When the mass content of linear carboxylic acid ester solvent is less than or equal to 70% based on the total mass of organic solvents, the degree of side reactions of linear carboxylic acid ester solvents can be reduced, and the consumption of lithium ions caused by side reactions can be reduced, thereby helping to improve the cycle life of the battery cell.
[0076] In some embodiments, the electrolyte comprises an electrolyte salt, which includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, and lithium difluorooxalateborate.
[0077] Lithium hexafluorophosphate is easily dissociated and moderately priced, making it suitable as a primary electrolyte salt in electrolyte solutions. Lithium difluorosulfonylimide, lithium bis(trifluoromethanesulfonylimide), lithium difluorophosphate, and lithium difluorooxalate borate have improved thermal stability and can be used as additives or partial substitutes for lithium hexafluorophosphate. They can also be reduced to LiF, which can form a more stable SEI film on graphite surfaces, thus improving the cycle life of individual battery cells. In addition, they can reduce the risk of HF attacking the positive electrode due to the hydrolysis of lithium hexafluorophosphate, leading to the dissolution of metal ions and damage to the SEI film of the negative electrode, further enhancing the cycle life of individual battery cells.
[0078] In a second aspect, a battery device is provided, comprising the battery cell of the first aspect and any of the embodiments thereof.
[0079] Thirdly, an electrical device is provided, comprising a battery cell of the first aspect and any of the embodiments thereof, or a battery device of the second aspect, wherein the battery cell or battery device is used to store or provide electrical energy. Attached Figure Description
[0080] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0081] Figure 1 This is a schematic diagram of a vehicle according to an embodiment of this application;
[0082] Figure 2 This is a schematic diagram of a battery device according to an embodiment of this application;
[0083] Figure 3 This is a schematic diagram of the negative electrode sheet according to an embodiment of this application;
[0084] Figure 4 This is a schematic diagram of the positive electrode sheet according to an embodiment of this application;
[0085] Figure 5 This is a schematic diagram of a battery cell according to an embodiment of this application. Detailed Implementation
[0086] Embodiments of the battery cell, battery device, and electrical appliance of this application have been described in detail with appropriate reference to the accompanying drawings; however, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0087] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0088] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0089] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0090] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0091] This application aims to develop a battery cell with high energy density and long cycle life. The battery cell includes: a negative electrode sheet comprising a negative electrode active material, the negative electrode active material comprising graphite, the specific capacity of the graphite being 360 mAh / g to 370 mAh / g; and an electrolyte comprising a first additive, the first additive comprising a compound represented by formula (I):
[0092]
[0093] Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano.
[0094] In individual battery cells, the degradation of cycle life primarily stems from the loss of active lithium at the negative electrode. The reconstruction of the SEI film after its destruction at the negative electrode leads to the consumption of active lithium. The solvent in the electrolyte participates in the formation of the SEI film at the negative electrode, and the resulting SEI film is mostly composed of organic components. This results in a relatively loose structure and poor stability of the SEI film. During battery cell cycling and storage, repeated destruction and reconstruction of the SEI film lead to the consumption of active lithium, thus affecting the cycle life of the battery cell. In battery cells containing high-specific-capacity graphite, although graphite has a high specific capacity, which is beneficial for improving the energy density of the battery cell, during charge-discharge cycles, high-specific-capacity graphite exhibits greater rebound and is more prone to generating significant stress. This further exacerbates the destruction of the SEI film, leading to repeated destruction and reconstruction, further consuming active lithium, making it difficult to simultaneously achieve high energy density and cycle performance of the battery cell.
[0095] This application provides a battery cell whose negative electrode active material includes graphite with a specific capacity of 360 mAh / g to 370 mAh / g, giving the battery cell a high energy density. The electrolyte of the battery cell includes a first additive, which comprises a compound of formula (I). In the compound of formula (I), R includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (e.g., hexafluorophosphate ions) in the electrolyte, thereby generating an SEI film rich in inorganic components, which is beneficial for improving the stability of the SEI film. The high density and compactness of the graphite reduce the risk of repeated SEI film rupture and reconstruction caused by the large stress exerted by graphite on the SEI film, thus reducing lithium-ion consumption and improving the cycle life of the battery cell. Furthermore, the π-π interaction between the benzene ring in the compound shown in formula (I) and graphite allows the compound to preferentially adsorb onto the graphite surface and enter the inner Helmholtz layer of the electrode / electrolyte interface double layer. This facilitates the enrichment of more anions on the graphite surface anode, further promoting the formation of an SEI film rich in inorganic components, resulting in a longer cycle life for the battery cell. Therefore, the battery cell of this application embodiment exhibits high energy density and a long cycle life.
[0096] The technical solutions described in the embodiments of this application are applicable to various electrical devices that use battery devices.
[0097] Electrical equipment can include vehicles, mobile phones, portable devices, laptops, ships, spacecraft, electric toys, and power tools, etc. Vehicles can be gasoline-powered cars, natural gas-powered cars, or new energy vehicles; new energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. Spacecraft include airplanes, rockets, space shuttles, and spacecraft, etc. Electric toys include stationary or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys, etc. Power tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers, etc. This application does not impose any special limitations on the above-mentioned electrical equipment.
[0098] For ease of explanation, the following embodiments use a vehicle as an example of electrical equipment.
[0099] For example, such as Figure 1 The diagram shown is a structural schematic of a vehicle 1 according to one embodiment of this application. Vehicle 1 can be a gasoline-powered vehicle, a natural gas-powered vehicle, or a new energy vehicle. New energy vehicles can be pure electric vehicles, hybrid electric vehicles, or range-extended electric vehicles, etc. A motor 40, a controller 30, and a battery device 10 can be installed inside vehicle 1. The controller 30 controls the battery device 10 to supply power to the motor 40. For example, the battery device 10 can be installed at the bottom, front, or rear of vehicle 1. The battery device 10 can be used to power vehicle 1. For example, the battery device 10 can serve as the operating power source for vehicle 1, for example, to meet the electrical system requirements of vehicle 1, such as for starting, navigation, and operation. In another embodiment of this application, the battery device 10 can not only serve as the operating power source for vehicle 1, but also as the driving power source for vehicle 1, replacing or partially replacing gasoline or natural gas to provide driving power for vehicle 1.
[0100] Figure 2 A partial structural schematic diagram of the battery device 10 according to an embodiment of this application is shown. For example, as... Figure 2 As shown, the battery device 10 of this application embodiment may include a plurality of battery cells 3 to meet different power usage requirements. The shape of the battery cell 3 in this application embodiment can be set according to actual application. For example, the battery cell 3 can be cylindrical, or it can be cuboid or other shapes, and this application embodiment is not limited to this.
[0101] It should be understood that, such as Figure 2As shown, the battery device 10 of this embodiment may further include a housing 11, which can be used to accommodate multiple battery cells 3. The housing 11 of this embodiment has a hollow interior, and the multiple battery cells 3 are accommodated within the housing 11. The housing 11 may include two parts, referred to herein as a first housing portion 111 and a second housing portion 112, which are fastened together. The shapes of the first housing portion 111 and the second housing portion 112 can be determined according to the shape of the components housed inside, for example, according to the shape of the combination of the multiple battery cells 3 housed inside. At least one of the first housing portion 111 and the second housing portion 112 has an opening. For example, as... Figure 2 As shown, the first housing portion 111 and the second housing portion 112 can both be hollow cuboids with one open side each. The openings of the first housing portion 111 and the second housing portion 112 are opposite to each other, and the first housing portion 111 and the second housing portion 112 are interlocked to form a housing 11 with a closed chamber, which can be used to accommodate multiple battery cells 3. The multiple battery cells 3 are connected in parallel, series, or mixed and placed inside the housing 11 formed by the interlocking of the first housing portion 111 and the second housing portion 112.
[0102] For example, unlike Figure 2 As shown, either the first housing portion 111 or the second housing portion 112 may have only one hollow cuboid with an opening, while the other is plate-shaped to cover the opening. Taking the second housing portion 112 as a hollow cuboid with one opening and the first housing portion 111 as a plate-shaped example, then the first housing portion 111 covers the opening of the second housing portion 112 to form a housing 11 with a closed chamber, which can be used to accommodate multiple battery cells 3.
[0103] In this embodiment of the application, the battery cell can be a secondary battery, which refers to a battery cell that can be recharged to activate the active materials and continue to be used after the battery cell has been discharged.
[0104] The battery cell can be a lithium-ion battery.
[0105] During the charging process of a single battery cell, lithium ions are released from the positive electrode active material, move and embed into the negative electrode; while during the discharging process, lithium ions are released from the negative electrode, move and embed into the positive electrode active material.
[0106] It should be understood that the “intercalation” process described in this application refers to the process by which lithium ions are intercalated in the positive electrode active material or the negative electrode due to an electrochemical reaction, and the “extraction” process described in this application refers to the process by which lithium ions are extracted from the positive electrode active material or the negative electrode due to an electrochemical reaction.
[0107] Typically, a battery cell includes a positive electrode, a negative electrode, an electrolyte, and a separator. The following section describes the battery cell and its components provided in this application.
[0108] [Battery cell]
[0109] This application provides a battery cell, including an electrolyte and a negative electrode.
[0110] The negative electrode sheet includes a negative electrode active material, which includes graphite. The graphite may include at least one of natural graphite or artificial graphite.
[0111] The specific capacity of graphite is from 360 mAh / g to 370 mAh / g, for example, it can be 360 mAh / g, 361 mAh / g, 362 mAh / g, 363 mAh / g, 364 mAh / g, 365 mAh / g, 366 mAh / g, 367 mAh / g, 368 mAh / g, 369 mAh / g, 370 mAh / g or any value within the above range.
[0112] The specific capacity of graphite can be measured as follows: A negative electrode slurry is prepared by mixing graphite, a conductive agent, a binder, and a solvent. This slurry is then coated onto copper foil to obtain a negative electrode sheet. The negative electrode sheet is then assembled with a lithium foil to form a coin cell. The coin cell is discharged at a constant current rate of 0.05C to 0.005V, and then charged at a constant current rate to 2V. The charging capacity of the coin cell is then measured. The specific capacity of graphite is calculated as: charging capacity / mass of graphite.
[0113] Before testing the specific capacity of graphite, the graphite obtained from the battery cell can be disassembled in the reverse phase. As an example, the battery cell is discharged at a constant current of 0.33C to 2.0V at 25°C to obtain a battery cell with 0% SOC. The battery cell is then disassembled to obtain the negative electrode sheet. The negative electrode film layer of the negative electrode sheet is scraped off to obtain the powder of the negative electrode film layer. The powder of the negative electrode film layer is then mixed with water, filtered, and dried to obtain graphite.
[0114] It should be noted that graphite with different basis weights can have different volume average particle size Dv50, different particle size distribution, different powder compaction density, and different degrees of graphitization.
[0115] The electrolyte includes a first additive, which includes a compound represented by formula (I):
[0116]
[0117] Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano.
[0118] As an example, the halogen element includes at least one of fluorine, chlorine, and bromine; the C1-C3 alkyl group includes at least one of methyl, ethyl, and propyl; the halogen-substituted C1-C3 alkyl group includes at least one of fluorine, chlorine, or bromine-substituted C1-C3 alkyl group; and the C1-C3 alkoxy group includes at least one of methoxy, ethoxy, and propoxy.
[0119] X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Any two groups can be the same group or different groups.
[0120] In X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When all components are hydrogen, the first additive can have the following structure:
[0121]
[0122] In X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When each of the following groups independently includes at least one of halogen elements (e.g., fluorine, chlorine, bromine), nitro, sulfonic acid, cyano, C1-C3 alkoxy (e.g., methoxy, ethoxy), or halogen-substituted C1-C3 alkyl (e.g., trifluoromethyl, trichloromethyl, tribromomethyl), the above groups (hereinafter collectively referred to as X groups) are electron-withdrawing groups and can form X-electron-rich centers. When X groups are combined with R, the positive and negative charge centers of the compound molecule shown in formula (I) are separated to form a dipole moment. Through ionic dipole interaction, anion enrichment is induced, and anion decomposition is promoted to form a more stable SEI film rich in inorganic components.
[0123] In the compound shown in formula (I), R includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (such as hexafluorophosphate ions) in the electrolyte. The decomposition of the anions participates in the formation of the SEI film, thereby generating an anion-derived SEI film rich in inorganic components at the negative electrode. The inorganic-rich SEI film is denser than the organic-rich SEI film, which reduces the risk of organic solvents in the electrolyte penetrating the SEI film and contacting the graphite at the negative electrode. This reduces the risk of forming an organic-rich SEI film and is more conducive to forming an inorganic-rich SEI film. The inorganic-rich SEI film has better thermal stability and mechanical properties than the organic-rich SEI film. It is less prone to breakage during the charge-discharge cycle of the battery cell, which can reduce the active lithium consumed by repeated breakage and reconstruction of the SEI film due to the large stress of graphite on the SEI film, thus improving the cycle life of the battery cell.
[0124] The benzene ring in the compound shown in formula (I) has a π-π interaction with the graphite, allowing the compound to enter the inner Helmholtz layer of the electrical double layer at the graphite / electrolyte interface. Since the electrical double layer is closer to the graphite surface than the electrolyte phase, and the SEI film is a solid electrolyte membrane at the graphite / electrolyte interface, the entry of the compound in formula (I) into the electrical double layer facilitates its preferential adsorption on the graphite surface, inducing more anions to accumulate on the graphite surface anode. This, in turn, is more conducive to the formation of anion-derived, inorganic-rich SEI film, thereby improving the cycle life of the battery cell.
[0125] Furthermore, the compound shown in formula (I) is a molecular compound, which is not easily dissociated in the electrolyte and is more conducive to adsorption on the surface of graphite. This allows for the formation of a higher quality SEI film on the graphite surface, which helps reduce the lithium ions consumed by repeated rupture and reconstruction of the SEI film, resulting in a longer cycle life for the battery cell.
[0126] In this embodiment, the negative electrode active material of the battery cell includes graphite with a specific capacity of 360 mAh / g to 370 mAh / g, giving the battery cell a high energy density. The electrolyte of the battery cell includes a first additive, which comprises a compound of formula (I). The R in the compound of formula (I) includes at least one of B, P, and BOB. The R group has empty electron orbitals, making it easier to attract anions (e.g., hexafluorophosphate ions) in the electrolyte, thereby generating an SEI film rich in inorganic components, which is beneficial for improving the stability and cohesiveness of the SEI film. The high density of the graphite reduces the risk of repeated breakage and reconstruction of the SEI film due to the large stress exerted by graphite on it, thus reducing lithium-ion consumption and improving the cycle life of the battery cell. Furthermore, the benzene ring in the compound shown in formula (I) has a π-π interaction with the graphite, allowing the compound to preferentially adsorb onto the graphite surface and enter the inner Helmholtz layer of the electrode / electrolyte interface double layer. This facilitates the enrichment of more anions on the graphite surface anode, further promoting the formation of an SEI film rich in inorganic components and resulting in a longer cycle life for the battery cell. Therefore, the battery cell in this embodiment has a long cycle life.
[0127] In some embodiments, R includes one of boron or phosphine, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X33 X 34 X 35 Each component independently includes at least one of the following: hydrogen, fluorine, chlorine, bromine, nitro, sulfonic acid, cyano, methyl, ethyl, methoxy, ethoxy, trifluoromethyl, trichloromethyl, and tribromomethyl. This facilitates the formation of an SEI film rich in inorganic components, thereby reducing lithium ion consumption.
[0128] In some embodiments, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It consists of at least two different atoms and includes different heteroatoms.
[0129] Heteroatoms are atoms other than carbon and hydrogen. For example, heteroatoms include at least one of O, N, F, Cl, and Br.
[0130] In the above technical solution, the substituents on the benzene ring have at least two different groups and include different heteroatoms, which is beneficial for generating an SEI film rich in different inorganic components, thereby facilitating the diffusion of lithium ions and reducing the impedance of the battery cell.
[0131] As an example, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35The generated SEI film, rich in inorganic components, can contain at least two different heteroatoms, including components such as LiF, Li₂O, Li₂CO₃, Li₃N, Li₂SO₃, and Li₂SO₄. These diverse components contribute to grain boundary diversification, allowing lithium ions to conduct and diffuse through these boundaries. This diversification facilitates lithium ion diffusion, thereby reducing the impedance of the battery cell. Furthermore, reduced impedance also helps lower the temperature rise of the battery cell, thus mitigating the exacerbation of side reactions within the cell at higher temperatures and ultimately improving the cycle life of the battery cell.
[0132] In some embodiments, X 12 X 13 X 14 X 15 X 22 X 23 X 24 X 25 X 32 X 33 X 34 X 35 For hydrogen, X 11 X 21 X 31 Each independently includes at least one of fluorine, chlorine, bromine, nitro, sulfonic acid, cyano, methyl, ethyl, methoxy, ethoxy, trifluoromethyl, trichloromethyl, and tribromomethyl. Thus, R and X in the compound shown in formula (I) 11 X 21 X 31 The combination of functional groups is beneficial to the separation of the positive and negative charge centers of the compound molecules shown in formula (I) to form a dipole moment, thereby inducing the accumulation of anions at the negative electrode interface to generate an SEI film rich in inorganic components. The first additive has a better effect and is beneficial to improving the cycle life of the battery cell.
[0133] As an example, the compound shown in formula (I) has the following structure:
[0134]
[0135] As an example, X11, X21, and X31 each independently include at least one of fluorine, chlorine, bromine, trifluoromethyl, trichloromethyl, and tribromomethyl.
[0136] As a predictable mechanism, the first additive has a strong adsorption effect on anions, which is more conducive to the formation of an SEI film rich in inorganic components, reducing the risk of repeated rupture and reconstruction of the SEI film, reducing the consumption of lithium ions, and thus helping to improve the cycle life of the battery cell.
[0137] In the above embodiments, the first additive has a better effect and is beneficial to improving the cycle life of the battery cell.
[0138] In some embodiments, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It contains 0 to 3 hydrogen atoms.
[0139] X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 The number of hydrogen atoms can be 0, 1, 2, or 3.
[0140] In X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When the number of hydrogen atoms is 0, all positions on the benzene ring have substituents.
[0141] The more substituents on the benzene ring, the lower the LUMO energy level of the first additive becomes. The first additive has a higher reduction potential, which in turn makes the difference between the reduction potential of the first additive and the organic solvent in the electrolyte larger. This makes it easier for the first additive to decompose preferentially relative to the organic solvent in the electrolyte, thereby reducing the risk of poor SEI film quality caused by solvent decomposition.
[0142] In this embodiment, the benzene ring has a large number of substituent groups, and the first additive has a lower LUMO energy level and a higher reduction potential, making it easier to decompose preferentially relative to the organic solvent in the electrolyte. This can reduce the risk of poor SEI film quality caused by solvent decomposition, which is beneficial to reduce lithium ion consumption and improve the cycle life of the battery cell.
[0143] As an example, in X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 When fluorine is included, the number of fluorine substitutions on each benzene ring is less than 5. If the number of fluorine substitutions on each benzene ring is too high (e.g., 5), defluorination may generate more HF, increasing the risk of metal ion dissolution in the positive electrode active material. The dissolved metal ions are then reduced to elemental metals on the negative electrode side, increasing the risk of damaging the SEI film. Compared to cases with fewer fluorine substitutions (e.g., 4 fluorine substitutions per benzene ring), this is detrimental to further improving cycle life.
[0144] In some embodiments, the first additive includes at least one of 2,4,6-tris(4-fluorophenyl)cycloboroxane, tris(4-fluorophenyl)phosphine, tris(pentafluorophenyl)phosphine, tris(4-chlorophenyl)phosphine, triphenylphosphine, triphenylphosphine oxide, triphenylborane, and tris(pentafluorophenyl)borane.
[0145] The aforementioned first additive has a good effect and is beneficial to improving the cycle life of battery cells.
[0146] In some embodiments, the mass content of the first additive is 0.001% to 8% based on the total mass of the electrolyte.
[0147] Based on the total mass of the electrolyte, the mass content of the first additive can be 0.001%, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, or any value within the above range.
[0148] The aforementioned mass content of the first additive includes both the mass content during the battery cell preparation process and the mass content after the battery cell has been formed. For example, after the battery cell has been formed, the mass content of the first additive may be 0.001% based on the total mass of the electrolyte. As another example, during the battery cell preparation process, the mass content of the first additive may be 8% based on the total mass of the electrolyte.
[0149] During the formation of a battery cell, the first additive undergoes at least partial decomposition. After the battery cell is formed, the first additive may be completely consumed or remain partially. It should be noted that "complete consumption of the first additive" here can refer to a situation where the first additive cannot be detected due to exceeding the instrument's detection precision. As an example, if the mass content of the first additive is 0.001% based on the total mass of the electrolyte, it can be considered that the first additive has been completely consumed.
[0150] As an example, if the mass content of the first additive is greater than or equal to 1% based on the total mass of the electrolyte before the battery cell is formed, there will be some residue of the first additive after formation.
[0151] Furthermore, as an example, if a battery cell is stored at room temperature (e.g., 25°C) for a short period (e.g., 2 months) after formation, the mass content of the first additive within the battery cell is essentially the same as that in a freshly formed battery cell. As another example, if a battery cell is stored at a higher temperature (e.g., 45°C) for a short period (e.g., within 30 days) after formation, the mass content of the first additive within the battery cell is essentially the same as that in a freshly formed battery cell. As yet another example, if a battery cell is stored at a higher temperature (e.g., 45°C) for a longer period (e.g., more than 180 days) after formation, the first additive can be completely consumed.
[0152] If the first additive is not completely consumed, its mass content can be determined by gas chromatography, gas chromatography-mass spectrometry (GC-MS), ion chromatography (IC), liquid chromatography (LC), nuclear magnetic resonance spectroscopy (NMR), or inductively coupled plasma optical emission spectrometry (ICP-OES). As an example, the battery cell is discharged at a constant current of 0.33C to 2.0V at 25°C. The battery cell is then disassembled, and the electrolyte is extracted (if the electrolyte content in the battery cell is low, the positive and negative electrode plates can be centrifuged to obtain the electrolyte from them). Next, 500 μl of deuterated reagent was added to the NMR tube in an argon-filled glove box. Then, 100 μl of the electrolyte sample was added to the NMR tube. The NMR tube was shaken to dissolve the non-aqueous electrolyte in the deuterated reagent. The composition and mass of the first additive in the electrolyte were tested using an Oxford Instruments X-Pulse benchtop NMR spectrometer. The mass content of the first additive in the electrolyte was calculated by dividing the mass of the first additive by the mass of the entire electrolyte.
[0153] When the first additive is depleted, it can be determined whether the first additive was added during the electrolyte preparation process by testing the benzene ring structure in the electrolyte and the content of inorganic lithium compounds in the solid electrolyte interphase (SEI) film on the surface of the negative electrode. For example, if the first additive cannot be detected by nuclear magnetic resonance spectroscopy, but the benzene ring structure in the electrolyte is detected and the peak area of the lithium element in the negative electrode at 53.8 ± 0.2 eV accounts for less than 45%, then it can be inferred that the first additive was included in the electrolyte during the preparation of the battery cell.
[0154] The content of inorganic lithium compounds in the solid electrolyte interphase (SEI) film on the surface of the negative electrode layer can be determined as follows: At 25°C, the battery cell is discharged at a constant current of 0.33C to 2.0V, and then the battery cell is disassembled to obtain the negative electrode. The inorganic lithium compounds in the SEI film on the surface of the negative electrode layer can be detected by X-ray photoelectron spectroscopy (XPS). Using the negative electrode as a sample and an Al target as the X-ray source at a power of 300W, X-rays are used to bombard the surface of the negative electrode layer, exciting the inner-shell electrons or valence electrons of atoms or molecules. The C1s peak (284.8 eV) is used as the XPS reference peak position to analyze surface elements (e.g., lithium) and functional groups. As an example, the X-ray photoelectron spectrum of lithium in the negative electrode is tested, and the peak area at 53.8 ± 0.2 eV is measured and recorded. This peak represents the organic component lithium ethylene dicarbonate (LEDC). Adding the first additive is beneficial for generating a higher content of inorganic lithium compounds at the negative electrode (i.e., the inorganic component in the SEI film becomes higher). The lower the proportion of the peak area at 53.8±0.2eV, the more inorganic lithium compounds are in the SEI film.
[0155] When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the cycle life of the battery cell. When the mass content of the first additive is less than or equal to 8% based on the total mass of the electrolyte, it can reduce the risk of the first additive causing side reactions in the battery cell due to excessive content, thereby reducing the adverse effect of side reactions on the cycle life of the battery cell.
[0156] In some embodiments, the mass content of the first additive is 0.5% to 8% based on the total mass of the electrolyte.
[0157] The mass content of the first additive mentioned above refers to the mass content of the battery cell before formation, or it can refer to the mass content of the first additive during the preparation of the battery cell.
[0158] Before the formation of the battery cell, based on the total mass of the electrolyte, the mass content of the first additive can be 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.5%, 1.8%, 2%, 2.2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.8%, 4%, 4.2%, 4.5%, 4.8%, 5%, 5.2%, 5.5%, 5.8%, 6%, 6.2%, 6.5%, 6.8%, 7%, 7.2%, 7.5%, 7.8%, 8%, or any value within the above range.
[0159] Before cell formation, when the mass content of the first additive is greater than or equal to 0.5% based on the total mass of the electrolyte, it has a good effect on improving the cycle life of the cell. When the mass content of the first additive is less than or equal to 8% based on the total mass of the electrolyte, it can reduce the risk of side reactions of the first additive in the cell due to excessive content, thereby reducing the adverse effect of side reactions on the cycle life of the cell.
[0160] In some embodiments, the mass content of the first additive is 1.5% to 6% based on the total mass of the electrolyte. Thus, before the battery cell is formed, if the mass content of the first additive based on the total mass of the electrolyte meets the above range, the battery cell has a longer cycle life.
[0161] In some embodiments, the mass content of the first additive is from 0.001% to 3.6% based on the total mass of the electrolyte.
[0162] The mass content of the first additive mentioned above refers to the mass content of the battery cell after formation. Here, "formed battery cell" can refer to a fresh battery cell, such as a battery cell that has just been manufactured and has not yet been driven in a vehicle, or a battery cell that has just been removed from the warehouse and has not yet been installed in a vehicle.
[0163] After the battery cell is formed, based on the total mass of the electrolyte, the mass content of the first additive can be 0.001%, 0.01%, 0.02%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.5%, 1.9%, 2%, 2.5%, 2.8%, 3%, 3.2%, 3.5%, 3.6% or any value within the above range.
[0164] When the mass content of the first additive is greater than or equal to 0.001% based on the total mass of the electrolyte, it has a good effect on improving the cycle life of the battery cell. When the mass content of the first additive is less than or equal to 3.6% based on the total mass of the electrolyte, it can reduce the risk of the first additive causing side reactions in the battery cell due to excessive residual first additive after formation, thereby reducing the adverse effect of side reactions on the cycle life of the battery cell.
[0165] In some embodiments, the mass content of the first additive is 0.2% to 1.8% based on the total mass of the electrolyte. Thus, after the battery cell is formed, if the mass content of the first additive based on the total mass of the electrolyte meets the above range, the battery cell has a longer cycle life.
[0166] In some embodiments, in the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for less than 45%.
[0167] In the X-ray photoelectron spectrum of lithium in the negative electrode, the percentage of the peak area at 53.8 ± 0.2 eV can be 44%, 43%, 42%, 40%, 38%, 35%, 33%, 30%, 28%, 25%, 22%, 20%, 18%, 16%, 14%, 12%, 10%, 8%, or any value within the above range.
[0168] The peak position at 53.8±0.2 eV corresponds to organic matter in the SEI membrane. The proportion of the peak area at 53.8±0.2 eV can reflect the content of organic matter in the SEI membrane. The smaller the proportion of the peak area at 53.8±0.2 eV, the less organic matter in the SEI membrane, the more inorganic components in the SEI membrane, and the denser and more stable the SEI membrane.
[0169] As an example, before the formation of the battery cell, based on the total mass of the electrolyte, when the mass content of the first additive is 0.5%, the peak area at the peak position of 53.8±0.2 eV accounts for approximately 38.2%; without the addition of the first additive, the peak area at the peak position of 53.8±0.2 eV accounts for approximately 57.5%.
[0170] In the embodiments of this application, the peak area of the peak at 53.8±0.2eV accounts for less than 45%, the content of inorganic components in the SEI film is relatively high, the SEI film is more dense and stable, which helps to reduce the risk of repeated breakage and reconstruction of the SEI film, reduce the consumption of lithium ions, and thus help to improve the cycle life of the battery cell.
[0171] In some embodiments, in the X-ray photoelectron spectroscopy of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for 10% to 40%. This results in a denser and more stable SEI film, reducing the risk of repeated breakage and reconstruction, which helps reduce lithium-ion consumption and thus improves the cycle life of the battery cell.
[0172] In some embodiments, the graphitization degree of graphite is greater than or equal to 94%.
[0173] The degree of graphitization of graphite can be 94%, 94.2%, 94.5%, 94.7%, 94.9%, 95%, 95.2%, 95.5%, 95.8%, 96%, 96.2% or any value within the above range.
[0174] When the graphitization degree of graphite is greater than or equal to 94%, graphite can have a higher specific capacity and a higher powder compaction density, which is beneficial to improving the energy density of battery cells.
[0175] In some embodiments, the graphitization degree of graphite is 94% to 96%. In this way, graphite can have a higher specific capacity and a higher powder compaction density, which is beneficial to improving the energy density of the battery cell.
[0176] In some embodiments, the volume average particle size Dv50 of graphite is 14 μm to 18 μm.
[0177] The volume average particle size (Dv50) of graphite represents the particle size corresponding to a cumulative volume distribution percentage of 50%, and can be determined using instruments and methods known in the art. As an example, graphite powder is obtained after disassembling battery cells (the method for obtaining graphite powder by disassembling battery cells can be found above and will not be repeated here). The particle size is conveniently determined using a laser particle size analyzer, referring to GB / T19077-2016, Particle Size Distribution by Laser Diffraction. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0178] The volume average particle size Dv50 of graphite can be 14 μm, 14.1 μm, 14.2 μm, 14.3 μm, 14.5 μm, 14.8 μm, 15 μm, 15.2 μm, 15.5 μm, 15.8 μm, 16 μm, 16.2 μm, 16.5 μm, 16.8 μm, 17 μm, 17.2 μm, 17.5 μm, 17.8 μm, 18 μm or any value within the above range.
[0179] When the volume average particle size (Dv50) of graphite is between 14 μm and 18 μm, graphite exhibits high powder compaction density and specific capacity, which is beneficial for improving the energy density of individual battery cells. Furthermore, when the volume average particle size (Dv50) of graphite is less than or equal to 18 μm, lithium ions have a suitable diffusion path length, facilitating lithium ion diffusion and improving the fast-charging performance of individual battery cells.
[0180] In some embodiments, the volumetric particle size distribution (Dv90-Dv10) / Dv50 of graphite is 0.9 to 1.25, where Dv90 is the particle size corresponding to a cumulative particle size distribution of 90%, Dv10 is the particle size corresponding to a cumulative particle size distribution of 10%, and Dv50 is the particle size corresponding to a cumulative particle size distribution of 50%.
[0181] The Dv90 and Dv10 can be measured using the same testing method as the Dv50, so it will not be repeated here.
[0182] The volumetric particle size distribution (Dv90-Dv10) / Dv50 of graphite can be 0.9, 0.92, 0.95, 0.98, 1, 1.05, 1.1, 1.15, 1.2, 1.25 or any value within the above range.
[0183] In the above embodiments, the volume particle size distribution of graphite meets the above range, which is beneficial to improving the compaction density of the negative electrode film layer, thereby giving the battery cell a higher energy density. In addition, it is also beneficial to form a reasonable pore structure between the particles of the negative electrode film layer, which is beneficial to improving the transport performance of active ions and electrons in the negative electrode film layer, and thus beneficial to improving the dynamic performance of the battery cell.
[0184] In some embodiments, the compacted density of graphite powder under a pressure of 50,000 N is 1.9 g / cm³. 3 Up to 2.1 g / cm 3 For example, it could be 1.9 g / cm³. 3 1.92g / cm 3 1.95g / cm 3 1.98g / cm 3 2.0g / cm 3 2.02 g / cm 3 2.05g / cm 3 2.08 g / cm 3 2.09 g / cm 3 2.1g / cm 3 Or any value within the above range.
[0185] As an example, graphite powder is obtained after disassembling a battery cell. The compacted density of the powder can be determined using an electronic pressure testing machine (e.g., UTM7305) according to standard GB / T24533-2009. An exemplary test method is as follows: Weigh 1g of material and add it to a container with a base area of 1.327cm². 2 In the mold, the pressure is increased to 50,000 N, held for 30 seconds, then the pressure is released and held for 10 seconds. The compaction density of the powder under a force of 50,000 N is then recorded and calculated.
[0186] In the above embodiments, graphite has a high powder compaction density and is not easily broken under high pressure, which is beneficial to improving the compaction density of the negative electrode film layer, and thus beneficial to improving the energy density of the battery cell.
[0187] In some embodiments, graphite comprises secondary particles.
[0188] Secondary particles can be formed by the aggregation of multiple primary particles. A primary particle can refer to a single particle, which is the smallest unit of a particle within a certain observation range. A primary particle may contain defects of any form, but it is impossible to define smaller particles within a primary particle.
[0189] When graphite includes secondary particles, it helps to reduce the orientation of the graphite structure and helps to buffer the volume change of graphite during the cycle of the battery cell. As a result, the graphite and the negative electrode film have better structural stability, which is beneficial to improving the cycle life of the battery cell.
[0190] In some embodiments, graphite includes at least one of artificial graphite or natural graphite.
[0191] In this embodiment, graphite may include natural graphite, artificial graphite, or a mixture of natural and artificial graphite.
[0192] Figure 3 This is a schematic diagram of the negative electrode sheet according to an embodiment of this application. In some embodiments, such as Figure 3 As shown, the negative electrode sheet 6 includes a negative electrode current collector 60 and a negative electrode film layer 61 disposed on at least one side surface of the negative electrode current collector 60. The negative electrode film layer 61 includes a negative electrode active material, and the negative electrode sheet satisfies at least one of the following conditions:
[0193] The compaction density of the negative electrode film is 1.62 g / cm³. 3 Up to 1.77 g / cm 3 ;
[0194] The porosity of the negative electrode sheet is 25% to 60%;
[0195] The areal density of one side of the negative electrode film is 7 mg / cm³. 2 Up to 12 mg / cm 2 .
[0196] The negative electrode current collector 60 has two opposing surfaces along its own thickness direction. The negative electrode film layer 61 can be disposed on one side surface of the negative electrode current collector 60 or on both sides surface of the negative electrode current collector 60.
[0197] The aforementioned compaction density of the negative electrode film can be considered as the compaction density of the negative electrode film when the battery cell is in a fully discharged state. Here, "fully discharged state" refers to the state of charge (SOC) of the battery cell being 0%. Specifically, at 25°C, a battery cell is discharged at a constant current of 0.33C to 2.0V; at this point, the battery cell has a 0% SOC.
[0198] The compaction density of the negative electrode film can be 1.62 g / cm³. 31.65g / cm 3 1.68g / cm 3 1.70g / cm 3 1.72g / cm 3 1.73g / cm 3 1.74 g / cm 3 1.75g / cm 3 1.76 g / cm 3 1.77g / cm 3 Or any value within the above range, the unilateral density of the negative electrode film can be 7 mg / cm³. 2 7.5 mg / cm 2 8mg / cm 2 8.5 mg / cm 2 9mg / cm 2 9.5 mg / cm 2 10mg / cm 2 10.5 mg / cm 2 11mg / cm 2 11.5 mg / cm 2 12mg / cm 2 The porosity of the negative electrode sheet can be 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, or any value within the above range.
[0199] The compaction density of the negative electrode film layer is greater than or equal to 1.62 g / cm³. 3 Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the negative electrode film is less than or equal to 1.77 g / cm³, it is beneficial to improve the energy density of individual battery cells. 3 In this case, it is beneficial to reduce the risk of particle breakage of negative electrode active material due to the high compaction density of the negative electrode film layer. It can reduce the side reactions between broken particles and electrolyte, reduce lithium ion consumption, and thus help reduce the adverse impact on the cycle life of battery cells.
[0200] When the porosity of the negative electrode sheet is greater than or equal to 25%, it facilitates the transport and diffusion of lithium ions, which is beneficial to improving the fast charging performance of the battery cell. When the porosity of the negative electrode sheet is less than or equal to 60%, the negative electrode sheet has a more suitable strength, which can reduce the risk of cracking of the negative electrode sheet and is beneficial to improving the cycle life of the battery cell.
[0201] The density on one side of the negative electrode film layer is greater than or equal to 7 mg / cm³. 2Under certain conditions, this is beneficial for improving the energy density of individual battery cells; when the density on one side of the negative electrode film is less than or equal to 12 mg / cm³, it is conducive to improving the energy density of individual battery cells. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial to improving the fast-charging performance of the battery cell. In addition, the combination of the first additive with the areal density and compaction density of the negative electrode film within the above-mentioned range is also beneficial to giving the battery cell a longer cycle life.
[0202] The areal density and compaction density of the negative and positive electrode films can be measured as follows: At 25°C, the battery cell is discharged at a constant current of 0.33C to 2.0V to obtain a battery cell with 0% SOC. Then, the positive and negative electrode sheets are removed from the battery cell, and the thickness of the electrode sheet and the current collector are measured respectively. The electrode sheet is then cut into small circular pieces with an area of S1 (if it is a double-sided coated electrode sheet, the film layer on one side can be wiped off first), and its weight is recorded as M1. Then, the film layer of the weighed electrode sheet is wiped off, and the weight of the current collector is recorded as M0. The areal density of one side = (M1 - M0) / S1. The compaction density = areal density / (electrode thickness - current collector thickness).
[0203] The porosity of the negative and positive electrode sheets can be determined according to the standard procedure GB / T 24586-2009. The specific test procedure is as follows: Select more than 20 round sheets with good appearance and no powder falling off the edges using tweezers and place them into a sample cup. Record the number of sheets and calculate the apparent volume V1. Then, place the sample cup containing the sample into a true density tester AccuPycⅡ1340, seal the test system, and introduce helium gas according to the procedure. By detecting the gas pressure in the sample chamber and expansion chamber, and then calculating the true volume V2 according to Bohr's Law (PV=nRT), the porosity of the sample to be tested is obtained as P=(V1-V2) / V1×100%.
[0204] In some embodiments, the negative electrode sheet satisfies at least one of the following conditions:
[0205] The compaction density of the negative electrode film is 1.62 g / cm³. 3 Up to 1.68 g / cm 3 ;
[0206] The porosity of the negative electrode sheet is 25% to 35%;
[0207] The single-sided density of the negative electrode film is 8 mg / cm³. 2 Up to 10 mg / cm 2 .
[0208] The compaction density of the negative electrode film layer is 1.62 g / cm³. 3 Up to 1.68 g / cm 3Under these conditions, the battery cell exhibits high energy density and long cycle life; with a negative electrode porosity of 25% to 35%, the battery cell demonstrates good fast-charging performance and long cycle life; and with a single-sided surface density of 8 mg / cm³ for the negative electrode film... 2 Up to 10 mg / cm 2 Under these conditions, the battery cells have high energy density and good fast charging performance.
[0209] Figure 4 This is a schematic diagram of a positive electrode sheet according to an embodiment of this application. In some embodiments, such as Figure 4 As shown, the battery cell includes a positive electrode 5, the positive electrode 5 includes a positive current collector 50 and a positive electrode film 51 disposed on at least one side surface of the positive current collector 50, the positive electrode film 51 includes a positive electrode active material, the positive electrode active material includes lithium phosphate.
[0210] The positive electrode current collector 50 has two opposing surfaces along its own thickness direction. The positive electrode film layer 51 can be disposed on one side surface of the positive electrode current collector 50 or on both sides surface of the positive electrode current collector 50.
[0211] Lithium-containing phosphates can refer to lithium-containing transition metal phosphates with an olivine structure, such as lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate, and their modified forms. The modification can be either doping or surface modification. For example, in doping modification, elements such as titanium can be doped into lithium iron phosphate; in surface modification, a coating layer can be applied to the surface of lithium iron phosphate.
[0212] Lithium phosphates have high structural stability, and lithium phosphate-containing battery cells have long cycle life.
[0213] In some embodiments, at least a portion of the surface of the lithium phosphate contains a carbon coating. This helps to improve the conductivity of the lithium phosphate, facilitates the utilization of the battery cell's capacity, and improves the cycle life of the battery cell.
[0214] In some embodiments, the positive electrode film layer includes a conductive agent and a positive electrode active material, wherein the mass content of the conductive agent is 0% to 1.5% based on the total mass of the positive electrode film layer.
[0215] Based on the total mass of the positive electrode film, the mass content of the conductive agent can be 0%, 0.2%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, or any value within the above range.
[0216] When the lithium phosphate surface has a carbon coating layer, the mass content of the conductive agent in the positive electrode film can be 0%. When the mass content of the conductive agent is greater than 0% based on the total mass of the positive electrode film, the positive electrode film has good conductivity, which facilitates the utilization of the battery cell's capacity and helps to improve the cycle life of the battery cell. When the mass content of the conductive agent is less than or equal to 1.5% based on the total mass of the positive electrode film, the positive electrode active material in the positive electrode film has a high content, which helps to improve the energy density of the battery cell.
[0217] In some embodiments, lithium phosphates include components having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes one or more of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.1.
[0218] In the above general formula, m can be 0.8, 0.82, 0.85, 0.88, 0.9, 0.92, 0.95, 0.98, 1, 1.0, 1.15 or any value within the above range; x can be 0.9, 0.92, 0.95, 0.98, 1 or any value within the above range; y can be 0.95, 0.96, 0.97, 0.98, 0.99, 1 or any value within the above range; j can be 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value within the above range; and q can be 0.01, 0.02, 0.04, 0.05, 0.06, 0.08, 0.09, 0.1 or any value within the above range.
[0219] During the charging and discharging process of a single battery cell, the molar content of lithium, oxygen, and other elements in the lithium phosphate cathode active material changes within a certain range.
[0220] The elements and their contents in the positive electrode active material can be determined using an argon ion cross-section polisher (model JEOLIB-19530CP) and a scanning electron microscope (model Zeiss Sigma 300) (equipped with an X-ray energy dispersive spectrometer (EDS, model Oxford X-Max-50mm2)).
[0221] As an example, the battery cell was discharged at a constant current of 0.33C to 2.0V at 25°C to obtain a battery cell with 0% SOC. Then, the positive electrode was removed from the battery cell, and a longitudinal cross-section of the positive electrode film was obtained using an ion section polisher. The cross-section of the positive electrode active material particles was then scanned using a scanning electron microscope to test the elements and their content.
[0222] In some embodiments, the lithium phosphate-containing cathode active material includes at least one of LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4. The aforementioned lithium phosphate-containing cathode active materials exhibit high structural stability, which helps to improve the cycle life of individual battery cells.
[0223] During the charging and discharging process, lithium (Li) undergoes insertion / extraction and consumption within a single battery cell. The molar content of Li in the positive electrode active material varies depending on the discharge state of the cell. In the examples of positive electrode active materials in this application, the molar content of Li refers to the initial state of the material, i.e., the state before feeding. After charge-discharge cycles, the molar content of Li changes when the positive electrode active material is applied to the battery system. Similarly, the molar content of O in the examples of positive electrode active materials in this application is only an ideal value. Oxygen release from the crystal lattice causes changes in the molar content of O, resulting in fluctuations in the actual molar content of O.
[0224] In some embodiments, the specific capacity of the positive electrode active material is from 135 mAh / g to 150 mAh / g.
[0225] The specific capacity of the positive electrode active material can be measured as follows: A positive electrode slurry is prepared by mixing the positive electrode active material, conductive agent, binder, and solvent. This slurry is then coated onto aluminum foil to obtain the positive electrode sheet. The positive electrode sheet is then assembled with a lithium foil to form a coin cell. The coin cell is charged at a constant current rate of 0.1C to 3.8V, and then discharged at a constant current rate to 2.0V. The discharge capacity of the coin cell is then measured. The specific capacity of the positive electrode active material is calculated as: discharge capacity / mass of the positive electrode active material.
[0226] As an example, the positive electrode active material is obtained by disassembling a battery cell. At 25°C, the battery cell is discharged at a constant current of 0.33C to 2.0V to obtain a battery cell with 0% SOC. The positive electrode sheet is then disassembled to obtain the positive electrode plate. The positive electrode film layer of the positive electrode plate is scraped off, and the positive electrode film layer powder is dissolved in NMP solvent. After filtration and drying, the positive electrode active material is obtained.
[0227] The specific capacity of the positive electrode active material can be 135mAh / g, 138mAh / g, 140mAh / g, 142mAh / g, 145mAh / g, 146mAh / g, 148mAh / g, 150mAh / g or any value within the above range.
[0228] In this embodiment, the positive electrode active material has a suitable specific capacity, and the battery cell has a suitable energy density.
[0229] In some embodiments, the positive electrode film layer satisfies at least one of the following conditions:
[0230] The compaction density of the positive electrode film is 2.52 g / cm³. 3 Up to 2.78 g / cm 3 ;
[0231] The areal density of one side of the positive electrode film is 12 mg / cm³. 2 Up to 22 mg / cm 2 .
[0232] The compaction density of the positive electrode film mentioned above can be the compaction density of the positive electrode film when the battery cell is in a fully discharged state, where the fully discharged state refers to the state of charge (SOC) of the battery cell being 0%.
[0233] The compaction density of the positive electrode film can be 2.52 g / cm³. 3 2.55g / cm 3 2.57g / cm 3 2.59g / cm 3 2.6g / cm 3 2.62 g / cm 3 2.65g / cm 3 2.68g / cm 3 2.7g / cm 3 2.72 g / cm 3 2.75g / cm 3 2.78g / cm 3 Or any value within the above range, the unilateral density of the positive electrode film can be 12 mg / cm³. 2 13mg / cm 2 14mg / cm 2 15mg / cm 2 16mg / cm 2 17mg / cm 2 18mg / cm 2 19mg / cm 2 20mg / cm 2 21mg / cm 2 22mg / cm 2 Or any value within the above range.
[0234] The compaction density of the positive electrode film layer is greater than or equal to 2.52 g / cm³. 3Under these conditions, it is beneficial to improve the energy density of individual battery cells; when the compaction density of the positive electrode film is less than or equal to 2.78 g / cm³. 3 Under these conditions, it is beneficial for the transport of lithium ions, thereby improving the fast charging performance of individual battery cells.
[0235] The density on one side of the positive electrode film is greater than or equal to 12 mg / cm³. 2 Under certain conditions, this is beneficial for improving the energy density of individual battery cells; when the density on one side of the positive electrode film is less than or equal to 22 mg / cm³, it is advantageous for improving the energy density of individual battery cells. 2 Under these conditions, it facilitates the diffusion and transport of lithium ions, which is beneficial for improving the fast-charging performance of individual battery cells. Furthermore, the combination of the first additive with the areal density and compaction density of the positive electrode film within the aforementioned range also helps to give the individual battery cells a longer cycle life.
[0236] In some embodiments, the electrolyte further includes at least one of a second additive and a third additive, wherein the second additive includes a carbonate additive and the third additive includes a sulfur-containing additive.
[0237] Carbonate additives facilitate the formation of polymer coatings on graphite surfaces, which can buffer the volume expansion of battery cells during charge and discharge processes. They also help repair damaged sites in the SEI film during long-term charge and discharge cycles, thereby improving the cycle life of battery cells.
[0238] The film formed on the graphite surface by sulfur-containing additives has good ion-conducting ability, which helps to reduce the increase of DC resistance in the battery cell and thus improves the kinetic isoelectric performance of the battery cell. In addition, the combined use of carbonate additives and sulfur-containing additives helps to balance the cycle life and kinetic performance of the battery cell.
[0239] In some embodiments, the carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate. These additives have a good effect on improving the cycle life of individual battery cells.
[0240] In some embodiments, the carbonate additive includes vinylene carbonate (VC), and the mass content of vinylene carbonate is 0.5% to 5% based on the total mass of the electrolyte, for example, it can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or any value within the range above.
[0241] In some embodiments, the carbonate additive includes fluoroethylene carbonate (FEC), and the mass content of fluoroethylene carbonate is 0.1% to 3% based on the total mass of the electrolyte, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3% or any value within the above range.
[0242] In some embodiments, the sulfur-containing additive includes at least one selected from vinyl sulfate, vinyl disulfate, butenyl sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate. These additives have a good effect on improving the kinetic performance of the battery cell.
[0243] In some embodiments, the sum of the mass contents of the second and third additives is 0.5% to 10% based on the total mass of the electrolyte.
[0244] The sum of the mass contents of the second and third additives mentioned above can be the sum of the mass contents of the second and third additives after the battery cell has been formed.
[0245] As an example, the second and third additives are consumed during the charge-discharge cycles of the formed battery cell and throughout the entire life cycle of the battery cell.
[0246] Based on the total mass of the electrolyte, the mass content of the second and third additives can be 0.5%, 0.8%, 1%, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, or any value within the above range.
[0247] When the mass content of the second and third additives is greater than or equal to 0.5% based on the total mass of the electrolyte, the battery cell has a longer cycle life. When the mass content of the second and third additives is less than or equal to 10% based on the total mass of the electrolyte, it is beneficial to reduce the risk of more severe side reactions in the battery cell caused by the higher content of the second and third additives, and can reduce the adverse effects of side reactions on the cycle life of the battery cell.
[0248] In some embodiments, the combined mass content of the second and third additives is 2% to 8% based on the total mass of the electrolyte. This results in a longer cycle life for the battery cell.
[0249] In some embodiments, the electrolyte further includes a fourth additive, which includes a lithium salt additive, and the lithium salt additive includes at least one of lithium difluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium dioxalate borate.
[0250] The aforementioned additives facilitate the formation of an SEI film at the negative electrode, which can reduce the risk of lithium-ion consumption due to SEI film rupture and improve the cycle life of individual battery cells.
[0251] In this embodiment, the second, third, and fourth additives can be tested using nuclear magnetic resonance spectroscopy. The specific procedure is as follows: 500 μl of deuterated reagent is added to an NMR tube in an argon-filled glove box. 100 μl of non-aqueous electrolyte sample is then added to the NMR tube. The NMR tube is shaken to dissolve the non-aqueous electrolyte in the deuterated reagent. The composition and mass of the electrolyte are tested using an Oxford Instruments X-Pulse benchtop NMR spectrometer. The method for obtaining the electrolyte sample is described above and will not be repeated here.
[0252] In some embodiments, the electrolyte includes an organic solvent, which includes cyclic carbonate solvents, including at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
[0253] Cyclic carbonate solvents have high dielectric constants and mainly play a role in dissociating lithium salts. This helps to increase the transport number of lithium ions, reduce the internal resistance of battery cells, and thus reduce the risk of increased lithium ion consumption due to higher battery cell temperatures, thereby improving the cycle life of battery cells.
[0254] In some embodiments, the cyclic carbonate solvent content is 20% to 40% by mass, based on the total mass of the organic solvent; for example, it can be 20%, 25%, 30%, 35%, 40%, or any value within the above range. This results in a electrolyte with suitable ionic conductivity, thereby giving the battery cell suitable fast-charging performance.
[0255] In some embodiments, the electrolyte includes an organic solvent, which includes linear carboxylic acid ester solvents, including at least one of methyl formate, methyl acetate, ethyl acetate, methyl butyrate, ethyl propionate, ethyl butyrate, butyl acetate, methyl propionate, and propyl butyrate.
[0256] The aforementioned linear carboxylic acid ester solvents have low viscosity and high ionic conductivity, which is beneficial for improving the fast charging performance of battery cells.
[0257] In addition, linear carbonate solvents have lower viscosity, which can compensate for the shortcomings of cyclic carbonate solvents, such as high viscosity, poor fluidity and wettability. By using linear carbonate solvents in combination with cyclic carbonate solvents, the electrolyte can achieve a balance between suitable viscosity and suitable ionic conductivity, which is beneficial for lithium-ion transport and facilitates the improvement of the fast-charging performance of battery cells.
[0258] In some embodiments, the mass content of the linear carboxylic acid ester solvent is 10% to 70% based on the total mass of the organic solvent, for example, it can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, or any value within the range above.
[0259] When the mass content of linear carboxylic acid ester solvent is greater than or equal to 10% based on the total mass of organic solvents, the electrolyte has lower viscosity and higher ionic conductivity, thus giving the battery cell better fast-charging performance. When the mass content of linear carboxylic acid ester solvent is less than or equal to 70% based on the total mass of organic solvents, the degree of side reactions of linear carboxylic acid ester solvents can be reduced, and the consumption of lithium ions caused by side reactions can be reduced, thereby helping to improve the cycle life of the battery cell.
[0260] In some embodiments, the electrolyte further includes a linear carbonate solvent, which includes at least one of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate.
[0261] In the embodiments of this application, the test methods for linear carbonate solvents, linear carboxylic acid ester solvents, and cyclic carbonate solvents can refer to the standard GB / T9722-2006 to quantitatively analyze the content of linear carbonates, cyclic carbonates, and linear carboxylic acid esters in the electrolyte using organic gas chromatography.
[0262] In some embodiments, the electrolyte comprises an electrolyte salt, which includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, and lithium difluorooxalateborate.
[0263] Lithium hexafluorophosphate is easily dissociated and moderately priced, making it suitable as a primary electrolyte salt in electrolyte solutions. Lithium difluorosulfonylimide, lithium bis(trifluoromethanesulfonylimide), lithium difluorophosphate, and lithium difluorooxalate borate have improved thermal stability and can be used as additives or partial substitutes for lithium hexafluorophosphate. They can also be reduced to LiF, which can form a more stable SEI film on graphite surfaces, thus improving the cycle life of individual battery cells. In addition, they can reduce the risk of HF attacking the positive electrode due to the hydrolysis of lithium hexafluorophosphate, leading to the dissolution of metal ions and damage to the SEI film of the negative electrode, further enhancing the cycle life of individual battery cells.
[0264] Figure 5 This is a schematic diagram of the structure of a battery cell according to an embodiment of this application. In one embodiment of this application, for example, referring to... Figure 5 As shown, the battery cell 3 includes a housing 31, an end cap assembly 32, and an electrode assembly 33. The housing 31 has an opening for accommodating the electrode assembly 33, and the end cap assembly 32 is used to close the opening. The electrode assembly 33 may include a positive electrode, a negative electrode, and a separator located between the positive electrode and the negative electrode.
[0265] The electrode assembly 33 can be prepared by a winding or stacking process from a positive electrode sheet, a negative electrode sheet, and an insulating element. As an example, the electrode assembly 33 is prepared by a winding process from a positive electrode sheet, a negative electrode sheet, and an insulating element.
[0266] In some embodiments, the end cap assembly 32 includes electrode terminals 322, such as Figure 5 As shown, the end cap assembly 32 includes two electrode terminals 322, one of which is a positive electrode terminal and the other is a negative electrode terminal.
[0267] The battery cell 3 also includes a connecting member 34 for connecting the tab 331 and the electrode terminal 322 of the electrode assembly 33. For example, one connecting member 34 is used to connect the tab of the positive electrode and the positive electrode terminal, and another connecting member 34 is used to connect the tab of the negative electrode and the negative electrode terminal.
[0268] [Positive electrode plate]
[0269] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0270] In some embodiments, the positive electrode active material may be a known positive electrode active material for batteries. As an example, the positive electrode active material may include one or more of the following materials: lithium phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides include, but are not limited to, lithium cobalt oxides (such as LiCoO2), lithium nickel oxides (such as LiNiO2), lithium manganese oxides (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (such as LiNi). 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also known as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also known as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also known as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also known as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also known as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi) 0.85 Co 0.1 Al 0.05 One or more of the following: O2) and its modified compounds. Examples of lithium phosphates with an olivine structure include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium iron phosphate and carbon composites, lithium manganese phosphate (such as LiMnPO4), lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, and lithium manganese iron phosphate and carbon composites.
[0271] During the charging and discharging process of a battery, Li undergoes insertion / extraction and consumption. The molar content of Li in the positive electrode active material varies depending on the discharge state. In the examples of positive electrode active materials in this application, the molar content of Li refers to the initial state of the material, i.e., the state before feeding. After charge-discharge cycles, the molar content of Li changes when the positive electrode active material is applied to the battery system. Similarly, the molar content of O in the examples of positive electrode active materials in this application is only an ideal value. Oxygen release from the crystal lattice causes changes in the molar content of O, and the actual molar content of O will fluctuate.
[0272] In some embodiments, the positive electrode film layer further includes a binder. As an example, the binder may include at least one selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0273] In some embodiments, the positive electrode film layer further includes a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0274] In one embodiment, the positive electrode sheet can be prepared by forming a positive electrode slurry using the components described above. For example, the positive electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., N-methylpyrrolidone) to form the positive electrode slurry. The positive electrode slurry is then coated onto a positive electrode current collector, and after drying, cold pressing, and other processes, the positive electrode sheet is obtained.
[0275] [Negative electrode plate]
[0276] In some embodiments, the negative electrode current collector can be a metal foil or a composite negative electrode current collector. The negative electrode current collector can be a copper foil. The composite negative electrode current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0277] The negative electrode film includes a negative electrode active material. The negative electrode active material can be any negative electrode active material known in the art for use in batteries. As an example, besides graphite, the negative electrode active material can include at least one of the following materials: soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. The silicon-based material can be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material can be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries can also be used. These negative electrode active materials can be used alone or in combination of two or more.
[0278] The negative electrode film layer may also optionally include a binder. As an example, the binder may include at least one of styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), water-soluble unsaturated resin SR-1B, waterborne acrylic resins (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0279] The negative electrode film may optionally include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0280] In one embodiment, the negative electrode sheet can be prepared by forming a negative electrode slurry using the components described above. For example, the negative electrode active material, conductive agent, binder, and any other components are dispersed in a solvent (e.g., deionized water) to form the negative electrode slurry. The negative electrode slurry is then coated onto a negative electrode current collector, and after drying, cold pressing, and other processes, the negative electrode sheet is obtained.
[0281] This application provides a battery device, including the battery cell in any of the above embodiments.
[0282] This application provides an electrical device including a battery cell or battery device as described in any of the above embodiments, wherein the battery cell or battery device is used to store or provide electrical energy.
[0283] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0284] [Example]
[0285] Example 1
[0286] (1) Preparation of negative electrode sheet
[0287] The negative electrode active material graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are mixed in a deionized water solvent system at a mass ratio of 96.5:0.5:1.8:1.2 to obtain a negative electrode slurry. The negative electrode slurry is uniformly coated on the negative electrode current collector copper foil, and then dried, cold-pressed, and slit to obtain the negative electrode sheet.
[0288] The graphite exhibits a specific capacity of 362 mAh / g, a volume average particle size (Dv50) of 16.2 μm, a volume particle size distribution (Dv90-Dv10) / Dv50 of 1.1, a degree of graphitization of 94.2%, and a powder compaction density of 2.0 g / cm³ under 50,000 N pressure. 3 Graphite includes artificial graphite with secondary particles.
[0289] With the battery cell at 0% SOC, the compaction density of the negative electrode film is 1.67 g / cm³. 3 The single-sided density of the negative electrode film is 9.0 mg / cm³. 2 .
[0290] (2) Preparation of positive electrode sheet
[0291] Lithium iron phosphate (LiFePO4), carbon black (CNY), and polyvinylidene fluoride (PVDF) (PVDF) binder were mixed thoroughly in an N-methylpyrrolidone (NMP) solvent system at a mass ratio of 97:0.7:2.3 to obtain a positive electrode slurry. This slurry was then uniformly coated onto an aluminum foil current collector, followed by drying, cold pressing, and slitting to obtain the positive electrode sheet. With the battery cell at 0% SOC, the compaction density of the positive electrode film was 2.55 g / cm³. 3 The single-sided density of the positive electrode film is 20.5 mg / cm³. 2 .
[0292] (3) Preparation of electrolyte
[0293] In an argon-atmospheric glove box (H2O content <10ppm, O2 content <1ppm), the electrolyte salt lithium hexafluorophosphate (LiPF6) was dissolved in a mixture of organic solvents ethylene carbonate (EC) and diethyl carbonate (DEC) and stirred until homogeneous. Then, a first additive, a second additive, and a third additive were added. The first additive included tris(4-fluorophenyl)phosphine, the second additive included vinylene carbonate (VC), and the third additive included 1,3-propanesulfonic acid lactone.
[0294] Based on the total mass of the electrolyte, the mass content of the first additive is 1.5%, the mass content of the second additive is 6%, and the mass content of the third additive is 0.5%. It should be noted that the mass contents of the first, second, and third additives mentioned here refer to the mass contents during the preparation process (before the battery cell formation).
[0295] Based on the total mass of the electrolyte, the mass content of the electrolyte salt LiPF6 is 12.5%, the mass content of EC is 25%, and the mass content of DEC is 54.5%.
[0296] (4) Separating membrane
[0297] The separator includes a base film, which is a polyethylene (PE) film with a thickness of 7 μm. An inorganic coating with a thickness of 2 μm is disposed on the side of the base film facing the negative electrode. The inorganic coating includes alumina ceramic particles.
[0298] (5) Preparation of battery cells
[0299] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to isolate them. This is then wound to form an electrode assembly. The tabs of the electrode assembly are connected to the end caps (e.g., by welding the tabs to the end caps using connecting components). The electrode assembly is placed in an aluminum casing and dried at 85°C for 6 hours. Electrolyte is then injected at an injection rate of 3.0 g / Ah. After vacuum sealing, settling, formation, and shaping, a battery cell is obtained. The formation process involves charging the battery cell to 30% State of Charge (SOC) at 0.04C.
[0300] Examples 2-4
[0301] The difference between Examples 2-4 and Example 1 is that the mass content of the first additive is different based on the total mass of the electrolyte.
[0302] Examples 5-8
[0303] The difference between Examples 5-8 and Example 1 is that the type of the first additive is different.
[0304] In Example 5, the first additive included tris(pentafluorophenyl)borane; in Example 6, the first additive included tris(pentafluorophenyl)borane and tris(4-fluorophenyl)phosphine; in Example 7, the first additive included triphenylphosphine; and in Example 8, the first additive included bis(2-trifluorophenyl)(3-sulfonylphenyl)phosphine.
[0305] Examples 9-13
[0306] The difference between Examples 9-13 and Example 1 is that the specific gravity of graphite is different.
[0307] Accordingly, graphite with different basis weights can correspond to different degrees of graphitization, volume average particle size Dv50, volume particle size distribution (Dv90-Dv10) / Dv50, and powder compaction density.
[0308] Example 14
[0309] The difference between Example 14 and Example 1 is that the graphite used is natural graphite. The specific capacity of the graphite is 367 mAh / g, the volume average particle size Dv50 is 17.5 μm, the volume particle size distribution (Dv90-Dv10) / Dv50 is 1.04, the degree of graphitization is 94.2%, and the powder compaction density of the graphite under 50000 N pressure is 1.9 g / cm³. 3 Graphite includes natural graphite with secondary particles.
[0310] With the battery cell at 0% SOC, the compaction density of the negative electrode film is 1.62 g / cm³. 3 The single-sided density of the negative electrode film is 9 mg / cm³. 2 .
[0311] Comparative Example 1
[0312] The difference between Comparative Example 1 and Example 1 is that the electrolyte does not contain the first additive.
[0313] Comparative Example 2
[0314] The difference between Comparative Example 2 and Example 1 is that the specific capacity of graphite is less than 360 mAh / g, specifically 350 mAh / g. In Comparative Example 2, the volume average particle size Dv50 of graphite is 10.5 μm, the volume particle size distribution (Dv90-Dv10) / Dv50 is 0.85, the degree of graphitization is 93.2%, and the powder compaction density of graphite under 50000 N pressure is 1.8 g / cm³. 3 .
[0315] Comparative Example 3
[0316] The difference between Comparative Example 3 and Example 1 is that the specific capacity of graphite is greater than 370 mAh / g, specifically 375 mAh / g. In Comparative Example 3, the volume average particle size Dv50 of graphite is 18 μm, the volume particle size distribution (Dv90-Dv10) / Dv50 is 1.06, the degree of graphitization is 97.6%, and the powder compaction density of graphite under 50000 N pressure is 2.05 g / cm³. 3 .
[0317] Table 1 Test data for the examples and comparative examples
[0318]
[0319] Table 2 Data from some embodiments
[0320]
[0321]
[0322] It should be noted that in Comparative Example 1, since no first additive was added, the type of the first additive, its mass content before and after formation are indicated by " / " in Table 1; in Comparative Examples 2 and 3, the main focus is on the effect of graphite specific capacity, therefore the mass content of the first additive after formation was not tested in Table 1, and the mass content of the first additive after formation is indicated by " / " in Table 1; in Examples 5-8, the type of the first additive is different from that in Example 1, and since the cycle life in Examples 5-8 is slightly shorter than that in Example 1, the mass content of the first additive after formation in Examples 5-8 was not tested, and the mass content of the first additive after formation in Examples 5-8 is indicated by " / " in Table 1; in Examples 9-14, the main focus is on the effect of graphite specific capacity on cycle life, therefore the mass content of the first additive after formation was not tested, and the mass content of the first additive after formation is indicated by " / " in Table 1.
[0323] In this embodiment, the cycle life of a battery cell can be represented by its cycle life. Cycle life is defined as the number of cycles a battery cell completes to 90% SOH (State of Health). The more cycles a cell completes, the longer its cycle life.
[0324] As shown in Examples 1-14 and Comparative Example 1, the addition of the first additive is beneficial to improving the cycle life of the battery cell. As shown in Examples 1 and Comparative Example 2, when the specific capacity of graphite is below 360 mAh / g, although the combination with the first additive results in a longer cycle life, the energy density of the battery cell is low. As shown in Examples 1 and Comparative Example 3, when the specific capacity of graphite is above 370 mAh / g, although the combination with the first additive results in a higher energy density, the cycle life of the battery cell is short. Therefore, by combining the first additive with graphite having a specific capacity between 360 mAh / g and 370 mAh / g, the battery cell achieves both higher energy density and a longer cycle life.
[0325] As shown in Examples 1-4, during the preparation of battery cells (before battery cell formation), when the mass content of the first additive is 0.5% to 8% based on the total mass of the electrolyte, the battery cells have a longer cycle life; during the preparation of battery cells (before battery cell formation), when the mass content of the first additive is 1.5% to 6% based on the total mass of the electrolyte, the battery cells have an even longer cycle life.
[0326] As shown in Examples 1-4, after the battery cell is formed, the battery cell has a longer cycle life when the mass content of the first additive is 0.001% to 3.6% based on the total mass of the electrolyte; and after the battery cell is formed, the battery cell has an even longer cycle life when the mass content of the first additive is 0.2% to 1.8% based on the total mass of the electrolyte.
[0327] As shown in Examples 1 and 5-8, the first additive comprising one or more components is beneficial for improving the cycle life of the battery cell. As shown in Examples 5-8, R in the first additive, including boron or phosphine, has a good effect on improving cycle life. As shown in Examples 5-7, setting a substituent (e.g., fluorine) on the benzene ring of the first additive is beneficial for further improving the cycle life of the battery cell. As shown in Example 5, when the number of fluorine substituents on each benzene ring is 5, the improvement in cycle life is small. This is because excessive fluorine substituents lead to an increase in HF, which in turn increases the risk of metal ion dissolution in the positive electrode active material. The risk of dissolved metal ions being reduced to elemental metals on the negative electrode side and thus damaging the SEI film increases, leading to increased lithium ion consumption.
[0328] As shown in Examples 9-14, when the specific capacity of graphite is 360mAh / g to 370mAh / g, combining it with the first additive is beneficial to improving the cycle life and energy density of the battery cell; and graphite with different specific capacities can correspond to different degrees of graphitization, volume average particle size Dv50, volume particle size distribution (Dv90-Dv10) / Dv50 and powder compaction density.
[0329] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
[0330] 1. Cycle life testing
[0331] At 25°C, charge the battery cell to 3.8V at a charging rate of 0.5C, then charge it to 0.05C at a constant voltage of 3.8V, let it stand for 10 minutes, and then discharge it to the discharge cutoff voltage (e.g., 2.0V) at a discharge rate of 0.33C, and let it stand for 10 minutes. One charge-discharge cycle is one cycle. The test is stopped when the capacity of the battery cell decays to 90% of the discharge capacity of the first cycle. This number is recorded as the number of cycles at 90% SOH. The more cycles, the longer the cycle life and the better the cycle performance.
[0332] 2. Energy density testing
[0333] At 25℃, the battery cell is charged at a constant current of 0.33C to the upper limit cutoff voltage of 3.8V, then charged at a constant voltage to a current of 0.05C, left to stand for 10 minutes, and then discharged at a constant current of 0.33C to the discharge cutoff voltage of 2.0V. The discharge capacity at this time is recorded and the discharge energy E0 is obtained, in Wh. The length, width and height of the battery cell are measured with calipers, and the volume V0 of the battery cell is calculated, in L. The volumetric energy density (Wh / L) = discharge energy E0 / volume V0 of the battery cell.
Claims
1. A battery cell, characterized in that, include: A negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, wherein the negative electrode active material comprises graphite, and the specific capacity of the graphite is 360 mAh / g to 370 mAh / g; An electrolyte comprising a first additive, the first additive comprising a compound of formula (I): Wherein, R includes at least one of B, P, and BOB, and X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of the following independently includes at least one of hydrogen, halogen, C1-C3 alkyl, C1-C3 alkoxy, halogen-substituted C1-C3 alkyl, nitro, sulfonic acid, and cyano.
2. The battery cell according to claim 1, characterized in that, The R includes one of boron or phosphine, and the X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 Each of these groups independently includes at least one of hydrogen, chlorine, bromine, fluorine, nitro, sulfonic acid, cyano, trifluoromethyl, trichloromethyl, tribromomethyl, methyl, ethyl, methoxy, and ethoxy.
3. The battery cell according to claim 1 or 2, characterized in that, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It consists of at least two different atoms and includes different heteroatoms.
4. The battery cell according to any one of claims 1-3, characterized in that, X 12 X 13 X 14 X 15 X 22 X 23 X 24 X 25 X 32 X 33 X 34 X 35 For hydrogen, X 11 X 21 X 31 Each of these groups independently includes at least one of the following: chlorine, bromine, fluorine, nitro, sulfonic acid, cyano, trifluoromethyl, trichloromethyl, tribromomethyl, methyl, ethyl, methoxy, and ethoxy.
5. The battery cell according to any one of claims 1-3, characterized in that, X 11 X 12 X 13 X 14 X 15 X 21 X 22 X 23 X 24 X 25 X 31 X 32 X 33 X 34 X 35 It contains 0 to 3 hydrogen atoms.
6. The battery cell according to any one of claims 1-3, characterized in that, The first additive includes at least one of 2,4,6-tris(4-fluorophenyl)cycloboroxane, tris(4-fluorophenyl)phosphine, tris(pentafluorophenyl)phosphine, tris(4-chlorophenyl)phosphine, triphenylphosphine, triphenylborane, tris(pentafluorophenyl)borane, and triphenylphosphine oxide.
7. The battery cell according to any one of claims 1-6, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is from 0.001% to 10%.
8. The battery cell according to claim 7, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 0.5% to 8%.
9. The battery cell according to claim 8, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 1.5% to 6%.
10. The battery cell according to claim 7, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is from 0.001% to 3.6%.
11. The battery cell according to claim 10, characterized in that, Based on the total mass of the electrolyte, the mass content of the first additive is 0.2% to 1.8%.
12. The battery cell according to any one of claims 1-11, characterized in that, In the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area at 53.8 ± 0.2 eV accounts for less than 45%.
13. The battery cell according to claim 12, characterized in that, In the X-ray photoelectron spectrum of lithium in the negative electrode, the peak area of the peak at 53.8±0.2 eV accounts for 10% to 40%.
14. The battery cell according to any one of claims 1-13, characterized in that, The graphite has a graphitization degree greater than or equal to 94%.
15. The battery cell according to any one of claims 1-14, characterized in that, The graphite has a graphitization degree of 94% to 96%.
16. The battery cell according to any one of claims 1-15, characterized in that, The volume average particle size Dv50 of the graphite is 14 μm to 18 μm.
17. The battery cell according to any one of claims 1-16, characterized in that, The volumetric particle size distribution (Dv90-Dv10) / Dv50 of the graphite is 0.9 to 1.
25.
18. The battery cell according to any one of claims 1-17, characterized in that, The graphite comprises secondary particles.
19. The battery cell according to any one of claims 1-18, characterized in that, The graphite includes at least one of artificial graphite and natural graphite.
20. The battery cell according to any one of claims 1-19, characterized in that, The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including the negative electrode active material, and the negative electrode sheet satisfies at least one of the following conditions: The compaction density of the negative electrode film is 1.62 g / cm³. 3 Up to 1.77 g / cm 3 ; The porosity of the negative electrode sheet is 25% to 60%; The one-sided density of the negative electrode film is 7 mg / cm³. 2 Up to 12 mg / cm 2 .
21. The battery cell according to claim 20, characterized in that, The negative electrode sheet satisfies at least one of the following conditions: The compaction density of the negative electrode film is 1.62 g / cm³. 3 Up to 1.68 g / cm 3 ; The porosity of the negative electrode sheet is 25% to 35%; The single-sided density of the negative electrode film is 8 mg / cm³. 2 Up to 10 mg / cm 2 .
22. The battery cell according to any one of claims 1-21, characterized in that, The battery cell includes a positive electrode sheet, the positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side surface of the positive current collector, the positive electrode film layer includes a positive electrode active material, and the positive electrode active material includes lithium phosphate.
23. The battery cell according to claim 22, characterized in that, At least a portion of the surface of the lithium phosphate has a carbon coating.
24. The battery cell according to claim 22 or 23, characterized in that, The lithium-containing phosphate includes components having the following general formula: Li m Fe x P y O j Q q Wherein, Q includes at least one of Al, Na, K, Mg, Cu, Mn, Cr, Zn, Pb, Ca, Co, Ni, Sr, Nb, V, Ti, B, S, Si, N, F, Cl, and Br, with 0.8≤m≤1.15, 0.9≤x≤1, 0.95≤y≤1, 3.5≤j≤4, and 0<q≤0.
1.
25. The battery cell according to any one of claims 22-24, characterized in that, The specific capacity of the positive electrode active material is from 135 mAh / g to 150 mAh / g.
26. The battery cell according to any one of claims 22-25, characterized in that, The positive electrode film layer satisfies at least one of the following conditions: The compaction density of the positive electrode film is 2.52 g / cm³. 3 Up to 2.78 g / cm 3 ; The areal density of one side of the positive electrode film is 12 mg / cm³. 2 Up to 22 mg / cm 2 .
27. The battery cell according to any one of claims 1-26, characterized in that, The electrolyte further includes at least one of a second additive and a third additive, wherein the second additive includes a carbonate additive and the third additive includes a sulfur-containing additive.
28. The battery cell according to claim 27, characterized in that, The carbonate additives include at least one of vinylene carbonate and fluoroethylene carbonate.
29. The battery cell according to claim 27 or 28, characterized in that, The sulfur-containing additive includes at least one of vinyl sulfate, vinyl disulfate, butene sulfite, 1,3-propanesulfonate lactone, vinyl sulfite, and methylene disulfonate.
30. The battery cell according to any one of claims 27-29, characterized in that, Based on the total mass of the electrolyte, the sum of the mass contents of the second additive and the third additive is 0.5% to 10%.
31. The battery cell according to claim 30, characterized in that, Based on the total mass of the electrolyte, the mass content of the second additive and the third additive is 2% to 8%.
32. The battery cell according to any one of claims 1-31, characterized in that, The electrolyte further includes a fourth additive, which includes a lithium salt additive, and the lithium salt additive includes at least one of lithium difluorophosphate, lithium difluorooxalate borate, lithium tetrafluoroborate, and lithium dioxalate borate.
33. The battery cell according to any one of claims 1-32, characterized in that, The electrolyte includes an organic solvent, which includes cyclic carbonate solvents, and the cyclic carbonate solvents include at least one of ethylene carbonate, propylene carbonate, and butene carbonate.
34. The battery cell according to claim 33, characterized in that, Based on the total mass of the organic solvents, the mass content of the cyclic carbonate solvents is 20% to 40%.
35. The battery cell according to any one of claims 1-34, characterized in that, The electrolyte includes an organic solvent, which includes linear carboxylic acid ester solvents, including at least one of methyl formate, methyl acetate, ethyl acetate, methyl butyrate, ethyl propionate, ethyl butyrate, butyl acetate, methyl propionate, and propyl butyrate.
36. The battery cell according to claim 35, characterized in that, Based on the total mass of the organic solvents, the mass content of the linear carboxylic acid ester solvent is 10% to 70%.
37. The battery cell according to any one of claims 1-36, characterized in that, The electrolyte comprises an electrolyte salt, which includes at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, and lithium difluorooxalateborate.
38. A battery device, characterized in that, include: Multiple battery cells according to any one of claims 1-37.