A molecularly induced electrolyte for suppressing the Ginger-Taylor effect in lithium-rich manganese cathodes
By introducing functional inducing additives into the electrolyte to form coordination bonds with Mn3+, the cathode material is stabilized, solving the Gyntelle distortion problem of lithium-rich manganese cathode materials and improving the structural stability and cycle performance of the battery.
Patent Information
- Application Number
- CN202611152615.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot reduce the Jan Taylor distortion in lithium-rich manganese cathode materials from a thermodynamic perspective, leading to structural instability, severe manganese dissolution and interfacial reactions, which affect battery life and performance.
Functional inducing additives, such as phosphonates, silanized phosphate derivatives, and nitrogen-containing multidentate ligands, are introduced into the electrolyte to stabilize Mn3+ through molecular coordination, inhibit Ginger-Tyler distortion, and form a stable interfacial film.
It effectively suppresses lattice distortion, reduces manganese dissolution, improves battery structural stability and cycle life, maintains battery energy density, and improves cycle performance at high rates.
Smart Images

Figure CN123120883A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, and more specifically, relates to a molecularly induced electrolyte that suppresses the Jan Taylor effect in lithium-rich manganese cathodes. Background Technology
[0002] Lithium-rich manganese-based cathode materials (general formula: xLi₂MnO₃·(1-x)LiMO₂, where M = Mn, Ni, Co, etc.) are considered highly promising cathode materials for next-generation high-energy-density lithium-ion batteries due to their high specific capacity (>250 mAh / g) and high operating voltage. However, their commercial application is severely constrained by a series of problems, among which the Jamette effect of manganese (Mn) ions is one of the key bottlenecks. The Jamette effect refers to the phenomenon where high-spin Mn... 3+ In the presence of an octahedral coordination field, to reduce the system energy, the octahedral structure undergoes spontaneous distortion (elongation or flattening), causing the crystal structure to decrease from cubic symmetry to tetragonal symmetry. In lithium-rich manganese-based cathode materials, with increasing charging depth, Mn... 3+ Increased JT content can lead to severe JT distortion, resulting in: crystal structure deterioration, dissolution of transition metal ions, intensified interfacial side reactions, and phase transition caused by oxygen loss.
[0003] To address the aforementioned issues, several innovative strategies were proposed, primarily including electrolyte optimization and interface control, and direct control of Mn. 3+ The local electronic structure and coordination field of the cathode material, as well as the modification of the cathode material (coating, surface modification), are considered, among which electrolyte optimization and interface control are the most direct and flexible strategies. Zhang et al. proposed an additive, trimethyl borate (TMB), which is paired with a commercial carbonate electrolyte to construct a highly conductive fluorine-rich and boron-rich interface on the solid electrolyte interface (SEI / CEI). Using a general electrolyte of 1 wt% TMB, a 4.7V lithium-ion battery can be stably cycled for more than 100 cycles with 70% capacity retention (Journal of Energy Chemistry, 2024, 92, 639-647). Wang et al. designed an inherently non-flammable electrolyte using 1M lithium difluorooxalate borate (LiDFOB) in triethyl phosphate (TEP) and N-methyl-N-propyl-pyrrolidine bis(trifluoromethanesulfonyl)imine ionic liquids. Unique Li + The solvation structure can induce a stable anion-derived electrolyte / electrode interface, effectively suppressing lithium dendrite growth and side reactions between the TEP and the electrode. LiNi using this electrolyte... 0.9 Co 0.05 Mn 0.05O2-encapsulated (NCM90) / Li-encapsulated batteries provide stable cycling even at 4.5V and 60°C. Furthermore, the 2.2Ah NCM90 / Li pouch cell simultaneously exhibits outstanding safety, consistently passing nail penetration tests, and a high gravimetric energy density of 470Wh / kg at 4.4V (Advanced Functional Materials, 2023, 33, 2215065).
[0004] Patent CN120767412A discloses a battery electrolyte additive suitable for manganese-based cathodes, comprising an electron-donating compound and a coordinating compound. The electron-donating compound is a nitrile compound or a phosphate ester compound; the coordinating compound is a heterocyclic compound, a fluorophosphate ester compound, or a fluorocarbonate compound.
[0005] Existing patented technologies primarily target the overall interface of the cathode material. Through interfacial reactions or adsorption, a more stable CEI film is formed. This film physically isolates the electrolyte from the active material, thus mitigating the consequences of the JT effect and manganese leaching. However, it lacks precise targeting of Mn... 3+ It itself forms chemical coordination bonds, directly altering Mn 3+ The local electron cloud distribution and ligand field environment cannot fundamentally weaken the driving force of JT distortion, thus "suppressing" rather than "alleviating" JT distortion. This invention introduces a certain amount of compounds with electron-donating centers or coordination capabilities as additives into the electrolyte system of a battery containing a manganese-based cathode. Through interfacial chemical regulation, it can effectively alleviate problems such as the Jan Taylor effect and manganese dissolution that occur in manganese-based batteries during charge-discharge cycles, limiting structural collapse caused by repeated volume changes, thereby significantly extending battery life and improving battery charge-discharge capacity and cycle performance. Summary of the Invention
[0006] To address the aforementioned technical problems, this invention provides a molecularly induced electrolyte that suppresses the Jan Taylor effect in lithium-rich manganese cathodes, thus solving the problem that existing molecularly induced electrolytes lack precise interaction with Mn. 3+ It itself forms chemical coordination bonds, directly altering Mn 3+ The local electron cloud distribution and ligand field environment cannot fundamentally reduce the technical problem of JT distortion.
[0007] The purpose and effect of the molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes of the present invention are achieved by the following specific technical means: A molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes comprises a lithium salt, an organic solvent, and a functional inducing additive; the functional inducing additive is an organic compound capable of coordinating with manganese ions, which stabilizes Mn in the cathode material through molecular coordination. 3+ To suppress the Ginger-Tyler aberration.
[0008] In a preferred embodiment, the functional inducing additive includes one or more functional groups selected from phosphonic acid, phosphate ester, polydentate nitrogen-containing heterocycle, amino, carboxyl, or crown ether structures.
[0009] In a preferred embodiment, the functional inducing additive is selected from one or more combinations of the following compound classes: phosphonates, silanized phosphate derivatives, nitrogen-containing polydentate ligands, amino acid compounds, crown ethers or azacrown ethers.
[0010] In a preferred embodiment, the phosphonate compound is dimethyl methylphosphonate or diethyl vinylphosphonate, the silanized phosphate derivative is tris(trimethylsilane) phosphate, the nitrogen-containing polydentate ligand is 1,10-phenanthroline or 2,2'-bipyridine and its derivatives, the amino acid compound is glycine or alanine, and the crown ether or azacrown ether compound is 18-crown-6-ether or 1,4,7-triazacyclononane.
[0011] In a preferred embodiment, the functional inducing additive has a mass percentage concentration of 0.1% to 5.0% in the electrolyte, preferably 0.5% to 2.0%.
[0012] In a preferred embodiment, the lithium salt is one or more of lithium hexafluorophosphate, lithium difluorosulfonylimide, lithium difluorophosphate, lithium tetrafluoroborate, and lithium perchlorate, and the molar concentration of the lithium salt is from 0.8 mol / L to 1.5 mol / L.
[0013] In a preferred embodiment, the organic solvent is a mixture of two or more of cyclic carbonates, chain carbonates, carboxylic acid esters, and ether solvents; the cyclic carbonates include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate; and the chain carbonates include dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate.
[0014] A lithium-ion battery includes a positive electrode, a negative electrode, a separator, and a molecularly induced electrolyte as described in any one of claims 1 to 7.
[0015] In a preferred embodiment, the positive electrode comprises a lithium-rich manganese-based positive electrode material, the general formula of which is: , where M is one or more of Mn, Ni, Co, Al, Fe, Cr, Ti, Zr, and Ru, and 0 < x < 1, and M contains at least the element Mn; The diaphragm is one or more of PP diaphragm, glass fiber diaphragm, and PI electrospun diaphragm; The conductive agent is one or more of acetylene black, Super (including P), and graphene.
[0016] An application of a functional inducing additive in the preparation of a molecularly induced electrolyte, wherein the application is to use the functional inducing additive to suppress the Jamin-Taylor effect in lithium-rich manganese-based cathode materials.
[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. Functional inducing additives interact with Mn in the cathode material through the functional groups in their molecular structure. 3+ Direct strong coordination occurs, regulating Mn at the atomic / molecular level. 3+ The local coordination field and electron configuration directly weaken the Jeunesse-Taylor driving force that causes distortion of the octahedral structure of the crystal from a thermodynamic perspective. This effect can effectively suppress structural distortion and internal stress accumulation of the crystal lattice under deep lithium-ion insertion / extraction conditions, fundamentally improve the reversibility of the bulk structure of LRM materials, avoid irreversible structural collapse of materials during cycling, and improve the structural stability of lithium-rich manganese-based cathode materials.
[0018] 2. The molecularly induced stabilizing layer formed by functional inducing additive molecules on the surface of lithium-rich manganese-based cathodes can tightly anchor Mn ions and reduce Mn content. 3+ The dissolution kinetics rate is reduced, decreasing the dissolution of transition metal ions from the cathode material. This mitigates the damage to the SEI caused by dissolved manganese ions migrating to the anode, reducing irreversible lithium loss and continuous electrolyte consumption, thereby extending the cycle life of the full battery. Furthermore, the additives of this invention, while functioning as coordination stabilizers, can synergistically interact with the base lithium salt and organic solvents to construct a thin and dense CEI layer. This interfacial film, rich in organic and inorganic composite components, possesses good mechanical stability, adapting to volume changes in the cathode material during charge and discharge, and exhibits excellent lithium-ion conductivity, helping to reduce the interfacial impedance between the electrode and electrolyte and improving the battery's cycle performance under high-rate conditions.
[0019] 3. The average discharge voltage decay of lithium-rich manganese-based cathode materials during cycling is mainly due to irreversible phase transitions occurring within the material. JT distortion is a significant contributing factor to these irreversible phase transitions. By suppressing JT distortion at its source, the process of irreversible phase transitions within the cathode material can be slowed down, reducing the decrease in electrochemical activity caused by phase transitions. LRM batteries using the electrolyte of this invention can better maintain their average discharge voltage level during long-term cycling, thereby effectively maintaining the battery's energy density and improving its performance over long-term use. Attached Figure Description
[0020] Figure 1 This is a schematic diagram comparing the impedance of Embodiment 1 and Comparative Example 1 in this invention; Figure 2 This is a cyclic curve diagram of Embodiment 2 and Comparative Example 1 in this invention. Detailed Implementation
[0021] The embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are used to illustrate the technical solutions of the present invention, but should not be used to limit the scope of protection of the present invention.
[0022] Example 1:
[0023] As attached Figures 1 to 2 As shown: This invention provides a molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes. The electrolyte comprises a lithium salt, an organic solvent, and a functional inducing additive. The lithium salt dissociates in the organic solvent to generate migratable lithium ions, providing charge carriers for the battery's charge and discharge processes and ensuring sufficient charge and discharge capacity. The organic solvent dissolves the lithium salt and the functional inducing additive, and also serves as a continuous medium for lithium ion transport, adjusting the electrolyte's viscosity, dielectric constant, and liquid temperature range. The functional inducing additive is an organic compound capable of coordinating with manganese ions, stabilizing Mn in the cathode material through molecular coordination. 3+ To suppress Gingeryl distortion, functional inducing additives include one or more functional groups from the following structures: phosphonic acid group, phosphate ester group, polydentate nitrogen-containing heterocycle, amino group, carboxyl group, or crown ether group. All of these functional groups contain heteroatoms that can provide lone pair electrons and can react with Mn. 3+ The empty orbitals form stable coordinate bonds, enabling the control of Mn 3+ Targeted binding and electronic structure regulation.
[0024] Functional inducing additives are selected from one or more combinations of the following compound categories: phosphonates, silanized phosphate derivatives, nitrogen-containing multidentate ligands, amino acid compounds, crown ethers or azacrown ethers. Different categories of compounds can be combined to form multifunctional synergistic coordination systems, covering Mn in different coordination environments on the cathode surface. 3+ Sites that improve overall stability.
[0025] Phosphonate esters, such as dimethyl methylphosphonate or diethyl vinylphosphonate, exhibit good electrolyte compatibility and moderate coordination strength, enabling them to form a uniform adsorption layer on the cathode surface. Silanized phosphate derivatives, such as tris(trimethylsilane)phosphate, possess silane groups that enhance the compound's oxidation resistance and interfacial film-forming ability. Nitrogen-containing polydentate ligands, such as 1,10-phenanthroline or 2,2'-bipyridine and their derivatives, have polydentate coordination sites that can bind with Mn. 3+ To form a chelating structure and enhance coordination stability, the amino acid compounds are glycine or alanine. These compounds contain both amino and carboxyl bifunctional groups, which can improve compatibility with the electrode surface. Crown ethers or aza-crown ethers are 18-crown-6-ethers or 1,4,7-triazacyclononanes. These compounds have a cavity structure of a specific size, which can selectively chelate Mn. 3+ ion.
[0026] In this embodiment, the electrolyte is prepared in an argon-filled glove box with a water and oxygen content of less than 0.5 ppm. First, cyclic carbonate and chain carbonate in a preset ratio are mixed evenly to obtain a base solvent. Lithium salt is added to the base solvent and stirred until completely dissolved to form a base electrolyte. Then, a preset mass percentage of functional inducing additive is added to the base electrolyte and stirred at a constant speed until the additive is completely dissolved to obtain a clear and transparent molecularly induced electrolyte. The prepared electrolyte is sealed and stored in an argon-filled glove box to prevent deterioration due to contact with moisture and oxygen.
[0027] Furthermore, functional inducing additives interact with Mn in the cathode material through the functional groups in their molecular structure. 3+ Direct strong coordination occurs, regulating Mn at the atomic / molecular level. 3+ The local coordination field and electron configuration directly weaken the Jeunesse-Taylor driving force that causes distortion of the octahedral structure of the crystal from a thermodynamic perspective. This coordination effect occurs dynamically with the battery charge-discharge cycle and can continuously stabilize the newly generated Mn during the cycle. 3+The presence of ions effectively suppresses structural distortion and internal stress accumulation in the lattice during deep lithium-ion insertion / extraction, fundamentally improving the reversibility of the bulk structure of LRM materials, preventing irreversible structural collapse during cycling, and enhancing the structural stability of lithium-rich manganese-based cathode materials. At the same time, the stable coordination structure reduces the release of lattice oxygen on the cathode surface, suppresses interfacial side reactions between the electrolyte and the cathode active material, reduces the rate of increase in interfacial impedance, and ensures the long-cycle performance of the battery.
[0028] The functional inducing additive has a mass percentage concentration of 0.1% to 5.0% in the electrolyte, and this concentration range is based on the Mn content in the lithium-rich manganese-based cathode material. 3+ The content and coordination requirements of the additive, as well as the overall electrochemical performance of the electrolyte, determine the optimal concentration. When the additive concentration is below 0.1%, the number of functional groups in the electrolyte that can participate in coordination is insufficient, making it impossible to coordinate the Mn atoms on the cathode surface and near the surface. 3+ While effective coverage and stability are achieved, it's difficult to suppress the effects of Ginger-Taylor distortion. When the additive concentration exceeds 5.0%, it leads to an increase in electrolyte viscosity, reducing the migration rate of lithium ions in the electrolyte. Simultaneously, excessive additives can cause over-decomposition on the electrode surface, forming an excessively thick interfacial layer, increasing the interfacial impedance between the electrode and the electrolyte, and affecting the battery's rate performance. A concentration range of 0.5% to 2.0% is preferred, as this range ensures adequate coverage of Mn. 3+ While forming sufficient and stable coordination, the electrolyte maintains suitable physicochemical properties and electrochemical performance, avoiding negative impacts on the battery's charge / discharge capacity and rate characteristics. The lithium salt is one or more of lithium hexafluorophosphate, lithium difluorosulfonylimide, lithium difluorophosphate, lithium tetrafluoroborate, and lithium perchlorate. Lithium hexafluorophosphate can form a stable solid electrolyte interface film on the negative electrode surface, while also possessing moderate ionic conductivity and cost advantages. Lithium difluorosulfonylimide exhibits high thermal stability and oxidation resistance, improving electrolyte stability under high-voltage conditions. Lithium difluorophosphate can participate in the positive and negative electrode interfaces. The formation of the membrane improves interfacial compatibility. Lithium tetrafluoroborate has good low-temperature performance, which can broaden the operating temperature range of the electrolyte. Lithium perchlorate has a high degree of dissociation, which can provide sufficient lithium-ion carriers for the electrolyte. The molar concentration of lithium salt is 0.8 mol / L to 1.5 mol / L. This concentration range can ensure that the electrolyte has a sufficient lithium-ion concentration to meet the charge transport requirements during battery charging and discharging. At the same time, it avoids the problems of excessively high lithium salt concentration leading to excessive electrolyte viscosity and decreased lithium-ion migration rate, or insufficient electrolyte conductivity and increased interfacial impedance due to excessively low concentration.
[0029] The organic solvent is a mixture of two or more of cyclic carbonates, chain carbonates, carboxylic acid esters, and ether solvents. Cyclic carbonates include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate. Cyclic carbonates have a high dielectric constant, which can effectively promote the dissociation of lithium salts and participate in the formation of a solid electrolyte interfacial film on the electrode surface. Chain carbonates include dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate. Chain carbonates have a low viscosity, which can reduce the overall viscosity of the electrolyte and increase the migration rate of lithium ions. Carboxylic acid ester solvents have a wide liquid temperature range, which can improve the low-temperature performance of the electrolyte. Ether solvents have good solvation ability, which can optimize the solvation structure of lithium ions. Mixing multiple organic solvents in different proportions can synergistically adjust the dielectric constant, viscosity, liquid temperature range, and interfacial film-forming properties of the electrolyte, so that the electrolyte can simultaneously meet the requirements of ionic conductivity, thermal stability, electrochemical stability, and low-temperature performance.
[0030] Specifically, the electrolyte preparation was carried out in an argon-filled glove box with a water and oxygen content of less than 0.5 ppm. First, a dry, clean glass container was placed inside the glove box. Fluoroethylene carbonate (FEC) and ethyl propionate (EP) were measured and added to the glass container at a 1:2 volume ratio. The mixture was stirred at a constant speed until the two solvents were completely miscible, resulting in a clear and transparent mixed solvent. FEC enhances the intrinsic antioxidant stability of the electrolyte and participates in the formation of the positive electrode surface interfacial film. Ethyl propionate reduces the overall viscosity of the mixed solvent, improving the lithium-ion migration rate and the low-temperature performance of the electrolyte. Then, 2M lithium bis(fluorosulfonyl)imide (LiFSI) was slowly added to the mixed solvent while stirring at a constant speed to avoid localized mixing. Excessive lithium salt concentration can lead to uneven dissolution or clumping. Stirring is continued until the lithium salt is completely dissolved, resulting in a homogeneous and transparent basic electrolyte. Lithium difluorosulfonylimide, as a lithium salt, can fully dissociate in the mixed solvent, providing migratable lithium-ion carriers for the battery charging and discharging process, while also improving the electrolyte's thermal stability and oxidation resistance. Then, 1.0 wt% dimethyl methylphosphonate is added to the basic electrolyte, and stirring is continued at 500 rpm until the dimethyl ... 3+ Strong coordination occurs, stabilizing Mn 3+ It can influence the electronic structure and coordination environment of the electrode, suppress the occurrence of Ginger-Taylor distortion, and participate in the construction of the interface film on the positive electrode surface, thereby improving the interfacial compatibility between the electrode and the electrolyte.
[0031] A lithium-ion battery includes a positive electrode, a negative electrode, a separator, and a molecularly induced electrolyte. The positive electrode serves as the site of the redox reaction, releasing lithium ions during charging and inserting them during discharging, thus achieving the interconversion of electrical energy and chemical energy. The negative electrode receives and stores lithium ions during charging and releases them during discharging, working in conjunction with the positive electrode to complete the battery's charge-discharge cycle. The separator physically separates the positive and negative electrodes, preventing direct contact and internal short circuits. Its porous structure also adsorbs and retains the electrolyte, providing a continuous channel for lithium ion transport. The molecularly induced electrolyte, acting as an ion transport medium, fills the gaps between the positive, separator, and negative electrodes, providing a pathway for lithium ion migration between the electrodes. It also participates in the formation of the interfacial film on the electrode surface, regulating the interfacial reaction between the electrode and the electrolyte. The positive electrode comprises a lithium-rich manganese-based positive electrode material, a conductive agent, and a binder. The general formula for the lithium-rich manganese-based positive electrode material is... Where M is one or more of Mn, Ni, Co, Al, Fe, Cr, Ti, Zr, and Ru, and 0 < x < 1, and M contains at least the element Mn. The (1-x)LiMO2 phase can provide additional specific capacity to the cathode material, improving the energy density of the battery. The (1-x)LiMO2 phase can maintain the crystal structure stability of the material, ensuring the cycle performance of the battery. Combinations of different transition metal elements can regulate the electronic structure and electrochemical activity of the material, adapting to different battery performance requirements. The separator is one or more of PP separator, glass fiber separator, and PI electrospun separator. PP separator has good chemical stability and mechanical strength, and low cost, meeting the usage requirements of conventional lithium-ion batteries. Glass fiber separator has high liquid absorption and retention capacity, and excellent high-temperature resistance, adapting to the battery usage requirements under high-temperature conditions. PI electrospun separator has high... Porosity and mechanical strength can improve electrolyte retention and battery safety. The conductive agent is one or more of acetylene black, SuperP, and graphene. The conductive agent is used to build continuous electron transport channels between the positive electrode active material particles and between the active material and the current collector, thereby improving the electronic conductivity of the positive electrode and reducing the internal resistance of the battery. Acetylene black has low cost and good conductivity, SuperP has high specific surface area and dispersibility, and graphene has excellent electronic conductivity and layered structure, which can form a continuous conductive network. The binder is used to bond the positive electrode active material particles and the conductive agent together and attach them to the surface of the current collector to ensure the mechanical strength and structural integrity of the positive electrode.
[0032] Specifically, the positive electrode preparation process involves preparing the positive electrode active material Li... 1.16 Ni 0.2 Co 0.08 Mn 0.56O2, a composite conductive agent composed of graphene and SuperP in a 1:1 mass ratio, and PVDF binder are added to NMP solvent in a 95:2.5:2.5 mass ratio. The mixture is stirred at a constant speed until a uniform, particle-free positive electrode slurry is formed. The positive electrode slurry is then uniformly coated onto the surface of an aluminum foil current collector, which collects electrons generated by the positive electrode and transmits them to an external circuit. The coated aluminum foil is dried in a vacuum oven to remove the NMP solvent, and then rolled to obtain a positive electrode sheet with a certain compaction density. The negative electrode uses a graphite negative electrode or a silicon-based composite negative electrode, and its preparation process is similar to that of the positive electrode, using copper foil as the current collector and a polyimide (PI) electrospun separator. The prepared positive electrode sheet, separator, and negative electrode sheet are stacked sequentially, with the active material side of the positive electrode sheet and the active material side of the negative electrode sheet facing the two sides of the separator, respectively. CR2O3 is placed in an argon-filled glove box with a water and oxygen content of less than 0.5 ppm. In the Type 2 battery case, 65 μL of the molecularly induced electrolyte prepared above was added dropwise to fully wet the electrode and separator. Then, the case was sealed to complete battery assembly. The assembled battery was left to stand at room temperature for 12 hours. This standing process allows the electrolyte to fully penetrate into the internal pores of the positive and negative electrode plates, ensuring the continuity of the lithium-ion transport channels and promoting the formation of an initial interface layer between the electrodes and the electrolyte. The charge and discharge voltage range of the battery was set to 2.0-4.8V. This voltage range can fully utilize the high specific capacity characteristics of the lithium-rich manganese-based cathode material while avoiding excessive decomposition of the electrolyte due to excessive voltage. Long-cycle testing was conducted at a 1C rate. The 1C rate represents the current density at which the battery completes a full charge or full discharge within 1 hour. The long-cycle test is used to evaluate the battery's capacity retention and cycle stability during multiple charge and discharge cycles. After 100 cycles, the battery capacity was 210 mAh / g, with a capacity retention rate of 87.5%.
[0033] Furthermore, the molecularly induced stabilizing layer formed by functional inducible additive molecules on the surface of the lithium-rich manganese-based cathode can tightly anchor Mn ions and reduce Mn content. 3+The dissolution kinetics rate is reduced, decreasing the dissolution of transition metal ions from the cathode material lattice. This mitigates the reduction reaction and deposition of dissolved manganese ions on the anode surface after migration, preventing the deposited manganese ions from damaging the solid electrolyte interphase (SEI) film on the anode surface. This reduces irreversible loss of active lithium and continuous electrolyte consumption caused by SEI film rupture and reformation, thereby extending the cycle life of the full battery. Furthermore, the additive of this invention, while playing a coordination stabilizing role, can synergistically work with the basic lithium salt and organic solvent to participate in the construction of a thin and dense cathode electrolyte interphase (CEI) film on the cathode surface. This interphase film is rich in organic and inorganic composite components. The organic components provide a certain degree of flexibility, while the inorganic components provide good mechanical strength and ion conductivity, enabling the interphase film to adapt to the volume changes of the cathode material during charging and discharging, preventing the interphase film from rupturing and failing. At the same time, it has excellent lithium-ion conductivity, which helps to reduce the interfacial impedance between the electrode and the electrolyte, reduce energy loss during lithium-ion transport, and improve the cycle performance and charge-discharge efficiency of the battery under high-rate conditions.
[0034] The application of a functional inducing additive in the preparation of molecularly induced electrolytes utilizes the functional inducing additive to suppress the Ginger-Taylor effect in lithium-rich manganese-based cathode materials.
[0035] Example 2:
[0036] 1. Electrolyte; Prepare a locally high-concentration electrolyte solution according to the LiTFSI: DMC ratio of 1:2.2 (molar ratio), and then add... Dissolve 0.8 wt% of 1,10-phenanthroline by stirring at 500 rpm.
[0037] 2. Battery (positive electrode, separator, electrolyte); Positive electrode: Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.
[0038] The conductive agent is Ketjen Black, and the PVDF binder is 94:3:3.
[0039] Diaphragm: PP diaphragm.
[0040] The electrode sheets and the prepared electrolyte (80 μL) were assembled into a CR2032 battery and allowed to stand for 12 hours. The battery's charge / discharge voltage range was 2.0–4.8 V, and charge / discharge tests were conducted at 0.5 C. After 200 cycles, the battery's capacity was 229 mAh / g, with a capacity retention of 92.3%.
[0041] Example 3:
[0042] 1. Electrolyte; Dissolve 1.0 M LiODFB in a 3:7 mixture of ethylene carbonate (EC) and ethyl acetate (EA) by volume, then add 1.5 wt% tris(trimethylsilane) phosphate and 0.5 wt% 2,2'-bipyridine, and stir at 500 rpm to dissolve.
[0043] 2. Battery (positive electrode, separator, electrolyte); Positive electrode: Li 1.2 Mn 0.6 Ni 0.2 O2.
[0044] The conductive agent is Super P, and the PVDF binder is 96:2:2.
[0045] Diaphragm: 9μm polyethylene (PE) diaphragm.
[0046] The electrode sheets and the prepared electrolyte (55 μL) were assembled into a CR2032 battery and allowed to stand for 12 h to ensure complete immersion. The battery's charge / discharge voltage range was 2.0–4.8 V, and long-term cycling tests were conducted at a high rate of 2 C. After 300 cycles, the battery's capacity was 185 mAh / g, with a capacity retention of 82.2%.
[0047] Example 4:
[0048] 1. Electrolyte; 1.2 M LiPF6 was dissolved in a mixed solvent of fluoroethylene carbonate (FEC) and succinate (SN) in a volume ratio of 2:8, and then 0.2 wt% of diethyl vinylphosphonate was added. The mixture was stirred at 500 rpm to dissolve.
[0049] 2. Battery (positive electrode, negative electrode, separator, electrolyte); Positive electrode: Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.
[0050] The conductive agent is a composite of carbon nanotubes (CNT) and acetylene black (1:4), and the PVDF binder is (96:2:2).
[0051] Separator: Polyimide (PI) electrospun separator.
[0052] The electrode sheets and the prepared electrolyte (60 μL) were assembled into a CR2032 battery and allowed to stand for 12 h. The battery's charge / discharge voltage range was 2.0–4.8 V, and long-cycle testing was conducted at a 0.5 C rate. After 100 cycles, the battery's capacity was 203 mAh / g, with a capacity retention of 85.3%.
[0053] Example 5:
[0054] 1. Electrolyte; 1.5 M LiFSI was dissolved in a 1:1 mixture of perfluoro-2-propoxypropane (FPP) and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE), and then 1.0 wt% glycine was added. The mixture was stirred at 600 rpm to dissolve.
[0055] 2. Battery (positive electrode, separator, electrolyte); Positive electrode: Li3PO4 nanoparticles coated on the surface 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.
[0056] The conductive agent is acetylene black, and the binder is PVDF (96:2:2).
[0057] Diaphragm: Glass fiber diaphragm.
[0058] The electrode sheets and the prepared electrolyte (70 μL) were assembled into a CR2032 battery and allowed to stand for 24 h. The battery's charge / discharge voltage range was 2.0–4.8 V, and long-cycle testing was conducted at 0.2 C. After 150 cycles, the battery's capacity was 199 mAh / g, with a capacity retention of 87.3%.
[0059] Comparative Example 1: 1. Electrolyte; 2 M LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 3:7, and stirred at 500 rpm.
[0060] 2. Battery (positive electrode, separator, electrolyte); Positive electrode: Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 O2.
[0061] The conductive agent is acetylene black, and the binder is PVDF (96:2:2).
[0062] Separator: PP / PE / PP three-layer composite separator.
[0063] The electrode sheets and the prepared electrolyte (80 μL) were assembled into a CR2032 battery and allowed to stand for 12 h. The battery's charge / discharge voltage range was 2.0–4.8 V, and long-term cycling tests were conducted at 1 C. After 200 cycles, the battery's capacity was 158 mAh / g, with a capacity retention of 65.8%.
[0064] The above-described embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be included within the protection scope of the present invention.
Claims
1. A molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes, characterized in that: It includes lithium salt, organic solvent, and functional inducing additive; the functional inducing additive is an organic compound capable of coordinating with manganese ions, which stabilizes Mn in the cathode material through molecular coordination. 3+ To suppress the Ginger-Tyler aberration.
2. The molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes according to claim 1, characterized in that: The functional inducing additives include one or more functional groups selected from phosphonic acid groups, phosphate ester groups, polydentate nitrogen-containing heterocycles, amino groups, carboxyl groups, or crown ether structures.
3. A molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes according to claim 1 or 2, characterized in that: The functional inducing additive is selected from one or more combinations of the following compound categories: phosphonates, silanized phosphate derivatives, nitrogen-containing polydentate ligands, amino acid compounds, crown ethers or azacrown ethers.
4. The molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes according to claim 3, characterized in that: The phosphonate compound is dimethyl methylphosphonate or diethyl vinylphosphonate, the silanized phosphate derivative is tris(trimethylsilane) phosphate, the nitrogen-containing polydentate ligand is 1,10-phenanthroline or 2,2'-bipyridine and its derivatives, the amino acid compound is glycine or alanine, and the crown ether or azacrown ether compound is 18-crown-6-ether or 1,4,7-triazacyclononane.
5. The molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes according to claim 1, characterized in that: The functional inducing additive has a mass percentage concentration of 0.1% to 5.0% in the electrolyte, preferably 0.5% to 2.0%.
6. The molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes according to claim 1, characterized in that: The lithium salt is one or more of lithium hexafluorophosphate, lithium difluorosulfonylimide, lithium difluorophosphate, lithium tetrafluoroborate, and lithium perchlorate, and the molar concentration of the lithium salt is from 0.8 mol / L to 1.5 mol / L.
7. The molecularly induced electrolyte for suppressing the Jan Taylor effect in lithium-rich manganese cathodes according to claim 1, characterized in that: The organic solvent is a mixture of two or more of the following: cyclic carbonates, chain carbonates, carboxylic acid esters, and ether solvents. The cyclic carbonates include ethylene carbonate, propylene carbonate, and fluoroethylene carbonate; the chain carbonates include dimethyl carbonate, diethyl carbonate, and methyl ethyl carbonate.
8. A lithium-ion battery, characterized in that: It includes a positive electrode, a negative electrode, a separator, and a molecularly induced electrolyte as described in any one of claims 1 to 7.
9. A lithium-ion battery according to claim 8, characterized in that: The positive electrode includes a lithium-rich manganese-based positive electrode material, the general formula of which is: , where M is one or more of Mn, Ni, Co, Al, Fe, Cr, Ti, Zr, and Ru, and 0 < x < 1, and M contains at least the element Mn; The diaphragm is one or more of PP diaphragm, glass fiber diaphragm, and PI electrospun diaphragm; The conductive agent is one or more of acetylene black, Super (including P), and graphene.
10. The application of a functional inducing additive in the preparation of molecularly induced electrolytes, characterized in that: The application involves using the functional inducing additive to suppress the Ginger-Taylor effect in lithium-rich manganese-based cathode materials.
Citation Information
Patent Citations
Electrolyte additive suitable for manganese-based positive electrode, electrolyte and battery
CN120767412A