An electrolyte and a lithium-ion battery
By using a composite additive of organic sulfides and organophosphorus silicon compounds in the electrolyte of lithium-ion batteries, a stable interfacial film was constructed, solving the interface problem of lithium-ion batteries under high voltage and high temperature, and achieving a high-efficiency improvement in battery performance.
Patent Information
- Application Number
- CN202611298787.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion batteries face interface challenges under high voltage and high temperature conditions, including electrolyte oxidation and decomposition, cathode material structure degradation, transition metal dissolution, and SEI film damage, leading to capacity decay and low initial efficiency.
A composite additive system, including organosulfur ether compounds and organophosphorus silicon compounds, is used to construct dense composite CEI and SEI films on the positive and negative electrode sides, respectively, to inhibit electrolyte oxidative decomposition and reduce active lithium consumption, and prevent transition metal ion deposition.
It improves the initial coulombic efficiency, room temperature cycle performance, and high temperature storage performance of lithium-ion batteries, with an initial coulombic efficiency of over 85%, and significantly improved capacity retention after 500 cycles and high temperature storage performance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This application relates to the technical field of lithium-ion batteries, specifically to an electrolyte and a lithium-ion battery. Background Technology
[0002] As terminal devices increasingly demand longer battery life, developing high-energy-density lithium-ion batteries has become an industry consensus. Increasing the operating voltage is a key path to achieving this goal.
[0003] However, when the charging cutoff voltage rises to 4.4V, the battery faces severe interface challenges: conventional electrolytes oxidize and decompose on the positive electrode surface, forming an unstable CEI film, which triggers side reactions, dissolution of transition metals and loss of lattice oxygen, leading to capacity decay; trace water and HF generated from fluorinated lithium salts corrode the positive electrode, and dissolved metal ions migrate to the negative electrode to destroy the SEI film; the problem is exacerbated at high temperatures, and the initial efficiency is low.
[0004] Electrolyte additives are an economical and effective solution, but the function of a single additive is limited. Therefore, developing composite additive systems that can synergistically address multiple interfacial failures under high voltage and high temperature is crucial for promoting the development of high-voltage, long-life batteries. Summary of the Invention
[0005] In a first aspect, this application provides an electrolyte for use in lithium-ion batteries, the electrolyte comprising a first additive and a second additive. The first additive is selected from organic sulfide compounds, and the second additive is selected from organic phosphorus-silicon compounds.
[0006] In some optional embodiments of the first aspect of this application, the first additive is selected from at least one of dimethyl sulfide, methyl ethyl sulfide, dimethyl disulfide, and dimethyl trisulfide.
[0007] In some optional embodiments of the first aspect of this application, the first additive is selected from dimethyl sulfide.
[0008] In some optional embodiments of the first aspect of this application, the second additive is selected from at least one of bis(trimethylsilyl)fluorophosphate, tri(trimethylsilyl)phosphate and bis(trimethylsilyl)vinyl phosphate.
[0009] In some optional embodiments of the first aspect of this application, the second additive is selected from bis(trimethylsilyl)fluorophosphate.
[0010] In some optional embodiments of the first aspect of this application, the mass ratio of the first additive to the second additive is 1:(0.15~6).
[0011] In some optional embodiments of the first aspect of this application, the mass ratio of the first additive to the second additive is 1:(0.3~3).
[0012] In some optional embodiments of the first aspect of this application, the mass ratio of the first additive to the second additive is 1:1.
[0013] In some optional embodiments of the first aspect of this application, the sum of the mass fraction of the first additive and the mass fraction of the second additive is 1% to 4% based on the mass of the electrolyte.
[0014] In some optional embodiments of the first aspect of this application, the sum of the mass fraction of the first additive and the mass fraction of the second additive is 2% based on the mass of the electrolyte.
[0015] In some optional embodiments of the first aspect of this application, the mass fraction of the first additive is 0.3% to 2%.
[0016] In some optional embodiments of the first aspect of this application, the mass fraction of the second additive is 0.3% to 2%.
[0017] In some optional embodiments of the first aspect of this application, the electrolyte further includes a solvent and a lithium salt, wherein the solvent is selected from carbonate solvents and the lithium salt is selected from fluorinated lithium salts.
[0018] A second aspect of this application provides a lithium-ion battery, which includes a positive electrode, a negative electrode, a separator, and an electrolyte as described above.
[0019] In some optional embodiments of the second aspect of this application, the positive electrode comprises a ternary material, and the negative electrode comprises at least one of graphite and silicon-carbon composite materials.
[0020] In some optional embodiments of the second aspect of this application, the ternary material is selected from lithium nickel cobalt manganese oxide ternary materials, the chemical formula of which is LiNi x Mn y Co z O2, where x ≥ 0.6, x+y+z=1.
[0021] Beneficial effects: The electrolyte provided in the first aspect of this application, by compounding a first additive, an organic sulfide compound, and a second additive, an organic phosphorus-silicon compound, in the electrolyte, forms a dense, stable composite CEI film rich in elements such as sulfur and phosphorus on the positive electrode side, effectively inhibiting the oxidative decomposition of the electrolyte under high voltage and the structural degradation of the positive electrode material; the first additive and the second additive participate in the formation of a robust and uniform SEI film on the negative electrode side, reducing the initial irreversible consumption of active lithium, preventing the destructive deposition of transition metal ions, and improving the first coulombic efficiency.
[0022] The lithium-ion battery provided in the second aspect of this application has an initial coulombic efficiency of over 85%, a capacity retention rate of over 83% after 500 cycles at 1C, and a capacity retention rate of over 85% after 30 days of storage at 60℃. The lithium-ion battery has high initial coulombic efficiency, good room temperature cycle performance, and high temperature storage performance. Detailed Implementation
[0023] The present application will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are only for explaining the present application and are not intended to limit the present application.
[0024] In one embodiment, an electrolyte is provided for use in a lithium-ion battery, the electrolyte comprising a first additive and a second additive; The first additive is selected from organic sulfide compounds, and the second additive is selected from organic phosphorus-silicon compounds.
[0025] In the above scheme, by compounding the first additive organic sulfide compound and the second additive organic phosphorus silicon compound in the electrolyte, the positive and negative electrode interfaces of the lithium-ion battery are optimized, thereby improving the first coulombic efficiency, room temperature cycle performance and high temperature storage performance of the lithium-ion battery.
[0026] Specifically, the first and second additives preferentially construct a dense, stable composite CEI film rich in elements such as sulfur and phosphorus on the positive electrode side, effectively inhibiting the oxidative decomposition of the electrolyte under high voltage and the structural degradation of the positive electrode material. On the negative electrode side, the first and second additives participate in the formation of a robust and uniform SEI film, reducing the initial irreversible consumption of active lithium, preventing the destructive deposition of transition metal ions, and improving the first coulombic efficiency.
[0027] The lone pair of electrons on the sulfur atom in organosulfur ether compounds endows them with a high HOMO energy level and a strong electron-donating ability, enabling them to preferentially oxidize and form a film on the cathode surface and quench reactive oxygen species released from the cathode. Organophosphorus silicon compounds effectively remove HF from the electrolyte, thereby reducing side reactions and chemical corrosion of the electrodes.
[0028] In some optional embodiments of this application, the first additive is selected from at least one of dimethyl sulfide, methyl ethyl sulfide, dimethyl disulfide, and dimethyl trisulfide.
[0029] Dimethyl sulfide, abbreviated as DMS, has the molecular formula (CH3)2S. Methyl ethyl sulfide has the molecular formula CH3SC2H5. Dimethyl disulfide, abbreviated as DMDS, has the molecular formula CH3SSCH3. Dimethyl trisulfide has the molecular formula CH3SSSCH3. Dimethyl sulfide, methyl ethyl sulfide, dimethyl disulfide, and dimethyl trisulfide were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.
[0030] In some optional embodiments of this application, the second additive is selected from at least one of bis(trimethylsilyl)fluorophosphate, tri(trimethylsilyl)phosphate, and bis(trimethylsilyl)vinyl phosphate.
[0031] bis(trimethylsilyl)fluorophosphate, abbreviated as BTSPFA, has the molecular formula C6H 18 FO3PSi2. Tris(trimethylsilyl)phosphate, abbreviated as TMSP, has the molecular formula C9H. 27 O4PSi3. Bis(trimethylsilyl)vinyl phosphate, abbreviated as DTMSVP. Bis(trimethylsilyl)fluorophosphate, tris(trimethylsilyl)phosphate and bis(trimethylsilyl)vinyl phosphate, purchased from Dongwoo Fine Chemicals Co., Ltd.
[0032] In some optional embodiments of this application, the first additive is selected from dimethyl sulfide.
[0033] In some optional embodiments of this application, the second additive is selected from bis(trimethylsilyl)fluorophosphate. The molecular structural formula of bis(trimethylsilyl)fluorophosphate is (CH3)3SiOP(F)(=O)OSi(CH3)3.
[0034] The following example, using dimethyl sulfide as the first additive and bis(trimethylsilyl)fluorophosphate as the second additive, further illustrates the mechanism of action of this embodiment: (1) Dimethyl sulfide has a high HOMO energy level, and its chemical stability is lower than that of conventional carbonate solvents (such as ethylene carbonate, methyl ethyl carbonate, etc.). During the first charge of the battery, when the positive electrode potential increases, the dimethyl sulfide molecules in the electrolyte preferentially lose electrons and undergo electrochemical oxidation. The sulfur atoms in the dimethyl sulfide molecules carry lone pairs of electrons and have a strong electron-donating ability, which allows them to be oxidized preferentially on the positive electrode surface before solvent molecules. The oxidation products of dimethyl sulfide (mainly sulfur-containing oligomers and polysulfides) are deposited on the positive electrode surface, forming a sulfur-rich CEI film. This sulfur-rich CEI film has good electronic insulation and good lithium-ion conductivity, which can effectively inhibit the continuous oxidation and decomposition of the electrolyte solvent under high pressure, while physically blocking the direct contact between the positive electrode active material and the electrolyte, reducing the dissolution of transition metal ions.
[0035] At high voltages (e.g., 4.4V), high-nickel cathode materials (e.g., NCM811) are in a deep delithiation state, where lattice oxygen loses electrons to form highly reactive superoxide radicals (O2). -This superoxide radical is released into the electrolyte. Superoxide radicals have extremely strong oxidizing properties and can attack carbonate solvent molecules, triggering a chain reaction of oxidative decomposition in the electrolyte, leading to continuous electrolyte consumption, increased gas production, and a sharp deterioration in battery performance. The sulfur atom in the dimethyl sulfide molecule, due to its lone pair of electrons and low oxidation potential, can undergo an electron transfer reaction with the superoxide radical. The electron-donating group of the dimethyl sulfide transfers electrons to the superoxide radical, reducing it to a stable peroxide or oxide species (such as O2). 2- Or O 2- This process effectively quenches the activity of superoxide radicals. This quenching process effectively interrupts the initiation step of the chain oxidation decomposition of the electrolyte, effectively inhibiting the continued decomposition of the electrolyte.
[0036] (2) Trace amounts of water in the electrolyte will react with fluorinated lithium salts such as LiPF6 to generate highly corrosive HF: LiPF6 + H2O → POF3 + LiF + 2HF. HF will attack the cathode material and exacerbate the dissolution of transition metal ions. The bis(trimethylsilyl)fluorophosphate molecule contains two trimethylsilyl groups (-Si(CH3)3), whose silicon atoms are oxyphilic. When bis(trimethylsilyl)fluorophosphate encounters HF, the Si-O bond (silicon ether bond) in the bis(trimethylsilyl)fluorophosphate molecule is broken, and the trimethylsilyl group combines with the fluorine atom in HF to generate trimethylfluorosilane ((CH3)3SiF), thereby efficiently removing HF from the electrolyte. The reaction can be illustrated as: (CH3)3Si-OP(O)(F)-O-Si(CH3)3 + 2HF → 2(CH3)3SiF + HOP(O)(F)OH. Through this reaction, bis(trimethylsilyl)fluorophosphate can effectively eliminate the chemical corrosion of the positive electrode material by HF, reducing the dissolution of transition metal ions and their migration and deposition to the negative electrode. During the electrochemical process, the phosphorus-oxygen double bond (P=O) and phosphorus-fluorine bond (PF) structural units in the bis(trimethylsilyl)fluorophosphate molecule can participate in the construction of the electrode interface film.
[0037] (3) Dimethyl sulfide and bis(trimethylsilyl)fluorophosphate work together at the electrode interface. On the positive electrode side, dimethyl sulfide, with its high HOMO energy level, preferentially oxidizes to form a sulfur-rich CEI film. The decomposition products of bis(trimethylsilyl)fluorophosphate (containing phosphorus oxygen / phosphorus fluoride species) are deposited together with the sulfur-rich CEI film on the positive electrode surface, forming a composite CEI film rich in PO, PF, and S. This composite CEI film has both good chemical stability and ionic conductivity, effectively suppressing high-voltage interfacial side reactions.
[0038] On the negative electrode side, dimethyl sulfide and bis(trimethylsilyl)fluorophosphate can form a more stable SEI film, reducing initial lithium consumption and improving the initial coulombic efficiency, room temperature cycle performance, and high-temperature storage performance of lithium-ion batteries. Specifically, during the first charge, the electrolyte undergoes reductive decomposition on the negative electrode surface to form an SEI film, a process that irreversibly consumes active lithium ions. Dimethyl sulfide participates in the formation of a sulfur-rich SEI film on the negative electrode surface, which has better lithium-ion conductivity and structural stability. Simultaneously, the decomposition products of bis(trimethylsilyl)fluorophosphate (containing phosphorus / silicon species) also participate in the construction of the SEI film, forming a denser and more uniform composite SEI film, inhibiting the continuous reductive decomposition of the electrolyte on the negative electrode, and reducing the active lithium consumption required for SEI film formation during the first charge and discharge process. Furthermore, due to the HF removal by bis(trimethylsilyl)fluorophosphate, the erosion of the SEI film by HF is reduced, making the SEI film more stable in subsequent cycles, further reducing the continuous consumption of active lithium.
[0039] In some optional embodiments of this application, the mass ratio of the first additive to the second additive is 1:(0.15~6).
[0040] With this configuration, when the mass ratio of the first additive to the second additive is 1:(0.15~6), the two additives can exert a better synergistic effect. Under this ratio, the first additive and the second additive can form a dense interfacial film on the positive and negative electrode surfaces, effectively suppressing the continuous oxidative decomposition and side reactions of the electrolyte under high voltage, and improving the initial coulombic efficiency, room temperature cycle performance, and high temperature storage performance of lithium-ion batteries.
[0041] Specifically, the mass ratio of the first additive to the second additive can be 1:0.15, 1:0.3, 1:0.45, 1:0.6, 1:0.75, 1:0.9, 1:1.05, 1:1.2, 1:1.35, 1:1.5, 1:1.65, 1:1.8, 1:1.95, 1:2.1, 1:2.25, 1:2.4, 1:2.55, 1:2.7, 1:2.85, 1 :3, 1:3.15, 1:3.3, 1:3.45, 1:3.6, 1:3.75, 1:3.9, 1:4.05, 1:4.2, 1:4.35, 1:4.5, 1:4.65, 1:4.8, 1:4.95, 1:5.1, 1:5.25, 1:5.4, 1:5.55, 1:5.7, 1:5.85, 1:6, or a range selected from any two of the above values.
[0042] In some optional embodiments of this application, the mass ratio of the first additive to the second additive is 1:(0.3~3). This configuration enhances the synergistic effect between the first and second additives, further improving the initial coulombic efficiency, room-temperature cycle performance, and high-temperature storage performance of the lithium-ion battery.
[0043] In some optional embodiments of this application, the mass ratio of the first additive to the second additive is 1:1. This configuration further enhances the synergistic effect between the first and second additives.
[0044] In some optional embodiments of this application, the sum of the mass fraction of the first additive and the mass fraction of the second additive is 1% to 4% based on the mass of the electrolyte.
[0045] With this configuration, the total mass of the first and second additives is controlled within the range of 1% to 4%. Within this range, the first and second additive systems can construct a composite interface film with moderate thickness and good mechanical strength on the positive and negative electrode surfaces. This effectively inhibits electrolyte oxidation and transition metal dissolution under high voltage, while also avoiding excessively thick interface films or surges in impedance due to excessive additives. Thus, while ensuring high initial coulombic efficiency, it also improves the room temperature cycle performance and high temperature storage performance of lithium-ion batteries.
[0046] Specifically, the sum of the mass fraction of the first additive and the mass fraction of the second additive can be 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, or a range selected from any two of the above values.
[0047] In some optional embodiments of this application, the sum of the mass fractions of the first additive and the second additive is 2% based on the mass of the electrolyte. This configuration further improves the initial coulombic efficiency, room-temperature cycle performance, and high-temperature storage performance of the lithium-ion battery.
[0048] In some optional embodiments of this application, the mass fraction of the first additive is 0.3% to 2% based on the mass of the electrolyte. With this setting, the mass fraction of the first additive is controlled within the range of 0.3% to 2%, which can effectively preferentially oxidize and form a film on the positive electrode surface and quench the active oxygen species released by the positive electrode, and participate in the formation of a robust and uniform SEI film on the negative electrode side, while avoiding an excessively thick interface film.
[0049] In some optional embodiments of this application, the mass fraction of the second additive is 0.3% to 2% based on the mass of the electrolyte. This setting controls the mass fraction of the second additive within the range of 0.3% to 2%, effectively removing HF from the electrolyte, thereby reducing side reactions and chemical corrosion of the electrodes. Simultaneously, it effectively participates in the formation of the interface film between the positive and negative electrodes, preventing the interface film from becoming too thick.
[0050] In some optional embodiments of this application, the electrolyte further includes a solvent and a lithium salt, wherein the solvent is selected from carbonate solvents and the lithium salt is selected from fluorinated lithium salts.
[0051] Carbonate solvents are selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.
[0052] The fluorinated lithium salt is selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorophosphate, and lithium bis(fluorosulfonyl)imide. The concentration of the fluorinated lithium salt in the electrolyte is 0.8 mol / L to 1.5 mol / L.
[0053] In another embodiment, a lithium-ion battery is provided, comprising a positive electrode, a negative electrode, a separator, and an electrolyte as described above.
[0054] In some optional embodiments of this application, the positive electrode comprises a ternary material, and the negative electrode comprises at least one of graphite and silicon-carbon composite materials.
[0055] In some optional embodiments of this application, the ternary material is selected from lithium nickel cobalt manganese oxide ternary materials, the chemical formula of which is LiNi. x Mn y Co z O2, where x ≥ 0.6, x+y+z=1.
[0056] The present application is further illustrated below with reference to embodiments and comparative examples. Unless otherwise specified, the raw materials, reagents, materials and equipment used in this application are all commercially available products conventionally used in the art.
[0057]
Example 1
[0058]
Example 2
[0059]
Example 3
[0060]
Example 4
[0061]
Example 5
[0062]
Example 6
[0063]
Example 7
[0064]
Example 8
[0065]
Example 9
[0066] Comparative Example 1 The difference between this comparative example and Example 1 is that the electrolyte does not contain any additives. Specifically: Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a mass ratio of EC:EMC = 3:7. After mixing, 1.0 mol / L lithium hexafluorophosphate (LiPF6) was added, stirred and dissolved, and the electrolyte was obtained after stirring evenly.
[0067] Comparative Example 2 The difference between this comparative example and Example 1 is that the electrolyte does not contain bis(trimethylsilyl)fluorophosphate additive (only 1% dimethyl sulfide). Specifically: Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a mass ratio of EC:EMC = 3:7. After mixing, 1.0 mol / L lithium hexafluorophosphate (LiPF6) was added and stirred to dissolve. After the lithium hexafluorophosphate was completely dissolved, 1% (based on the mass of the electrolyte) of dimethyl sulfide additive was added and stirred evenly to obtain the electrolyte.
[0068] Comparative Example 3 The difference between this comparative example and Example 1 is that the electrolyte does not contain dimethyl sulfide additive (it contains only 1% bis(trimethylsilyl)fluorophosphate). Specifically: Ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a mass ratio of EC:EMC = 3:7. After mixing, 1.0 mol / L lithium hexafluorophosphate (LiPF6) was added and stirred to dissolve. After the lithium hexafluorophosphate was completely dissolved, 1% (based on the mass of the electrolyte) of bis(trimethylsilyl)fluorophosphate additive was added and stirred evenly to obtain the electrolyte.
[0069] Table 1 summarizes some experimental parameters from each embodiment and comparative example.
[0070] Table 1
[0071] [Performance Testing] Lithium-ion pouch batteries were prepared based on the electrolytes obtained in Examples 1 to 9 and Comparative Examples 1 to 3, and their electrochemical performance was tested. The test results are shown in Table 2.
[0072] The specific manufacturing steps for lithium-ion pouch batteries are as follows: (1) Preparation of positive electrode sheet: The active material lithium nickel cobalt manganese oxide (NCM811), conductive agent (acetylene black) and binder (polyvinylidene fluoride) are mixed evenly in N-methylpyrrolidone solvent system at a mass ratio of 95:2.5:2.5. The slurry is coated on the current collector aluminum foil, and the lithium-ion battery positive electrode sheet that meets the requirements is obtained by slitting, die cutting and rolling.
[0073] (2) Preparation of negative electrode sheet: The graphite negative electrode is mixed with conductive agent (Ketjen Black), thickener (sodium carboxymethyl cellulose) and binder (styrene-butadiene rubber) in a deionized water solvent system at a mass ratio of 90:3:2:5. The slurry is then coated onto the current collector copper foil. After slitting, rolling and die cutting, the lithium-ion battery negative electrode sheet that meets the requirements is obtained.
[0074] (3) Preparation of lithium-ion batteries: The positive electrode, negative electrode and separator prepared according to the above process are used to obtain bare cells according to the process of stacked cells. The bare cells are then placed in aluminum-plastic film for pre-encapsulation, injected with the prepared electrolyte and then encapsulated to obtain the required lithium-ion soft pack battery.
[0075] The specific steps for electrochemical performance testing are as follows: (1) The prepared lithium-ion pouch batteries were formed and capacity tested using a battery testing cabinet. The formation process consisted of constant current charging at 0.02 C to 3.4 V, constant current charging at 0.1 C to 3.6 V, and constant current charging at 0.2 C to 3.8 V. The aging process was then carried out at 45 ℃ for 48 hours. The capacity testing process consisted of constant current and constant voltage charging at 0.33 C to 4.4 V, with a cutoff current of 0.05 C, followed by constant current discharging at 0.33 C to 2.5 V. The charge-discharge cycle was repeated 5 times. Based on the above capacity testing data, the discharge capacity and charge capacity of the 5th cycle were extracted, and the first coulombic efficiency was calculated.
[0076] (2) Room temperature cycle test: The lithium-ion pouch battery was placed in a constant temperature environment of 25 ℃ and subjected to constant current and constant voltage cycle test at a charge / discharge rate of 1C / 1C. The voltage range was set to 2.5V~4.4V. The discharge capacity of the first cycle was recorded as the initial capacity, and the cycle was continued until the 500th cycle. The discharge capacity was recorded, and the capacity retention rate at 1C for 500 cycles was calculated.
[0077] (3) High temperature storage test: The lithium-ion soft pack battery was fully charged and stored in a constant temperature chamber at 60℃ for 30 days. After the storage period, the battery was taken out and allowed to return to normal temperature. The full charge and discharge test was performed again. By comparing the discharge capacity before and after storage, the capacity retention rate after 30 days of storage at 60℃ was calculated.
[0078] Table 2
[0079] As can be seen from the data in Table 2: (a) The initial coulombic efficiency of Examples 1 to 9 ranged from 85.5% to 87.8%, and the initial coulombic efficiency of Comparative Examples 1 to 3 ranged from 82.5% to 85.0%.
[0080] The capacity retention rate of Examples 1 to 9 after 500 cycles at 1°C ranged from 83.9% to 92.5%, while the capacity retention rate of Comparative Examples 1 to 3 after 500 cycles at 1°C ranged from 58.3% to 80.1%.
[0081] After 30 days of storage at 60°C, the capacity retention rate of Examples 1 to 9 ranged from 85.7% to 92.7%, while that of Comparative Examples 1 to 3 ranged from 68.5% to 85.3%. All examples exhibited high initial coulombic efficiency, good room temperature cycling performance, and high-temperature storage performance.
[0082] In terms of initial coulombic efficiency, capacity retention after 500 cycles at 1 C, and capacity retention after 30 days of storage at 60°C, all examples were superior to the comparative example. This indicates that a synergistic effect occurred between the first and second additives, which promoted the formation of a highly efficient interface film on the positive and negative electrode surfaces and significantly reduced the active lithium ions consumed in the formation of SEI / CEI.
[0083] (II) Comparison of Examples 1, 4 to 7 In Examples 1, 4 to 7, the total amount of the second additive was the same. However, a comparison showed that the data for Examples 4 and 7 were slightly lower than those for Examples 1, 5, and 6. This indicates that an excessively high or low proportion of the first or second additive weakened their synergistic effect, resulting in a slight decrease in performance. In Examples 1, 5, and 6, the first and second additives exhibited a better synergistic effect. Data from Example 1 shows that the lithium-ion battery prepared in Example 1 has superior overall performance.
[0084] It should be noted that, in this document, "comprising," "including," or any other variation thereof is intended to cover non-exclusive inclusion, such that a process, method, or article that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, or article.
[0085] The various embodiments in this specification are described in a related manner. The same or similar parts between the various embodiments can be referred to each other. Each embodiment focuses on describing the differences from other embodiments.
[0086] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the principles of this application should be included within the scope of protection of this application.
Claims
1. An electrolyte, characterized in that, The electrolyte is used in lithium-ion batteries, and the electrolyte includes a first additive and a second additive. The first additive is selected from organosulfur compounds, and the second additive is selected from organophosphorus silicon compounds.
2. The electrolyte as described in claim 1, characterized in that, The first additive is selected from at least one of dimethyl sulfide, methyl ethyl sulfide, dimethyl disulfide, and dimethyl trisulfide; Preferably, the first additive is selected from dimethyl sulfide.
3. The electrolyte as described in claim 1, characterized in that, The second additive is selected from at least one of bis(trimethylsilyl)fluorophosphate, tri(trimethylsilyl)phosphate and bis(trimethylsilyl)vinyl phosphate; Preferably, the second additive is selected from bis(trimethylsilyl)fluorophosphate.
4. The electrolyte according to any one of claims 1 to 3, characterized in that, The mass ratio of the first additive to the second additive is 1:(0.15~6). Preferably, the mass ratio of the first additive to the second additive is 1:(0.3~3). Preferably, the mass ratio of the first additive to the second additive is 1:
1.
5. The electrolyte according to any one of claims 1 to 3, characterized in that, Based on the mass of the electrolyte, the sum of the mass fractions of the first additive and the second additive is 1% to 4%. Preferably, based on the mass of the electrolyte, the sum of the mass fraction of the first additive and the mass fraction of the second additive is 2%.
6. The electrolyte as described in claim 5, characterized in that, Based on the mass of the electrolyte, the mass fraction of the first additive is 0.3% to 2%.
7. The electrolyte as described in claim 5, characterized in that, Based on the mass of the electrolyte, the mass fraction of the second additive is 0.3% to 2%.
8. The electrolyte according to any one of claims 1 to 3, characterized in that, The electrolyte also includes a solvent and a lithium salt, wherein the solvent is selected from carbonate solvents and the lithium salt is selected from fluorinated lithium salts.
9. A lithium-ion battery, characterized in that, The lithium-ion battery includes a positive electrode, a negative electrode, a separator, and an electrolyte as described in any one of claims 1 to 8.
10. The lithium-ion battery as described in claim 9, characterized in that, The positive electrode comprises a ternary material, and the negative electrode comprises at least one of graphite and silicon-carbon composite materials; Preferably, the ternary material is selected from lithium nickel cobalt manganese oxide ternary materials, and the chemical formula of the lithium nickel cobalt manganese oxide ternary material is LiNi. x Mn y Co z O2, where x ≥ 0.6, x+y+z=1.