Electrolyte, secondary battery, and electric device

Through the synergistic design of specific electrolyte additives, the problems of water corrosion in electrolytes, insufficient SEI film performance, and single function of additives have been solved, achieving high cycle life, high and low temperature performance, and high voltage stability of batteries, and making them suitable for silicon-based anodes and high energy density batteries.

CN123120886APending Publication Date: 2026-11-17EVE ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611318667.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing electrolyte systems suffer from problems such as water content in the electrolyte and corrosion by HF, difficulty in achieving comprehensive performance of the SEI membrane, and limited functionality of additives, which can easily lead to antagonistic effects when compounded, resulting in short battery cycle life, poor low-temperature performance, and insufficient high-voltage stability.

Method used

By employing specific first electrolyte additives containing sulfur- and/or nitrogen-containing aromatic heterocycles and their functional substituents, deep dehydration and acid suppression, high conductivity film formation, and long-term interface stability are achieved through synergistic design. This includes precise regulation of groups such as Boc-amino and aldehyde groups, forming a highly conductive, flexible, and stable SEI film that is compatible with silicon-based anodes and high-energy-density battery systems.

Benefits of technology

It effectively suppresses lithium salt hydrolysis, reduces interface impedance, and improves battery cycle life, high and low temperature performance, and high voltage stability, solving multiple performance problems of batteries in high energy density battery systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_14
    Figure SMS_14
  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

This application provides an electrolyte, a secondary battery, and an electrical device. The electrolyte includes a first electrolyte additive, which comprises a sulfur- and / or nitrogen-containing aromatic heterocycle and functional substituents on the sulfur- and / or nitrogen-containing aromatic heterocycle. The functional substituents include a first substituent and a second substituent, wherein the first substituent is selected from Boc-amino and the second substituent is selected from aldehyde. This first electrolyte additive, through the synergistic design of single-molecule multi-groups, achieves multifunctional integration of deep water removal and acid suppression, high-conductivity film formation, and long-term interface stability. It overcomes the technical bottlenecks of existing additives with single functions and antagonistic compounding, and can simultaneously improve the battery's cycle life, high and low temperature performance, and high-voltage stability, perfectly adapting to high-energy-density battery systems such as silicon-based anodes and high-nickel ternary batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of battery technology and relates to an electrolyte, a secondary battery, and an electrical device. Background Technology

[0002] With the large-scale application of lithium-ion batteries in new energy vehicles, consumer electronics, and energy storage, the market has placed higher demands on battery cycle life, high and low temperature performance, high voltage stability, and safety performance. As a key component of lithium-ion batteries, the stability of the electrolyte directly determines the core performance of the battery, and electrolyte additives are crucial for regulating electrolyte performance and optimizing electrode interface characteristics.

[0003] The existing electrolyte system still has the following problems:

[0004] (1) The problems of water content in the electrolyte and corrosion by HF are prominent: Trace amounts of free water in the electrolyte can cause lithium salts (especially the mainstream lithium hexafluorophosphate) to hydrolyze, generating highly corrosive HF. HF will continuously corrode the interface film between the positive and negative electrodes, destroy the layered structure of the positive electrode material, cause the dissolution of transition metals, and at the same time cause the negative electrode SEI film to repeatedly rupture and regenerate, consuming active lithium and electrolyte, ultimately causing rapid capacity decay and a significant reduction in cycle life. Existing dehydration additives generally have the problems of low dehydration efficiency and single function, and cannot fundamentally inhibit the chain reaction of lithium salt hydrolysis.

[0005] (2) The comprehensive performance of SEI film (solid electrolyte interface film) is difficult to achieve: the SEI film formed by existing film-forming additives generally has the contradiction of "conductivity and stability cannot be achieved at the same time". The inorganic phase-based SEI film has poor ionic conductivity and high interfacial impedance, while the organic phase-based SEI film has insufficient mechanical strength and is easy to decompose under high temperature / high pressure. In particular, when adapted to silicon-based anodes, the existing SEI film cannot withstand the 300% volume expansion of silicon materials and is very easy to break during cycling, and cannot achieve long-term interface protection.

[0006] (3) Additives have a single function and are prone to antagonistic effects when compounded: Existing electrolyte additives can generally only achieve a single function. When multiple additives such as dehydrating agents, film-forming agents and impedance reducing agents are compounded, problems such as reduction / oxidation potential mismatch, interfacial film formation competition and poor solvent compatibility are likely to occur. Not only can they not achieve synergistic performance, but they will also lead to increased interfacial impedance and deterioration of battery performance. They cannot solve the multiple problems of high electrolyte water content, poor interfacial stability, insufficient high and low temperature performance and poor high voltage adaptability at the same time. Summary of the Invention

[0007] The purpose of this application is to provide an electrolyte, a secondary battery, and an electrical device. The electrolyte contains a specific first electrolyte additive. Through the synergistic design of single-molecule multi-groups, the first electrolyte additive achieves multi-functional integration of deep water removal and acid suppression, high conductivity film formation, and long-term interface stability. It breaks through the technical bottleneck of existing additives having single functions and antagonistic compounding, and can simultaneously improve the cycle life, high and low temperature performance, and high voltage stability of the battery. It is perfectly compatible with high-energy-density battery systems such as silicon-based anodes and high-nickel ternary batteries.

[0008] To achieve the purpose of this application, the following technical solution is adopted:

[0009] In a first aspect, this application provides an electrolyte comprising a first electrolyte additive, wherein the first electrolyte additive comprises a sulfur- and / or nitrogen-containing aromatic heterocycle and functional substituents on the sulfur- and / or nitrogen-containing aromatic heterocycle.

[0010] The functional substituent includes a first substituent and a second substituent, wherein the first substituent is selected from Boc-amino and the second substituent is selected from aldehyde.

[0011] The electrolyte described in this application contains a specific first electrolyte additive. In the first electrolyte additive, a sulfur- and / or nitrogen-containing aromatic heterocycle is the main ring, and the main ring contains Boc-amino and aldehyde substituents. The sulfur atoms on the sulfur- and / or nitrogen-containing aromatic heterocycle can be preferentially reduced and decomposed on the negative electrode surface to generate sulfur-containing components with high ionic conductivity such as Li2S and LiNCS, which participate in the construction of the SEI film, significantly reducing interfacial impedance and improving interfacial conductivity. At the same time, the sulfur-containing SEI film has excellent flexibility and mechanical strength, which can adapt to the volume expansion of silicon-based negative electrodes and avoid the film structure from breaking during cycling. The nitrogen atoms on the sulfur- and / or nitrogen-containing aromatic heterocycle can synergistically participate in film formation to form a stable SEI film. Meanwhile, the conjugated heterocyclic structure of the aromatic heterocycle can improve oxidation resistance and stability under high voltage.

[0012] In addition, in the Boc-amino group (referring to the amino group protected by tert-butoxycarbonyl, t-Bu-OC(=O)-NH-) in the first electrolyte additive, the tert-butoxycarbonyl (Boc) forms a protective blockade on the amino group, preventing the amino group from undergoing premature side reactions during the electrolyte storage stage of the cell. During the cell formation stage, the protection can be controlled by adjusting the potential, and the released amino group participates in the formation of the SEI film, forming a nitrogen-containing stable component, which improves the thermal and chemical stability of the SEI film and significantly optimizes the battery cycle performance. The aldehyde group (-CHO) in the first electrolyte additive of this application can undergo a directional condensation reaction with free water in the electrolyte and the alcohol hydroxyl groups generated by the hydrolysis of carbonate solvents, which efficiently consumes free water in the system and inhibits the production of HF by the hydrolysis of lithium salts such as LiPF6 from the source, reducing interface corrosion. At the same time, the condensation reaction products can synergistically participate in the interface film formation, further enhancing the compactness and stability of the SEI film. Therefore, this application achieves multi-functional integration of deep water removal and acid suppression, high conductivity film formation, and long-term interface stability through the precise design and site separation of the three functional groups. It breaks through the technical bottleneck of single function and antagonistic compounding of existing additives, and can simultaneously improve the cycle life, high and low temperature performance and high voltage stability of the battery, perfectly adapting to high energy density battery systems such as silicon-based anodes and high-nickel ternary batteries.

[0013] In some embodiments, the sulfur- and / or nitrogen-containing aromatic heterocycle is selected from any one of thiazole rings, thiophene rings, imidazole rings, or oxazole rings, preferably thiazole rings.

[0014] Because the thiazole ring possesses three core advantages—sulfur-containing film-forming sites, nitrogen-containing coordination sites, and the antioxidant properties of conjugated heterocyclic rings—it can simultaneously achieve the synergistic effects of impedance reduction, film stabilization, and high-pressure resistance. Replacing it with other heterocyclic groups would not be able to simultaneously achieve the above properties. For example, the absence of nitrogen atoms in the thiophene ring affects film formation, resulting in a weaker SEI film stability and lower antioxidant properties compared to the thioazole ring. It is also more prone to decomposition under high voltage, leading to lower overall performance. The imidazole ring, a five-membered aromatic heterocycle containing two nitrogen atoms, lacks sulfur atoms, hindering the formation of highly conductive sulfur-containing components. Its interfacial impedance is higher than that of the thioazole ring system, and its free radical scavenging ability decreases, leading to reduced high-temperature stability and consequently lower rate and low-temperature performance. The oxazole ring, a five-membered aromatic heterocycle containing oxygen and nitrogen atoms, also lacks sulfur atoms. While it can improve the compatibility of the first electrolyte additive with the carbonate solvent, the absence of sulfur atoms affects the formation of a highly conductive SEI film, increasing interfacial impedance, reducing film-forming activity, and decreasing the effectiveness of suppressing the volume expansion of the silicon-based anode. Similarly, the pyridine ring, lacking sulfur atoms, results in reduced interfacial conductivity, increased ring steric hindrance, decreased film-forming activity, and lower SEI film density, ultimately reducing the battery's cycle and rate performance.

[0015] In some embodiments, the functional substituent further includes a third substituent selected from halogen substituents, wherein the halogen substituent is selected from at least one of Cl, Br, or F.

[0016] When sulfur- and / or nitrogen-containing aromatic heterocycles also contain halogen substituents, the electronic effects and interfacial behavior of the molecules can be further optimized. Specifically, halogen substituents (especially fluorine and chlorine) have a strong electron-withdrawing inductive effect, which can moderately reduce the electron cloud density of sulfur and nitrogen atoms on the thiazole ring, thereby precisely controlling the reduction decomposition potential of the additive on the negative electrode surface, avoiding premature or delayed decomposition, and achieving controllable gradient film formation during the formation stage. At the same time, the introduction of halogen atoms can enhance the proportion of inorganic components (such as LiF and LiCl) in the SEI film. These components have higher interfacial energy and better lithium-ion migration ability, which can reduce interfacial impedance and improve the compactness and mechanical strength of the SEI film, thereby more effectively suppressing the risk of film rupture caused by the volume expansion of silicon-based negative electrodes. In addition, halogen substituents can further enhance the antioxidant capacity of aromatic heterocycles, suppress side reactions of additives on the surface of high-voltage positive electrodes, broaden the electrochemical window of the electrolyte, and enhance the cycle stability of the battery at high voltages of 4.4V and above. In summary, the halogen (especially fluorine) substituents, together with the Boc-amino, aldehyde, and thiazole ring core structures, form a "four-effect synergy," achieving multiple benefits beyond deep dehydration and acid suppression, including adjustable film formation potential, reduced interfacial impedance, and improved high-voltage stability.

[0017] In some embodiments, the chemical formula of the first electrolyte additive is shown in Formula I):

[0018] ;

[0019] Formula I);

[0020] Wherein, R1 is selected from Boc-amino, R2 is selected from aldehyde, and R3 is selected from hydrogen or halogen substituent, wherein the halogen substituent is selected from at least one of Cl, Br or F.

[0021] The preferred chemical formula of the first electrolyte additive is shown in Formula I), which separates the sites of each functional group so that they do not affect each other.

[0022] In some embodiments, the first electrolyte additive includes (CAS: 391668-77-2) (CAS: 2241514-59-8) or Any one or at least two of the following (CAS: 388594-31-8):

[0023] In some embodiments, the content of the first electrolyte additive in the electrolyte is 0.05wt% to 3.0wt%, for example, it can be 0.05wt%, 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt% or 3wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable, preferably 0.2wt% to 1.5wt%.

[0024] In some embodiments, the electrolyte further includes any one or a combination of at least two of a second electrolyte additive, a third electrolyte additive, a fourth electrolyte additive, and a fifth electrolyte additive, which are different from the first electrolyte additive. The second electrolyte additive includes 1,3-propanesulfonate lactone and / or vinyl sulfate, the third electrolyte additive includes fluoroethylene carbonate and / or vinylene carbonate, the fourth electrolyte additive includes lithium difluorophosphate and / or lithium difluorooxalate borate, and the fifth electrolyte additive includes lithium tetrafluoroborate.

[0025] The first electrolyte additive can be used in combination with any one or at least two of the second, third, fourth, and fifth electrolyte additives. The second electrolyte additive, as a sulfur-containing additive, synergizes with the thiazole ring of the first electrolyte additive to further increase the sulfur content of the SEI film, reduce interfacial impedance, and enhance the film's flexibility and high-temperature stability. The third electrolyte additive, as a film-forming additive, assists in constructing a stable negative electrode SEI film, forming an organic-inorganic composite structure with the film-forming component of the first electrolyte additive, improving the film's mechanical strength and adapting to the volume expansion of the silicon-based negative electrode. The fourth electrolyte additive, as a dehydration and acid removal / impedance reduction additive, forms a dual dehydration and acid removal system with the first electrolyte additive, further removing trace amounts of water and HF from the system, while simultaneously reducing interfacial impedance and improving rate performance. The fifth electrolyte additive, as a lithium salt stabilizer, enhances the hydrolytic stability of lithium salts, synergistically inhibiting lithium salt hydrolysis with the first electrolyte additive, and enhancing the high-voltage and high-temperature stability of the electrolyte.

[0026] In some embodiments, the content of the second electrolyte additive in the electrolyte is 0.1wt% to 2.0wt%, for example, it can be 0.1wt%, 0.5wt%, 1wt%, 1.5wt% or 2wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0027] In some embodiments, the content of the third electrolyte additive in the electrolyte is 0.5wt% to 8.0wt%, for example, it can be 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt% or 8wt%, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0028] In some embodiments, the content of the fourth electrolyte additive in the electrolyte is 0.1wt% to 2.0wt%, for example, it can be 0.1wt%, 0.5wt%, 1wt%, 1.5wt% or 2wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0029] In some embodiments, the content of the fifth electrolyte additive in the electrolyte is 0.1wt% to 1.0wt%, for example, it can be 0.1wt%, 0.3wt%, 0.5wt%, 0.7wt%, 0.9wt% or 1.0wt%, but is not limited to the listed values. Other unlisted values ​​within the range are also applicable.

[0030] In some embodiments, the electrolyte further includes an organic solvent.

[0031] In some embodiments, the mass percentage of organic solvent in the electrolyte is 80wt% to 90wt%, for example, it can be 80wt%, 82wt%, 84wt%, 86wt%, 88wt% or 90wt%, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0032] In some embodiments, the organic solvent includes cyclic carbonates and chain carbonates.

[0033] In some embodiments, the mass ratio of the cyclic carbonate to the chain carbonate is (20~40):(60~80), for example, it can be 20:80, 25:75, 30:70, 35:65 or 40:60, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0034] The mass ratio of the cyclic carbonate to the chain carbonate is within a specific range, which can balance condensation dewatering efficiency, dielectric constant, low viscosity and high and low temperature compatibility.

[0035] In some embodiments, the cyclic carbonate includes ethylene carbonate and / or propylene carbonate, preferably ethylene carbonate.

[0036] A condensable cyclic carbonate + low-viscosity chain carbonate mixed system is used as an organic solvent to balance the water removal effect of aldehyde groups, the lithium salt dissociation ability and ion transport efficiency. Among them, the cyclic carbonate that can undergo condensation reaction with aldehyde groups can undergo acetal reaction with formaldehyde groups to synergistically consume free water by hydrolyzing the diol hydroxyl group generated by hydrolysis.

[0037] In some embodiments, the chain carbonate includes any one or a combination of at least two of dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate, preferably dimethyl carbonate and methyl ethyl carbonate.

[0038] In some embodiments, the electrolyte further includes lithium salt.

[0039] In some embodiments, the lithium salt includes any one or a combination of at least two of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, or lithium difluorooxalateborate.

[0040] In some embodiments, the concentration of lithium salt in the electrolyte is 0.8 mol / L to 1.5 mol / L, for example, it can be 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L or 1.5 mol / L, and the content (mass percentage) of lithium salt is 10 wt% to 15 wt%, for example, it can be 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt% or 15 wt%, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0041] In some embodiments, the preparation method of the electrolyte includes the following steps: in an argon atmosphere glove box with a water oxygen content of <1ppm, organic solvents are mixed in a preset ratio and stirred at room temperature until completely homogeneous to obtain an organic solvent mixture system; lithium salt is slowly added to the organic solvent mixture system and stirred continuously until completely dissolved to obtain a basic electrolyte; the first electrolyte additive and optional other electrolyte additives are added to the basic electrolyte in a preset ratio and stirred at room temperature until completely dissolved to obtain the target electrolyte.

[0042] Secondly, this application provides a secondary battery, the secondary battery comprising the electrolyte as described in the first aspect.

[0043] In some embodiments, the secondary battery includes a negative electrode sheet, the negative electrode sheet includes a negative current collector and a negative electrode active layer on at least one side surface of the negative current collector, the negative electrode active layer includes 80wt%-88wt% of negative electrode material, for example, it can be 80wt%, 82wt%, 84wt%, 96wt% or 88wt%, but is not limited to the listed values, and other unlisted values ​​within the value range are also applicable.

[0044] In some embodiments, the negative electrode material in the secondary battery includes a silicon-based negative electrode material (such as a silicon-carbon negative electrode material), wherein the silicon content in the silicon-based negative electrode material is 45% to 55%, for example, it can be 45%, 47%, 49%, 51%, 53% or 55%, but is not limited to the listed values, and other unlisted values ​​within the range are also applicable.

[0045] In some embodiments, the secondary battery includes a positive electrode sheet, the positive electrode sheet includes a positive current collector and a positive active layer on at least one side surface of the positive current collector, the positive active layer includes 93wt%-98wt% of positive electrode material, for example, it can be 93wt%, 94wt%, 95wt%, 96wt%, 97wt% or 98wt%, but is not limited to the listed values, other unlisted values ​​within the range are also applicable.

[0046] In some embodiments, the positive electrode material in the secondary battery includes a high-nickel positive electrode material, the general chemical formula of which is LiNi. x Co y Mn 1-x-y O2, 0.8≤x<1, for example, it can be 0.8, 0.85, 0.9 or 0.95, 0≤y≤0.2, for example, it can be 0, 0.05, 0.1, 0.15 or 0.2, but not limited to the listed values, other unlisted values ​​within the range also apply.

[0047] Thirdly, this application provides an electrical device that includes a secondary battery as described in the second aspect.

[0048] Compared with the prior art, this application has the following advantages:

[0049] (1) It solves the problems of high free water content in electrolyte, HF generated by lithium salt hydrolysis leading to interface corrosion and rapid capacity decay. Through the directional condensation reaction of formaldehyde groups, the free water in the system is efficiently consumed, and lithium salt hydrolysis is suppressed from the source. The HF inhibition rate is >90%, thereby greatly reducing electrode interface corrosion.

[0050] (2) It solves the problems of poor interfacial conductivity, insufficient mechanical strength and easy breakage of traditional SEI membranes. By generating highly conductive sulfur-containing components through thiazole rings, a low impedance and highly flexible SEI membrane is constructed to adapt to the volume expansion of silicon-based anodes and achieve long-term interfacial protection during cycling.

[0051] (3) It solves the problems of uncontrollable film formation and poor storage stability of existing additives. Through the protection of amino groups by Boc groups and the controllable deprotection design, it achieves precise control of "storage stability-gradient film formation", avoids premature side reactions of additives, and improves the storage stability and film uniformity of electrolyte.

[0052] (4) It solves the problem of existing additives having a single function and multiple additives being prone to antagonistic effects. Through the synergistic design of the three major functional groups of a single molecule, it simultaneously achieves water removal and acid suppression, film formation and impedance reduction, and high and low temperature / high pressure performance improvement, avoiding film formation competition and performance deterioration in multiple additive combinations.

[0053] (5) It solves the problem that high energy density battery systems cannot simultaneously achieve high and low temperature performance and cycle performance. Through a low impedance SEI film and a stable electrolyte system, it simultaneously improves the high temperature cycle life and low temperature discharge performance of the battery, and is perfectly compatible with high energy density systems such as high nickel ternary and silicon-based anodes. Detailed Implementation

[0054] The technical solution of this application will be further described below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely to help understand this application and should not be regarded as specific limitations on this application.

[0055] Example 1

[0056] This embodiment provides an electrolyte, which includes a first electrolyte additive, wherein the first electrolyte additive is... (CAS: 391668-77-2, purchased from Zhengzhou Alpha Chemical Co., Ltd.)

[0057] The electrolyte comprises 1 wt% of the first electrolyte additive of this embodiment, 1 wt% of the second electrolyte additive, 3 wt% of the third electrolyte additive, 1 wt% of the fourth electrolyte additive, 0.5 wt% of the fifth electrolyte additive, 11.5 wt% of lithium hexafluorophosphate, and the balance being an organic solvent.

[0058] The second electrolyte additive is 1,3-propanesulfonate lactone, the third electrolyte additive is fluoroethylene carbonate, the fourth electrolyte additive is lithium difluorooxalate borate, the fifth electrolyte additive is lithium tetrafluoroborate, and the organic solvent is ethylene carbonate, methyl ethyl carbonate, and dimethyl carbonate in a mass ratio of 30:40:30.

[0059] The preparation method of the electrolyte includes the following steps:

[0060] In an argon-atmospheric glove box, an organic solvent is stirred at room temperature for 30 minutes according to a preset ratio to obtain an organic solvent mixture. Lithium hexafluorophosphate is slowly added to the organic solvent mixture and stirred continuously for 60 minutes until completely dissolved to obtain a basic electrolyte. The first electrolyte additive, the second electrolyte additive, the third electrolyte additive, the fourth electrolyte additive, and the fifth electrolyte additive of this embodiment are added to the basic electrolyte according to a preset ratio and stirred at room temperature for 40 minutes until completely dissolved to obtain the electrolyte.

[0061] Example 2

[0062] This embodiment provides an electrolyte, which includes a first electrolyte additive, wherein the first electrolyte additive is... (CAS: 391668-77-2, purchased from Zhengzhou Alpha Chemical Co., Ltd.)

[0063] The electrolyte comprises 1.5 wt% of the first electrolyte additive of this embodiment, 0.1 wt% of the second electrolyte additive, 0.5 wt% of the third electrolyte additive, 2.0 wt% of the fourth electrolyte additive, 0.1 wt% of the fifth electrolyte additive, 10.8 wt% of lithium hexafluorophosphate, and the balance being an organic solvent.

[0064] The second electrolyte additive is ethylene sulfate, the third electrolyte additive is vinylene carbonate, the fourth electrolyte additive is lithium difluorophosphate, the fifth electrolyte additive is lithium tetrafluoroborate, and the organic solvent is ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a mass ratio of 40:30:30.

[0065] The preparation method of the electrolyte includes the following steps:

[0066] In an argon-atmospheric glove box, an organic solvent is stirred at room temperature for 30 minutes according to a preset ratio to obtain an organic solvent mixture. Lithium hexafluorophosphate is slowly added to the organic solvent mixture and stirred continuously for 60 minutes until completely dissolved to obtain a basic electrolyte. The first electrolyte additive, the second electrolyte additive, the third electrolyte additive, the fourth electrolyte additive, and the fifth electrolyte additive of this embodiment are added to the basic electrolyte according to a preset ratio and stirred at room temperature for 40 minutes until completely dissolved to obtain the electrolyte.

[0067] Example 3

[0068] This embodiment provides an electrolyte, which includes a first electrolyte additive, wherein the first electrolyte additive is... (CAS: 391668-77-2, purchased from Zhengzhou Alpha Chemical Co., Ltd.)

[0069] The electrolyte comprises 0.2 wt% of the first electrolyte additive of this embodiment, 2.0 wt% of the second electrolyte additive, 3 wt% of the third electrolyte additive, 0.1 wt% of the fourth electrolyte additive, 1.0 wt% of the fifth electrolyte additive, and 13.7 wt% of lithium hexafluorophosphate, and the balance being an organic solvent.

[0070] The second electrolyte additive is 1,3-propanesulfonate lactone, the third electrolyte additive is vinylene carbonate, the fourth electrolyte additive is lithium difluorophosphate, the fifth electrolyte additive is lithium tetrafluoroborate, and the organic solvent is ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a mass ratio of 20:40:40.

[0071] The preparation method of the electrolyte includes the following steps:

[0072] In an argon-atmospheric glove box, an organic solvent is stirred at room temperature for 30 minutes according to a preset ratio to obtain an organic solvent mixture. Lithium hexafluorophosphate is slowly added to the organic solvent mixture and stirred continuously for 60 minutes until completely dissolved to obtain a basic electrolyte. The first electrolyte additive, the second electrolyte additive, the third electrolyte additive, the fourth electrolyte additive, and the fifth electrolyte additive of this embodiment are added to the basic electrolyte according to a preset ratio and stirred at room temperature for 40 minutes until completely dissolved to obtain the electrolyte.

[0073] Example 4

[0074] This embodiment provides an electrolyte, wherein the electrolyte contains, in addition to the first electrolyte additive, [the following is also present]. Except for (CAS: 2241514-59-8, purchased from Shanghai Haohong Biomedical Technology Co., Ltd.), everything else is the same as in Example 1.

[0075] Example 5

[0076] This embodiment provides an electrolyte, wherein the electrolyte contains, in addition to the first electrolyte additive, [the following is also present]. Except for (CAS: 388594-31-8, purchased from Shanghai Haohong Biomedical Technology Co., Ltd.), everything else is the same as in Example 1.

[0077] Example 6

[0078] This embodiment provides an electrolyte, wherein the electrolyte contains, in addition to the first electrolyte additive, [the following is also present]. Except for (CAS: 199296-40-7, purchased from Shanghai Hongchuang Pharmaceutical Technology Co., Ltd.), everything else is the same as in Example 1.

[0079] Example 7

[0080] This embodiment provides an electrolyte, which is the same as that in Example 1 except that the content of the first electrolyte additive is 0.05 wt%.

[0081] Example 8

[0082] This embodiment provides an electrolyte, which is the same as that in Embodiment 1 except that the content of the first electrolyte additive is 3 wt%.

[0083] Example 9

[0084] This embodiment also provides an electrolyte, which is the same as that in Example 1 except that it does not contain the second electrolyte additive, the third electrolyte additive, the fourth electrolyte additive and the fifth electrolyte additive.

[0085] Comparative Example 1

[0086] This comparative example provides an electrolyte that is identical to that of Example 1, except that it does not include the first electrolyte additive of Example 1.

[0087] Comparative Example 2

[0088] This comparative example provides an electrolyte, wherein the electrolyte contains, in addition to the additive in the first electrolyte, [the following is also present]. Except for (CAS: 1003-61-8, purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.), everything else is the same as in Example 1.

[0089] Comparative Example 3

[0090] This comparative example provides an electrolyte, wherein the electrolyte contains, in addition to the additive in the first electrolyte, [the following is also present]. Except for (CAS: 170961-15-6, purchased from Shanghai Haohong Biomedical Technology Co., Ltd.), everything else is the same as in Example 1.

[0091] Comparative Example 4

[0092] This comparative example provides an electrolyte, wherein the electrolyte contains, except for the first electrolyte additive, […]. Except for (CAS: 176980-36-2, purchased from Shanghai Haohong Biomedical Technology Co., Ltd.), everything else is the same as in Example 1.

[0093] The electrolytes described in the above embodiments and comparative examples were used to prepare lithium-ion batteries with positive electrode sheets, separators, and negative electrode sheets. The preparation process is as follows:

[0094] (1) Preparation of positive electrode sheet

[0095] Ternary material NCM (LiNi) 0.8 Co 0.1 Mn 0.1 O2, PVDF (polyvinylidene fluoride) and SP (conductive carbon black) are mixed with N-methylpyrrolidone in a mass ratio of 96:1.8:2.2 to obtain a positive electrode slurry with a solid content of 55wt%. The positive electrode slurry is then coated onto aluminum foil through a coating process, followed by drying and cold pressing to obtain the positive electrode sheet.

[0096] (2) Preparation of negative electrode sheet

[0097] Silicon-carbon anode material (with a silicon content of 50 wt%), SP (conductive carbon black), SWCNT (single-walled carbon nanotubes), and PAA (polyacrylic acid) are mixed with deionized water in a mass ratio of 83.5:8:0.5:8 to obtain anode slurry (with a solid content of 30%). The anode slurry is then coated onto copper foil through a coating process, followed by vacuum drying and cold pressing to obtain the anode sheet.

[0098] (3) Selection of separator membrane

[0099] Polyethylene separators with ceramic coatings are selected as the separators for lithium-ion batteries.

[0100] (4) Preparation of lithium-ion batteries

[0101] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation, thus obtaining a bare cell. The bare cell is placed in an outer packaging shell, dried, and then injected with the electrolyte described in the above embodiments and comparative examples. After vacuum sealing, settling, formation, and shaping processes, a lithium-ion battery is obtained.

[0102] The electrochemical performance of the lithium-ion battery was tested at room temperature (25℃) using the LAND battery testing system of Wuhan Jinno Electronics Co., Ltd., with the charge / discharge voltage limited to 2.5V~4.4V. The specific test method is as follows:

[0103] 1) Testing of storage performance at 60℃, free water content and HF content

[0104] ① Standard charge and discharge: At 25℃, charge the lithium-ion battery at a constant current and constant voltage rate of 0.33C to 4.2V, let it stand for 10 minutes, then discharge the lithium-ion battery at a constant current rate of 0.33C to 2.5V, and let it stand for 10 minutes.

[0105] ② Initial performance test: The performance of the sample battery was tested using battery testing equipment at room temperature (25℃). The battery was charged and discharged three times at 0.33C standard, and the capacity after the third discharge was recorded as the initial capacity C0.

[0106] ③ High temperature storage: At room temperature (25℃), the lithium-ion battery is charged to 4.2 V at a constant current and constant voltage rate of 0.33C, left to stand for 30 minutes, and the cell thickness t1 is measured; then the cell is placed in a 60℃ oven for high temperature storage for 7 days.

[0107] ④ Post-storage performance test: After the storage time is reached, the battery is taken out of the high-temperature test chamber and left at room temperature for 3 hours to allow the battery temperature to return to room temperature. The cell thickness is tested and recorded as t2. The lithium-ion battery is discharged at a constant current of 0.33C to 2.5V and left to stand for 10 minutes. The discharge capacity is the retention capacity C1. Then, the battery is charged and discharged at 0.33C standard for 3 cycles. The capacity of the 3rd discharge is recorded as the post-storage capacity C2.

[0108] Cell thickness expansion rate (%) = (t2-t1) / t1×100%; Capacity retention rate = C1 / C0×100%; Capacity recovery rate = C2 / C0×100%.

[0109] Free water content and HF content testing: The free water content of the electrolyte after preparation and storage at 60℃ for 7 days was tested using a Karl Fischer moisture analyzer; the HF content of the electrolyte after storage at 60℃ for 7 days was tested using acid-base titration.

[0110] 2) Capacity retention rate after 1000 cycles at room temperature (1°C) / 1°C

[0111] At 25°C, the lithium-ion battery was charged at a constant current and constant voltage of 1C to 4.4V, with a cutoff current of 0.05C. After resting for 10 minutes, the lithium-ion battery was discharged at a constant current of 1C to 2.5V and then rested for 10 minutes. This constitutes one charge-discharge cycle. The lithium-ion battery was subjected to 1000 charge-discharge cycles using the above method. The capacity retention rate of the lithium-ion battery after 1000 charge-discharge cycles at 1C / 1C was calculated.

[0112] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity of the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0113] 3) Room temperature 6C rate performance - constant current charge ratio

[0114] At 25℃, the lithium-ion battery was discharged at a constant current rate of 1C to 2.5V, left to stand for 10 minutes, and then charged at a constant current and constant voltage rate of 6C to 4.2V with a cutoff current of 0.05C. After standing for 10 minutes, the constant current charging capacity Q1 and the total constant current and constant voltage charging capacity Q2 of the lithium-ion battery were recorded. The constant current charge ratio of the 6C rate charging was calculated according to the following formula: 6C rate charging constant current charge ratio = constant current charging capacity Q1 / total constant current and constant voltage charging capacity Q2 × 100%.

[0115] 4) Capacity retention rate at 45℃, 1C / 1C cycle for 1000 cycles

[0116] At 45°C, the lithium-ion battery was charged at a constant current and constant voltage of 1C to 4.4V, with a cutoff current of 0.05C. After resting for 10 minutes, the lithium-ion battery was discharged at a constant current of 1C to 2.5V and then rested for 10 minutes. This constitutes one charge-discharge cycle. The lithium-ion battery was subjected to 1000 charge-discharge cycles using the above method. The capacity retention rate of the lithium-ion battery after 1000 charge-discharge cycles at 1C / 1C was calculated.

[0117] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity of the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0118] The test results are shown in Table 1 below:

[0119] Table 1

[0120]

[0121] As can be seen from Table 1 above:

[0122] As shown in Example 1 and Comparative Example 1, the first electrolyte additive of this application achieves multi-functional integration of deep water removal and acid suppression, high conductivity film formation, and long-term interface stability, improving the battery's cycle performance, rate performance, and high-temperature storage performance, and does not exhibit antagonistic issues when used in combination with other additives. As shown in Example 1 and Comparative Example 2, the amino group in the first electrolyte additive of this application is protected by a tert-butoxycarbonyl group, which can prevent premature side reactions of the amino group and allow the amino group to participate in SEI film formation, further improving the battery's cycle performance. As shown in Example 1 and Comparative Example 3, the aldehyde group in the first electrolyte additive of this application can reduce the water content and HF content in the electrolyte, further enhancing the density and stability of the SEI film, thereby further improving the overall performance of the battery. As shown in Example 1 and Comparative Example 4, the main ring of this application is a sulfur-containing and / or nitrogen-containing aromatic heterocycle, which can achieve functions such as impedance reduction, film stabilization, and high voltage resistance. Further enhancing the overall performance of the battery; as shown in Examples 1 and 4-5, the main ring of the first electrolyte additive in this application also contains halogen substituents, which can cooperate with other functional groups to further enhance the overall performance of the battery; as shown in Examples 1 and 6, the sulfur-containing and / or nitrogen-containing aromatic heterocycles in this application are preferably thiazole rings containing both sulfur and nitrogen. If it is a pyridine ring as in Example 6, the interfacial conductivity is poor, the ring steric hindrance is large, the film-forming activity is insufficient, the SEI film density is low, and the cycle and rate performance of the battery will be greatly degraded; as shown in Examples 1 and 7-8, the content of the first electrolyte additive in the electrolyte of this application is preferably within a specific range, which can give full play to the optimal role of the first electrolyte additive and ensure the overall performance of the battery; as shown in Examples 1 and 9, other auxiliary additives in the electrolyte of this application can further synergize with the first electrolyte additive to further enhance the overall performance of the battery.

[0123] The above description is only a specific embodiment of this application, but the protection scope of this application is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in this application fall within the protection and disclosure scope of this application.

Claims

1. An electrolyte, characterized by, The electrolyte includes a first electrolyte additive, which includes a sulfur- and / or nitrogen-containing aromatic heterocycle and functional substituents on the sulfur- and / or nitrogen-containing aromatic heterocycle. The functional substituent includes a first substituent and a second substituent, wherein the first substituent is selected from Boc-amino and the second substituent is selected from aldehyde.

2. The electrolyte according to claim 1, characterized in that, The sulfur- and / or nitrogen-containing aromatic heterocycles are selected from any one of thiazole rings, thiophene rings, imidazole rings, or oxazole rings; And / or, the functional substituent further includes a third substituent selected from halogen substituents.

3. The electrolyte according to claim 2, characterized in that, The sulfur- and / or nitrogen-containing aromatic heterocycles are selected from thiazole rings; And / or, the chemical formula of the first electrolyte additive is shown in Formula I): ; Formula I); R1 is selected from Boc-amino, R2 is selected from aldehyde, and R3 is selected from hydrogen or halogen substituents.

4. The electrolyte additive according to claim 1 or 2, characterized in that, The first electrolyte additive comprises , or any one or a combination of at least two.

5. The electrolyte according to claim 1 or 2, characterized in that, The content of the first electrolyte additive in the electrolyte is 0.05wt%~3.0wt%; And / or, the electrolyte further includes any one or a combination of at least two of the following: a second electrolyte additive, a third electrolyte additive, a fourth electrolyte additive, and a fifth electrolyte additive, different from the first electrolyte additive; the second electrolyte additive includes 1,3-propanesulfonate lactone and / or vinyl sulfate; the third electrolyte additive includes fluoroethylene carbonate and / or vinylene carbonate; the fourth electrolyte additive includes lithium difluorophosphate and / or lithium difluorooxalate borate; and the fifth electrolyte additive includes lithium tetrafluoroborate.

6. The electrolyte according to claim 5, characterized in that The content of the second electrolyte additive in the electrolyte is 0.1wt%~2.0wt%; And / or, the content of the third electrolyte additive in the electrolyte is 0.5wt%~8.0wt%; And / or, the content of the fourth electrolyte additive in the electrolyte is 0.1wt%~2.0wt%; And / or, the content of the fifth electrolyte additive in the electrolyte is 0.1wt%~1.0wt%.

7. The electrolyte according to claim 1 or 2, characterized in that, The electrolyte also includes an organic solvent, which includes cyclic carbonates and chain carbonates, wherein the mass ratio of the cyclic carbonates to the chain carbonates is (20~40):(60~80), the cyclic carbonates include ethylene carbonate and / or propylene carbonate, and the chain carbonates include any one or a combination of at least two of dimethyl carbonate, diethyl carbonate, or methyl ethyl carbonate. The electrolyte also includes lithium salts, which include any one or a combination of at least two of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, or lithium difluorooxalateborate. The content of lithium salts in the electrolyte is 10wt% to 15wt%.

8. A secondary battery characterized by comprising: The secondary battery includes the electrolyte as described in any one of claims 1-7.

9. The secondary battery according to claim 8, characterized by The negative electrode material in the secondary battery includes a silicon-based negative electrode material; And / or, the positive electrode material in the secondary battery comprises a ternary material, a chemical general formula of the ternary material is LiNi x Co y Mn 1-x-y O2, 0.8≤x<1, 0≤y≤0.

2.

10. An electric device, characterized by The electrical equipment includes the secondary battery as described in claim 8 or 9.