An electrolyte and a battery

By adding compound of formula I to the electrolyte in synergy with vinylene carbonate and methane disulfonate, and by controlling the pore size of the positive electrode active material, the problems of electrolyte turbidity and high-temperature gas generation in lithium iron phosphate batteries are solved, thereby improving the high-temperature cycle stability and lifespan of the battery.

CN123120889APending Publication Date: 2026-11-17GUANGZHOU TINCI MATERIALS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611613510.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing electrolytes are prone to turbidity when containing methylene disulfonate (MMDS), and lithium iron phosphate batteries are prone to gas generation under high-temperature cycling, affecting the battery's high-temperature cycling stability and lifespan.

Method used

By adding the compound shown in Formula I to the electrolyte in synergistic effect with vinylene carbonate and methane disulfonate, the additive ratio and pore size of the positive electrode active material are controlled, forming a stable interface layer, inhibiting OC bond breaking and ferrous ion dissolution, and improving the stability of the electrolyte and lithium ion transport.

Benefits of technology

It effectively alleviates the problem of electrolyte turbidity, reduces the rate of change of battery impedance during high-temperature cycling, and increases the battery's cycle life and high-temperature storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120889A_ABST
    Figure CN123120889A_ABST
Patent Text Reader

Abstract

This application discloses an electrolyte and a battery. The electrolyte includes a first additive, a second additive, and a third additive; the first additive includes a compound with the structural formula shown in Formula I: Formula I; in Formula I, R1 and R2 are each independently selected from straight-chain alkyl or branched-chain alkyl groups having 1 to 3 carbon atoms; the second additive is vinylene carbonate; the third additive is methane disulfonate; based on the total mass of the electrolyte, the mass percentage of the first additive is 0.5% to 5%. This application improves the electrolyte formulation, thereby enhancing the stability of the electrolyte, reducing the impedance change rate of the battery during high-temperature cycling, and increasing cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of battery technology, specifically relating to an electrolyte and a battery. Background Technology

[0002] With the rapid development of new energy technologies, electrochemical energy storage batteries are increasingly widely used in 3C digital devices, electric bicycles, electric vehicles, power tools, electric aircraft, drones, and other fields. Therefore, the performance and safety requirements for electrochemical energy storage batteries are becoming increasingly stringent. However, the high-temperature performance of existing batteries is insufficient to meet these demands; for example, under high-temperature conditions, the battery's internal resistance increases, and its cycle performance decreases.

[0003] Especially in the application of lithium iron phosphate (LFP) batteries in power and energy storage fields, higher requirements are placed on the high-temperature cycle life and calendar life of LFP batteries. This necessitates electrolytes that can significantly improve the high-temperature cycle stability and high-temperature storage stability of lithium batteries. Methylene methane disulfonate (MMDS) possesses excellent high-temperature performance; it can not only improve the initial efficiency of lithium batteries but also significantly improve the capacity retention rate and inhibit the growth of DCR during high-temperature storage, making it an excellent high-temperature resistant additive for improving the high-temperature performance of LFP batteries. However, we have found that MMDS encounters stability issues in practical use. Electrolytes containing MMDS are prone to turbidity during preparation, storage, and transportation, leading to abnormal turbidity and ultimately failing to meet shipping standards. Existing technologies do not provide in-depth analysis of this problem or offer targeted solutions, severely impacting the application of MMDS in LFP battery systems.

[0004] Furthermore, the inventors noted that lithium iron phosphate batteries are prone to gas production under high-temperature cycling conditions when they are at a low or high state of charge. Accumulated gas can crowd out the pores of the secondary particles in the positive electrode and hinder electrolyte wetting, thereby degrading cycle performance. Existing technologies have not yet found a specific solution to address the stability issues of MMDS-containing electrolytes while simultaneously suppressing the aforementioned gas production problem. Summary of the Invention

[0005] This application aims to at least partially address one of the technical problems in the related art. To this end, this application proposes an electrolyte that, by synergistically acting the compound shown in Formula I with vinylene carbonate and methylene disulfonate, can alleviate the electrolyte turbidity problem caused by methylene disulfonate, and reduce the rate of change of battery impedance and increase cycle life during high-temperature cycling.

[0006] The first aspect of this application protects an electrolyte comprising a first additive, a second additive, and a third additive; The first additive includes a compound with the structural formula shown in Formula I:

[0007] Formula I; In Formula I, R1 and R2 are each independently selected from straight-chain alkyl or branched alkyl groups having 1 to 3 carbon atoms; The second additive is vinylene carbonate; The third additive is methylene methane disulfonate; Based on the total mass of the electrolyte, the mass percentage of the first additive is a%, and 0.5 ≤ a ≤ 5.

[0008] In some implementations, at least one of the following is satisfied: Based on the total mass of the electrolyte, the mass percentage of the second additive is b%, and 0.5 ≤ b ≤ 5. Based on the total mass of the electrolyte, the mass percentage of the third additive is c%, and 0.1 ≤ c ≤ 4.

[0009] In some embodiments, the electrolyte satisfies at least one of the following (I) to (III): (I) 1 ≤ a ≤ 4; (II) 1≤b≤4; (III) 0.3 ≤ c ≤ 1.5.

[0010] In some embodiments, in Formula I, R1 and R2 are each independently selected from straight-chain alkyl groups having 1 to 3 carbon atoms.

[0011] In some implementations, (2a+b) / c ≥ 2.5; In some embodiments, the first additive includes: Formula I-1 , Formula I-2 , Formula I-3 , Formula I-4 , Formula I-5 Any one or more of the following.

[0012] In some embodiments, the electrolyte further includes an electrolyte salt and a solvent; and satisfies at least one of the following (i) to (iii): (i) The electrolyte salt includes one or more of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium bis(oxalate)borate, lithium difluorooxalateborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethane)sulfonylimide, lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, and lithium tetrafluorooxalate phosphate. (ii) Solvents include carbonate solvents; carbonate solvents include one or more of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate; (iii) The solvent includes carboxylic acid ester solvents, which include one or more of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate, and ethyl butyrate.

[0013] This application, by synergistically combining the compound shown in Formula I with methylene disulfonate and vinylene carbonate, can alleviate the turbidity changes caused by the instability of methylene disulfonate in the formulation, and solve the problem of electrolyte turbidity that is easily caused by electrolyte formulations containing methylene disulfonate. It can achieve the technical effect of better controlling the quality of the shipped electrolyte. At the same time, the electrolyte formulation has a good improvement effect in reducing the impedance change rate of the battery during high-temperature cycling and increasing the cycle life.

[0014] Furthermore, by controlling the dosage of the three additives shown in Formula I, methylene disulfonate, and vinylene carbonate to be (2a+b) / c≥2.5, the problem of turbidity changes caused by the instability of methylene disulfonate in the formulation can be solved, achieving a better technical effect of controlling the quality of the electrolyte shipment.

[0015] The second aspect of this application provides a battery, including a positive electrode, a negative electrode, a separator, and an electrolyte provided in the first aspect of this application. The positive electrode includes a positive active material layer, the positive active material layer includes a positive active material, and the positive active material includes lithium iron phosphate material. The average pore size of the secondary particles of the lithium iron phosphate material is D nm, where 5 ≤ D ≤ 40. The battery satisfies the following conditions: 6≤( )D+aD≤353; Based on the total mass of the electrolyte, the mass percentage of the first additive is a%, the mass percentage of the second additive is b%, and the mass percentage of the third additive is c.

[0016] In some embodiments, the surface of the positive electrode active material particles is at least partially coated with carbon material.

[0017] In some implementations, the battery satisfies at least one of the following (α) and (β): (α)10≤D≤25; (β)11≤( )D+aD≤300.

[0018] Furthermore, by designing the average pore size of the secondary particles of lithium iron phosphate positive electrode active material, as well as the relevant formulas for the dosage of three additives—compound of formula I, methylene disulfonate, and vinylene carbonate—the gas generation problem of lithium iron phosphate batteries under high and low SOC conditions is improved, while also exhibiting good high-temperature performance of the battery.

[0019] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Detailed Implementation

[0020] The embodiments of this application are described in detail below and are intended to explain this application, but should not be construed as limiting this application.

[0021] The following explanation uses a lithium-ion battery as an example. The battery includes an electrolyte. Methylene methane disulfonate (chemical formula C2H4O6S2, CAS number 99591-74-9, abbreviated as MMDS) used in the electrolyte has excellent high-temperature performance. It can not only improve the initial coulombic efficiency of lithium-ion batteries, but also significantly improve the capacity retention rate and inhibit the growth of DCR during high-temperature storage. However, MMDS is prone to causing precipitation in the electrolyte, which greatly shortens the shelf life of the electrolyte. Further research has found that hydrogen fluoride (HF) byproducts are difficult to avoid in the electrolyte. The OC bond in the MMDS molecule is prone to breakage in the presence of trace amounts of hydrogen fluoride to form an unstable intermediate state. Free lithium ions in the electrolyte combine with this unstable intermediate state and easily form precipitates.

[0022] Therefore, a first aspect of the embodiments of this application provides an electrolyte including a first additive, a second additive, and a third additive; The first additive comprises a compound with the structural formula shown in Formula I:

[0023] Formula I; In Formula I, R1 and R2 are each independently selected from straight-chain alkyl or branched alkyl groups having 1 to 3 carbon atoms. The second additive is vinylene carbonate; The third additive is methylene disulfonate; Based on the total mass of the electrolyte, the mass percentage of the first additive is a%, and 0.5 ≤ a ≤ 5.

[0024] As an example, a is a range of values ​​between 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8, 5.0, or any two of these.

[0025] The embodiments of this application, by synergistically combining the compound shown in Formula I with methylene methane disulfonate and vinylene carbonate, can alleviate the electrolyte turbidity problem caused by methylene methane disulfonate. At the same time, the electrolyte formulation has a good effect on reducing the impedance change rate of the battery during high-temperature cycling and increasing cycle life.

[0026] Research has shown that the compound shown in Formula I can improve the structural stability of methylene disulfonate, which helps to block the formation of precipitates, thereby alleviating the problem of easy turbidity in electrolytes containing methylene disulfonate and improving the stability of the electrolyte. Specifically, the N atom on the -N-SO2-F group provided in the compound shown in Formula I has a lone electron, which can combine with the C atom on the OC bond of methylene disulfonate, providing an additional electron cloud for the OC bond of methylene disulfonate, making it more stable, significantly reducing the risk of OC bond breakage, thereby blocking the process of CO breakage leading to the combination of O atoms with free lithium ions, significantly blocking the process of precipitate formation, thus alleviating the problem of easy turbidity in electrolytes containing methylene disulfonate and reducing the turbidity of the electrolyte.

[0027] However, relying solely on the compound shown in Formula I to alleviate the turbidity of the methane disulfonate-containing electrolyte is insufficient to meet the shipment standards. It was found that adding vinylene carbonate along with the compound shown in Formula I can further reduce the turbidity of the methane disulfonate-containing electrolyte, thus bringing the electrolyte quality up to the shipment standard. The simultaneous presence of the compound shown in Formula I and vinylene carbonate (CAS No. 872-36-6) effectively shields the contact between hydrofluoric acid and methane disulfonate in the electrolyte, better preventing the breakage of the OC bonds in the molecule in the presence of trace amounts of hydrogen fluoride. The specific mechanism is as follows: The N atom on the -N-SO2-F group provided in the compound shown in Formula I has lone electrons, which is conducive to its attraction of hydrogen ions in hydrofluoric acid. At the same time, the C atom on the C=O double bond in vinylene carbonate has a partially positive charge. When it approaches the F atom in hydrofluoric acid, due to the high electronegativity of the F atom, the two can have a weak interaction. Finally, the three form a cluster of compound shown in Formula I - hydrofluoric acid - vinylene carbonate, which prevents it from effectively attacking methane disulfonate methylene ester.

[0028] In summary, through the synergistic effect of the compound shown in Formula I and vinylene carbonate, as well as the effect of the N atom on the -N-SO2-F group of the compound shown in Formula I, the high turbidity problem caused by the instability of methylene disulfonate in the electrolyte formulation can be alleviated, achieving a better technical effect in controlling the quality of the shipped electrolyte. Simultaneously, the electrolyte formulation has a significant effect in reducing the rate of change in battery impedance and increasing cycle life during high-temperature cycling.

[0029] Further investigation revealed that when the amounts of the compound shown in Formula I, vinylene carbonate, and methylene disulfonate, based on the total mass of the electrolyte, are a%, b%, and c%, respectively, satisfying the formula (2a+b) / c≥2.5, the compound shown in Formula I can better enhance the structural stability of methylene disulfonate. Ultimately, in the presence of both the compound shown in Formula I and vinylene carbonate, the clusters of the compound shown in Formula I—hydrofluoric acid—vinylene carbonate are better formed. This further reduces the amount of freely moving hydrofluoric acid in the electrolyte, preventing hydrofluoric acid from effectively contacting or attacking methylene disulfonate. This improves the stability of the electrolyte formulation containing methylene disulfonate and meets the controllable shipping standard requirements.

[0030] In some implementations, the electrolyte satisfies at least one of the following: Based on the total mass of the electrolyte, the mass percentage of the second additive is b%, and 0.5 ≤ b ≤ 5. Based on the total mass of the electrolyte, the mass percentage of the third additive is c%, 0.1≤c≤4.

[0031] As an example, b is a value ranging from 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.2, 1.4, 1.6, 1.8, 2.0, 2.2, 2.4, 2.6, 2.8, 3.0, 3.2, 3.4, 3.6, 3.8, 4.0, 4.2, 4.4, 4.6, 4.8, 5.0, or any two of these values.

[0032] For example, c is 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.5, 2.0, 2.5, 3.0. 3.5, 4.0, or any value between the two.

[0033] In some embodiments, the electrolyte satisfies at least one of the following (I) to (III): (I) 1 ≤ a ≤ 4; (II) 1≤b≤4; (III) 0.3 ≤ c ≤ 1.5.

[0034] In some embodiments, in Formula I, R1 and R2 are each independently selected from straight-chain alkyl groups having 1 to 3 carbon atoms.

[0035] The compound shown in Formula I uses alkyl groups instead of non-alkyl groups such as alkenyl, alkynyl, or benzene rings. This is primarily because the aforementioned non-alkyl groups would increase the overall activity of the molecule, leading to its rapid consumption during battery charging and discharging. Furthermore, alkyl groups are electron-donating groups for the N and S groups on the molecule, slightly increasing the electron cloud density on the N atom, thus enhancing its stabilizing effect on methylene disulfonate. Further, short-chain alkyl groups are chosen due to steric hindrance. If the molecular chain is too long, the interaction between the compound of Formula I and methylene disulfonate and vinylene carbonate (VC) becomes more difficult, making it harder to solve the stability problem of electrolyte formulations containing methylene disulfonate. Simultaneously, suitable alkyl groups and chain lengths have the effect of reducing the battery's DCR rate and improving its cycle performance.

[0036] In some embodiments of this application, the first additive includes: Formula I-1 , Formula I-2 , Formula I-3 , Formula I-4 , Formula I-5 Any one or more of the following. Among them, the CAS number of the compound represented by Formula I-1 is 354-44-9; the CAS number of the compound represented by Formula I-2 is 1458771-72-6; the CAS number of the compound represented by Formula I-3 is 2826747-29-7; the CAS number of the compound represented by Formula I-4 is 382-97-8; and the CAS number of Formula I-5 is 3136357-24-6.

[0037] The compounds shown in Formulas I-1 to I-5 above can exert a better synergistic effect with methylene disulfonate and vinylene carbonate, better alleviate the electrolyte turbidity problem caused by methylene disulfonate, and further reduce the battery impedance change rate and increase cycle life during high-temperature cycling.

[0038] In some embodiments of this application, the electrolyte further includes an electrolyte salt and a solvent; and satisfies at least one of the following (i) to (iii): (i) The electrolyte salt includes one or more of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium bis(oxalate)borate, lithium difluorooxalateborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethane)sulfonylimide, lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, and lithium tetrafluorooxalate phosphate. (ii) Solvents include carbonate solvents; carbonate solvents include one or more of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate; (iii) The solvent includes carboxylic acid ester solvents, which include one or more of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate, and ethyl butyrate.

[0039] The electrolyte salt in the embodiments of this application can be a lithium salt known in the art. For example, it can include, but is not limited to, one or more of lithium hexafluorophosphate (LiPF6), lithium hexafluoroarsenate (LiAsF6), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiB(C2O4)2 or lithium di(oxalato)borate), lithium difluorooxalato)borate (LiBF2C2O4), lithium bis(fluorosulfonyl)imide (LiN(SO2F)2), lithium bis(trifluoromethane)sulfonyl)imide (LiN(SO2CF3)2), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalato)phosphate (LiPF2(C2O4)2 or lithium difluorobis(oxalato)phosphate), and lithium tetrafluorooxalato)phosphate (LiPF4C2O4).

[0040] Furthermore, the electrolyte salt used in this embodiment can be lithium hexafluorophosphate (LiPF6). Since trace amounts of moisture are unavoidable in the electrolyte during production processes, lithium hexafluorophosphate decomposes upon contact with moisture, releasing hydrogen fluoride. This hydrogen fluoride reacts with methylene methane disulfonate to form a precipitate. This embodiment uses a combination of the compound shown in Formula I, methylene methane disulfonate, and vinylene carbonate as additives to improve the precipitation problem, better adapt to the lithium hexafluorophosphate electrolyte system, improve electrolyte stability, and enhance the battery's high-temperature performance.

[0041] In this application, the solvent may be a solvent known in the art. As an example, it may include, but is not limited to, one or a combination of carbonate solvents and carboxylic acid ester solvents.

[0042] A second aspect of this application provides a battery, including a positive electrode, a negative electrode, a separator, and an electrolyte provided in the first aspect of this application. The positive electrode includes a positive active material layer, the positive active material layer includes a positive active material, and the positive active material includes lithium iron phosphate material. The average pore size of the secondary particles of the lithium iron phosphate material is D nm, where 5 ≤ D ≤ 40. The battery satisfies the following conditions: 6≤( )D+aD≤353; Based on the total mass of the electrolyte, the mass percentage of the first additive is a%, the mass percentage of the second additive is b%, and the mass percentage of the third additive is c.

[0043] As an example, the average pore size D of the secondary particles of lithium iron phosphate material is 5nm, 7nm, 9nm, 11nm, 13nm, 15nm, 17nm, 19nm, 20nm, 23nm, 25nm, 27nm, 29nm, 31nm, 33nm, 35nm, 37nm, 39nm, 40nm or any value between the two.

[0044] As an example, ( The value of D+aD is 6, 20, 40, 60, 80, 100, 120, 140, 160, 180, 200, 220, 240, 260, 280, 300, 320, 340, 350, 353 or any value between the two.

[0045] Lithium iron phosphate (LFP) batteries are prone to gas generation under high-temperature cycling conditions, particularly in areas with low or high charge levels. This phenomenon is closely related to internal battery polarization: under high and low charge states, internal polarization increases significantly, reducing the stability of the LFP positive electrode active material or the LFP lattice formed after delithiation. This makes it easier for ferrous ions to break through the lattice and dissolve. The dissolved ferrous ions shuttle between the positive and negative electrodes during charging and discharging, catalyzing the decomposition of the electrolyte solvent on the electrode surface and generating gas. The continuous accumulation of gas occupies the pores within the secondary particles of the LFP material, hindering the electrolyte's penetration into the secondary particles, obstructing lithium-ion transport channels, and ultimately degrading battery cycle performance.

[0046] To address the aforementioned problems, this application's implementation method simultaneously controls the electrolyte additive system and the microporous structure of the lithium iron phosphate material, ensuring that the contents of the compounds shown in Formula I (a%), vinylene carbonate (b%), and methylene disulfonate (c%), along with the average pore size D of the secondary particles in the lithium iron phosphate material, synergistically satisfy the following relationship: 6≤( )D+aD≤353.

[0047] In the formula, a / (b+c) represents the ratio of the compound shown in Formula I to the total content of vinylene carbonate and methane disulfonate, reflecting the electrolyte bulk interaction among the three additives. Specifically, methane disulfonate is prone to OC bond breakage during interfacial film formation, and the oxygen atoms generated by the breakage will capture free lithium ions in the system. Vinylene carbonate is a film-forming additive, but it is continuously consumed under high temperature and long cycle, and its window of action is short.

[0048] When a / (b+c) is at an appropriate level, the compound shown in Formula I can fully exert its dual synergistic effect: on the one hand, it inhibits the side reaction in which oxygen atoms generated from the decomposition of methane disulfonate combine with free lithium ions; on the other hand, it continuously protects the interfacial film formed by vinylene carbonate, prolonging the effective duration of vinylene carbonate in the cycling system. If a / (b+c) is too small, the proportion of the compound shown in Formula I is insufficient, making it difficult to fully regulate the decomposition side reaction of methane disulfonate and maintain the long-term film-forming effect of vinylene carbonate; if a / (b+c) is too large, the excessive amount of LiF and sulfate / sulfite-dominated interfacial components spontaneously formed by the compound shown in Formula I will lead to an abnormally high interfacial film impedance, hindering lithium ion conduction.

[0049] ( Item D, a / (b+c) multiplied by the average pore size D, characterizes the ability of the ternary additives to exert interface regulation in the pore space of the positive electrode active material under this additive ratio; Item aD couples the absolute amount of the compound shown in Equation I with the average pore size of the secondary particles, characterizing the effective enrichment level of the compound shown in Equation I in the pores of the positive electrode active material and its comprehensive potential for capturing iron ions. This combined formula no longer limits the electrolyte ratio and the pore structure of the positive electrode active material as two independent parameters, but constructs a unified synergistic formula: the bulk interaction between additives in the electrolyte matches the pore space scale of the secondary particles in the positive electrode lithium iron phosphate material, which is beneficial to suppress the gas generation problem caused by the dissolution of divalent iron under high temperature and high and low charge ranges from the root. The specific mechanism is as follows: ① Within the parameter range that satisfies the above relationship, during the electrolyte injection stage, the electrolyte can fully penetrate and wet the secondary pores of the lithium iron phosphate material. The capillary force is sufficient, the pore connectivity is good, and the bubbles are easily discharged. The compound shown in Formula I, methylene disulfonate, and vinylene carbonate enter the interparticle gaps simultaneously with the electrolyte wetting.

[0050] ② The electron cloud of the compound shown in Formula I is concentrated in the -SO2F group, exhibiting electron-rich characteristics. It can capture ferrous ions dissolved by the battery under low or high charge conditions in the Helmholtz-Perrin double layer at the positive electrode-electrolyte interface. At the same time, D is controlled in the range of 5nm~40nm to ensure the lithium ion transport efficiency in the secondary particles. This promotes the formation of an interface component mainly composed of LiF and sulfate / sulfite at the positive electrode interface of the compound shown in Formula I, inhibiting the migration of ferrous ions to the electrolyte and negative electrode side, and weakening the reaction pathway of ferrous ions catalyzing the decomposition of electrolyte solvent to produce gas.

[0051] ③ The average pore size of the secondary particles, ranging from 5 nm to 40 nm, provides suitable space for the synergistic formation of polyvinyl carbonate interfacial components with embedded sulfonate groups during the formulation and compatibility stage of the compound shown in Formula I, methylene disulfonate, and vinylene carbonate. This interfacial component, on the one hand, fills the pores within the secondary particles, suppressing the gas generated under high and low charge states from crowding out the pore space; on the other hand, it possesses good ionic conductivity, providing a continuous pathway for lithium-ion transport and ensuring normal lithium-ion insertion / extraction on the positive electrode side in the later stages of cycling.

[0052] The interface layer formed by the synergy of these three components possesses electronic insulation, thermal stability, and mechanical toughness, exhibiting low negative impact on the lithium-ion intercalation / deintercalation process during the formation and capacity testing phase. It simultaneously achieves a comprehensive effect of extending electrolyte shelf life, improving battery high-temperature cycle life, suppressing DCR growth under high-temperature storage, and reducing battery expansion rate at high temperatures. The battery electrochemical performance is no longer an independent superposition of the effects of the electrolyte additive system and the pore structure of the cathode active material, but rather, under the constraints of the aforementioned joint mathematical relationship, the interaction of the ternary electrolyte additives and the matching and synergistic effect of the pore microstructure of the cathode active material solve the core problem of iron dissolution induced by polarization and gas generation clogging pores in the lithium iron phosphate system at high temperatures and between high and low charge ranges.

[0053] Secondary particles of positive electrode active materials refer to larger aggregates (or composite particles) formed by the aggregation and bonding of multiple small primary particles (crystals) through weak interaction forces.

[0054] The average pore size of the secondary particles of the positive electrode active material affects the wetting effect of the electrolyte, and thus affects the performance of each additive in the electrolyte. In the embodiments of this application, the average pore size of the secondary particles of the lithium iron phosphate material is designed to be 5nm-40nm, which is beneficial to improve the wetting effect of the electrolyte, enhance the synergistic effect of the first additive, the second additive, and the third additive on the electrolyte and the battery, and better improve the high-temperature cycle and storage performance of the battery.

[0055] As an example, the average pore size D of secondary particles in lithium iron phosphate materials can be detected by gas adsorption (i.e., static volumetric method). This method is based on the principle of gas adsorption. By measuring the amount of gas adsorbed by the material under different relative pressures, the adsorption-desorption isotherms are obtained, and then the specific surface area and pore size distribution parameters are calculated.

[0056] In this application, there are no particular restrictions on the preparation method of the positive electrode active material, as long as the purpose of this application can be achieved. For example, in the process of preparing lithium iron phosphate material by solid-phase synthesis, the average pore size of the secondary particles of lithium iron phosphate material can be controlled by controlling parameters such as processing temperature, processing time, and heating rate.

[0057] As an example, a method for preparing secondary particles of lithium iron phosphate material is provided. In the solid-phase synthesis process, the average pore size of the secondary lithium iron phosphate particles is controlled by adjusting relevant step parameters. Exemplarily, a solution is prepared using lithium, iron, and phosphorus sources as raw materials. The solution is dispersed by high-speed shearing, followed by spray drying, pre-sintering treatment, and high-temperature calcination to obtain lithium iron phosphate material or lithium iron phosphate material with a carbon coating. During the preparation process, the average pore size of the secondary lithium iron phosphate particles can be controlled by adjusting the spray pressure, spray drying temperature, and calcination temperature.

[0058] Furthermore, the average pore size of the secondary particles in the lithium iron phosphate material can be controlled by adjusting the spray pressure (0.08 MPa-0.5 MPa), the inlet air temperature (180℃-240℃), and the calcination temperature (580-750℃). For example, the lithium iron phosphate material in this application can be prepared by the following preparation method: (1) Preparation of precursor slurry: Weigh out the lithium source (Li₂CO₃), iron source (Fe(NO₃)₃·9H₂O), phosphorus source (NH₄H₂PO₄), and carbon source (glucose) according to stoichiometric ratios, maintaining a Li:Fe:P:carbon source molar ratio of 1:1:1:1 (considering volatilization losses during high-temperature calcination, the lithium source can be added in excess by 3%-5%). Dissolve the above raw materials in deionized water to prepare a mixed suspension with a solid content of 10 wt%–20 wt%. Place the mixed suspension in a planetary ball mill and ball mill for 15 h using deionized water as the medium to fully refine and homogenize the raw materials, obtaining a precursor slurry. After preparing the slurry, directly ball mill for 15 h to fully refine and homogenize the raw materials.

[0059] (2) Two-fluid spray drying: The precursor slurry was atomized and dried using a two-fluid nozzle spray dryer (Yamato ADL311S, nozzle diameter 0.4 mm). The operating parameters were set as follows: Spray pressure: 0.08 MPa-0.5 MPa; Inlet air temperature: 180℃-240℃; Air outlet temperature: 80℃-103℃; Feed rate: 4.5 mL / min - 15 mL / min.

[0060] During spray drying, the precursor solution is pumped to a two-fluid nozzle, where compressed air tears the slurry into micron-sized droplets. These droplets come into contact with hot air inside the drying tower, causing rapid evaporation of moisture. The suspended primary particles aggregate to form porous spherical or annular secondary particles. The dried powder is collected by a cyclone separator as the precursor powder.

[0061] (3) Calcination treatment: The collected precursor powder was first dried at 120 °C for 5 h to remove residual moisture. It was then placed in a tube furnace and calcined under an argon (Ar) atmosphere. The calcination regime was as follows: the temperature was increased to 350-450 °C at a rate of 2-5 °C / min and held for 3-6 h (pre-calcination stage). After the pre-sintered intermediate product was allowed to cool naturally, it was then ground to break up any possible soft agglomerates. The ground powder was then placed back in the tube furnace and subjected to high-temperature crystallization calcination under a flowing inert atmosphere (argon or a nitrogen-argon mixture), increasing the temperature to 580-750 °C at a rate of 3-5 °C / min and holding for 8-15 h. Finally, it was allowed to cool naturally to room temperature to obtain the lithium iron phosphate / carbon-coated composite material. The cooled sintered block was removed, mechanically ground, and passed through a 400-mesh sieve to obtain the lithium iron phosphate / carbon-coated composite material.

[0062] In some embodiments of this application, the surface of the positive electrode active material particles is at least partially coated with carbon material.

[0063] By coating the surface of the positive electrode active material particles with carbon material, the conductivity of the positive electrode side can be improved and the battery impedance can be reduced.

[0064] In some embodiments of this application, the battery satisfies at least one of the following (α) and (β): (α)10≤D≤25; This facilitates better compatibility between the compound shown in Formula I, methylene disulfonate, vinylene carbonate, and secondary particles of the positive electrode active material, thereby improving the battery's high-temperature cycle and storage performance and reducing gas production.

[0065] (β)11≤( )D+aD≤300. The battery exhibits better high-temperature cycle and high-temperature storage performance, which is beneficial for better solving the gas generation problem of lithium iron phosphate batteries at high and low SOC.

[0066] In some embodiments of this application, the negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one side surface of the negative current collector, the negative electrode film layer including a negative electrode active material.

[0067] In some embodiments of this application, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, and lithium titanate, etc. Silicon-based materials may include at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may include at least one of elemental tin, tin oxide compounds, and tin alloys.

[0068] In some embodiments of this application, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).

[0069] In some embodiments of this application, the negative electrode film layer may optionally include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), sodium carboxymethyl cellulose (CMC), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0070] In some embodiments of this application, the negative electrode film layer may optionally include a conductive agent. The conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0071] In some embodiments of this application, the positive electrode sheet includes a positive current collector and a positive electrode film layer disposed on at least one side surface of the positive current collector, the positive electrode film layer including a positive electrode active material.

[0072] In some embodiments of this application, the positive electrode current collector may include a metal foil or a composite positive electrode current collector. For example, the metal foil may be aluminum foil. The composite positive electrode current collector may include a polymer material substrate and a metal layer formed on at least one surface of the polymer material substrate. For example, the composite negative electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).

[0073] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.

[0074] In some embodiments of this application, the positive electrode film layer may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0075] In some embodiments of this application, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.

[0076] In some embodiments of this application, the battery further includes a separator, which includes, but is not limited to, glass fiber, nonwoven fabric, polyethylene, polypropylene, or polyvinylidene fluoride.

[0077] The present application will now be described with reference to specific embodiments. It should be noted that these embodiments are merely descriptive and do not limit the present application in any way. The reagents used in the embodiments are all from Aladdin Biochemical Technology Co., Ltd.

[0078] [Performance Testing] 1. High-temperature cycling performance test: Place the lithium-ion battery in a 60℃ constant temperature test chamber and let it stand for 30 minutes to allow it to reach a constant temperature. Charge it at a constant current of 1.0C to 3.65V, then charge it at a constant voltage until the cutoff current is 0.05C. Let it stand for 30 minutes, then discharge it at a constant current of 1.0C to 2.0V. Record this as the discharge capacity C0. Repeat this process until the capacity decays to 80% of C0. Record the number of cycles, which is the "number of cycles at 60℃ high temperature to 80% SOH".

[0079] 2. Expansion rate during 60℃ high-temperature cycling: The lithium-ion battery was placed in a 60℃ constant temperature test chamber and left to stand for 30 minutes to reach a constant temperature. Its initial thickness was measured using a thickness gauge and recorded as T1. Then, the lithium-ion battery was transferred to the 60℃ constant temperature test chamber for high-temperature cycle performance testing. Specifically: the lithium-ion battery was placed in the 60℃ constant temperature test chamber and left to stand for 30 minutes to reach a constant temperature. It was then charged at a constant current of 1.0C to 3.65V, then charged at a constant voltage to a cutoff current of 0.05C, left to stand for 30 minutes, and then discharged at a constant current of 1.0C to 2.0V, which was recorded as the discharge capacity C0. This cycle was repeated until the capacity decayed to 80% of C0. The thickness of the battery after high-temperature cycling was measured using a thickness gauge and recorded as T2. The battery expansion rate after 60℃ high-temperature cycling is calculated as 100% × (T2 - T1) / T1.

[0080] 3. DCR change rate after storage at 60℃: The lithium-ion battery was placed in a 25°C constant temperature chamber and left to stand for 30 minutes. Then, it was charged at a constant current of 1.0C to a voltage of 3.65V, discharged at a constant current of 1.0C for 30 minutes, left to stand for 1 hour, and then discharged at a current I1 corresponding to a 2.0C rate for 10 seconds. The corresponding voltage was recorded as V1. The DC resistance (DCR) of the lithium-ion battery at 50% state of charge (SOC), i.e., the initial DCR = V1 / I1, is denoted as R1, with units of mΩ. After charging the lithium-ion battery at a constant current of 1.0C to a voltage of 3.65V, it was transferred to 60°C and stored for 30 days. The DCR after high-temperature storage was tested using the above method and recorded as R2. The DCR change rate of the battery stored at 60°C is 100% × (R2 - R1) / R1.

[0081] 4. Electrolyte stability: The electrolytes prepared in the examples and comparative examples were respectively placed in sealed aluminum bottles, which were vacuum-sealed with aluminum-plastic film and stored in a constant temperature chamber set at 25°C. Samples were taken in a glove box after 15 days of storage, and the turbidity of the electrolyte was measured using a turbidimeter (instrument model: HACH 2100N), with the unit being NTU.

[0082] 5. Test method for the average pore size of secondary particles in cathode materials: The gas adsorption method (i.e., static volumetric method) was used for determination. This method is based on the principle of gas adsorption; by measuring the amount of gas adsorbed by the material under different relative pressures, adsorption-desorption isotherms are obtained, and then the specific surface area and pore size distribution parameters are calculated. The specific test steps are as follows: (1) Sample pretreatment: The cathode material sample is placed in a vacuum degassing device and degassed at 150℃~300℃ for 4~12 hours to thoroughly remove adsorbed moisture and impurity molecules from the sample surface and pores, ensuring sample surface cleanliness. The degassing temperature should not be too high to avoid damaging the porous structure of the material.

[0083] (2) Determination of adsorption-desorption isotherms: Using high-purity nitrogen (N2) as the adsorbate, the adsorption-desorption isotherms of the samples were determined by static volumetric method at liquid nitrogen temperature (-196℃). During the measurement, nitrogen was gradually and quantitatively injected into the sample tube, and the amount of nitrogen adsorbed at each equilibrium pressure was recorded until saturation adsorption was reached; then the pressure was gradually reduced, and the desorption curve was recorded. The pore size measurement range is generally 0.35 nm to 500 nm, which can cover the target pore size range of 5 nm to 40 nm in the embodiments of this application.

[0084] (3) Calculation of specific surface area: Based on adsorption isotherm data, the total specific surface area of ​​the sample was calculated using the BET (Brunauer-Emmett-Teller) multilayer adsorption theory.

[0085] (4) Calculation of average aperture: The desorption isotherm was analyzed using the Barrett-Joyner-Halenda (BJH) model to calculate the pore size distribution curve. The BJH method, based on capillary condensation theory, is suitable for analyzing the pore size distribution of mesoporous (2 nm to 50 nm) materials.

[0086] The formula for calculating the average aperture D is: D = 4V / S.

[0087] in: V is the total pore volume (cm³) 3 / g), which is calculated from the adsorption amount at a relative pressure P / P0≈0.99 by the adsorption isotherm; S is the BET specific surface area (m²) 2 / g); D is the average aperture (nm), assuming the pore is a cylindrical model.

[0088] (5) Testing instruments The Micromeritics ASAP 2460 fully automated surface area and porosity analyzer (pore size analysis range 0.35nm~500nm) was used.

[0089] Preparation of positive electrode active materials (1) Preparation of precursor slurry: Weigh out lithium source (Li₂CO₃), iron source (Fe(NO₃)₃·9H₂O), phosphorus source (NH₄H₂PO₄), and carbon source (glucose) according to stoichiometric ratios, maintaining a Li:Fe:P:carbon source molar ratio of 1:1:1:1 (considering volatilization losses during high-temperature calcination, lithium source can be added in excess by 3%). Dissolve the above raw materials in deionized water to prepare a mixed suspension with a solid content of 15 wt%. Place the mixed suspension in a planetary ball mill and ball mill for 15 h using deionized water as the medium to fully refine and homogenize the raw materials, obtaining a precursor slurry. After preparing the slurry, directly ball mill for 15 h to fully refine and homogenize the raw materials.

[0090] (2) Two-fluid spray drying: The precursor slurry was atomized and dried using a two-fluid nozzle spray dryer (Yamato ADL311S, nozzle diameter 0.4 mm). The operating parameters were set as follows: Spray pressure: 0.08 MPa; Inlet air temperature: 180℃; Air outlet temperature: 90℃; Feed rate: 10 mL / min; During spray drying, the precursor solution is pumped to a two-fluid nozzle, where compressed air tears the slurry into micron-sized droplets. These droplets come into contact with hot air inside the drying tower, causing the moisture to evaporate rapidly. The dried powder is then collected by a cyclone separator as the precursor powder.

[0091] (3) Calcination treatment: The collected precursor powder was first dried at 120 °C for 5 h to remove residual moisture. It was then placed in a tube furnace and calcined under an argon (Ar) atmosphere. The calcination temperature was increased to 380 °C at a rate of 5 °C / min and held for 4 h (pre-calcination stage). After the pre-sintered intermediate product was allowed to cool naturally, it was ground to break up any possible soft agglomerates. The ground powder was then placed back in the tube furnace and subjected to high-temperature crystallization calcination under a flowing inert atmosphere (argon), increased to 580 °C at a rate of 5 °C / min and held for 8 h. Finally, it was allowed to cool naturally to room temperature to obtain the lithium iron phosphate / carbon-coated composite material. The cooled sintered block was removed, mechanically ground, and passed through a 400-mesh sieve to obtain a lithium iron phosphate / carbon-coated composite material. Static volumetric testing confirmed that the average pore size of the secondary lithium iron phosphate particles was 5 nm. By adjusting process parameters such as spray drying pressure, spray drying inlet air temperature, and calcination temperature, lithium iron phosphate materials with different average pore sizes of secondary particles were prepared and named "1#", "2#", "3#", "4#", "5#", "6#", and "7#", respectively. The specific preparation process parameters and average pore size parameters of secondary particles are shown in Table 1.

[0092] Table 1

[0093] [Preparation of electrolyte and battery cells] Example 1 (1) Preparation of electrolyte: Under an inert atmosphere (water < 0.1 ppm, oxygen < 1 ppm), the basic solvents ethylene carbonate and ethyl methyl carbonate were mixed at a volume ratio of 1:2. After uniform mixing, lithium bis(fluorosulfonyl)imide (LiFSI) and lithium hexafluorophosphate (LiPF6) were added. The mass percentage of LiFSI in the electrolyte was 6 wt%, and the mass percentage of LiPF6 in the electrolyte was 7 wt%. Then, the first additive (the compound shown in Formula I-1), the second additive (VC), and the third additive (MMDS) were added. The mass percentage of the first additive (the compound shown in Formula I-1) was 3%, the mass percentage of the second additive (VC) was 2.5%, and the mass percentage of the third additive (MMDS) was 0.7%.

[0094] (2) Preparation of positive electrode sheet: The positive active material with the corresponding average pore size of the secondary particles prepared above (as shown in Table 1), conductive carbon black and binder polyvinylidene fluoride (PVDF) are dispersed in N-methylpyrrolidone (NMP) solvent at a mass ratio of 98:1:1. The mixture is stirred and mixed thoroughly to form a uniform positive electrode slurry (the solid content in the positive electrode slurry is 56wt%). The positive electrode slurry is coated on the upper and lower surfaces of aluminum foil and dried. After cold pressing, the positive electrode sheet is then cut, diced and slit to form a positive electrode sheet.

[0095] (3) Preparation of negative electrode sheet: The negative electrode active material graphite, conductive agent conductive carbon black, thickener carboxymethyl cellulose (CMC), and binder styrene-butadiene rubber (SBR) are mixed in deionized water at a mass ratio of 95.3:1.7:1.6:1.4 to prepare a negative electrode slurry (the solid content in the negative electrode slurry is 51wt%). The negative electrode slurry is coated on the upper and lower surfaces of copper foil and dried. Then, it is cold-pressed, trimmed, cut into sheets, and slit to prepare a negative electrode sheet.

[0096] (4) Separator: A 16μm polyethylene film is used as the separator.

[0097] (5) Battery preparation: The above-mentioned positive electrode, separator and negative electrode are stacked in sequence, with the separator between the positive electrode and the negative electrode to play a role in isolation. Then, they are wound to obtain a bare cell, which is placed in an outer packaging shell, dried, and then injected with electrolyte. After vacuum sealing, standing, formation and shaping, the battery preparation is completed.

[0098] Comparative Example 1 The battery was prepared using the method of Example 1, except that the first additive was not added to the electrolyte.

[0099] Comparative Example 2 The battery was prepared using the method of Example 1, except that no second additive was added to the electrolyte.

[0100] Comparative Example 3 The battery was prepared using the method of Example 3, except that no second additive was added to the electrolyte.

[0101] Examples 2-5 Examples 2-5 were prepared using the method of Example 1, with the difference being that the type of the first additive (the compound shown in Formula I) was different, as shown in Table 2.

[0102] Examples 6-9 Examples 6-9 were prepared using the method of Example 1, with the following differences: the amount of the first additive was different, the mass percentage of the base solvent was changed accordingly, and the percentage of other components in the electrolyte remained unchanged. The rest were the same as in Example 1, as shown in Table 2.

[0103] Comparative Examples 4-5 Comparative Examples 4 and 5 were prepared using the method of Example 1, with the following differences: the amount of the first additive added was different, the mass percentage of the base solvent changed accordingly, and the percentage of other components in the electrolyte remained unchanged. The rest were the same as in Example 1, as shown in Table 2.

[0104] Examples 10-15 Examples 10-15 were prepared using the method of Example 1, with the difference being that the amount of the third additive was different, the mass percentage of the base solvent changed accordingly, and the percentage of other components in the electrolyte remained unchanged. The rest were the same as in Example 1, as shown in Table 2.

[0105] Examples 16-21 Examples 16-21 were prepared using the method of Example 1, with the difference being that the amount of the second additive was different, the mass percentage of the base solvent changed accordingly, and the percentage of other components in the electrolyte remained unchanged. The rest were the same as in Example 1, as shown in Table 2.

[0106] Examples 22-26 Examples 22-26 were prepared using the method of Example 1, with the difference being that the average pore size of the secondary particles of the positive electrode active material was different, as shown in Table 2.

[0107] Examples 27-37 Examples 25-38 were prepared using the method of Example 1, with the difference being: the electrolyte additive formulation was adjusted (the amounts of the first, second, and third additives were adjusted individually or simultaneously) and the average pore size of the secondary particles of the positive electrode active material was adjusted. When the specific amount of additives was adjusted, the mass percentage of the base solvent changed accordingly. Except for the percentage of other components in the electrolyte, the rest was the same as in Example 1, as shown in Table 2.

[0108] Comparative Example 6 Comparative Example 6 uses the method of Example 1 to prepare a battery, except that the amount of the first and third additives in the electrolyte additive formulation is adjusted, the mass percentage of the base solvent is changed accordingly, and the percentage of other components in the electrolyte remains unchanged. Otherwise, it is the same as Example 1, as shown in Table 2.

[0109] Table 2

[0110] Note: In Table 1, " / " indicates that the corresponding preparation parameters or substances do not exist.

[0111] Table 3

[0112] The electrolytes and batteries obtained in Examples 1-37 and Comparative Examples 1-6 were tested, and the results are shown in Table 3.

[0113] As shown in Examples 1 and Comparative Examples 1-3, the three-component additive combination of the first additive (the compound shown in Formula I-1), the second additive (VC), and the third additive (MMDS) in Example 1 significantly reduced the turbidity of the resulting electrolyte, reduced precipitation, and increased electrolyte stability. The problem of gas generation during high-temperature cycling at low SOC was improved, exhibiting a lower expansion rate after high-temperature cycling. At the same time, the resulting battery had a higher number of cycles at 60°C to 80% capacity retention and a lower high-temperature storage DCR growth rate, proving that the first additive (the compound shown in Formula I-1), the second additive (VC), and the third additive (MMDS) have a good synergistic effect, which is beneficial for maintaining the stability of the electrolyte and improving the electrochemical performance at high temperatures, thus solving the high-temperature gas generation problem unique to lithium iron phosphate under high and low SOC conditions.

[0114] As shown in Examples 1-5, when the first additive can be compounds shown in Formula I-1, Formula I-2, Formula I-3, Formula I-4, and Formula I-5, the turbidity of the resulting electrolyte is significantly improved, the problem of gas generation during high-temperature cycling with low SOC is alleviated, and a lower expansion rate after high-temperature cycling is exhibited. Simultaneously, the resulting battery has a higher number of cycles to 80% capacity retention at 60°C and a lower high-temperature storage DCR growth rate. These compounds, as the first additive, are more compatible with the electrolyte system in terms of overall activity, maintaining a relatively low consumption rate during battery charging and discharging, better extending the duration of vinylene carbonate's action, and further achieving the goal of mitigating the increase in the cycle DCR change rate caused by VC consumption and film formation. In the compounds shown in Formula I, the alkyl group is an electron-donating group for the N and S groups on the molecule, which can slightly increase the electron cloud density on the N atom, thus enhancing its stabilizing effect on MMDS. Furthermore, the aforementioned alkyl groups have lower molecular steric hindrance, which helps reduce the difficulty of interaction between the compound shown in Formula I and MMDS and VC, better exerting the synergistic effect, helping to maintain the stability of the electrolyte and improve electrochemical performance at high temperatures, and solving the high-temperature gas generation problem unique to lithium iron phosphate under high and low SOC conditions. In addition, comparing the performance data obtained from Examples 1-5, the overall trend of changes in electrolyte turbidity and battery high-temperature performance is relatively gradual. Specific differences are as follows: Comparing Examples 1, 2, and 3, and comparing Examples 4 and 5, it can be seen that as the alkyl chain shortens, the high-temperature cycle life of the battery shows an increasing trend, the high-temperature storage DCR growth rate and high-temperature cycle expansion rate show a decreasing trend, and the turbidity of the electrolyte shows a decreasing trend. This is because the shorter alkyl chain length reduces steric hindrance, weakening the difficulty of interaction between the compound shown in Formula I and MMDS and VC, leading to an increasing trend in the improvement effect of the synergistic effect. Furthermore, when R1 and R2 groups are the same, the molecular structure is symmetrically distributed, which also increases the performance improvement effect on the battery and electrolyte.

[0115] Compared with Examples 1, 6-7, 27, 29, and Comparative Example 2, and Examples 14-15 and Comparative Example 4, when the formula (2a+b) / c≥2.5 is satisfied, the improvement effect on electrolyte precipitation is enhanced, and the turbidity is controlled below 0.9. When the ratio (2a+b) / c is less than 2.5, the electrolyte turbidity is greater than 0.9. We believe that if the electrolyte turbidity is between 0.9 and 1, there is still a risk that the turbidity will further increase after shipment and storage. However, the value of the above formula is not necessarily better the larger it is. As shown in Example 32 and Comparative Example 6, if the ratio of (2a+b) / c is too large, for example, if the amount of Formula I-1 exceeds 5%, the possible reason is that the proportion of the polyvinyl carbonate interfacial component with embedded sulfonate groups or the organic interfacial component formed by the compound shown in Formula I-1, MMDS, and VC during the formulation and compatibility stage decreases. This leads to an increase in the brittleness of the electrode-electrolyte interface. In the later stage of high-temperature cycling, with the expansion of the active material on the negative electrode side, there is a risk of solvent decomposition triggered by interface rupture, which is not conducive to improving high-temperature performance.

[0116] As shown in Examples 1 and 10-15, with the increase of the amount of the third additive (MMDS) in the electrolyte, the high-temperature cycling performance of the battery shows a trend of first increasing and then decreasing, the DCR growth rate during high-temperature storage shows a trend of first decreasing and then increasing, and the battery expansion rate after high-temperature cycling shows a trend of first decreasing and then increasing. In addition, the turbidity of the electrolyte shows a trend of gradually increasing. This is because, with the amount of the compound shown in Formula I-1 in the electrolyte remaining constant, as the amount of MMDS added to the electrolyte gradually increases, the blocking effect of the compound shown in Formula I-1 on the overall precipitation of MMDS gradually weakens, the amount of precipitation in the electrolyte increases, the turbidity of the electrolyte gradually increases, and this also affects the high-temperature performance of the electrolyte. Furthermore, the amount of MMDS that can actually exert high-temperature performance decreases, and the improvement effect of the high-temperature storage process on the capacity retention rate and the inhibition of DCR growth during high-temperature storage weakens.

[0117] As shown in Examples 1 and 16-21, the addition of the second additive (VC) to the electrolyte has a relatively small impact on the turbidity, showing a trend of slow decrease followed by a slow increase. The high-temperature cycling performance of the battery shows a trend of first increasing and then decreasing, while the DCR growth rate during high-temperature storage shows a relatively flat trend followed by a significant decrease. The battery expansion rate after high-temperature cycling shows a trend of first decreasing and then increasing. With the increase of VC, while VC repairs the SEI film during cycling, it also leads to a significant increase in battery impedance. Therefore, its impact on the high-temperature storage DCR growth rate and high-temperature cycling performance is quite significant.

[0118] As shown in Examples 1 and 22-26, the average pore size of the secondary particles in the positive electrode active material affects the high-temperature performance of the battery. The turbidity of the electrolyte is only related to the properties of the additive components and is not affected by the average pore size of the secondary particles, but it has a significant impact on the high-temperature performance of the battery. The high-temperature cycling performance of the battery initially increases and then decreases; the DCR growth rate of the battery during high-temperature storage initially decreases and then increases; and the battery expansion after high-temperature cycling initially decreases and then increases. A smaller average pore size of the secondary particles hinders electrolyte wetting and ion diffusion transport; a larger average pore size allows ferrous ions to diffuse more into the electrolyte and negative electrode side, increasing the problem of ferrous ions catalyzing electrolyte solvent decomposition and gas generation; and larger interparticle gaps make it easier for gases generated at low or high charge levels to occupy the pores between particles. Therefore, high-temperature cycling gas generation increases, and the improvement effect on high-temperature cycling and storage decreases.

[0119] Based on the overall performance results in Table 3, especially compared with Examples 1, 27-34 and Examples 35-37 and Comparative Example 6, the unified synergistic formula for electrolyte additive formulation and positive electrode lithium iron phosphate secondary particle pore construction, compared with Examples 35-37 and Comparative Example 6 which are outside the formula range, shows that the electrolyte bulk interaction between additives and the spatial scale of positive electrode lithium iron phosphate secondary particle pores are well matched. This helps to suppress the gas generation problem caused by the dissolution of divalent iron at high temperature and high and low charge ranges from the root, and improve the high temperature performance of the battery.

[0120] Therefore, the interaction between the ternary additives in the electrolyte and the synergistic matching of the microstructure of the cathode pores help to better solve the core problems of iron dissolution induced by polarization and gas generation blocking pores in the lithium iron phosphate system at high temperatures and high and low charge ranges, thereby improving the high-temperature performance of the battery. When 11≤( If D+aD≤300, the battery will have better high-temperature cycle and high-temperature storage performance.

[0121] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to specific features, structures, materials, or characteristics described in connection with that embodiment or example, which are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.

[0122] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.

Claims

1. An electrolyte, characterized by, Including the first additive, the second additive, and the third additive; The first additive comprises a compound with the structural formula shown in Formula I: Formula I; In Formula I, R1 and R2 are each independently selected from straight-chain alkyl or branched alkyl groups having 1 to 3 carbon atoms. The second additive is vinylene carbonate; The third additive is methylene disulfonate; Based on the total mass of the electrolyte, the mass percentage of the first additive is a%, and 0.5 ≤ a ≤ 5.

2. The electrolyte according to claim 1, characterized in that, Meet at least one of the following: Based on the total mass of the electrolyte, the mass percentage of the second additive is b%, and 0.5 ≤ b ≤ 5. Based on the total mass of the electrolyte, the mass percentage of the third additive is c%, 0.1≤c≤4.

3. The electrolyte of claim 1, wherein Satisfy at least one of the following (I) to (III): (I) 1 ≤ a ≤ 4; (II) 1≤b≤4; (III) 0.3 ≤ c ≤ 1.

5.

4. The electrolyte according to any one of claims 1 to 3, characterized in that, It satisfies: (2a+b) / c≥2.

5.

5. The electrolyte according to any one of claims 1 to 3, characterized in that, In Formula I, R1 and R2 are each independently selected from straight-chain alkyl groups having 1 to 3 carbon atoms.

6. The electrolyte according to any one of claims 1 to 3, characterized in that, The first additive includes: any one or more of formulae I-1 , formula I-2 , formula I-3 , formula I-4 , formula I-5 .

7. The electrolyte according to any one of claims 1 to 3, characterized in that, The electrolyte further includes an electrolyte salt and a solvent; and satisfies at least one of the following (i) to (iii): (i) The electrolyte salt includes one or more of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium bis(oxalate)borate, lithium difluorooxalateborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethane)sulfonylimide, lithium difluorophosphate, lithium difluorobis(oxalate) phosphate, and lithium tetrafluorooxalate phosphate. (ii) The solvent includes carbonate solvents; the carbonate solvent includes one or more of ethylene carbonate, propylene carbonate, butene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, and methyl propyl carbonate. (iii) The solvent includes carboxylic acid ester solvents, which include one or more of methyl formate, methyl acetate, methyl propionate, methyl butyrate, ethyl acetate, ethyl propionate, propyl propionate, and ethyl butyrate.

8. A battery, characterized by The battery includes a positive electrode, a negative electrode, a separator, and an electrolyte as described in any one of claims 1 to 6; the positive electrode includes a positive active material layer, the positive active material layer includes a positive active material, and the positive active material includes lithium iron phosphate material; The average pore size of the secondary particles in the lithium iron phosphate material is D nm, where 5 ≤ D ≤ 40. The battery satisfies: 6≤ )D+aD≤353; Based on the total mass of the electrolyte, the mass percentage of the first additive is a%, the mass percentage of the second additive is b%, and the mass percentage of the third additive is c.

9. The battery of claim 8, wherein, The surface of the positive electrode active material particles is at least partially coated with carbon material.