Secondary battery cells and their manufacturing methods, energy storage devices
By measuring the DC internal resistance reduction of dry and wet cells, the problem of inaccurate judgment of resting time in sodium-ion battery production was solved, achieving efficient and precise wetting control, and improving production efficiency and cell quality.
Patent Information
- Application Number
- CN202611340058.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
In existing sodium-ion battery production, the judgment of the resting time is inaccurate, resulting in insufficient or excessive immersion, which affects the performance and safety of the cell. Furthermore, the sampling and disassembly method has problems of missed detection and material waste.
By measuring the DC internal resistance and its decrease in dry and wet cells, and using low-current short-time pulse testing and periodic monitoring, the wetting state is determined to ensure that each cell is formed at the optimal time, thus avoiding disassembly and waste.
It enables precise identification of the wetting status of each battery cell, improving production efficiency and yield, avoiding performance problems and safety hazards caused by insufficient resting time, and reducing material waste.
Smart Images

Figure CN123120897A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to new energy technologies, and in particular to a method for producing a secondary battery cell, the secondary battery cell, and an energy storage device. Background Technology
[0002] In the production of sodium-ion batteries, the settling period after electrolyte injection is a crucial step. Ideally, the settling should end immediately after the positive and negative electrodes are fully wetted, and formation should proceed. Otherwise, excessive settling time will reduce production efficiency and increase manufacturing costs. Conversely, ending the settling period too early, resulting in insufficient wettability of the positive and negative electrodes, may lead to safety issues such as sodium deposition during cell formation. The formed cells may also exhibit electrochemical performance problems such as low capacity and high internal resistance.
[0003] The relevant technology uses a sampling disassembly method to determine when the settling period ends. That is, during the settling process, samples are taken from the same batch of cells at multiple intervals for disassembly. When it is observed that the positive and negative electrode plates are fully wetted, it is considered that the entire batch of cells has been fully wetted and can enter the formation process.
[0004] However, this approach has several drawbacks. First, spot checks can only cover a very small number of cells within a batch, failing to fully reflect the true wetting status of all cells in the same batch, thus posing a risk of missed detections. If poorly wetting cells are not detected and flow into subsequent formation processes, it may lead to cell performance failure or even create safety hazards. Second, spot checks are destructive testing; disassembled cells are directly scrapped, resulting in wasted raw materials and lowering the overall product yield. Summary of the Invention
[0005] This application provides a method for producing a secondary battery cell, the secondary battery cell itself, and an energy storage device.
[0006] This application provides a method for producing a secondary battery cell, including: We provide positive electrode plates, negative electrode plates, and electrolytes; The positive electrode and the negative electrode are wound to obtain a dry cell; Measure the first DC internal resistance of the dry cell; The electrolyte is injected into the dry battery cell to obtain a wet battery cell; The second DC internal resistance of the wet battery cell is monitored during the static storage process. When the decrease in the second DC internal resistance relative to the first DC internal resistance is greater than a predetermined threshold, the cell is converted into a wet cell to obtain the cell of the secondary battery.
[0007] The method for producing secondary battery cells according to this application determines the wetting state by measuring the DC internal resistance and its decrease in dry and wet cells. This accurately identifies the moment when each cell reaches its optimal wetting state, allowing for immediate initiation of formation without disassembling the cells. This ensures production efficiency while preventing subsequent formation problems caused by insufficient resting time. Furthermore, each cell can be independently inspected, avoiding the risk of missed inspections during sampling. In addition, inspected cells can still proceed normally to subsequent formation processes, eliminating scrap caused by disassembly and significantly improving production yield.
[0008] In some embodiments, measuring the first DC internal resistance of the dry cell includes: The dry cell is charged and / or discharged at a constant current for a first time using a first current. Measure the first voltage change of the dry cell; The first DC internal resistance is calculated based on the first voltage change value and the first current.
[0009] This implementation method uses a small current and short-time pulse test to test the dry-state battery cell, which can obtain the reference internal resistance R1 without damaging the electrode, providing a reliable reference value for subsequent calculation of the reduction K.
[0010] In some embodiments, monitoring the second DC internal resistance of the wet cell during the resting process of the wet cell includes: During the resting process of the wet battery cell, the second DC internal resistance is measured once at predetermined intervals.
[0011] The method for producing a secondary battery cell according to the present application periodically measures the DC internal resistance of the wet cell at predetermined intervals during the resting process. This allows for the tracking of the change trend of the internal resistance with the immersion time in a discrete sampling manner. This avoids frequent disturbances to the cell state caused by continuous monitoring and can also capture the inflection point where the internal resistance decreases from below the threshold to above the threshold.
[0012] In some implementations, the predetermined time is 2-8 hours.
[0013] Experiments show that using the above range can capture cells with slower wetting speeds while avoiding the waste of resources caused by excessive testing.
[0014] In some embodiments, measuring the second DC internal resistance at predetermined intervals includes: The wet cell is charged and / or discharged at a constant current for a second time at predetermined intervals; Measure the second voltage change value of the wet battery; The second DC internal resistance is calculated based on the second voltage change value and the second current.
[0015] In this way, firstly, it ensures that the first DC resistance and the second DC resistance are measured under exactly the same conditions, so the reduction can truly reflect the impedance change caused by immersion and eliminate the systematic error introduced by the difference in test methods; secondly, the DC internal resistance measured by the constant current charge-discharge method includes ohmic resistance and activation polarization resistance, which can more comprehensively reflect the actual impedance characteristics of the cell and is more accurate than the AC internal resistance method (which only measures ohmic resistance).
[0016] In some implementations, the first current and / or the second current is 0.05-0.2 times, and the first time and / or the second time is 5-30 seconds.
[0017] Experiments show that only within the above-mentioned range can measurement accuracy and cell safety be well guaranteed.
[0018] In some implementations, the predetermined threshold is 55%-70%.
[0019] Experiments show that 55% is the lower limit for ensuring safety, and 70% is the upper limit for ensuring efficiency.
[0020] In some embodiments, the method further includes: If the decrease is still not less than the predetermined threshold after a predetermined time period, the wet cell is determined to be unqualified.
[0021] This avoids: indefinitely leaving the battery stationary, wasting production capacity and equipment; mixing defective cells into the formation process, leading to waste in subsequent processes (formation also consumes time and electricity); and defective cells flowing into customers, causing safety accidents.
[0022] In some implementations, the predetermined duration is 36-72 hours.
[0023] The lower limit of 36 hours ensures that normal cells have enough time to reach the threshold; the upper limit of 72 hours avoids indefinite delays in the production line due to individual abnormal cells.
[0024] In some embodiments, the secondary battery is a sodium-ion battery.
[0025] The positive and negative electrode materials of sodium-ion batteries (such as polyanionic and hard carbon) are highly sensitive to electrolyte wetting, and sodium ions have a large radius, making them more prone to sodium deposition and capacity decay when wetting is insufficient. The cell manufacturing method for secondary batteries according to the embodiments of this application can precisely control the standing time endpoint of sodium-ion cells, effectively avoiding sodium deposition caused by insufficient wetting, and significantly improving the manufacturing yield and safety performance of sodium-ion batteries. Therefore, the cell manufacturing method for secondary batteries according to the embodiments of this application is particularly suitable for sodium-ion batteries.
[0026] In some embodiments, the positive electrode sheet includes a polyanionic positive electrode material, a carbon nanotube conductive agent, a superconducting carbon black conductive agent, and a polyvinylidene fluoride binder; the polyanionic positive electrode material has a mass percentage of 90.0% to 98.0%, the carbon nanotube conductive agent has a mass percentage of 0.5% to 3.0%, the superconducting carbon black conductive agent has a mass percentage of 0.5% to 4.0%, and the polyvinylidene fluoride binder has a mass percentage of 1.2% to 3.0%.
[0027] Experiments show that the formulation ratio of the positive electrode directly affects its electronic conductivity, electrolyte wettability, and the stability of its dry-state internal resistance R1. By limiting the range of material composition and mass percentage of the positive electrode, the reduction in DC internal resistance can sensitively reflect the degree of wettability.
[0028] In some embodiments, the mass percentage of the polyanionic cathode material is 93.0% to 95.0%, the mass percentage of the carbon nanotube conductive agent is 1.0% to 2.5%, the mass percentage of the superconducting carbon black conductive agent is 1.0% to 2.5%, and the mass percentage of the polyvinylidene fluoride binder is 1.2% to 2.5%.
[0029] Experiments show that within this range, the electronic resistance and porosity of the electrode reach the optimal balance: the dry internal resistance R1 is stable at 180-250 mΩ, the wetting curve is smooth after liquid injection, and the K value is stable at over 60% within 36-44 h.
[0030] In some embodiments, the negative electrode sheet comprises hard carbon active material, superconducting carbon black conductive agent, sodium carboxymethyl cellulose thickener, and styrene-butadiene rubber binder; the mass percentage of the hard carbon active material is 90.0%~95.0%, the mass percentage of the superconducting carbon black conductive agent is 0.5%~4.0%, the mass percentage of the sodium carboxymethyl cellulose thickener is 0.2%~2.5%, and the mass percentage of the styrene-butadiene rubber binder is 1.2%~3.0%.
[0031] Experiments show that by limiting the material composition and mass percentage range of the negative electrode, the negative electrode can be ensured to have suitable porosity and hydrophilicity.
[0032] In some embodiments, the hard carbon active material has a mass percentage of 93.0% to 94.5%, the superconducting carbon black conductive agent has a mass percentage of 1.0% to 3.0%, the sodium carboxymethyl cellulose thickener has a mass percentage of 0.5% to 2.0%, and the styrene-butadiene rubber binder has a mass percentage of 1.5% to 2.5%.
[0033] Experiments show that using the above range results in better wetting consistency of the negative electrode sheet and a smoother curve of K value change with standing time, which is beneficial for accurately capturing the threshold inflection point within a 2-8 hour interval.
[0034] In some embodiments, the bifacial density of the positive electrode sheet coated on the positive current collector is 13.0 mg / cm² to 30.4 mg / cm², and the bifacial density of the negative electrode sheet coated on the negative current collector is 5.2 mg / cm² to 12.6 mg / cm².
[0035] The areal density range in this embodiment ensures that the electrolyte can substantially wet the entire thickness direction of the electrode within 48 hours.
[0036] In some embodiments, the bifacial density of the positive electrode coating is 13.5 mg / cm² to 25.2 mg / cm², and the bifacial density of the negative electrode coating is 5.4 mg / cm² to 10.2 mg / cm².
[0037] Experiments show that the above range represents the optimal balance between ensuring battery energy density (meeting commercial requirements) and wetting efficiency. At this areal density, the monitoring method described in this application (0.1C / 10s test, 4-hour interval, 60% threshold, 48h upper limit) can accurately distinguish between cells with sufficient and insufficient wetting.
[0038] In some embodiments, providing the positive electrode, negative electrode, and electrolyte includes: Using N-methylpyrrolidone as a solvent, polyanionic cathode material, carbon nanotube conductive agent, superconducting carbon black conductive agent and polyvinylidene fluoride binder are mixed, stirred and dispersed to prepare cathode slurry; The positive electrode slurry is coated onto the surface of the positive electrode aluminum foil current collector, dried, and rolled to obtain the positive electrode sheet; Using deionized water as a solvent, hard carbon active material, superconducting carbon black conductive agent, sodium carboxymethyl cellulose thickener and styrene-butadiene rubber binder are mixed, stirred and dispersed to prepare negative electrode slurry; The negative electrode slurry is coated onto the surface of the negative electrode aluminum foil current collector, dried, and rolled to obtain the negative electrode sheet.
[0039] The electrode prepared by the above method has good consistency in coating porosity, pore size distribution and surface roughness, which makes the dry internal resistance R1 of different cells fluctuate little (for example, between 180 and 220 mΩ), the wetting curve after liquid injection has good repeatability, and the standard deviation of the time point when the K value exceeds 60% is less than 2 hours.
[0040] This application also provides a secondary battery cell, which is manufactured using the aforementioned production method.
[0041] This application also provides an energy storage device, which includes the battery cell. Attached Figure Description
[0042] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, wherein: Figure 1-5 This is a schematic flowchart of a method for producing a cell of a secondary battery according to certain embodiments of this application.
[0043] Figure 6 This is a photograph of the positive electrode sheet obtained by disassembling a battery cell produced by a certain embodiment of the present application after it has been left to stand for 20 hours.
[0044] Figure 7 This is a photograph of the positive electrode obtained by disassembling a battery cell produced by a certain embodiment of the present application after it has been left to stand for 48 hours.
[0045] Figure 8 This is another schematic diagram of a method for producing a cell of a secondary battery according to certain embodiments of this application.
[0046] Figure 9 This is a perspective view of an energy storage device according to certain embodiments of this application.
[0047] Explanation of main component symbols Energy storage device 100, secondary battery cell 10. Detailed Implementation
[0048] The embodiments of this application are described in detail below. Examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the embodiments of this application, and should not be construed as limiting the embodiments of this application.
[0049] To better understand the specific embodiments of this application, the following uses a sodium-ion battery as an example to illustrate the current status and shortcomings of the production method for secondary battery cells. However, those skilled in the art should understand that the production methods of the specific embodiments of this application are also applicable to other types of secondary batteries such as lithium-ion batteries and potassium-ion batteries. The sodium-ion battery is only used to illustrate a typical application scenario of the specific embodiments of this application and does not constitute a limitation on the scope of protection of this application.
[0050] In the production of sodium-ion batteries, the settling period after electrolyte injection is a crucial step. Ideally, the settling should end immediately after the positive and negative electrodes are fully wetted, and formation should proceed. Otherwise, excessive settling time will reduce production efficiency and increase manufacturing costs. Conversely, ending the settling period too early, resulting in insufficient wettability of the positive and negative electrodes, may lead to safety issues such as sodium deposition during cell formation. The formed cells may also exhibit electrochemical performance problems such as low capacity and high internal resistance.
[0051] The relevant technology uses a sampling disassembly method to determine when the settling period ends. That is, during the settling process, samples are taken from the same batch of cells at multiple intervals for disassembly. When it is observed that the positive and negative electrode plates are fully wetted, it is considered that the entire batch of cells has been fully wetted and can enter the formation process.
[0052] However, this approach has several drawbacks. First, spot checks can only cover a very small number of cells within a batch, failing to fully reflect the true wetting status of all cells in the same batch, thus posing a risk of missed detections. If poorly wetting cells are not detected and flow into subsequent formation processes, it may lead to cell performance failure or even create safety hazards. Second, spot checks are destructive testing; disassembled cells are directly scrapped, resulting in wasted raw materials and lowering the overall product yield.
[0053] In view of this, please refer to Figure 1 The specific embodiments of this application provide a method for producing a secondary battery cell, including: S1: Provides positive electrode, negative electrode and electrolyte; S2: Wind the positive electrode and the negative electrode to obtain a dry cell; S3: Measure the first DC internal resistance of the dry cell; S4: Inject the electrolyte into the dry battery cell to obtain a wet battery cell; S5: Monitor the second DC internal resistance of the wet cell during the static placement process; S6: When the decrease in the second DC internal resistance relative to the first DC internal resistance is greater than a predetermined threshold, the cell is converted into a wet cell to obtain the cell of the secondary battery.
[0054] The method for producing secondary battery cells according to this application determines the wetting state by measuring the DC internal resistance and its decrease in dry and wet cells. This accurately identifies the moment when each cell reaches its optimal wetting state, allowing for immediate initiation of formation without disassembling the cells. This ensures production efficiency while preventing subsequent formation problems caused by insufficient resting time. Furthermore, each cell can be independently inspected, avoiding the risk of missed inspections during sampling. In addition, inspected cells can still proceed normally to subsequent formation processes, eliminating scrap caused by disassembly and significantly improving production yield.
[0055] In some embodiments, the secondary battery is a sodium-ion battery.
[0056] Sodium-ion batteries are secondary batteries that use sodium ions as charge carriers. Their working principle is similar to that of lithium-ion batteries: during charging, sodium ions are released from the positive electrode and inserted into the negative electrode; the reverse occurs during discharging. Sodium-ion batteries have advantages such as abundant sodium resources, low cost, and good safety, making them particularly suitable for large-scale energy storage and low-speed electric vehicles.
[0057] The positive and negative electrode materials of sodium-ion batteries (such as polyanionic and hard carbon) are highly sensitive to electrolyte wetting, and sodium ions have a large radius, making them more prone to sodium deposition and capacity decay when wetting is insufficient. The cell manufacturing method for secondary batteries according to the embodiments of this application can precisely control the standing time endpoint of sodium-ion cells, effectively avoiding sodium deposition caused by insufficient wetting, and significantly improving the manufacturing yield and safety performance of sodium-ion batteries. Therefore, the cell manufacturing method for secondary batteries according to the embodiments of this application is particularly suitable for sodium-ion batteries.
[0058] Of course, the secondary battery is not limited to sodium ion batteries, but in other embodiments it can be a lithium ion battery, a potassium ion battery or other types of secondary batteries.
[0059] Specifically, in step S1, the positive electrode refers to the electrode sheet that undergoes an oxidation reaction during charging and a reduction reaction during discharging of the secondary battery. It typically includes a positive current collector and a positive electrode coating applied to its surface. The positive electrode coating contains positive active material, a conductive agent, and a binder. The negative electrode refers to the electrode sheet that undergoes a reduction reaction during charging and an oxidation reaction during discharging of the secondary battery. It typically includes a negative current collector and a negative electrode coating applied to its surface. The negative electrode coating contains negative active material, a conductive agent, a thickener, and a binder. The electrolyte is an ion-conducting liquid containing electrolyte salts (such as sodium salts and lithium salts) and organic solvents (such as carbonates and ethers), used to transport metal ions between the positive and negative electrodes.
[0060] In some embodiments, the positive electrode sheet includes a polyanionic positive electrode material, a carbon nanotube conductive agent, a superconducting carbon black conductive agent, and a polyvinylidene fluoride binder; the polyanionic positive electrode material has a mass percentage of 90.0% to 98.0%, the carbon nanotube conductive agent has a mass percentage of 0.5% to 3.0%, the superconducting carbon black conductive agent has a mass percentage of 0.5% to 4.0%, and the polyvinylidene fluoride binder has a mass percentage of 1.2% to 3.0%.
[0061] Polyanionic cathode materials refer to a class of sodium-ion battery cathode materials with a three-dimensional framework structure, such as sodium vanadium phosphate (Na3V2(PO4)3), sodium iron pyrophosphate (Na2FeP2O7), and sodium vanadium fluorophosphate (Na3V2(PO4)2F3). They are characterized by structural stability and high safety, but have relatively low electronic conductivity, requiring the addition of conductive agents.
[0062] Carbon nanotube conductive agents are one-dimensional tubular carbon materials with excellent electronic conductivity and the ability to construct long-range conductive networks.
[0063] Superconducting carbon black conductive agent is a particulate carbon material with a high specific surface area (such as Super P and Ketjen Black) that fills the spaces between active material particles to form point contact conductivity.
[0064] Polyvinylidene fluoride (PVDF) is an oily adhesive, soluble in nitrogen. Methylpyrrolidone (NMP) provides electrode mechanical strength and current collector adhesion.
[0065] Experiments show that the formulation ratio of the positive electrode directly affects its electronic conductivity, electrolyte wettability, and the stability of its dry-state internal resistance R1. By limiting the range of material composition and mass percentage of the positive electrode, the reduction in DC internal resistance can sensitively reflect the degree of wettability.
[0066] If the proportion of polyanionic cathode material is below 90.0%, the active material ratio is too low, the battery capacity will decrease significantly, and the relatively excessive amount of conductive agent and binder will hinder electrolyte penetration; if it is above 98.0%, the conductive agent and binder will be insufficient, the electrode internal resistance will be too high, and the dry internal resistance R1 will be too large, causing the K value calculation benchmark to deviate.
[0067] If the carbon nanotube conductive agent content is below 0.5%, the conductive network will be discontinuous and the electronic resistance of the electrode will increase; if it is above 3.0%, the carbon nanotubes will easily agglomerate, reducing the uniformity of the coating.
[0068] If the superconducting carbon black conductive agent content is below 0.5%, the point contact conductivity is insufficient; if it is above 4.0%, the proportion of active material is compressed, and the excess carbon black absorbs the electrolyte, affecting the wetting kinetics.
[0069] If the polyvinylidene fluoride binder content is below 1.2%, the electrode is prone to powder shedding and cracking; if it is above 3.0%, the binder will block the pores, hindering electrolyte wetting and causing the wet internal resistance R2 to decrease slowly.
[0070] In some embodiments, the mass percentage of the polyanionic cathode material is 93.0% to 95.0%, the mass percentage of the carbon nanotube conductive agent is 1.0% to 2.5%, the mass percentage of the superconducting carbon black conductive agent is 1.0% to 2.5%, and the mass percentage of the polyvinylidene fluoride binder is 1.2% to 2.5%.
[0071] Experiments show that within this range, the electronic resistance and porosity of the electrode achieve the optimal balance: the dry internal resistance R1 is stable at 180–250 mΩ, the wetting curve is smooth after liquid injection, and the K value is stable at over 60% within 36–44 hours. If a wide range is used but exceeds this narrow range (e.g., 92% active material), although it can still work, the wetting time may be extended to more than 50 hours, affecting production efficiency.
[0072] As an example, the positive electrode composition is: 94.5% polyanion, 1.5% carbon nanotubes, 1.5% superconducting carbon black, and 2.5% PVDF. Correspondingly, the dry internal resistance R1 = 200 mΩ (typical value), and R2 drops to 69 mΩ within 40 hours after liquid injection, K = 65.5%, indicating sufficient wetting and no sodium precipitation.
[0073] As another example, using 93.5% polyanionic polymer + 2.0% carbon nanotubes + 2.0% superconducting carbon black + 2.5% PVDF, the dry internal resistance is 210mΩ, and K=62% after 42h of injection.
[0074] As another example, if 95.0% active material + 1.0% carbon nanotubes + 1.0% superconducting carbon black + 3.0% PVDF (PVDF exceeds the narrow range but is still within the wide range), the wetting time may be extended to 48h, K=61%, still above the threshold but with a slight decrease in efficiency.
[0075] In some alternative embodiments, some carbon nanotubes can be replaced with vapor-grown carbon fibers (VGCF), or superconducting carbon black can be replaced with acetylene black. Alternatively, polyacrylic acid (PAA) or sodium alginate can be used instead of PVDF, in which case the solvent needs to be changed to water or an alcohol-water mixture accordingly.
[0076] In some embodiments, the negative electrode sheet comprises hard carbon active material, superconducting carbon black conductive agent, sodium carboxymethyl cellulose thickener, and styrene-butadiene rubber binder; the mass percentage of the hard carbon active material is 90.0%~95.0%, the mass percentage of the superconducting carbon black conductive agent is 0.5%~4.0%, the mass percentage of the sodium carboxymethyl cellulose thickener is 0.2%~2.5%, and the mass percentage of the styrene-butadiene rubber binder is 1.2%~3.0%.
[0077] Specifically, hard carbon is an amorphous carbon material with a large interlayer spacing (approximately 0.37–0.40 nm), which is suitable for the insertion / extraction of sodium ions and is the mainstream anode material for sodium-ion batteries.
[0078] Sodium carboxymethyl cellulose (CMC) is a water-soluble thickener used to adjust the viscosity of negative electrode slurry, disperse conductive agents and active substances, and prevent sedimentation.
[0079] Styrene-butadiene rubber (SBR) is a water-based binder that provides electrode flexibility and elasticity, preventing cracking during winding.
[0080] Experiments show that by limiting the range of material composition and mass percentage of the negative electrode, suitable porosity and hydrophilicity are ensured. Exceeding this range can lead to poor wetting or electrode defects, rendering the K-value determination in this application inaccurate.
[0081] Specifically, if the hard carbon active material content is below 90.0%, the capacity loss is severe; if it is above 95.0%, the conductive agent and binder are insufficient, the internal resistance of the electrode increases and the peel strength decreases.
[0082] If the superconducting carbon black conductive agent content is below 0.5%, the conductive network is incomplete; if it is above 4.0%, the energy density is reduced and excessive liquid absorption may occur.
[0083] If the sodium carboxymethyl cellulose (CMC) thickener content is below 0.2%, the slurry stability is poor and it is prone to settling; if it is above 2.5%, the slurry viscosity is too high, making coating difficult, and the CMC will form an insulating film after drying, increasing the internal resistance of the electrode.
[0084] If the styrene-butadiene rubber binder content is below 1.2%, the electrode sheet will lack flexibility and will easily crack during winding; if it is above 3.0%, the binder will coat hard carbon particles, hindering electrolyte contact and sodium ion diffusion, resulting in a slow decrease in wet internal resistance.
[0085] In some embodiments, the hard carbon active material has a mass percentage of 93.0% to 94.5%, the superconducting carbon black conductive agent has a mass percentage of 1.0% to 3.0%, the sodium carboxymethyl cellulose thickener has a mass percentage of 0.5% to 2.0%, and the styrene-butadiene rubber binder has a mass percentage of 1.5% to 2.5%.
[0086] Experiments show that using the above range results in better wetting consistency of the negative electrode sheet and a smoother curve of K value change with standing time, which is beneficial for accurately capturing the threshold inflection point within a 2-8 hour interval.
[0087] As an example, the negative electrode composition is: 94.8% hard carbon, 2.0% superconducting carbon black, 1.2% CMC, and 2.0% SBR. The dry internal resistance R1, when combined with the positive electrode, is 200 mΩ. After liquid injection, the wetting is normal, and K = 65.5% after 40 h.
[0088] As another example, using 94.0% hard carbon + 2.5% superconducting carbon black + 1.5% CMC + 2.0% SBR, the dry internal resistance is 190mΩ, and K=61% after 38h of injection, with good results.
[0089] In some alternative embodiments, the conductive agent can be acetylene black or Ketjen black instead of superconducting carbon black. The thickener can be hydroxypropyl methylcellulose (HPMC) instead of CMC. The binder can be polyacrylate (PA) or polyimide (PI) instead of SBR.
[0090] In some embodiments, the bifacial density of the positive electrode sheet coated on the positive current collector is 13.0 mg / cm² to 30.4 mg / cm², and the bifacial density of the negative electrode sheet coated on the negative current collector is 5.2 mg / cm² to 12.6 mg / cm².
[0091] Double-sided density refers to the total mass of the dry coating applied to both sides (front and back) of the current collector divided by the coating area, expressed in mg / cm². It directly determines the electrode thickness and energy density.
[0092] Areal density is a key parameter affecting wetting rate. When areal density is too low (positive electrode < 13.0, negative electrode < 5.2), although wetting is rapid (K may exceed 60% within 10 hours), the battery energy density is too low, lacking commercial value. When areal density is too high (positive electrode > 30.4, negative electrode > 12.6), the electrode sheet is too thick, making it difficult for the electrolyte to penetrate to the underlying active material near the current collector through capillary action. This results in the surface being wetted but the interior remaining dry. In this case, the measured DC internal resistance R2 mainly reflects the surface layer impedance, and the K value may be artificially high, leading to misjudgment.
[0093] The areal density range in this embodiment ensures that the electrolyte can substantially wet the entire thickness direction of the electrode within 48 hours.
[0094] In some embodiments, the bifacial density of the positive electrode coating is 13.5 mg / cm² to 25.2 mg / cm², and the bifacial density of the negative electrode coating is 5.4 mg / cm² to 10.2 mg / cm².
[0095] Experiments show that the above range represents the optimal balance between ensuring battery energy density (meeting commercial requirements) and wetting efficiency. At this areal density, the monitoring method of this application (0.1C / 10s test, 4-hour interval, 60% threshold, 48h upper limit) can accurately distinguish between cells with sufficient and insufficient wetting.
[0096] As an example, the positive electrode has a bifacial density of 20.0 mg / cm², the negative electrode has a bifacial density of 8.0 mg / cm², and after liquid injection, the K at 40 hK is 65.5%. The cross-section of the disassembled electrode is uniformly wet with no dry areas.
[0097] As another example, with a positive electrode concentration of 18.0 mg / cm² and a negative electrode concentration of 7.2 mg / cm², the infiltration curves of the two examples almost overlap.
[0098] For designs with higher energy density, the bifacial density of the cathode can approach 30.4 mg / cm², but the upper limit of the static monitoring time needs to be extended (e.g., 72 hours), and the threshold may need to be lowered from 60% to 55% to compensate for the slower decrease in internal resistance.
[0099] Please see Figure 2 In some implementations, step S1 includes: S11: Using N-methylpyrrolidone as a solvent, polyanionic cathode material, carbon nanotube conductive agent, superconducting carbon black conductive agent and polyvinylidene fluoride binder are mixed, stirred and dispersed to prepare cathode slurry; S12: The positive electrode slurry is coated on the surface of the positive electrode aluminum foil current collector, dried and rolled to obtain the positive electrode sheet; S13: Using deionized water as a solvent, hard carbon active material, superconducting carbon black conductive agent, sodium carboxymethyl cellulose thickener and styrene-butadiene rubber binder are mixed, stirred and dispersed to prepare negative electrode slurry; S14: The negative electrode slurry is coated on the surface of the negative electrode aluminum foil current collector, dried and rolled to obtain the negative electrode sheet.
[0100] N Methylpyrrolidone (NMP) is a highly polar organic solvent that can effectively dissolve PVDF and is a commonly used solvent for oily cathode slurries.
[0101] Deionized water is used as a solvent for aqueous negative electrode slurries, which is environmentally friendly and low in cost.
[0102] Stepwise mixing refers to first preparing the adhesive solution (binder + solvent), then adding a conductive agent for dispersion, and finally adding the active substance to ensure uniformity.
[0103] The specific implementation methods involve the preparation of the positive electrode and the preparation of the negative electrode.
[0104] For cathode preparation, since PVDF is only soluble in NMP, NMP must be used as the solvent. During stirring, PVDF is first dissolved to form a gel, then superconducting carbon black and carbon nanotubes are added for dispersion (the carbon nanotubes need to be pre-dispersed into a gel state), and finally, polyanionic dry powder is added. This stepwise feeding method can avoid the agglomeration of active materials and ensure that the conductive agent is uniformly coated on the surface of the active materials. The coated electrode sheet needs to be dried at high temperature (about 120°C) to remove NMP, and then rolled to the target compaction density.
[0105] For anode preparation, CMC is soluble in deionized water. First, a CMC solution is prepared, then superconducting carbon black is added for dispersion, and finally, hard carbon powder is added. SBR is usually added last to avoid excessive shearing that could damage its latex particle structure. After coating, the anode needs to be dried at a relatively low temperature (approximately 80°C) to prevent the hard carbon micropores from collapsing.
[0106] The electrode prepared by the above method has good consistency in coating porosity, pore size distribution and surface roughness, which makes the dry internal resistance R1 of different cells fluctuate little (for example, between 180 and 220 mΩ), the wetting curve after liquid injection has good repeatability, and the standard deviation of the time point when the K value exceeds 60% is less than 2 hours.
[0107] In some alternative embodiments, dimethylacetamide (DMAC) can be used instead of NMP as the positive electrode solvent, but DMAC is slightly more toxic. A dual planetary mixer can be used instead of a powered mixer for negative electrode stirring; the order of addition can be adjusted, for example, adding CMC and SBR together first, but this may affect the dispersion effect. Transfer coating, gravure coating, etc., can be used instead of extrusion coating for coating. Hot air drying, infrared drying, or microwave drying can be used for drying.
[0108] In step S2, winding is the process of stacking long strips of positive electrode sheet, separator, and negative electrode sheet in sequence and winding them into a cylindrical or flat electrode assembly using a winding machine. After winding, the electrode assembly is installed into a pre-made battery casing and subjected to operations such as tab welding and sealing (leaving a liquid injection port) to obtain a dry cell. The dry cell undergoes a drying process to remove moisture from the electrode coating and prevent moisture from reacting with the electrolyte. A dry cell refers to a semi-finished cell that has not yet been injected with electrolyte. It is usually assembled from positive electrode sheet, negative electrode sheet, and the separator between them by winding or stacking, and installed in a battery casing (such as an aluminum-plastic film soft pack or a metal square shell), but has not yet been injected with electrolyte.
[0109] In step S3, the DC internal resistance (DCR) refers to the equivalent resistance exhibited by the cell under DC charging and discharging conditions, including ohmic resistance (electronic resistance, ionic resistance) and polarization resistance (electrochemical polarization resistance, concentration polarization resistance). The DC internal resistance is usually determined by applying a constant current and measuring the voltage change, i.e., R = ΔV / I, where ΔV is the change in the cell terminal voltage during the applied current I.
[0110] The first DC internal resistance (R1) refers to the DC internal resistance of a dry cell (without electrolyte). Since there is no electrolyte in the dry electrode, the ion conduction path is almost zero. Therefore, R1 mainly reflects the electronic resistance (electronic conductivity of the electrode coating, contact resistance of the current collector, etc.), and its value is usually much greater than the wet internal resistance.
[0111] Measuring the first DC internal resistance of a dry cell needs to be done before electrolyte injection. Since there is no electrolyte inside the dry cell, conventional high-current testing cannot be used, otherwise the electrodes may be damaged. Exemplarily, this application embodiment uses a low-current constant-current charge-discharge method, for example, charging and / or discharging the dry cell with a current of 0.05C to 0.2C for 5 to 30 seconds. The change in voltage across the cell during this period, ΔV, is measured, and the first DC internal resistance is calculated using the formula R1 = ΔV / I.
[0112] For details, please refer to Figure 3 In some implementations, step S3 includes: S31: The dry cell is charged and / or discharged at a constant current for a first time using a first current; S32: Measure the first voltage change of the dry cell; S33: Calculate the first DC internal resistance based on the first voltage change value and the first current.
[0113] The first current refers to the constant current applied when measuring the DC internal resistance of a dry cell. Since dry cells contain no electrolyte and have extremely poor ionic conductivity, the first current must be small to avoid irreversible damage to the electrodes. The first current is usually expressed as a factor (C) of the battery's rated capacity, for example, 0.05C to 0.2C. For cells of different capacities, the absolute current value corresponding to this factor is different (e.g., 0.1C for a 10Ah cell is 1A, and 0.1C for a 100Ah cell is 10A), but the factor definition makes the testing conditions universally applicable.
[0114] The first time refers to the duration for which the first current is applied. Too short a time will result in the voltage response not yet reaching steady state, and the measured value will contain capacitive transient components; too long a time may cause polarization accumulation, or even thermal damage to the dry electrode. The first time is typically 5–30 seconds, preferably 10 seconds.
[0115] The first voltage change (ΔV1) refers to the change in voltage between the positive and negative terminals of the battery cell during the application of the first current. For constant current discharge, ΔV1 = voltage before discharge begins. Voltage at the moment discharge ends; for constant current charging, ΔV1 = voltage at the moment charging ends. Voltage before charging begins.
[0116] The first DC internal resistance (R1) can be calculated according to Ohm's law: R1 = ΔV1 / I1, where I1 is the value of the first current (in amperes).
[0117] When measuring the DC internal resistance of a dry cell battery, special attention must be paid to its unique characteristics: because there is no electrolyte in the electrode coating, sodium ions (or other metal ions) cannot migrate in the solid phase. Therefore, the battery's impedance is extremely high, and it comes almost entirely from electronic resistance (including contact resistance between active material particles, interface resistance between the coating and the current collector, and electrode tab welding resistance). If a conventional large current (such as above 0.5C) is used, excessive Joule heating will be generated locally on the electrode, which may lead to softening of the binder, coating peeling, or diaphragm shrinkage. Therefore, the embodiments of this application use a small current (0.05C to 0.2C) and a short time (5 to 30 seconds) to avoid generating excessive Joule heating.
[0118] In some alternative implementations, a charging mode measurement can be used: charging at a constant current of 1A for 10 seconds, the voltage rises from 0.05V to 0.25V, ΔV1 = 0.20V, and R1 remains the same. For a 12Ah cell, a 0.15C = 1.8A charging time of 8 seconds can be used, yielding ΔV1 = 0.36V and R1 = 0.36 / 1.8 = 0.20Ω. A 20-second discharge can also be used; ΔV1 may increase slightly (due to polarization accumulation), but the calculated R1 value should remain relatively stable at around 200mΩ, indicating good robustness of the measurement method. Furthermore, five consecutive charge-discharge pulses are performed, and the average value of R1 is taken to further improve accuracy.
[0119] This implementation method uses a small current, short-time pulse test on the dry-state battery cell to obtain a reference internal resistance R1 without damaging the electrode, providing a reliable reference value for subsequent calculation of the reduction K. Compared to directly using empirical constants, the measured R1 can eliminate the differences in electronic resistance between different batches and electrode formulations, making the K value criterion universal.
[0120] In step S4, after measuring the DC internal resistance of the dry cell, a measured amount of electrolyte is injected into the dry cell through a pre-reserved injection port, and then the injection port is temporarily sealed (e.g., with a rubber stopper or heat seal). The amount of electrolyte injected is determined based on the cell's design capacity and the electrode porosity, typically 3–6 grams per ampere-hour. The cell after electrolyte injection is called a wet cell and enters the settling process. A wet cell refers to a cell where electrolyte injection has been completed; at this point, the electrolyte has not yet completely wetted the electrodes, but the diffusion and permeation process has begun.
[0121] In step S5, the second DC internal resistance (R2) refers to the DC internal resistance of the wet cell at a certain moment during the resting process. As the electrolyte gradually wets the electrode, the ion conduction pathway increases, and R2 will gradually decrease.
[0122] Monitoring involves placing the wet battery cell in a static environment (usually a constant temperature chamber, 25℃~45℃) after electrolyte injection. During this static period, the DC internal resistance R2 of the wet battery cell is measured at predetermined time intervals (e.g., 2~8 hours), using the same test method as for measuring R1 (same current ratio and time). After each measurement, the reduction K is calculated based on the measured R1 and the current R2. As the static time increases, R2 gradually decreases, and K gradually increases.
[0123] For details, please refer to Figure 4 In some implementations, step S5 includes: S51: During the resting process of the wet cell, the second DC internal resistance is measured once at predetermined intervals.
[0124] The predetermined time refers to the time interval between two consecutive DC internal resistance measurements.
[0125] The second DC internal resistance (R2) refers to the DC internal resistance of the wet cell measured at a specific moment during the resting process. The measurement method is exactly the same as that of R1 (the same current ratio and pulse time).
[0126] During the settling phase after electrolyte injection, the electrolyte gradually permeates into the pores of the electrode coating through capillary action, causing the ionic conductivity of the electrode to gradually increase. Therefore, R2 decreases monotonically over time. By measuring R2 at predetermined time intervals, a discrete curve of R2 versus time can be plotted, and the decrease K = (R1 / R2) can be calculated. The evolution of R2 / R1 over time. When K first exceeds the predetermined threshold, complete immersion is determined.
[0127] The method for producing a secondary battery cell according to the present application periodically measures the DC internal resistance of the wet cell at predetermined intervals during the resting process. This allows for the tracking of the change trend of the internal resistance with the immersion time in a discrete sampling manner. This avoids frequent disturbances to the cell state caused by continuous monitoring and can also capture the inflection point where the internal resistance decreases from below the threshold to above the threshold.
[0128] In some implementations, the scheduled time is 2-8 hours. Exemplarily, the scheduled time is 2, 3, 4, 5, 6, 7, or 8 hours.
[0129] Experiments show that using the above range can capture cells with slower wetting speeds while avoiding the waste of resources caused by excessive testing.
[0130] If the interval is less than 2 hours: the testing frequency is too high. On the one hand, each cell needs to be tested more than 24 times within 48 hours, which greatly increases the load on the testing equipment and the amount of data. In large-scale production, this will lead to increased equipment costs and data processing pressure. On the other hand, frequently applying charge and discharge pulses to cells that are still in a static state may cause unnecessary electrochemical disturbances to the electrode microstructure (especially areas that are not yet fully wetted). Although the test current is small, overly intensive testing may still affect the natural progress of the wetting process. Experiments show that an interval of less than 2 hours does not provide more effective information than an interval of 4 hours (because the change in internal resistance within 2 hours is less than the test error). Therefore, shorter intervals do not bring additional technical benefits but instead increase costs.
[0131] If the interval is greater than 8 hours: the sampling density is too low, and the critical inflection point of K value from below the threshold to above the threshold may be missed. According to experimental data, the K value is 0.545 at 20h (unwetting) and 0.655 at 40h (wetting), with the inflection point appearing approximately between 30 and 35h. If the interval is greater than 8 hours (e.g., 12 hours), the test time points may fall at 20h, 32h, and 44h. At 32h, K may still be around 55% (not up to standard), and at 44h it may be far above 60%, causing the cell to remain stationary for another 12 hours after meeting the standard, resulting in "over-settling" and reduced production efficiency. More seriously, if the inflection point happens to fall between two test points, it may go completely undetected, leading to the cell being misjudged as unqualified or entering the formation process too late.
[0132] As an example, a predetermined time of 4 hours is set. The first R2 is measured immediately after injection (t=0h) and recorded as R. 20 The second R measurement was taken 4 hours later. 24 The third R measurement was taken 8 hours later. 28 ...until R2 stabilizes or K exceeds the threshold. For example, if R1 = 200 mΩ, R... 20 =121mΩ → K=39.5%; R 24 =115mΩ → K=42.5%; R 28 =106mΩ → K=47%; R 212 =101mΩ → K=49.5%; R 216 =95mΩ → K=52.5%; R 220 =91mΩ → K=54.5%; R 224 =85mΩ → K=57.5%; R 228 =82mΩ → K=59%; R 232 =74mΩ → K=63%; at 32h, K=63%>60%, stop the settling process. Actual measurements only require 9 times (0, 4, 8, 12, 16, 20, 24, 28, 32h), significantly reducing the number of tests.
[0133] In some alternative implementations, variable interval measurements can be used. Initially, the immersion rate is relatively fast, so the interval can be set to 2 hours. Later, as the immersion rate approaches the threshold, the interval is increased to 1 hour, and then it can be stopped once the threshold is exceeded. For example: 0, 2, 4, 6, 8, 10, 12, 16, 20, 24, 28, 32h (gradually extended).
[0134] Long-interval measurements can also be used. For example, for a known stable process, an interval of 8 hours can be set directly. Although the exact inflection point may be missed, it can ensure that K>60% is found in about 40 hours.
[0135] Continuous monitoring and early warning can also be used. Online internal resistance monitoring equipment is used to automatically test every 5 minutes. When K exceeds the threshold twice in a row, formation is triggered.
[0136] Please see Figure 5 In some implementations, step S51 includes: S511: The wet cell is charged and / or discharged with a second current at a second time interval at the predetermined time interval; S512: Measure the second voltage change value of the wet battery cell; S513: Calculate the second DC internal resistance based on the second voltage change value and the second current.
[0137] The second current refers to the constant current applied when measuring the DC internal resistance of a wet battery cell. Its magnitude should be the same as the first current when measuring a dry battery cell (usually using the same test equipment and the same setting value) to ensure the comparability of R1 and R2. The second current is also a small current, for example, 0.05C to 0.2C.
[0138] The second time refers to the duration of the second current application, which is the same as the first time (e.g., 5 to 30 seconds).
[0139] Second voltage change value (ΔV2): The change in voltage at the wet cell terminals during the application of the second current.
[0140] In summary, the measurement method for the DC internal resistance of a wet-state battery cell is basically the same as that for a dry-state cell (constant current charge-discharge method). This ensures that R1 and R2 are measured under identical conditions, therefore the reduction K = (R1...) R2 / R1 can accurately reflect the impedance change caused by wetting, eliminating systematic errors introduced by differences in test methods; secondly, the DC internal resistance measured by the constant current charge-discharge method includes ohmic resistance and activation polarization resistance, which can more comprehensively reflect the actual impedance characteristics of the cell and is more accurate than the AC internal resistance method (which only measures ohmic resistance).
[0141] In practice, you can perform constant current discharge only, constant current charging only, or both and take the average value. For wet cells, since electrolyte has been injected, their open circuit voltage (OCV) is usually between 0.1V and 0.5V (sodium-ion batteries). Therefore, the ΔV measured during discharge and charging may be slightly asymmetrical. Taking the average value can eliminate the influence of polarization direction.
[0142] As an example, using the same equipment (such as a battery testing system) and parameters as the dry-state test: second current = 0.1C (1A for a 10Ah cell), second time = 10 seconds. After 20 hours of rest, the discharge ΔV2 is measured to be 0.091V, therefore R2 = 0.091V / 1A = 91mΩ. After 40 hours of rest, ΔV2 = 0.069V, R2 = 69mΩ.
[0143] In some alternative implementations, only the charging pulse can be used. For wet cells, the ΔV2 measured by the charging pulse is usually slightly smaller than that of the discharging pulse (due to different polarization directions), but the calculated R2 difference is within 5% and does not affect the K value judgment.
[0144] Alternatively, multi-pulse averaging can be used, for example, performing 5 consecutive charge-discharge pulses and taking the average value, which can improve repeatability.
[0145] In some implementations, the first current and / or the second current is 0.05-0.2 times, and the first time and / or the second time is 5-30 seconds.
[0146] The rate (C) represents the ratio of the charge / discharge current to the battery's rated capacity. For example, 1C means the current required to fully charge or discharge the battery to its rated capacity in one hour. Using a rate instead of absolute current (amperes) makes the testing method more universal for cells of different capacities.
[0147] Experiments show that the above range ensures measurement accuracy and cell safety. If the range is exceeded, for current ratios below 0.05C: for dry-state cells, the typical internal resistance R1 is 200mΩ, and the voltage change at 0.05C is ΔV = I × R1. Taking a 10Ah cell as an example, 0.05C = 0.5A, ΔV = 0.5 × 0.2 = 0.1V. While this value is measurable, for cells with low internal resistance (e.g., 150mΩ), ΔV is only 0.075V, potentially approaching the resolution (0.01V) and noise level of conventional testing equipment. This leads to poor measurement repeatability; the R1 fluctuation between two measurements of the same cell can reach ±10%, making the K value unreliable. For larger capacity cells (e.g., 100Ah), 0.05C = 5A and ΔV = 1V, which is sufficient for the signal. However, for smaller capacity cells (e.g., 1Ah), 0.05C = 0.05A and ΔV = 0.01V, resulting in an extremely weak signal. Therefore, 0.05C is the lower limit to ensure a clear voltage signal for cells of all capacity ranges.
[0148] Above 0.2C: For dry-state cells, there is almost no internal ionic conductivity, and the applied current is entirely converted into Joule heat. At 0.2C, taking a 10Ah cell as an example, a current of 2A and power P=I²R=4×0.2=0.8W, concentrated at the contact points between the tabs and the coating, may cause local temperature rises exceeding 50°C, leading to softening of the binder, shrinkage of the separator, or shedding of active materials. For semi-wet cells, large currents may exacerbate polarization and induce local sodium deposition. Experiments show that 0.2C is the upper limit that dry-state cells can safely withstand.
[0149] Regarding the time duration, if it is less than 5 seconds: When the constant current pulse time is too short, the cell terminal voltage has not yet reached a steady state and is still in the transient stage of capacitive charging and discharging (double-layer charging). The measured ΔV at this time contains a large transient component, deviating from the steady-state DC internal resistance. For example, the ΔV measured at 1 second may only be 60% to 80% of the steady-state value, leading to a lower calculated internal resistance. Repeatability is poor, with large fluctuations in results from multiple tests of the same cell.
[0150] If the pulse duration exceeds 30 seconds: As the pulse time increases, concentration polarization gradually develops inside the cell—the ion concentration gradient on the surface of the active material particles causes an additional voltage drop. This concentration polarization internal resistance is not directly related to the degree of wetting (concentration polarization still exists even after sufficient wetting), therefore, its inclusion will lead to a higher measured R² and a lower K value, resulting in a conservative judgment (i.e., a longer time is required to reach the threshold). Simultaneously, for dry-state cells, prolonged power-on will cause Joule heat accumulation, potentially leading to thermal damage. Experiments show that steady-state establishment can be completed within 30 seconds, and concentration polarization is not yet significant.
[0151] As another example, using a combination of 0.1C and 10 seconds, the measured dry-state internal resistance R1 was 200mΩ, with a standard deviation <2mΩ (repeated 5 times); the wet-state internal resistance R2 decreased monotonically with time, with a clear inflection point. If 0.03C and 10 seconds were used instead, the fluctuation of R1 increased to ±10mΩ, and the K value calculation became unstable. If 0.3C and 10 seconds were used instead, some dry-state cells showed electrode thermal damage, and the wetting curve after electrolyte injection was abnormal.
[0152] In some alternative implementations, a current of 0.08C and a time of 20 seconds or a current of 0.15C and a time of 6 seconds may be used.
[0153] In step S6, the reduction rate is defined as K = (R1 - R2) / R1, which is the percentage decrease in dry-state internal resistance. The monitoring terminates when the K value first exceeds a predetermined threshold, indicating that the cell is fully wetted.
[0154] In some implementations, the predetermined threshold is 55%-70%.
[0155] The predetermined threshold is the minimum internal resistance decrease K value required to determine sufficient wetting. When K is greater than this threshold, the electrode sheet is considered to be fully wetted, and can enter the formation process.
[0156] Experiments show that 55% is the lower limit to ensure safety, and 70% is the upper limit to ensure efficiency.
[0157] See Figure 6 , if K=0.545 after standing for 20 hours, obvious sodium precipitation is found on the surface of the negative electrode through disassembly and observation, indicating that the electrode sheet is not fully wetted. If a threshold lower than 55% (for example, 50%) is adopted, the cell will be judged as qualified at 20 hours and flow into the formation process. During the formation process, the unwetted area will cause problems such as sodium precipitation and capacity fading, leading to product performance failure and even potential safety hazards.
[0158] See Figure 7 , if K=0.655 after standing for 40 hours, disassembly shows that the surface color of the electrode sheet is uniform and there is no sodium precipitation, indicating that it is fully wetted. If a threshold higher than 70% (for example, 75%) is adopted, the cell still does not meet the condition at 40 hours and needs to continue standing. However, experimental data shows that the K value has stabilized at 0.69 at 48h (Table 1) and remains basically unchanged in the subsequent time, and may never reach 75%. This means that even if the cell is fully wetted, it will be left standing indefinitely or finally judged as unqualified, resulting in yield loss and reduced production efficiency.
[0159] Table 1 DC internal resistance table
[0160] As an example, a 60% threshold is adopted: for a certain cell, K=63% at 32h, formation is carried out immediately, no sodium precipitation is found after disassembly, and the cycle performance is excellent. A 55% threshold is adopted: for a certain cell, K=56% at 28h, formation is carried out in advance, no obvious sodium precipitation is found after disassembly (due to the small margin), but the risk increases during mass production. A 70% threshold is adopted: for a certain cell, K=65% at 40h, which still does not meet the standard, it continues to stand until 60h when the K value is still 66%, and is finally judged as unqualified, though it is actually fully wetted.
[0161] In some alternative embodiments, a dynamic threshold can be adopted. For example, different thresholds can be preset according to the positive and negative electrode materials, electrode sheet thickness, electrolyte viscosity, etc., for example, 55% for thick electrode sheets and 65% for thin electrode sheets. A dual threshold can also be adopted: a first threshold (such as 55%) is set for pre-formation (small-current pre-charging), and a second threshold (such as 60%) is set for main formation, to further optimize the process.
[0162] Formation refers to the process of performing the first charge and discharge on the cell injected with electrolyte, the purpose of which is to form a stable solid electrolyte interphase (SEI) film on the surface of the negative electrode and activate the positive and negative electrode materials.
[0163] Once the K value is detected to exceed a predetermined threshold, the cell is immediately transferred to the formation process. Formation typically involves constant current charging with a small current (e.g., 0.05C–0.2C) to a predetermined voltage (e.g., 4.0V for sodium-ion batteries), followed by a period of rest, and then discharge to the cutoff voltage. During the formation process, because the electrodes are fully wetted, a uniform and dense SEI film can be formed, avoiding localized sodium deposition.
[0164] Please see Figure 8 In some embodiments, the method further includes: S7: If the decrease is still not less than the predetermined threshold after a predetermined time period, the wet cell is determined to be unqualified.
[0165] The preset duration is the maximum set time for static monitoring. If this time is exceeded, even if the K value still does not exceed the threshold, the static monitoring will not continue, and the cell will be directly judged as a defective product and rejected.
[0166] The settling time for each battery cell cannot be extended indefinitely. On the one hand, a very small number of cells may experience extremely slow wetting or never reach the threshold due to manufacturing defects (such as overly dense electrode coating, partial blockage of the diaphragm, or insufficient electrolyte injection due to a faulty injection valve). On the other hand, the production line needs to maintain its pace and cannot allow the entire settling process to be blocked due to a few abnormal cells. Therefore, it is necessary to set a maximum allowable settling time (i.e., a predetermined duration).
[0167] If the K value still does not exceed the threshold after the predetermined settling time, it indicates that the battery cell has an irreversible wetting defect. At this point, the system should automatically mark the battery cell as unqualified and remove it from the production line (e.g., move it to the defective product area) and prevent it from entering the formation process. This avoids: ① Indefinite settling wastes production capacity and equipment; ② Mixing defective cells into the formation process leads to waste in subsequent processes (formation also consumes time and electricity); ③ Defective cells flowing to the customer and causing safety accidents.
[0168] As an example, the preset duration is set to 48 hours. If a certain battery cell measures K=58% after 48 hours (not reaching 60%), the system determines it to be unqualified, automatically removes it from the resting tray, and records it as a defective product with poor wetting.
[0169] In some alternative implementations, a tiered judgment can be used. If the K value is very low (e.g., <30%) within a predetermined time period, it can be directly judged as a serious non-conformity; if it is close to the threshold (e.g., 55%–60%), retesting or monitoring can be extended for 2–4 hours before a final judgment is made. Manual verification can also be used. For non-conforming products close to the threshold, manual retesting or disassembly verification can be allowed to optimize process parameters.
[0170] In some implementations, the predetermined duration is 36-72 hours. For example, the predetermined duration can be 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, or 72 hours.
[0171] The scheduled duration is the maximum time for static monitoring, and it is also the time point at which failure is determined if the time limit is exceeded.
[0172] The lower limit of 36 hours ensures that normal cells have enough time to reach the threshold; the upper limit of 72 hours avoids indefinite delays in the production line due to individual abnormal cells.
[0173] If the time is less than 36 hours, in one example, the dry-state internal resistance R1 = 200mΩ, and the wet-state internal resistance is 91mΩ (K=54.5%) at 20h, 74mΩ (K=63%) at 32h, and 69mΩ (K=65.5%) at 40h. Normal cells typically reach K>60% between 30 and 35h. If the predetermined time is set to less than 36 hours (e.g., 30h), many normal cells may still have a K value of around 58% at 30h (not yet reaching 60%), and will be incorrectly judged as unqualified, leading to a serious yield loss (it is estimated that more than 30% of normal cells will be misjudged). Therefore, 36 hours is the lower limit to ensure that normal cells have a chance of meeting the standard.
[0174] If the time exceeds 72 hours: For normal cells, the K-value stabilizes at 69% within 48 hours and hardly changes thereafter. If the predetermined time is set to exceed 72 hours (e.g., 96 hours), the production line needs to reserve a settling window of up to 4 days for each cell. Even if the vast majority of cells have completed soaking within 40 hours, they still need to wait 72 hours before being judged as qualified or unqualified (because the timeout judgment only occurs after 72 hours). This will lead to a surge in the settling area of the production line, a backlog of work-in-process inventory, and a severe reduction in production efficiency. In addition, a very small number of abnormal cells cannot meet the standard even after 96 hours of settling, so extending the upper limit is not beneficial.
[0175] As an example, a predetermined timeframe of 48 hours is set: normal cells that meet the standards within 32-44 hours are directly transferred to the formation process; abnormal cells that still fail to meet the standards within 48 hours are deemed unqualified and discarded. The production line's resting cycle is controllable.
[0176] If the time limit is set to 36 hours: a certain cell has a K=59% at 36 hours (due to slightly thicker electrode sheets) and is judged to be unqualified. In reality, it can reach 63% at 40 hours, which leads to a misjudgment.
[0177] If the time limit is set to 72 hours: a certain battery cell has met the standard after 40 hours, but the static equipment still needs to keep it for 72 hours before it can be released (if it is managed in batches), which will cause the production line to be blocked.
[0178] In some alternative implementations, a dynamic predetermined duration can be used: the predetermined duration is dynamically adjusted based on the cell's historical data (such as the size of the dry-state internal resistance R1): cells with smaller R1 (lower electronic resistance) are generally wetted faster and can be set to a shorter duration (such as 36h); cells with larger R1 can be set to a longer duration (such as 60h).
[0179] A phased warning approach can also be adopted: if the K value still does not reach 80% of the threshold (e.g., 48%) at 80% of the predetermined duration (e.g., 80% of 48h, i.e., 38.4h), an early warning will be issued to indicate that it may be unqualified, facilitating manual intervention.
[0180] Please see Figure 9 The specific embodiments of this application also provide a secondary battery cell 10, which is produced using the aforementioned production method.
[0181] Please see Figure 9 This application also provides an energy storage device 100, which includes the battery cell 10. For example, the energy storage device 100 may include one or more of the following: an emergency start-up power supply, a start-stop power supply, an outdoor energy storage device, a portable energy storage device, and a power tool power supply.
[0182] In this specification, the terms "specifically," "furthermore," "particularly," "understandably," etc., refer to specific features, structures, materials, or characteristics described in connection with embodiments or examples that are included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0183] Any process or method description in the flowchart or otherwise herein can be understood as representing a module, segment, or portion of executable request code comprising one or more steps for implementing a particular logical function or process, and the scope of the preferred embodiments of this application includes additional implementations in which functions may be performed not in the order shown or discussed, including substantially simultaneously or in reverse order according to the functions involved, as should be understood by those skilled in the art to which embodiments of this application pertain.
[0184] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A method for producing a cell for a secondary battery, characterized in that, include: We provide positive and negative electrode plates; The positive electrode and the negative electrode are wound to obtain a dry cell; Measure the first DC internal resistance of the dry cell; Electrolyte is injected into the dry cell to obtain a wet cell; The second DC internal resistance of the wet battery cell is monitored during the static storage process. When the decrease in the second DC internal resistance relative to the first DC internal resistance is greater than a predetermined threshold, the cell is converted into a wet cell to obtain the cell of the secondary battery.
2. The method as described in claim 1, characterized in that, The measurement of the first DC internal resistance of the dry cell includes: The dry cell is charged and / or discharged at a constant current for a first time using a first current. Measure the first voltage change of the dry cell; The first DC internal resistance is calculated based on the first voltage change value and the first current.
3. The method as described in claim 1, characterized in that, The monitoring of the second DC internal resistance of the wet battery cell during the static storage process includes: During the resting process of the wet battery cell, the second DC internal resistance is measured once at predetermined intervals.
4. The method as described in claim 3, characterized in that, The scheduled time is 2-8 hours.
5. The method as described in claim 3, characterized in that, The step of measuring the second DC internal resistance at predetermined intervals includes: The wet cell is charged and / or discharged at a constant current for a second time at predetermined intervals; Measure the second voltage change value of the wet battery; The second DC internal resistance is calculated based on the second voltage change value and the second current.
6. The method as described in claim 2 or 5, characterized in that, The first current and / or the second current is 0.05-0.2 times, and the first time and / or the second time is 5-30 seconds.
7. The method as described in claim 1, characterized in that, The predetermined threshold is 55%-70%.
8. The method as described in claim 1, characterized in that, The method further includes: If the decrease is still not less than the predetermined threshold after a predetermined time period, the wet cell is determined to be unqualified.
9. The method as described in claim 8, characterized in that, The scheduled duration is 36-72 hours.
10. The method according to any one of claims 1-9, characterized in that, The secondary battery is a sodium-ion battery.
11. The method as described in claim 10, characterized in that, The positive electrode sheet comprises a polyanionic positive electrode material, a carbon nanotube conductive agent, a superconducting carbon black conductive agent, and a polyvinylidene fluoride binder; the polyanionic positive electrode material has a mass percentage of 90.0% to 98.0%, the carbon nanotube conductive agent has a mass percentage of 0.5% to 3.0%, the superconducting carbon black conductive agent has a mass percentage of 0.5% to 4.0%, and the polyvinylidene fluoride binder has a mass percentage of 1.2% to 3.0%.
12. The method as described in claim 11, characterized in that, The mass percentage of the polyanionic cathode material is 93.0%~95.0%, the mass percentage of the carbon nanotube conductive agent is 1.0%~2.5%, the mass percentage of the superconducting carbon black conductive agent is 1.0%~2.5%, and the mass percentage of the polyvinylidene fluoride binder is 1.2%~2.5%.
13. The method as described in claim 10, characterized in that, The negative electrode sheet comprises hard carbon active material, superconducting carbon black conductive agent, sodium carboxymethyl cellulose thickener, and styrene-butadiene rubber binder; the mass percentage of the hard carbon active material is 90.0%~95.0%, the mass percentage of the superconducting carbon black conductive agent is 0.5%~4.0%, the mass percentage of the sodium carboxymethyl cellulose thickener is 0.2%~2.5%, and the mass percentage of the styrene-butadiene rubber binder is 1.2%~3.0%.
14. The method as described in claim 13, characterized in that, The hard carbon active material has a mass percentage of 93.0% to 94.5%, the superconducting carbon black conductive agent has a mass percentage of 1.0% to 3.0%, the sodium carboxymethyl cellulose thickener has a mass percentage of 0.5% to 2.0%, and the styrene-butadiene rubber binder has a mass percentage of 1.5% to 2.5%.
15. The method as described in claim 10, characterized in that, The bifacial density of the positive electrode sheet coated on the positive current collector is 13.0 mg / cm² to 30.4 mg / cm², and the bifacial density of the negative electrode sheet coated on the negative current collector is 5.2 mg / cm² to 12.6 mg / cm².
16. The method as described in claim 15, characterized in that, The positive electrode coating has a bifacial density of 13.5 mg / cm² to 25.2 mg / cm², and the negative electrode coating has a bifacial density of 5.4 mg / cm² to 10.2 mg / cm².
17. The method as described in claim 10, characterized in that, The provision of a positive electrode, a negative electrode, and an electrolyte includes: Using N-methylpyrrolidone as a solvent, polyanionic cathode material, carbon nanotube conductive agent, superconducting carbon black conductive agent and polyvinylidene fluoride binder are mixed, stirred and dispersed to prepare cathode slurry; The positive electrode slurry is coated onto the surface of the positive electrode aluminum foil current collector, dried, and rolled to obtain the positive electrode sheet; Using deionized water as a solvent, hard carbon active material, superconducting carbon black conductive agent, sodium carboxymethyl cellulose thickener and styrene-butadiene rubber binder are mixed, stirred and dispersed to prepare negative electrode slurry; The negative electrode slurry is coated onto the surface of the negative electrode aluminum foil current collector, dried, and rolled to obtain the negative electrode sheet.
18. A cell for a secondary battery, characterized in that, The battery cell is manufactured using the method described in any one of claims 1-17.
19. An energy storage device, characterized in that, The energy storage device includes the battery cell as described in claim 18.