A bromine-substituted polyaniline-based four-electron aqueous zinc-iodine battery and its preparation method
By using bromine-substituted polyaniline cathode and composite electrolyte in zinc-iodine batteries, a three-dimensional nanofiber structure was constructed, which solved the problems of polyiodine anion shuttle effect and I+ hydrolysis in zinc-iodine batteries, realized four-electron redox reaction, and improved the battery voltage, energy density and cycle life.
Patent Information
- Application Number
- CN202611622254.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing zinc-iodine batteries are difficult to achieve four-electron reactions, suffer from severe shuttle effects of polyiodine anions, have high self-discharge, short cycle life, and I+ is easily hydrolyzed in aqueous solution, making it difficult to stably achieve I0/I+ conversion.
A three-dimensional interwoven nanofiber network structure was constructed by using bromine-substituted polyaniline cathode material and ZnI2+ZnBr2 composite electrolyte. The electrostatic interaction inhibited the shuttle of polyiodine anions, generating a stable IBr2- complex and activating the four-electron redox reaction of iodine.
It significantly improves the rate performance and long-cycle stability of the battery, significantly increases the battery output voltage and energy density, reduces self-discharge, alleviates zinc anode corrosion, and extends cycle life.
Smart Images

Figure CN123120925A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of zinc-iodine battery technology, specifically relating to a bromine-substituted polyaniline-based four-electron aqueous zinc-iodine battery and its preparation method. Background Technology
[0002] With the ongoing energy transition, large-scale energy storage technologies urgently require electrochemical systems that are safe, low-cost, long-life, and environmentally friendly. Aqueous zinc-iodine batteries (ZIBs), with their advantages of high theoretical iodine capacity, abundant raw material reserves, low cost, and high safety, have become highly promising energy storage devices for large-scale energy storage. Traditional zinc-iodine batteries can only achieve I... - The two-electron redox reaction of I₂ has limited energy density. If it were possible to achieve I₂… - / I 0 / I + The four-electron reaction can further improve the battery's output voltage and energy density.
[0003] The existing technology has many technical bottlenecks: (1) Iodine has poor conductivity and slow redox kinetics; (2) Soluble polyiodide anions are easily generated during the charging and discharging process, resulting in a shuttle effect. Polyiodide anions pass through the diaphragm and corrode the zinc anode, causing loss of active material, severe self-discharge, and reduced cycle life; (3) I in aqueous solution + It is highly susceptible to hydrolysis and difficult to achieve stable I 0 / I + The four-electron redox reaction is difficult to activate effectively. How to achieve iodine four-electron redox, suppress the shuttle of polyiodine anions, and improve the rate capability and cycle life is a technical problem that urgently needs to be solved in this field. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of existing zinc-iodine batteries, such as difficulty in stably achieving four-electron reactions, severe polyiodide shuttling, high self-discharge, and poor long-cycle performance, and to provide a bromine-substituted polyaniline-based four-electron aqueous zinc-iodine battery and its preparation method.
[0005] This invention obtains a brominated polyaniline cathode material through the electrochemical copolymerization of aniline and 3-bromoaniline, constructing a three-dimensional interwoven nanofiber network structure; combined with a ZnI2+ZnBr2 composite electrolyte, Br - with I + Formation of stable IBr2 - Complex, inhibiting I + Hydrolysis successfully activated iodine I. - / I 0 / I + Four-electron redox reaction. Bromine-substituted nitrogen cations on the polyaniline chain anchor polyiodide anions through electrostatic interactions, reducing zinc anode corrosion, significantly reducing self-discharge, and improving battery rate performance and ultra-long cycle stability.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] A brominated polyaniline-based four-electron aqueous zinc-iodine battery includes a positive electrode, a negative electrode, a separator, and an electrolyte; the positive electrode is brominated polyaniline Br-PANI electropolymerized in situ on a stripped graphite foil EG substrate; the negative electrode is a modified zinc sheet; and the electrolyte is a mixed aqueous solution of ZnI2 and ZnBr2.
[0008] The preparation method of the above-mentioned brominated polyaniline-based four-electron aqueous zinc-iodine battery includes the following steps:
[0009] 1) Preparation of exfoliated graphite foil EG conductive substrate;
[0010] 2) Br-PANI-1:3 cathode was prepared on an EG electrode using cyclic voltammetry;
[0011] 3) Preparation of modified zinc sheet negative electrode: Graphite powder and PVDF are dissolved in NMP to make a slurry, the slurry is coated on the surface of zinc sheet and dried;
[0012] 4) Prepare a mixed aqueous solution of ZnI2 and ZnBr2 as the electrolyte;
[0013] 5) Place the Swagelok battery in the order of Br-PANI-1:3 positive electrode-separator-modified zinc sheet negative electrode. After placing the separator, inject the electrolyte. After placing the negative electrode, encapsulate the zinc-iodine battery.
[0014] Furthermore, in the above preparation method, step 1), the method for preparing the exfoliated graphite foil EG conductive substrate is as follows: in a three-electrode system, the substrate is cut to a size of 0.8 × 0.8 cm. 2 Using graphite foil as the working electrode, SCE as the reference electrode, and platinum sheet as the counter electrode, 10 cyclic voltammetric scans were first performed in 0.5M KOH solution at a scan rate of 20mV / s and a potential range of 0~1.8V. Then, the solution was continuously treated in 0.5M KNO3 solution at a constant potential of 1.8V for 600s, followed by 15 cyclic voltammetric scans at a voltage range of -1.3~1.2V and a scan rate of 20mV / s to obtain EG.
[0015] Furthermore, in the above preparation method, step 2), the method for preparing the Br-PANI-1:3 cathode on EG using cyclic voltammetry is as follows: 3-bromoaniline and aniline are dissolved in 1M HClO4 aqueous solution to prepare an electrochemical copolymerization deposition solution, and electrochemical deposition is performed using a three-electrode system: with SCE as the reference electrode, EG as the working electrode, and platinum sheet as the counter electrode, cyclic voltammetry scanning is performed; the working electrode is removed, thoroughly rinsed with deionized water, and dried to obtain Br-PANI-1:3.
[0016] Furthermore, in the above preparation method, in step 2), the concentration of 3-bromoaniline in the 1M HClO4 aqueous solution is 0.05M, and the concentration of aniline in the 1M HClO4 aqueous solution is 0.15M.
[0017] Furthermore, in the above preparation method, step 2), the parameters of the cyclic voltammetric scan are set as follows: voltage range of 0~1V, scan rate of 20mV / s, and number of cycles of 7.
[0018] Furthermore, in the above preparation method, step 2), the drying is performed at 60°C for 10 hours.
[0019] Furthermore, in the above preparation method, step 3), the method for preparing the modified zinc sheet negative electrode is as follows: graphite powder and PVDF are mixed and dissolved in NMP at a mass ratio of 1:1 to form a slurry and uniformly coated on the surface of a circular zinc sheet with a diameter of 1.0 cm, and dried at 100°C for 24 h.
[0020] Furthermore, in step 4) of the above preparation method, the electrolyte is a mixed aqueous solution of ZnI2 with a mass molar concentration of 0.35m and ZnBr2 with a mass molar concentration of 9m.
[0021] Furthermore, in the above preparation method, step 5), the assembly method of the zinc-iodine battery is as follows: using a Swagelok battery composed of a titanium rod and polytetrafluoroethylene, with Br-PANI-1:3 as the positive electrode, two glass fiber membranes are placed in, electrolyte is added, and modified zinc sheet is used as the negative electrode to assemble the zinc-iodine battery.
[0022] The beneficial effects of this invention are:
[0023] 1. In existing zinc-iodine batteries, I3 - I5 - The shuttle effect of polyiodine species leads to poor stability and makes it difficult to achieve I... 0 / I + Redox reactions can only result in two-electron energy storage reactions, limiting the improvement of battery energy density. This invention employs the electrochemical copolymerization of aniline and 3-bromoaniline to construct a bromosubstituted polyaniline Br-PANI-1:3 with a nanofiber network structure on a three-dimensional porous exfoliated graphite foil substrate. This three-dimensional porous network can provide a large number of iodine redox active sites; the polymer molecular chains contain a large number of nitrogen cations (-NH4+). + =、-N + -), can anchor iodine anions (I3) through strong electrostatic interactions. - I5 -This reduces the polyiodine ion shuttle effect at its source, mitigating the corrosive damage of polyiodine species to the zinc anode. The zinc anode surface remains smooth after battery cycling, indicating significant inhibition of zinc dendrite growth and improved battery cycle life.
[0024] 2. Existing zinc-iodine batteries can only achieve I - / I 0 Two-electron redox reactions, limited by I + It is readily hydrolyzed in aqueous solution and is difficult to trigger I. 0 / I + Redox conversion limits the energy density of batteries to a single low-voltage discharge plateau. This invention employs a bromine-substituted polyaniline cathode matched with a bromine-containing composite electrolyte. The Br in the electrolyte... - Can be used with I + Combined to form stable IBr2 - Complexes, overcoming I in aqueous solution + Overcoming the hydrolysis challenge, successfully achieving I- iodine synthesis. - / I 0 / I + A four-electron reversible redox energy storage system was constructed, featuring a dual-voltage platform at 1.2V and 1.5V, where I... 0 / I + The voltage plateau accounts for up to 37.4%, significantly improving the battery's output voltage and area-specific capacity. (At 1 mA·cm²) -2 At the specified current density, the areal specific capacity of the Zn / / Br-PANI-1:3 battery can reach 1.72 mAh·cm³. -2 This is significantly higher than the 0.70 mAh·cm⁻¹ of Zn / / EG batteries under the same conditions. -2 .
[0025] 3. Compared to traditional zinc-iodine batteries, the brominated polyaniline cathode of this invention significantly reduces charge transfer resistance to only 4.59 Ω, resulting in significantly improved redox reaction kinetics and excellent rate performance. (At 10 mA·cm⁻¹) -2 It can still maintain 0.84 mAh·cm³ under high current density conditions. -2 The specific capacity of the area is significantly improved. This invention can significantly alleviate the problem of battery self-discharge. After being fully charged and left to stand for 24 hours, the specific capacity of the Zn / / Br-PANI-1:3 battery can retain 73.16%, while the specific capacity of the Zn / / EG battery under the same conditions is only 26.68%.
[0026] 4. Existing zinc-iodine batteries generally suffer from short cycle life under high current, and ordinary host materials struggle to simultaneously achieve both polyiodine suppression and four-electron reaction activation. The battery assembled using the cathode material of this invention exhibits excellent long-term cycle stability at 10 mA·cm⁻¹. -2After 4,000 charge-discharge cycles at high current density, the area capacity retention rate can still reach 82.14%; in contrast, the Zn / / EG battery only experienced short-circuit failure after 512 cycles. Attached Figure Description
[0027] Figure 1 The Zn / / Br-PANI-1:3 battery of Example 1 and the Zn / / EG battery of Comparative Example 1 were compared at 1 mA·cm⁻¹. -2 Constant current charge-discharge curves at current density.
[0028] Figure 2 This is a comparison chart of the rate performance of the Zn / / Br-PANI-1:3 battery in Example 1 and the Zn / / EG battery in Comparative Example 1.
[0029] Figure 3 The Zn / / Br-PANI-1:3 battery of Example 1 and the Zn / / EG battery of Comparative Example 1 were compared at 5 mA·cm⁻¹. -2 Long-cycle performance curves at current density.
[0030] Figure 4 The Zn / / Br-PANI-1:3 battery of Example 1 and the Zn / / EG battery of Comparative Example 1 were compared at 10 mA·cm⁻¹. -2 Long-cycle performance curves at current density.
[0031] Figure 5 The graphs show the self-discharge performance of the Zn / / Br-PANI-1:3 battery of Example 1 and the Zn / / EG battery of Comparative Example 1 after being left to stand for 12 hours and 24 hours, respectively. In the graphs, a represents the Zn / / Br-PANI-1:3 battery after 12 hours of standing, b represents the Zn / / Br-PANI-1:3 battery after 24 hours of standing, c represents the Zn / / EG battery after 12 hours of standing, and d represents the Zn / / EG battery after 24 hours of standing.
[0032] Figure 6 The images show SEM images of the zinc anode after cyclic charging and discharging of the Zn / / EG battery (a) of Comparative Example 1 and the Zn / / Br-PANI-1:3 battery (b) of Example 1.
[0033] Figure 7 This is a schematic diagram of the structure of a bromine-substituted polyaniline cathode. Detailed Implementation
[0034] Example 1
[0035] This embodiment prepared a novel zinc-iodine battery using brominated polyaniline as the positive electrode, modified zinc sheet as the negative electrode, and a mixed aqueous solution of ZnI2 + ZnBr2 as the electrolyte. The specific preparation method includes the following steps:
[0036] 1) Positive electrode: First, the graphite foil is peeled off. In the three-electrode system, the graphite foil (0.8 × 0.8 cm) is used. 2 The electrode used is a saturated calomel electrode (SCE) as the working electrode, a platinum sheet as the counter electrode, and a 0.5M KOH solution as the electrolyte. The voltage is 20 mV / s. -1 The scan rate was 0–1.8 V, and cyclic voltammetry was performed for 10 cycles. Then the electrolyte was replaced with 0.5 M KNO3 solution, and the electrophoresis was maintained at a constant potential of 1.8 V for 600 s. Subsequently, the electrophoresis was performed at 20 mV s in the range of -1.3–1.2 V. -1 The scan rate was set at 15 CV cycles to obtain the exfoliated graphite foil (EG). 0.05 mol / L 3-bromoaniline and 0.15 mol / L aniline (molar ratio of 3-bromoaniline to aniline 1:3) were dissolved in 1M HClO4 aqueous solution as the deposition solution. Using EG as the working electrode, SCE as the reference electrode, and a platinum sheet as the counter electrode, the deposition was performed at 20 mV s⁻¹ within a potential window of 0–1 V. -1 At a scan rate of [value missing], 7 cyclic voltammetric scans were performed, and the electrode surface turned dark green. The working electrode was removed, thoroughly rinsed with deionized water, and dried in a 60℃ oven for 10 hours to obtain Br-PANI-1:3.
[0037] 2) Negative electrode: 30 mg of graphite powder and 30 mg of polyvinylidene fluoride (PVDF) are mixed evenly and dissolved in 1000 μL of N-methylpyrrolidone (NMP) to make a slurry. The slurry is coated on the surface of a 1.0 cm diameter circular zinc sheet and dried in a drying oven at 100 °C for 24 h to obtain a modified zinc sheet.
[0038] 3) Electrolyte: Use a mixed aqueous solution of 0.35m ZnI2 + 9m ZnBr2 (m is the molality, i.e. the amount of solute in each kilogram of solvent).
[0039] 4) Battery assembly: A Swagelok battery structure consisting of a titanium rod and polytetrafluoroethylene was adopted. The Br-PANI-1:3 prepared in step 1) was used as the positive electrode, two glass fiber membranes were placed in it, 60 μL of the electrolyte prepared in step 3) was injected, and the modified zinc sheet prepared in step 2) was used as the negative electrode to assemble a zinc-iodine battery (Zn / / Br-PANI-1:3).
[0040] Comparative Example 1
[0041] 1. The preparation process of zinc / / stripped graphite foil battery (Zn / / EG) is as follows:
[0042] Using the exfoliated graphite foil (EG) obtained in Example 1 as the positive electrode and the modified zinc sheet as the negative electrode, and using a mixed aqueous solution of 0.35mZnI2+9mZnBr2 as the electrolyte, a Swagelok battery was assembled to obtain the Zn / / EG battery.
[0043] 2. Performance Testing:
[0044] 1) Constant current charge-discharge test: Electrochemical tests were performed on the Zn / / Br-PANI-1:3 battery of Example 1, and a comparative experiment was conducted using the Zn / / EG battery of Comparative Example 1. The constant current charge-discharge test was performed at 1 mA·cm⁻¹. -2 Constant current charge-discharge tests were performed on these two types of batteries at current density.
[0045] like Figure 1 As shown, the discharge curve of the Zn / / EG battery only shows a distinct discharge plateau at approximately 1.2V (corresponding to I). 0 / I - (Conversion), at 1.5V (corresponding to I) 0 / I + The conversion platform is relatively short, accounting for only 20% of the total. Its area-to-capacity ratio is only 0.7 mAh·cm³. -2 The Coulomb efficiency is only 44.49%.
[0046] The Zn / / Br-PANI-1:3 battery exhibits two distinct discharge plateaus at the same current density: 1.2V and 1.5V. The 1.5V plateau accounts for a significant 37% of the total discharge, with an areal capacity of 1.72 mAh·cm³. -2 The coulomb efficiency was 83.99%, which was significantly better than the control group.
[0047] 2) Rate performance testing: Electrochemical tests were performed on the Zn / / Br-PANI-1:3 battery of Example 1, and a comparative experiment was conducted using the Zn / / EG battery of Comparative Example 1. Rate performance testing was performed at 1 mA·cm⁻¹. -2 2mA·cm -2 5mA·cm -2 10mA·cm -2 The areal capacity of the batteries was tested at different current densities.
[0048] like Figure 2 As shown, the areal specific capacity of Zn / / EG batteries under different current densities is 0.65 mAh·cm⁻¹. -2 0.52mAh·cm -2 0.32mAh·cm -2 0.20mAh·cm -2 The areal specific capacity of the Zn / / Br-PANI-1:3 battery in Example 1 at different current densities was 1.72 mAh·cm³. -2 1.52mAh·cm -2 1.19mAh·cm -2 0.84mAh·cm-2 The rate performance is far superior to that of Zn / / EG batteries at the corresponding current density, thanks to the improved redox kinetics of iodine by Br-PANI-1:3.
[0049] 3) Long-term cycle stability: Electrochemical tests were performed on the Zn / / Br-PANI-1:3 battery of Example 1, and a comparative experiment was conducted using the Zn / / EG battery of Comparative Example 1. At 5 mA·cm⁻¹ -2 and 10mA·cm -2 The cycle stability of the two battery groups was tested at current density.
[0050] like Figure 3 As shown, at 5mA·cm -2 At the given current density, the initial discharge areal capacity of the Zn / / EG battery is 0.325 mAh·cm³. -2 After 5 cycles, the specific capacity increased to 0.366 mAh·cm³. -2 Subsequently, the areal capacity significantly decreased, making it unable to maintain stable cycling; the Zn / / Br-PANI-1:3 battery system had an initial discharge areal capacity of 1.2 mAh·cm³. -2 After 70 cycles, it increased to 1.36 mAh·cm³. -2 No significant decay was observed during subsequent cycles, and the capacity retention rate was 96.4% after 500 cycles.
[0051] like Figure 4 As shown, at 10 mA·cm -2 At current density, the Zn / / EG battery failed due to short circuit after only 512 cycles because zinc dendrites pierced the separator; while the Zn / / Br-PANI-1:3 battery of this invention still maintained a capacity retention of 82.14% after 4000 charge-discharge cycles, demonstrating ultra-long cycle stability.
[0052] 4) Self-discharge performance test: Self-discharge tests were conducted on Zn / / Br-PANI-1:3 batteries and Zn / / EG batteries.
[0053] like Figure 5 As shown, the Zn / / Br-PANI-1:3 battery retained 75.54% of its capacity after 12 hours of rest and 73.16% of its areal capacity after 24 hours of rest. In comparison, the Zn / / EG battery only retained 35.39% (12h) and 26.68% (24h) of its capacity under the same conditions.
[0054] 5) SEM morphology verification: The Zn / / Br-PANI-1:3 battery and Zn / / EG battery after cyclic charge-discharge testing were disassembled, and the zinc anode was characterized by scanning electron microscopy (SEM).
[0055] like Figure 6 As shown, after cyclic charging and discharging, a large number of zinc dendrites are generated on the surface of the zinc anode in Zn / / EG batteries. These zinc dendrites accumulate and eventually puncture the separator, causing a short circuit. Therefore, Zn / / EG batteries have a relatively short cycle life. In contrast, the surface of the zinc anode in Zn / / Br-PANI-1:3 batteries is relatively smooth. This is because Br-PANI-1:3 anchors polyiodide anions during charging and discharging, protecting the zinc anode from corrosion and damage.
Claims
1. A brominated polyaniline-based four-electron aqueous zinc-iodine battery, characterized in that, The brominated polyaniline-based four-electron aqueous zinc-iodine battery includes a positive electrode, a negative electrode, a separator, and an electrolyte; the positive electrode is brominated polyaniline Br-PANI electropolymerized in situ on a stripped graphite foil EG substrate; the negative electrode is a modified zinc sheet; and the electrolyte is a mixed aqueous solution of ZnI2 and ZnBr2.
2. The method for preparing a brominated polyaniline-based four-electron aqueous zinc-iodine battery according to claim 1, characterized in that, Includes the following steps: 1) Preparation of exfoliated graphite foil EG conductive substrate; 2) Br-PANI-1:3 cathode was prepared on an EG electrode using cyclic voltammetry; 3) Preparation of modified zinc sheet negative electrode: Graphite powder and PVDF are dissolved in NMP to make a slurry, the slurry is coated on the surface of zinc sheet and dried; 4) Prepare a mixed aqueous solution of ZnI2 + ZnBr2 as the electrolyte; 5) Place the Swagelok battery in the order of Br-PANI-1:3 positive electrode-separator-modified zinc sheet negative electrode. After placing the separator, inject the electrolyte. After placing the negative electrode, encapsulate the zinc-iodine battery.
3. The preparation method according to claim 2, characterized in that, In step 1), the method for preparing the exfoliated graphite foil EG conductive substrate is as follows: in a three-electrode system, the substrate is cut to a size of 0.8 × 0.8 cm. 2 Using graphite foil as the working electrode, SCE as the reference electrode, and platinum sheet as the counter electrode, 10 cyclic voltammetric scans were first performed in 0.5M KOH solution at a scan rate of 20mV / s and a potential range of 0~1.8V. Then, the solution was continuously treated in 0.5M KNO3 solution at a constant potential of 1.8V for 600s, followed by 15 cyclic voltammetric scans at a voltage range of -1.3~1.2V and a scan rate of 20mV / s to obtain EG.
4. The preparation method according to claim 2, characterized in that, In step 2), the method for preparing the Br-PANI-1:3 cathode on the EG using cyclic voltammetry is as follows: 3-bromoaniline and aniline are dissolved in a 1M HClO4 aqueous solution to prepare an electrochemical copolymerization deposition solution. Electrochemical deposition is performed using a three-electrode system: SCE is used as the reference electrode, EG is used as the working electrode, and a platinum sheet is used as the counter electrode. Cyclic voltammetry scans are performed. The working electrode is then removed, thoroughly rinsed with deionized water, and dried to obtain Br-PANI-1:
3.
5. The preparation method according to claim 4, characterized in that, In step 2), the concentration of 3-bromoaniline in the 1M HClO4 aqueous solution is 0.05M, and the concentration of aniline in the 1M HClO4 aqueous solution is 0.15M.
6. The preparation method according to claim 4, characterized in that, In step 2), the parameters of the cyclic voltammetric scan are set as follows: voltage range of 0~1V, scan rate of 20mV / s, and number of cycles of 7.
7. The preparation method according to claim 4, characterized in that, In step 2), the drying process involves drying at 60°C for 10 hours.
8. The preparation method according to claim 2, characterized in that, In step 3), the method for preparing the modified zinc sheet negative electrode is as follows: graphite powder and PVDF are mixed and dissolved in NMP at a mass ratio of 1:1 to form a slurry and uniformly coated on the surface of a circular zinc sheet with a diameter of 1.0 cm, and dried at 100°C for 24 h.
9. The preparation method according to claim 2, characterized in that, In step 4), the electrolyte is a mixed aqueous solution of ZnI2 with a molar concentration of 0.35m and ZnBr2 with a molar concentration of 9m.
10. The preparation method according to claim 2, characterized in that, In step 5), the assembly method of the zinc-iodine battery is as follows: a Swagelok battery composed of a titanium rod and polytetrafluoroethylene is used, with Br-PANI-1:3 as the positive electrode, two glass fiber membranes are placed in, electrolyte is added, and a modified zinc sheet is used as the negative electrode to assemble the zinc-iodine battery.