A binder-free all-solid-state electrolyte based on the layered structure of phlogopite mica, its preparation method and application

By using a binder-free all-solid-state electrolyte based on the layered structure of phlogopite, the problems of polyiodide shuttle effect and zinc anode side reaction in aqueous zinc-iodine batteries have been solved, achieving high ion conductivity and long cycle stability, and improving the cycle life and safety of the battery.

CN123120927APending Publication Date: 2026-11-17HAINAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611437221.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Aqueous zinc-iodine batteries suffer from rapid capacity decay and short cycle life due to the superposition of polyiodide shuttle effect and zinc anode side reaction. Existing polymer-based composite solid electrolytes are difficult to balance high ionic conductivity and long cycle stability due to the low ionic conductivity of the polymer matrix, easy swelling and degradation, and large ion transport barrier at heterogeneous interfaces.

Method used

A binder-free all-solid electrolyte based on the layered structure of phlogopite was used. Zn2+ was loaded onto the interlayer domains and/or framework surface by stirring phlogopite powder in zinc salt electrolyte. The two-dimensional layered structure of phlogopite and the Mg-O polar bond were used to suppress the migration of polyiodide anions. Combined with drying treatment to remove free water, a self-supporting electrolyte sheet was prepared.

Benefits of technology

It achieves efficient and orderly migration of Zn2+, inhibits the migration of polyiodide ions to the zinc anode, reduces zinc dendrite growth, improves battery cycle life and safety, and the material is environmentally friendly and inexpensive.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123120927A_ABST
    Figure CN123120927A_ABST
Patent Text Reader

Abstract

This invention discloses a binder-free all-solid-state electrolyte based on the layered structure of phlogopite, its preparation method, and its application, belonging to the field of zinc-ion energy storage battery electrolyte technology. The preparation method includes: (1) adding phlogopite powder to a zinc salt electrolyte, stirring, centrifuging, discarding the supernatant, collecting the precipitate, washing, and drying to obtain zinc-loaded phlogopite inorganic powder; (2) grinding the obtained zinc-loaded phlogopite inorganic powder, without adding any binder, and directly pressing it into shape to obtain phlogopite-based all-solid-state electrolyte sheets. This invention utilizes the two-dimensional layered framework structure of phlogopite as Zn 2+ It provides a continuous conduction channel, utilizes the exposed Mg-O polar bonds on the surface of the phlogopite framework layer to suppress polyiodine shuttle, and eliminates free water through drying treatment to suppress hydrogen evolution side reactions. The resulting electrolyte can be used in aqueous zinc-iodine batteries and aqueous zinc-ion energy storage batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of zinc-ion energy storage battery electrolyte technology, specifically relating to a binder-free all-solid-state electrolyte based on a layered structure of phlogopite mica, its preparation method, and its application. Background Technology

[0002] Aqueous zinc-ion batteries, with their advantages of abundant zinc resources, high theoretical specific capacity, moderate redox potential, and inherent safety of aqueous electrolytes, are considered strong contenders for next-generation large-scale energy storage technology. Among various aqueous zinc-ion battery systems, aqueous zinc-iodine batteries, relying on the unique advantages of high theoretical capacity and low cost of iodine cathodes, further enhance their energy storage application value and possess broad industrialization prospects.

[0003] However, the combined effect of the polyiodide shuttle effect and the side reactions at the zinc anode leads to rapid capacity decay and short cycle life in aqueous zinc-iodine batteries, severely hindering their industrialization. Specifically, aqueous zinc-iodine batteries use an aqueous electrolyte as the ion transport medium. During charging and discharging, the reversible oxidation-reduction of the iodine cathode generates highly water-soluble I3. - I5 - Polyiodine anions are present. These anions readily diffuse through the electrolyte, penetrate the separator, and migrate to the zinc anode, where they undergo irreversible side reactions with metallic zinc. This leads to the loss of active material from the positive electrode, capacity decay, and continuous corrosion of the zinc anode, reducing the battery's coulombic efficiency. Furthermore, aqueous electrolytes contain a large amount of free active water. Metallic zinc exhibits poor thermodynamic stability in aqueous systems, making it prone to hydrogen evolution during charging. This generates insulating passivation products such as Zn(OH)2 and ZnO, which accumulate on the zinc anode surface, disrupting the interfacial structure. Due to the uneven microstructure of the zinc anode, localized electric field concentration and a sharp-point effect easily occur on its surface, leading to localized enrichment and disordered deposition of zinc ions, forming zinc dendrites. These side reactions accumulate and intensify over long cycles, causing continuous degradation of battery performance and rapid decline in cycle life. In severe cases, they can even lead to safety hazards such as separator puncture and battery short circuits.

[0004] To address this, existing technologies typically employ methods such as electrolyte additive modification, membrane modification, and the construction of solid-state electrolytes to attempt to weaken free water activity and block polyiodide ion migration, thereby improving the cycle stability of aqueous zinc-iodine batteries. Among these approaches, solid-state electrolytes, which can simultaneously suppress polyiodide shuttle and zinc anode side reactions, are considered the most promising direction for improvement.

[0005] Currently, the mainstream approach for solid-state electrolytes is a polymer-based composite system. This typically uses polymers such as polyethylene oxide, polyvinylidene fluoride, and polyacrylonitrile as the matrix for film formation, combined with inorganic ion-conducting fillers. The polymer's film-forming properties provide mechanical support, while the inorganic fillers improve ion transport capacity and optimize the system structure. However, the polymer matrix itself has low ionic conductivity, which is the main source of resistance to ion transport in this type of system. In aqueous circulation environments, polymer segments are prone to swelling and degradation, leading to a loose electrolyte structure, deteriorated electrode interface contact, and insufficient long-term service stability. Furthermore, the inorganic fillers and polymer matrix are heterogeneous composite structures, with a significant ion transport barrier at the interface, further restricting the rapid conduction of zinc ions. These interconnected problems make it difficult for existing polymer-based solid-state electrolytes to simultaneously meet the requirements of high ion conductivity and long-term cycling stability.

[0006] This application is submitted to address the above issues. Summary of the Invention

[0007] To address the problems of rapid capacity decay and short cycle life caused by the superposition of polyiodide shuttle effect and zinc anode side reaction in existing aqueous zinc-iodine batteries, and the technical defects of existing polymer-based composite solid electrolytes that are difficult to balance high ionic conductivity and long cycle stability due to the low ionic conductivity of the polymer matrix, easy swelling and degradation, and large ion transport barrier at heterogeneous interfaces, this invention provides a binder-free all-solid electrolyte based on phlogopite layered structure and its preparation method.

[0008] This invention utilizes the two-dimensional layered framework structure of natural phlogopite. By adding phlogopite powder to a zinc salt electrolyte and stirring, Zn... 2+ Zn is constructed by loading active sites onto the interlayer domains and / or surface of the framework of phlogopite. 2+ Continuous transport channels; utilizing the electrostatic adsorption of polyiodine anions by the Mg-O polar bonds exposed on the surface of the phlogopite framework layer, the polyiodine shuttle effect is effectively suppressed; through the drying treatment in step (1), the free active water molecules inside the powder are fully removed, significantly suppressing the hydrogen evolution side reaction of the zinc anode; at the same time, the two-dimensional interlayer channels of phlogopite can transfer Zn 2+ The migration path is constrained in multiple parallel channels, which makes the ion flux reaching the negative electrode interface uniformly distributed, avoiding local accumulation and tip deposition, thereby inhibiting the growth of zinc dendrites; in addition, by making full use of the overlapping and interlocking characteristics of natural phlogopite flakes, self-supporting electrolyte sheets can be obtained by high pressure pressing without adding any binder.

[0009] The technical solution adopted in this invention is:

[0010] This invention provides a method for preparing a binderless all-solid electrolyte based on the layered structure of phlogopite, comprising the following steps: (1) adding phlogopite powder to a zinc salt electrolyte, stirring, centrifuging, discarding the supernatant, collecting the precipitate, washing, and drying to obtain zinc-loaded phlogopite inorganic powder; (2) grinding the zinc-loaded phlogopite inorganic powder obtained in step (1), and pressing it directly into shape without adding any binder to obtain phlogopite-based all-solid electrolyte sheets.

[0011] Preferably, in step (1), the mass-to-volume ratio of the phlogopite powder to the zinc salt electrolyte is (1-4):(5-20), the concentration of the zinc salt electrolyte is 1-3 mol / L, the stirring time is 6-48 h, the number of washing cycles after centrifugation is 3-6, the drying temperature is 60-100℃, and the drying time is 6-12 h.

[0012] Preferably, in step (1), the zinc salt electrolyte is an aqueous solution of zinc sulfate, zinc acetate, zinc nitrate or zinc chloride.

[0013] Preferably, in step (2), the unidirectional pressure per unit area of ​​the pressing molding is 10-30 MPa, the holding time is 1-5 min, and the pressing molding is unidirectional pressing.

[0014] Preferably, the phlogopite powder is natural phlogopite mineral powder.

[0015] Preferably, in step (2), the grinding is done by dry grinding, and the particle size of the zinc-loaded phlogopite powder after grinding is 200-800 mesh.

[0016] The second aspect of the present invention provides a phlogopite-based all-solid-state electrolyte prepared by the preparation method provided in the first aspect, having a thickness of 0.1 to 0.5 mm.

[0017] Preferably, the phlogopite-based all-solid electrolyte is a self-supporting sheet that does not contain any organic binders, inorganic binders, or polymer matrix.

[0018] A third aspect of the present invention provides an aqueous zinc-iodine battery comprising the phlogopite-based all-solid-state electrolyte described in the second aspect.

[0019] The fourth aspect of this invention provides the application of the phlogopite-based all-solid-state electrolyte described in the second aspect in an aqueous zinc-iodine energy storage battery or an aqueous zinc-ion energy storage battery.

[0020] It should be noted that the "all-solid electrolyte" mentioned in this invention refers to a self-supporting sheet body obtained by pressing the zinc-loaded phlogopite inorganic powder obtained in step (1) into shape in step (2). This sheet does not contain any organic binder, inorganic binder, polymer matrix, or free water. During battery assembly, a trace amount of zinc salt interfacial wetting liquid can be introduced onto the surface of this sheet to improve interfacial contact. The amount of this interfacial wetting liquid does not exceed 5% of the mass of the electrolyte sheet and is only used to improve interfacial contact. It does not form a continuous liquid ion conduction pathway, and ion conduction is mainly carried out by the interlayer channels of phlogopite. Therefore, the battery containing this sheet can be understood as a quasi-solid / hybrid solid-state aqueous zinc-iodine battery with a phlogopite-based all-solid electrolyte sheet as the main body and the interface modified by a trace amount of wetting liquid.

[0021] The beneficial effects of this invention are:

[0022] 1. Phlogopite has a natural two-dimensional layered framework, consisting of negatively charged silicate layers and interlayer cations (mainly K). + Phlogopite is formed by electrostatic stacking, with cation sites between layers and active sites on the surface of the framework layer and in the interlayer domains. This invention utilizes the interlayer confinement and surface activity characteristics of phlogopite to place phlogopite powder in a zinc salt electrolyte and stir, allowing the Zn in the solution to... 2+ The active sites on the interlayer domains and / or framework surface of phlogopite are loaded, a process that does not disrupt the original layered framework structure of the mica. After treatment, Zn is formed in the interlayer domains and on the framework surface. 2+ The enrichment environment provides a basis for subsequent Zn enrichment. 2+ The migration provides a continuous coordination environment. Subsequent Zn... 2+ When traversing interlayer channels, Zn can utilize this coordination environment for orderly migration, significantly reducing migration resistance and thus transforming the interlayer gaps into a favorable environment for Zn migration. 2+ Continuous conduction migration channels. Simultaneously, the two-dimensional parallel layered structure of mica affects Zn. 2+ The migration of Zn has spatial confinement and guiding effects, making Zn 2+ The ordered and directional migration along the interlayer, unlike the free and disordered diffusion of ions in liquid electrolytes, further reduces migration resistance and realizes Zn 2+ Efficient conduction in solid electrolytes is beneficial for improving battery rate performance.

[0023] 2. The surface of the phlogopite framework layer exposes Mg-O polar bonds. The electronegativity difference between Mg and O is significant, and these polar bonds are strongly associated with polyiodide anions (I3). - I5 -It exhibits electrostatic adsorption. When soluble polyiodide anions are generated at the iodine cathode during charging and discharging, these polyiodide ions are adsorbed by Mg-O polar bonds on the surface of the phlogopite cathode as they pass through the electrolyte from the cathode side, thus reducing their migration towards the zinc anode. Simultaneously, the confined space of the interlayer channels in the phlogopite forms a physical barrier against polyiodide ions that fail to be adsorbed on the surface. The size of the interlayer channels preferentially allows Zn... 2+ Smaller ions can pass through, while larger species such as polyiodide ions are difficult to enter due to steric hindrance and are blocked outside the interlayer channels. The synergistic effect of surface adsorption and interlayer size exclusion effectively reduces the migration of polyiodide ions to the zinc anode, which not only avoids capacity decay caused by the loss of iodine active material from the positive electrode side, but also blocks the corrosion reaction that occurs after polyiodide ions come into contact with metallic zinc, thereby significantly extending the cycle life of the battery.

[0024] 3. In the preparation process of this invention, a drying treatment is performed to fully remove free water from the zinc-loaded phlogopite powder, resulting in a phlogopite-based all-solid-state electrolyte sheet that itself contains no free water. During battery assembly, only a trace amount of zinc salt electrolyte is introduced onto the surface of the electrolyte sheet to improve interfacial contact. This interfacial wetting solution does not bear the main responsibility for ion conduction; ion conduction is mainly carried out by the interlayer channels of the phlogopite. Due to the extremely low amount of electrolyte used, the total amount of free active water in the system is still significantly suppressed. The direct cause of the hydrogen evolution side reaction at the zinc anode is the electrochemical reduction reaction that occurs after free water molecules come into contact with metallic zinc. When the free water content in the system is extremely low, this reaction is significantly suppressed due to the lack of sufficient reactants, thereby significantly reducing the accumulation of insulating passivation products such as Zn(OH)2 and ZnO on the zinc anode surface and the interface degradation.

[0025] Meanwhile, the interlayer channels of phlogopite will connect Zn 2+ The migration path is constrained in a two-dimensional layered space, making Zn 2+ As it traverses the electrolyte layer, it migrates orderly along the interlayer, resulting in a more uniform ion flux distribution at the negative electrode interface. This differs from Zn in liquid electrolytes. 2+ The transport mechanism, which allows for free three-dimensional diffusion and easy local enrichment at the tip, along with the ordered constraint of interlayer channels, prevents local accumulation of ions on the negative electrode surface, thereby effectively suppressing the deposition and growth of zinc dendrites at the tips. The significant suppression of hydrogen evolution side reaction ensures the chemical stability of the negative electrode interface, while the suppression of dendrite growth ensures the structural integrity of the negative electrode interface. Together, these factors improve the cycle life and safety of the battery.

[0026] 4. This invention uses natural phlogopite as raw material, which is abundant, widely distributed, and inexpensive to mine in my country. Neither the raw material nor the preparation process involves toxic or harmful substances, meeting green and environmentally friendly requirements. Furthermore, phlogopite itself possesses excellent thermal stability (long-term operating temperature can reach over 700℃) and intrinsic electrical insulation, enabling it to maintain structural stability under battery charging and discharging temperature rise conditions. It also effectively isolates the positive and negative electrodes, preventing internal short circuits and further enhancing battery safety. Attached Figure Description

[0027] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0028] Figure 1 X-ray diffraction (XRD) patterns of phlogopite raw material and zinc-loaded phlogopite provided in the embodiments of the present invention;

[0029] Figure 2 A scanning electron microscope (SEM) cross-sectional image of a phlogopite-based all-solid-state electrolyte sheet provided in an embodiment of the present invention;

[0030] Figure 3 A comparison of the cycling performance of zinc-iodine full cells assembled with phlogopite-based all-solid electrolyte and comparative liquid electrolyte at a current density of 1 A / g, as provided in this embodiment of the invention.

[0031] Figure 4 The Zn||Zn symmetric cell assembled with the phlogopite-based all-solid-state electrolyte and the comparative liquid electrolyte provided in this embodiment of the invention operates at 0.5 mA / cm². 2 XRD comparison images of zinc anode after 50 cycles under the specified conditions;

[0032] Figure 5 The Zn||Zn symmetric cell assembled with the phlogopite-based all-solid-state electrolyte and the comparative liquid electrolyte provided in this embodiment of the invention operates at 0.5 mA / cm². 2 SEM comparison images of the zinc anode after 50 cycles under the specified conditions;

[0033] Figure 6 The image shows the UV-Vis absorption spectrum of test example 5. Detailed Implementation

[0034] The present invention will be further described in detail below with reference to embodiments, but this is not intended to limit the invention. Any modifications or improvements made based on the teachings of the present invention fall within the protection scope of the present invention. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in the art or in accordance with the product manual.

[0035] Example 1

[0036] This embodiment provides a method for preparing a binder-free all-solid-state electrolyte based on a layered structure of phlogopite mica, including the following steps:

[0037] (1) Commercially available phlogopite powder (purchased from Aladdin, purity ≥98%, particle size 200 mesh) was added to a 3 mol / L zinc sulfate aqueous solution at a mass-to-volume ratio of 1:5. The solution was stirred at room temperature for 24 h to allow the Zn concentration in the solution to rise. 2+ The zinc-loaded phlogopite was loaded onto the interlayer domains and / or surface active sites of the framework. After the reaction, the suspension was centrifuged (8000 rpm, 10 min), the supernatant was discarded, and the precipitate was collected. The precipitate was washed three times with deionized water to remove unbound free zinc salts from the powder surface. The washed precipitate was then dried in a 60℃ oven for 12 h to obtain zinc-loaded phlogopite inorganic powder.

[0038] (2) Grind the zinc-loaded phlogopite inorganic powder obtained in step (1) thoroughly in a mortar until it becomes fine powder, and pass it through a 200-mesh sieve. Weigh 0.1 g of the ground powder, spread it evenly in a stainless steel mold with a diameter of 13 mm, and press it under a unit area pressure of 20 MPa for 2 min using a tablet press. After demolding, a phlogopite-based all-solid electrolyte sheet with a thickness of about 0.3 mm is obtained.

[0039] The obtained zinc-loaded phlogopite inorganic powder was characterized by X-ray diffraction (XRD), and the results are as follows: Figure 1 As shown. Compared with the raw phlogopite, the (001) characteristic peak position of zinc-loaded phlogopite did not shift significantly, and the diffraction peaks did not show obvious broadening or new phase diffraction peaks, indicating that the zinc salt treatment process did not destroy the layered framework structure of phlogopite.

[0040] Example 2

[0041] The only difference between this embodiment and Example 1 is that in step (1), the zinc salt electrolyte is an aqueous solution of zinc acetate with a concentration of 2 mol / L, the mass-to-volume ratio of phlogopite powder to the aqueous solution of zinc acetate is 2:10, the stirring time is 48 h, the drying temperature is 80℃, and the drying time is 8 h. In step (2), the pressing pressure is 15 MPa, and the holding time is 3 min. The remaining steps are the same as in Example 1.

[0042] Example 3

[0043] The only difference between this embodiment and Embodiment 1 is that in step (1), the zinc salt electrolyte is an aqueous solution of zinc nitrate with a concentration of 1 mol / L, the mass-to-volume ratio of phlogopite powder to the aqueous solution of zinc nitrate is 4:20, the stirring time is 6 h, the washing is performed 6 times, the drying temperature is 100℃, and the drying time is 6 h. In step (2), the grinding is performed using dry ball milling, the particle size of the zinc-loaded phlogopite powder after grinding is 400 mesh, the pressing pressure is 30 MPa, and the holding time is 1 min. The remaining steps are the same as in Embodiment 1.

[0044] Comparative Example 1

[0045] This comparative example provides a liquid electrolyte for comparison, which is composed of zinc sulfate dissolved in deionized water to prepare a zinc sulfate aqueous solution with a concentration of 3 mol / L.

[0046] Test Example 1

[0047] The phlogopite-based all-solid-state electrolyte prepared in Example 1 and the 3 mol / L zinc sulfate liquid electrolyte of Comparative Example 1 were respectively assembled into zinc-iodine full cells. The specific assembly method was as follows: zinc foil was used as the negative electrode, iodine-loaded activated carbon (AC@I2) was used as the positive electrode, and the phlogopite-based all-solid-state electrolyte sheet served as both the separator and the electrolyte (for the liquid system, a glass fiber separator was used and liquid electrolyte was added) to assemble a coin cell.

[0048] A constant current charge-discharge cycle test was performed at a current density of 1 A / g, and the results are as follows: Figure 3 As shown, the battery using the liquid electrolyte in Comparative Example 1 exhibits rapid capacity decay in the early stages of cycling, while the battery using the mica-based all-solid-state electrolyte in Example 1 maintains stable capacity during cycling, demonstrating excellent cycle stability.

[0049] Test Example 2

[0050] The phlogopite-based all-solid-state electrolyte prepared in Example 1 and the 3 mol / L zinc sulfate liquid electrolyte of Comparative Example 1 were used to assemble Zn||Zn symmetric cells. The cells were tested at a current density of 0.5 mA / cm². 2 Surface capacity 0.5 mAh / cm 2 After cycling for 50 cycles under the specified conditions, the battery was disassembled, the zinc sheet was removed, and the surface was gently rinsed with anhydrous ethanol for XRD phase analysis and SEM morphology observation.

[0051] XRD results are as follows Figure 4As shown, obvious characteristic peaks of byproducts such as ZnO and Zn(OH)2 appeared on the surface of the zinc sheet using the liquid electrolyte of Comparative Example 1, while only the characteristic peak of metallic zinc was detected on the surface of the zinc sheet using the phlogopite-based all-solid electrolyte of Example 1, and the byproduct peaks were extremely weak. This indicates that the phlogopite-based all-solid electrolyte effectively suppressed the hydrogen evolution side reaction of the zinc anode.

[0052] SEM results are as follows Figure 5 As shown, the zinc sheet using the liquid electrolyte of Comparative Example 1 exhibits numerous dendritic protrusions and cracks on its surface, resulting in a loose and uneven deposition layer. In contrast, the zinc sheet using the phlogopite-based all-solid electrolyte of Example 1 has a dense and smooth deposition layer with no obvious dendrites, indicating that the interlayer channels of phlogopite are crucial for the deposition of Zn. 2+ The migration of these elements has a spatial confinement and guiding effect, effectively inhibiting the growth of zinc dendrites.

[0053] Test Example 3

[0054] The phlogopite-based all-solid-state electrolyte sheet prepared in Example 1 was sandwiched between two stainless steel blocking electrodes and subjected to electrochemical impedance spectroscopy (EIS) testing. The frequency range was 1 MHz to 0.01 Hz, the amplitude was 5 mV, and the testing temperature was room temperature (25°C). Before testing, the electrolyte sheet was dried in a vacuum oven at 60°C for 6 h to completely remove surface adsorbed water. The diameter of the stainless steel blocking electrodes was 10 mm, and the diameter of the electrolyte sheet was 13 mm, ensuring that the electrodes completely covered the effective area of ​​the electrolyte. The ionic conductivity was calculated according to the formula σ = L / (R × S), where L is the electrolyte thickness (L = 0.30 mm in this test), R is the bulk resistance (taken as the intersection of the semicircle in the high-frequency region of the Nyquist plot and the real axis), and S is the electrode area (S = 0.785 cm²). 2 ).

[0055] The results show that the room-temperature ionic conductivity of the phlogopite-based all-solid-state electrolyte is 10.75 mS / cm. For comparison, the room-temperature ionic conductivity of the mullite-based solid-state electrolyte reported in previous literature (Adv. Mater. 2024, 36, 2408213) is 7.8 mS / cm. -1 The ionic conductivity of the phlogopite-based all-solid-state electrolyte is higher than that of the mullite-based solid-state electrolyte, indicating that the two-dimensional layered structure of phlogopite is favorable for Zn production. 2+ The conduction.

[0056] Test Example 4

[0057] The phlogopite-based all-solid-state electrolyte prepared in Example 1 was used to assemble a zinc-iodine full cell. Zinc foil was used as the negative electrode and iodine-loaded activated carbon (AC@I2) was used as the positive electrode. Constant current charge-discharge cycle test was conducted at a current density of 1 A / g and the test temperature was room temperature (25°C).

[0058] The results show that the battery assembled with phlogopite-based all-solid-state electrolyte exhibits excellent capacity retention during cycling, with a capacity retention of 55.5% after 10,700 cycles.

[0059] Test Example 5

[0060] To investigate the adsorption capacity of zinc-loaded phlogopite for polyiodide anions, the zinc-loaded phlogopite powder prepared in Example 1 was added to a solution containing I3⁻ for adsorption experiments.

[0061] Preparation of the test solution: Dissolve potassium iodide and elemental iodine in deionized water at a molar ratio of 2:1, stir in the dark until completely dissolved, and bring to a final volume to obtain I3. - The test solution has a concentration of 10 mmol / L.

[0062] Adsorption experiment: Take 100 mL of the above I3 - The solution was mixed with 400 mg of zinc-loaded phlogopite powder and magnetically stirred at room temperature in the dark for 6 h. After stirring, the suspension was centrifuged (8000 rpm for 10 min), and the supernatant was collected. The absorbance of the supernatant at 288 nm and 352 nm was measured using a UV-Vis spectrophotometer, and the absorbance of the original I3 without powder was also measured. - The absorbance of the solution at the same wavelength was used as a control.

[0063] The results showed that the absorbance of the supernatant after zinc-loaded phlogopite treatment was 0.791 and 0.529 at 288 nm and 352 nm, respectively, which was lower than that of the original I3. - The absorbance of the solution decreased significantly at 1.609 and 1.033. Based on the absorbance changes, the zinc-loaded phlogopite was calculated to have a significant effect on I3. - The adsorption capacity is approximately 46.63 mg / g.

[0064] The above results indicate that zinc-loaded phlogopite has an adsorption effect on polyiodide anions, which is consistent with the electrostatic adsorption effect of Mg-O polar bonds on the surface of the phlogopite framework layer.

[0065] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of this application and are not intended to limit it. Although this application has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made to it in form and detail without departing from the scope defined by the claims of this application; the dimensions described in the drawings and embodiments are not related to the specific physical object and are not used to limit the protection scope of this application. The physical dimensions can be selected and changed according to actual needs.

Claims

1. A method for preparing a binder-free all-solid-state electrolyte based on a layered structure of phlogopite, characterized in that, Includes the following steps: (1) Add phlogopite powder to zinc salt electrolyte, stir, centrifuge, discard the supernatant, collect the precipitate, wash and dry to obtain zinc-loaded phlogopite inorganic powder; (2) Grind the zinc-loaded phlogopite inorganic powder obtained in step (1), and press it directly into shape without adding any binder to obtain phlogopite-based all-solid electrolyte sheet.

2. The preparation method according to claim 1, characterized in that, In step (1), the mass-to-volume ratio of the phlogopite powder to the zinc salt electrolyte is (1-4):(5-20), the concentration of the zinc salt electrolyte is 1-3 mol / L, the stirring time is 6-48 h, the number of washing cycles after centrifugation is 3-6, the drying temperature is 60-100℃, and the drying time is 6-12 h.

3. The preparation method according to claim 1, characterized in that, In step (1), the zinc salt electrolyte is an aqueous solution of zinc sulfate, zinc acetate, zinc nitrate or zinc chloride.

4. The preparation method according to claim 1, characterized in that, In step (2), the unit area pressure of the pressing molding is 10-30 MPa, the holding time is 1-5 min, and the pressing molding is unidirectional pressing.

5. The preparation method according to any one of claims 1 to 4, characterized in that, The phlogopite powder is a natural phlogopite mineral powder.

6. The preparation method according to any one of claims 1 to 4, characterized in that, In step (2), the grinding is done by dry grinding, and the particle size of the zinc-loaded phlogopite powder after grinding is 200-800 mesh.

7. A phlogopite-based all-solid-state electrolyte prepared by any one of claims 1 to 4, having a thickness of 0.1 to 0.5 mm.

8. The phlogopite-based all-solid-state electrolyte according to claim 7, characterized in that, The phlogopite-based all-solid electrolyte is a self-supporting sheet that contains no organic binders, inorganic binders, or polymer matrix.

9. An aqueous zinc-iodine battery comprising the phlogopite-based all-solid-state electrolyte as described in claim 7 or 8.

10. The application of the phlogopite-based all-solid-state electrolyte according to claim 7 or 8 in an aqueous zinc-iodine energy storage battery or an aqueous zinc-ion energy storage battery.