A soft-pack lithium-ion battery and its formation method
By combining segmented constant current charging with electrolyte additives, the problems of uneven CEI film deposition and Mn2+ dissolution in lithium-ion battery formation are solved, achieving high-efficiency interface stability and long cycle performance, which is suitable for pouch lithium-ion batteries.
Patent Information
- Application Number
- CN202611307383.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium-ion battery formation processes cannot adapt to the differentiated film formation potential windows of dual-phase cathode systems, resulting in the inability to independently control the deposition timing, thickness, and density of CEI films. This leads to high interface impedance dispersion, poor batch consistency, ineffective suppression of Mn2+ dissolution, high gas bag defect rate, and poor stability of composite cathode structures.
A segmented constant current charging formation method is adopted, in which the current is gradually increased from 0.02C to 0.2C, and the voltage is kept constant at 3.92V±0.02V during the segmented formation period. Combined with LiPO2F2 and ethylene sulfate additives, a composite CEI protective layer is formed. The electrolyte film formation process is optimized by combining segmented negative pressure-normal pressure alternating venting and stepped temperature and pressure aging process.
It enables independent molding and densification of CEI membranes, inhibits Mn2+ dissolution, reduces interfacial impedance dispersion, improves batch consistency, reduces gas bag defect rate, and enhances first coulombic efficiency and cycle life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This application belongs to the field of lithium-ion battery manufacturing technology, specifically relating to a soft-pack lithium-ion battery and its formation method. Background Technology
[0002] The formation and aging processes are the core links in the lithium-ion battery production process. They determine the initial quality of the negative electrode solid electrolyte interphase (SEI) and positive electrode electrolyte interphase (CEI), which in turn affects a series of key performance indicators such as initial coulombic efficiency, cycle life, internal resistance evolution, and gas expansion risk.
[0003] Existing lithium-ion battery formation and aging processes primarily target single-phase cathode systems (such as pure NCM or pure LFP / LMFP systems). When applied to LMFP@NCM622 composite cathode systems, they generally suffer from the following drawbacks: A single constant-current formation mode cannot adapt to the differentiated film formation potential windows of the two phases. Current mainstream formation processes often employ a fixed small current (typically 0.05-0.1C) to complete the entire charging process from open-circuit voltage to full-charge cutoff voltage in one pass, or use a crude two-stage current switching. These processes do not consider the significant misalignment in film formation potential between LMFP and NCM622—the main formation potential range of the CEI film on the NCM622 side is concentrated between 3.55-3.85V, while the main formation potential range of the CEI film on the LMFP side is concentrated between 3.88-4.02V. Using a single or coarse current through these two windows will prevent independent control of the deposition timing, thickness, and density of the two-phase CEI film, ultimately resulting in high interfacial impedance dispersion, poor batch consistency, and wide DCR distribution. Furthermore, the entire low-current formation process typically takes over 20 hours, creating a significant bottleneck in production capacity. There is a lack of specific Mn... 2+ Active inhibition mechanism of dissolution: In the composite cathode system, the LMFP phase will exhibit Mn dissolution after the charging potential exceeds approximately 3.95V. 2+ The sharp increase in dissolution rate, the dissolved Mn 2+ It can migrate through the diaphragm to the negative electrode side, disrupting the forming SEI membrane structure, leading to continuous SEI reconstruction, reduced coulombic efficiency, and significantly decreased cycle life during subsequent cycles. The formation process and electrolyte additive formulation are disconnected: existing formation processes and electrolyte formulations are usually designed independently, without optimizing the process and formulation for the decomposition and film-forming characteristics of specific additives at specific potentials, thus failing to fully release the role of additives in the formation of biphase CEI membranes. Furthermore, existing degassing processes mainly employ either full-process negative pressure formation or a single-stage vacuum degassing after formation, which cannot accurately match the misalignment rhythm of the gas generation peaks in the NCM622 and LMFP two-phase composite systems, resulting in a high defect rate for gas bags. Moreover, existing aging processes generally adopt a constant temperature and pressure static setting mode, lacking process integration and coordinated design with the dynamic electrochemical processes of the formation stage. Particularly for composite cathode systems, the SEI / CEI film remains metastable after formation, requiring densification reconstruction and interface impedance homogenization within a specific temperature-pressure window. A single constant temperature and pressure mode cannot activate film reconstruction or homogenize the two-phase interface impedance, which is detrimental to the structural stability of the composite cathode. Summary of the Invention
[0004] This application provides a soft-pack lithium-ion battery and its formation method, aiming to solve the problems of existing lithium-ion battery formation methods where the single constant current formation mode cannot adapt to the potential window of the two-phase differential formation film, resulting in the inability to independently control the deposition timing, thickness, and density of the two-phase CEI film, ultimately leading to high interface impedance dispersion, poor batch consistency, and wide DCR distribution; and lacking a method for Mn 2+ The active inhibition mechanism for dissolution addresses issues such as high gas bag defect rate and poor stability of composite cathode structure.
[0005] The first aspect of this application provides a method for forming a soft-pack lithium-ion battery, comprising the following steps: (1) Injecting electrolyte into a soft-pack lithium-ion battery and sealing it; the electrolyte includes the following raw materials: LiPO2F2, vinyl sulfate (DTD), fluoroethylene carbonate (FEC), vinylene carbonate (VC), LiPF6 and solvent; (2) The soft-pack lithium-ion battery is charged and formed in segments with a current gradually increasing from 0.02C to 0.2C. During the segmented formation, when the voltage is charged to 3.92V±0.02V, the constant voltage charging is maintained until the current decays to 0.01-0.02C, and then the next stage of charging and formation is carried out. (3) Perform first discharge and second charge activation treatment on the lithium-ion battery obtained in step (2); (4) The lithium-ion battery obtained in step (3) is subjected to aging treatment.
[0006] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the electrolyte comprises the following raw materials in parts by weight: 0.5-1.5 parts LiPO2F2, 0.3-0.8 parts vinyl sulfate, 3-5 parts fluoroethylene carbonate, 1-2 parts vinylene carbonate, 12-14 parts LiPF6, and 76-82 parts solvent.
[0007] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the mass ratio of LiPO2F2 to ethylene sulfate in the electrolyte is (1.5-2.5):1.
[0008] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the solvent includes one or more of ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate.
[0009] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, in step (2), the segmented constant current charging formation includes the initial nucleation SEI stage of the negative electrode, the CEI film deposition stage on the NCM side, the pre-deposition stage of the protective CEI layer on the LMFP side, the CEI film deposition completion stage on the LMFP side, the overall shaping of the CEI film on the positive electrode side, and the first full charge stage of the battery.
[0010] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the constant current charging current of the initial nucleation SEI stage of the negative electrode is 0.02C-0.03C, and the voltage range corresponding to the constant current charging is from the open circuit voltage to 3.55V. The constant current charging current during the NCM-side CEI film deposition stage is 0.04C-0.06C, and the corresponding voltage range for constant current charging is 3.55V to 3.85V; preferably, a first venting process is performed during this stage, and the first venting process takes 12-20 minutes. During the deposition of the protective CEI layer on the LMFP side, the constant current charging current is 0.04C-0.06C, and the voltage range corresponding to the constant current charging is 3.85V to 3.92V±0.02V; when the voltage reaches 3.92V±0.02V, the constant voltage charging is maintained until the current decays to 0.01-0.02C. The constant current charging current during the CEI film deposition completion stage on the LMFP side is 0.08C-0.12C, and the voltage range corresponding to the constant current charging is 3.92V-4.05V; preferably, a second venting process is performed at the end of this stage, more preferably, the venting negative pressure is -45 to -55kPa, and the time is 8-12min; The constant current charging current during the overall shaping of the CEI film on the positive electrode side and the first full charge stage of the battery is 0.15C-0.2C, and the voltage range corresponding to constant current charging is 4.05V to 4.25V; when the voltage reaches 4.25V, constant voltage charging is carried out until the current is ≤0.02C.
[0011] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, in step (3), the battery is first discharged until the voltage is 2.8V, and then the discharge is stopped; And / or, the secondary charge is activated to a voltage of 3.7V.
[0012] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, in step (4), the aging treatment includes an exhaust aging treatment stage, an interface reconstruction aging treatment stage, and a stabilization treatment stage.
[0013] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the temperature of the exhaust aging treatment stage is 20-30°C, the pressure is 0.03-0.08MPa, and the time is 20-26h; exhaust treatment is performed during the exhaust aging treatment stage.
[0014] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the pressure of the exhaust treatment is -90kPa to -100kPa, and the time is 3-8min.
[0015] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the temperature of the interface reconstruction aging treatment stage is 40-50℃, the pressure is 0.35-0.45MPa, and the charging voltage is 3.75V±0.02V. Under the above conditions, constant voltage charging is performed until the microcurrent decays to below 0.002C to complete the interface reconstruction aging treatment.
[0016] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the temperature of the stabilization treatment stage is 20-30°C, the pressure is 0.12-0.16 MPa, and the time is 20-26 h.
[0017] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the positive electrode of the soft-pack lithium-ion battery includes a composite system of lithium manganese iron phosphate (LMFP) and ternary material NCM.
[0018] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the ternary material NCM is selected from one or more of the NCM523, NCM622, NCM811, NCM9, and NCM613 systems.
[0019] According to some embodiments of the formation method of the soft-pack lithium-ion battery described in this application, the morphology of the ternary material NCM includes one or more of the following: single crystal, quasi-single crystal, and polycrystalline.
[0020] The second aspect of this application provides a pouch lithium-ion battery prepared by the formation method described in the first aspect of this application.
[0021] According to some embodiments of the pouch lithium-ion battery described in this application, the Mn in the SEI of the negative electrode of the pouch lithium-ion battery 2+ Deposition amount ≤25ppm; two-phase charge depth difference ΔSOC ≤5%; capacity retention ≥92% after 1000 cycles at 0.5C / 0.5C@25℃.
[0022] The beneficial effects of this application include: the formation method of the soft-pack lithium-ion battery described in this application uses segmented current formation to independently form the CEI film on the composite cathode system side within its optimal potential range, and uses a dual-additive electrolyte to avoid uneven CEI film thickness; and actively suppresses Mn through a constant voltage holding section at a specific potential. 2+ Dissolution protects the integrity of the negative electrode SEI film; a segmented negative pressure-normal pressure alternating venting strategy is designed to match the two-phase gas production rhythm and avoid gas bag risks; then, through a stepped temperature and pressure coupled aging process, the stable reconstruction of the CEI / SEI film and the homogenization of the interface impedance are completed in the later stage of formation, so that the soft-pack lithium-ion battery described in this application has high initial coulombic efficiency (≥90%), low interface impedance and small dispersion (DCR@50%SOC distribution CV≤5%), low gas bag defect rate (≤1%), and Mn 2+ It has advantages such as low deposition in the negative electrode SEI (≤25ppm), small difference in the two-phase charge depth ΔSOC (≤5%), long cycle life (capacity retention ≥92% after 1000 cycles at 0.5C / 0.5C@25℃), and excellent batch consistency. Detailed Implementation
[0023] The embodiments of the present invention are described in detail below. These embodiments are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention.
[0024] In this invention, the terms "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., refer to a specific feature, structure, material, or characteristic described in connection with that embodiment or example, which is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples. Moreover, without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification, as well as the features of different embodiments or examples.
[0025] This application provides a method for forming a soft-pack lithium-ion battery, including the following steps: (1) Injecting electrolyte into a soft-pack lithium-ion battery and sealing it; the electrolyte includes the following raw materials: LiPO2F2, vinyl sulfate, fluoroethylene carbonate, vinylene carbonate, LiPF6 and solvent; (2) The soft-pack lithium-ion battery is charged and formed in segments with a current gradually increasing from 0.02C to 0.2C. During the segmented formation, when the voltage is charged to 3.92V±0.02V, the constant voltage charging is maintained until the current decays to 0.01-0.02C, and then the next stage of charging and formation is carried out. (3) Perform first discharge and second charge activation treatment on the lithium-ion battery obtained in step (2); (4) The lithium-ion battery obtained in step (3) is subjected to aging treatment.
[0026] The formation method of the soft-pack lithium-ion battery described in this application introduces a constant voltage holding section within a potential window of 3.92V ± 0.02V during the first charge until the final current decays to 0.01-0.02C. At this time, LiPO2F2 in the electrolyte and vinyl sulfate (DTD) additive synergistically decompose to form a ternary composite CEI protective layer rich in Li3PO4 / LiF / Li2SO3, effectively suppressing Mn. 2+ Dissolution; after formation, during the battery aging process, unstable components such as ROCO2Li in the film layer are replaced by stable components such as Li2CO3 and LiF through microcurrent compensation for self-discharge, thereby achieving dynamic interface renewal; ultimately, the difference in charge depth between the two phases ΔSOC can be controlled within 5% (traditional processes are usually >12%), ensuring electrochemical stress balance and improved long-cycle performance.
[0027] In some embodiments of this application, the electrolyte comprises the following raw materials in parts by weight: 0.5-1.5 parts LiPO2F2, 0.3-0.8 parts vinyl sulfate, 3-5 parts fluoroethylene carbonate, 1-2 parts vinylene carbonate, 12-14 parts LiPF6, and 76-82 parts solvent.
[0028] In some embodiments of this application, the mass ratio of LiPO2F2 to vinyl sulfate in the electrolyte is (1.5-2.5):1. When the mass ratio of LiPO2F2 to DTD is controlled at (1.5-2.5):1, the two can co-decompose during the 3.92V constant voltage maintenance stage. The Li3PO4 / LiF generated from the decomposition of LiPO2F2 and the Li2SO3 generated from the decomposition of DTD are co-deposited on the surface of LMFP particles, forming a dense ternary composite CEI film with excellent ion conductivity. If the proportion of LiPO2F2 is too high (mass ratio > 2.5:1), the proportion of LiF in the CEI film is too high, the interfacial impedance increases, and the rate performance decreases; if the proportion of DTD is too high (mass ratio < 1.5:1), the excessive Li2SO3 component easily leads to a loose CEI film, Mn 2+ The dissolution inhibition effect is weakened, and the Mn in the negative electrode SEI is reduced. 2+ The amount of sediment has increased.
[0029] In some embodiments of this application, the solvent includes one or more of ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate. As a preferred embodiment, the solvent is composed of ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate in a volume ratio of 3:5:2.
[0030] In some embodiments of this application, step (2) of the segmented constant current charging formation includes the initial nucleation SEI stage on the negative electrode, the CEI film deposition stage on the NCM side, the pre-deposition stage of the protective CEI layer on the LMFP side, the completion stage of CEI film deposition on the LMFP side, the overall shaping of the CEI film on the positive electrode side, and the first full charge stage of the battery. Through segmented current and potential window control, the CEI film on the composite positive electrode system side is formed independently in its optimal potential range, and with the help of a dual-additive electrolyte, the problem of uneven CEI film thickness is avoided.
[0031] In some embodiments of this application, the constant current charging current during the initial nucleation SEI stage of the negative electrode is 0.02-0.03C, and the voltage range corresponding to the constant current charging is from the open circuit voltage to 3.55V; The constant current charging current during the NCM-side CEI film deposition stage is 0.04C-0.06C, and the corresponding voltage range for constant current charging is 3.55V to 3.85V. Preferably, the first venting process is performed during this stage. During venting, the vent valve of the formation cabinet is opened to vent at atmospheric pressure, forming the CEI film deposition on the NCM side of the composite cathode system (the main forming potential range of the CEI film on the NCM side is concentrated in 3.55-3.85V. This stage mainly involves the decomposition of VC and FEC to produce gas, and the gases such as CO2 and C2H4 produced by the decomposition of EC / DMC are discharged through atmospheric pressure venting).
[0032] During the deposition of the protective CEI layer on the LMFP side, the constant current charging current is 0.04C-0.06C, and the corresponding voltage range is 3.85V to 3.92V±0.02V. Once the voltage reaches 3.92V±0.02V, constant voltage charging is maintained until the current decays to 0.01-0.02C. During this constant voltage holding period, LiPO2F2 in the electrolyte continuously decomposes at 3.92V to generate Li3PO4 / LiF, and DTD continuously decomposes at 3.92V to generate Li2SO3. Both of these components together form a Li3PO4 / LiF / Li2SO3 ternary composite CEI protective layer on the LMFP surface through in-situ chemical deposition. Li3PO4 acts as a fast ion conductor layer to protect the Li... + Rapid transport; LiF acts as a high-mechanical-strength framework layer to suppress further electrolyte decomposition; Li2SO3 acts as a flexible buffer layer to alleviate volume strain during charging and discharging, thereby enabling Mn on the LMFP side... 2+ An effective protective layer is constructed before the dissolution threshold (3.95V) to prevent Mn from reaching the target level. 2+ Dissolution.
[0033] The constant current charging current during the LMFP side CEI film deposition completion stage is 0.08C-0.12C, and the corresponding voltage range for constant current charging is 3.92V-4.05V. Preferably, a second venting process is performed during this stage. More preferably, the venting negative pressure is -45 to -55kPa, and the time is 8-12min. The segmented negative pressure-normal pressure alternating venting strategy is designed to match the two-phase gas production rhythm and avoid the risk of gas bags.
[0034] The constant current charging current during the overall shaping of the CEI film on the positive electrode side and the first full charge stage of the battery is 0.15-0.2C, and the voltage range corresponding to constant current charging is 4.05V to 4.25V; when the voltage reaches 4.25V, constant voltage charging is carried out until the current is ≤0.02C.
[0035] In some embodiments of this application, in step (3), the battery is first discharged until the voltage is 2.8V, and then the discharge is stopped.
[0036] In some embodiments of this application, the secondary charging activation voltage is 3.7V.
[0037] In some embodiments of this application, step (4) includes an exhaust aging process, an interface reconstruction aging process, and a stabilization process. The stable reconstruction and interface impedance homogenization of the CEI / SEI film are completed in the later stages of formation through a stepped temperature-pressure coupled aging process.
[0038] In some embodiments of this application, the temperature of the exhaust aging treatment stage is 20-30°C, the pressure is 0.03-0.08MPa, such as 0.03MPa, 0.05MPa, 0.06MPa, 0.08MPa, etc., and the time is 20-26h; exhaust treatment is performed during the exhaust aging treatment stage.
[0039] In some embodiments of this application, the pressure of the exhaust treatment is -90kPa to -100kPa, such as -90kPa, -98kPa, -100kPa, etc., and the time is 3-8min; such as 3min, 5min, 6min, 8min, etc.
[0040] In some embodiments of this application, the temperature of the interface reconstruction aging process is 40-50℃, such as 40℃, 46℃, 50℃, etc., the pressure is 0.35-0.45MPa, such as 0.35MPa, 0.38MPa, 0.40MPa, 0.45MPa, etc., and the charging voltage is 3.75V±0.02V. Under the above conditions, constant voltage charging is performed until the microcurrent decays to below 0.002C, thus completing the interface reconstruction aging process. In the constant voltage maintenance state, a microcurrent is provided by a constant voltage power supply to compensate for self-discharge, and the microcurrent value is monitored in real time. This stage maintains constant voltage until the microcurrent decays to ≤0.002C (approximately 0.2% of the nominal capacity) and remains stable for more than 2 hours; this promotes the densification and reconstruction of the SEI / CEI film and homogenizes the interface impedance.
[0041] In some embodiments of this application, the stabilization treatment stage is carried out at a temperature of 20-30°C and a pressure of 0.12-0.16 MPa, such as 0.12 MPa, 0.13 MPa, 0.15 MPa, or 0.16 MPa, for a duration of 20-26 hours. This stage can complete the final stabilization of the membrane structure and mitigate aging stress.
[0042] In some embodiments of this application, the positive electrode of the soft-pack lithium-ion battery comprises a composite system of lithium manganese iron phosphate (LMFP) and ternary material NCM; preferably, the ternary material NCM is selected from one or more of NCM523, NCM622, NCM811, NCM9, and NCM613.
[0043] In some embodiments of this application, the morphology of the ternary material NCM includes one or more of the following: single crystal, quasi-single crystal, and polycrystalline.
[0044] This application also provides a soft-pack lithium-ion battery, which is prepared by the formation method described in the first aspect of this application.
[0045] In some embodiments of this application, the Mn in the SEI of the negative electrode of the pouch lithium-ion battery 2+ Deposition amount ≤25ppm; two-phase charge depth difference ΔSOC ≤5%; capacity retention ≥92% after 1000 cycles at 0.5C / 0.5C@25℃.
[0046] After aging is complete, the batteries are subjected to three 0.5C / 0.5C capacity grading cycles, and indicators such as discharge capacity, DC internal resistance (DCR@50%SOC) and open circuit voltage retention rate (OCV@72h) are measured. Unqualified batteries are rejected.
[0047] The technical solution of this application will be further described below with reference to specific embodiments.
[0048] Example 1 A method for forming a soft-pack lithium-ion battery includes the following steps: The nominal capacity of the soft-pack lithium-ion battery is 20Ah LMFP@NCM622 / / graphite soft-pack battery (positive electrode LMFP:NCM622=30:70, compaction density 3.27g / cm³). 3 ).
[0049] (1) Mix 1 part of LiPO2F2, 0.5 part of vinyl sulfate, 4 parts of fluoroethylene carbonate, 1.5 parts of vinylene carbonate, 13 parts of LiPF6 and 80 parts of solvent (a mixture of EC, EMC and DEC in a volume ratio of 3:5:2) to prepare an electrolyte (LiPO2F2:DTD mass ratio = 2:1); inject the electrolyte into a soft-pack lithium-ion battery and seal it, place it in a formation cabinet, and keep it at -85 kPa negative pressure and 25°C for 10 h; (2) The soft-pack lithium-ion battery is charged in segments with a gradually increasing current to form the battery. The specific operating steps are as follows: The above-mentioned soft-pack lithium-ion battery was charged from open-circuit voltage to 3.55V under a constant current of 0.02C, which took 3.2 hours; thus enabling the initial nucleation of the SEI film on the graphite anode. The voltage was charged from 3.55V to 3.85V by constant current charging at 0.05C. At the end of this charging stage, the exhaust valve of the formation cabinet was opened to exhaust at normal pressure for 15 minutes; the main body deposition of CEI film on the NCM622 side was completed. A constant current charge of 0.05C was applied to charge the voltage from 3.85V to 3.92V, followed by constant voltage maintenance for 87 minutes until the current decayed to 0.015C; this process was repeated on the LMFP surface using Mn. 2+ A protective CEI layer rich in LiF / Li3PO4 is pre-formed before the dissolution threshold (3.95V); in this constant voltage holding section, LiPO2F2 in the electrolyte continuously decomposes at 3.92V to generate Li3PO4 / LiF, and DTD continuously decomposes at 3.92V to generate Li2SO3. Together, they form a Li3PO4 / LiF / Li2SO3 ternary composite CEI protective layer on the LMFP surface. A constant current charge of 0.1C was applied to charge the voltage from 3.92V to 4.05V, completing the CEI film deposition on the LMFP side. At the end of this stage, a second negative pressure exhaust window was applied to exhaust the gas generated on the LMFP side under a negative pressure of -50kPa for 10 minutes. The voltage was charged from 4.05V to 4.25V using a constant current of 0.2C. Then, the voltage was kept constant until the current was 0.02C, which completed the overall shaping of the CEI film on the positive electrode side and the first full charge of the battery. The total formation time was about 22 hours.
[0050] (3) Discharge the lithium-ion battery obtained in step (2) to 3.5V at 0.05C, then discharge it to 2.8V at 0.1C; then charge it to 3.7V at 0.05C (corresponding to about 30% SOC) as the charge reference state before aging; (4) Aging treatment The specific operating steps are as follows: The lithium-ion battery obtained in step (3) was aged at 25°C and 0.05MPa for 24 hours; and the exhaust valve of the formation cabinet was opened to vacuum exhaust 12 hours after aging in this stage. The exhaust conditions were: -95kPa for 5 minutes and then resealed. Then, the battery was aged for 18 hours under constant voltage conditions of 45℃, 0.40MPa, and 3.75V. During this stage, the battery aging process was not an open-circuit resting process, but rather a constant voltage state of 3.75V. Micro-current was provided by the constant voltage power supply to compensate for self-discharge, and the micro-current value was monitored in real time. This constant voltage state was maintained until the micro-current decayed to ≤0.002C (approximately 0.2% of the nominal capacity) and remained stable for more than 2 hours (total 18 hours). Under constant voltage conditions, unstable components (ROCO2Li, Li2O, etc.) in the SEI / CEI film continued to dissolve and were replaced by stable components (Li2CO3, LiF, Li3PO4) under the drive of micro-current, achieving dynamic repair and densification of the film layer. At the same time, the two-phase charge depth was gradually equalized under voltage drive, ensuring electrochemical stress balance and improved long-cycle performance. Then, under the conditions of 25℃ and 0.15MPa, the film was aged for 24 hours to complete the final stabilization of the film structure and release the aging stress.
[0051] Example 2 The only difference between the formation method of the soft-pack lithium-ion battery in Example 2 and that in Example 1 is that the mass ratio of LiPO2F2 and ethylene sulfate in the injected electrolyte is different during the formation of the soft-pack lithium-ion battery in Example 2.
[0052] The specific operating steps include: (1) Mix 0.9 parts of LiPO2F2, 0.6 parts of vinyl sulfate, 4 parts of fluoroethylene carbonate, 1.5 parts of vinylene carbonate, 13 parts of LiPF6 and 80 parts of solvent (a mixture of EC, EMC and DEC in a volume ratio of 3:5:2) to prepare an electrolyte (LiPO2F2:DTD mass ratio = 1.5:1); inject the electrolyte into a soft-pack lithium-ion battery and seal it, place it in a formation cabinet, and keep it at -85 kPa negative pressure and 25°C for 10 h; The remaining operating steps are the same as in Example 1.
[0053] Example 3 The only difference between the formation method of the soft-pack lithium-ion battery in Example 3 and that in Example 1 is that the mass ratio of LiPO2F2 and ethylene sulfate in the injected electrolyte is different during the formation of the soft-pack lithium-ion battery in Example 3 compared to that in Example 1.
[0054] The specific operating steps include: (1) Mix 1.08 parts of LiPO2F2, 0.42 g of vinyl sulfate, 4 parts of fluoroethylene carbonate, 1.5 parts of vinylene carbonate, 13 parts of LiPF6 and 80 parts of solvent (a mixture of EC, EMC and DEC in a volume ratio of 3:5:2) to prepare an electrolyte (LiPO2F2:DTD mass ratio = 2.5:1); inject the electrolyte into a soft-pack lithium-ion battery and seal it, place it in a formation cabinet, and keep it at -85 kPa negative pressure and 25°C for 10 h; The remaining operating steps are the same as in Example 1.
[0055] Example 4 The only difference between the formation method of the soft-pack lithium-ion battery in Example 4 and that in Example 1 is that the mass ratio of LiPO2F2 and ethylene sulfate in the injected electrolyte is different during the formation of the soft-pack lithium-ion battery in Example 4 compared to that in Example 1.
[0056] The specific operating steps include: (1) Mix 1.2 parts of LiPO2F2, 0.3 parts of vinyl sulfate, 4 parts of fluoroethylene carbonate, 1.5 parts of vinylene carbonate, 13 parts of LiPF6 and 80 parts of solvent (a mixture of EC, EMC and DEC in a volume ratio of 3:5:2) to prepare an electrolyte (LiPO2F2:DTD mass ratio = 4:1); inject the electrolyte into a soft-pack lithium-ion battery and seal it, place it in a formation cabinet, and keep it at -85 kPa negative pressure and 25°C for 10 h; The remaining operating steps are the same as in Example 1.
[0057] Example 5 The only difference between the formation method of the soft-pack lithium-ion battery in Example 5 and that in Example 1 is that the soft-pack lithium-ion battery used in the formation method of the soft-pack lithium-ion battery in Example 5 is a 10Ah LMFP@NCM622 / / graphite soft-pack battery.
[0058] Example 6 The only difference between the formation method of the soft-pack lithium-ion battery in Example 6 and that in Example 1 is that the soft-pack lithium-ion battery used in the formation method of the soft-pack lithium-ion battery in Example 6 is a 30Ah LMFP@NCM622 / / graphite soft-pack battery.
[0059] Comparative Example 1 The only difference between the formation method of the soft-pack lithium-ion battery described in Comparative Example 1 and Example 1 is that, during the formation of the soft-pack lithium-ion battery described in Comparative Example 1, the gradually increasing current is used to perform segmented constant current charging on the soft-pack lithium-ion battery to form the protective CEI layer rich in LiF / Li3PO4 before the voltage is maintained at 3.92V. The other operation steps are the same as in Example 1.
[0060] Comparative Example 2 The only difference between the formation method of the soft-pack lithium-ion battery described in Comparative Example 2 and that in Example 1 is that the electrolyte injected during the formation of the soft-pack lithium-ion battery in Comparative Example 2 does not contain raw materials LiPO2F2 and DTD. The rest of the operation is the same as that in Example 1.
[0061] Comparative Example 3 The only difference between the formation method of the soft-pack lithium-ion battery described in Comparative Example 3 and Example 1 is that, during the formation of the soft-pack lithium-ion battery described in Comparative Example 3, no 3.75V voltage was applied during the aging process at 45°C, i.e., the battery was aged in an open-circuit static state.
[0062] Performance study of the pouch lithium-ion batteries described in Examples 1-6 and Comparative Examples 1-3 of this application Test method: (1) Initial Coulomb efficiency: After formation, charge to 4.25V at a rate of 0.1C (constant voltage to 0.02C), and then discharge to 2.8V at 0.1C. Calculate the ratio of the initial discharge capacity to the initial charge capacity.
[0063] (2) DCR@50%SOC: Adjust the battery to 50%SOC, let it stand for 1 hour, and then discharge it at 1C for 10 seconds. Record the voltage difference ΔV and current I before and after discharge. DCR=ΔV / I. Test 30 batteries in each group and calculate the mean and coefficient of variation CV.
[0064] (3) Gas bag defect rate: After the formation and aging are completed, visually inspect the appearance of 100 batteries in each group and count the percentage of batteries with bulging / gas bags caused by gas production.
[0065] (4) Mn in the negative electrode SEI 2+ Deposition amount: After the battery was cycled for 50 cycles, it was disassembled, the negative electrode sheet was cleaned with DMC 3 times and then vacuum dried, and the Mn content on the negative electrode surface was determined by ICP-MS.
[0066] (5) Two-phase charge depth difference ΔSOC: The battery was disassembled under full charge, and LMFP and NCM622 cathode powders were taken for XRD analysis. The actual amount of lithium delithiation between the two phases was calculated by the change of lattice parameters, and the charge depth difference ΔSOC = |SOC LMFP -SOC NCM622 |
[0067] (6) Cycle life: 1000 cycles at 25℃ with a 0.5C / 0.5C rate in the 2.8-4.25V range, and record the capacity retention rate.
[0068] The test results are shown in Table 1.
[0069] Table 1
[0070] As can be seen from Table 1: (1) A comparison of Examples 1-3 with Comparative Example 1 shows that introducing a constant voltage holding segment within a potential window of 3.92V ± 0.02V is effective in suppressing Mn. 2+ Key process steps for dissolution and construction of a high-quality CEI protective layer; in Comparative Example 1, where a constant voltage of 3.92V was not maintained, Mn 2+ The deposition rate was as high as 45 ppm (only 18 ppm in Example 1), and the capacity retention rate after 1000 cycles was only 86.2% (94.5% in Example 1).
[0071] (2) The comparison between Example 1 and Comparative Example 2 shows that the synergistic effect of LiPO2F2 and DTD dual additives on CEI membrane densification and Mn 2+ Inhibition is indispensable; without this dual additive, Mn 2+ The deposition rate increased to 68 ppm and the gas bag defect rate rose to 3.8%, indicating that the dual additive and formation process design are the core factors for the excellent performance of this application.
[0072] (3) The comparison between Example 1 and Comparative Example 3 shows that the stepped temperature and pressure aging process (especially the 45℃ / 3.75V constant voltage stage) has a significant effect on the densification of CEI / SEI film and the homogenization of two-phase charge depth; when this constant voltage aging step is missing, ΔSOC increases from 3.2% to 7.2%, and DCR dispersion CV increases from 3.2% to 9.1%.
[0073] (4) The performance of Examples 1-3 (LiPO2F2:DTD mass ratio in the range of 1.5-2.5:1) is better than that of Example 4 (mass ratio of 4:1 exceeds the preferred range), which verifies the rationality of the optimal mass ratio range of LiPO2F2 to DTD (1.5-2.5):1 proposed in this application.
[0074] (5) The comparison between Examples 5 and 6 and Example 1 shows that the formation method described in this application has good adaptability to soft-pack batteries with different capacity specifications of 10Ah-30Ah, and has excellent process universality and industrialization promotion value.
[0075] In summary, the formation method for the soft-pack lithium-ion battery described in this application improves the interface stability and Mn content of the LMFP@NCM composite cathode system soft-pack battery through a comprehensive process design that includes segmented constant current formation, dual-potential window partitioning for CEI film formation, dual-additive synergistic film formation, and segmented degassing and stepped temperature and pressure aging. 2+ Its suppression effect, charge balance, and long-cycle performance make it of significant value for industrial applications.
[0076] Although the above embodiments have been shown and described, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Any changes, modifications, substitutions and variations made to the above embodiments by those skilled in the art are within the protection scope of the present invention.
Claims
1. A method for forming a soft-pack lithium-ion battery, characterized in that, Includes the following steps: (1) Injecting electrolyte into a soft-pack lithium-ion battery and sealing it; the electrolyte includes the following raw materials: LiPO2F2, vinyl sulfate, fluoroethylene carbonate, vinylene carbonate, LiPF6 and solvent; (2) The soft-pack lithium-ion battery is charged and formed in segments with a current gradually increasing from 0.02C to 0.2C. During the segmented formation, when the voltage is charged to 3.92V±0.02V, the constant voltage charging is maintained until the current decays to 0.01-0.02C, and then the next stage of charging and formation is carried out. (3) Perform first discharge and second charge activation treatment on the lithium-ion battery obtained in step (2); (4) The lithium-ion battery obtained in step (3) is subjected to aging treatment.
2. The formation method of the soft-pack lithium-ion battery according to claim 1, characterized in that, The electrolyte comprises the following raw materials in parts by weight: 0.5-1.5 parts LiPO2F2, 0.3-0.8 parts vinyl sulfate, 3-5 parts fluoroethylene carbonate, 1-2 parts vinylene carbonate, 12-14 parts LiPF6, and 76-82 parts solvent. Preferably, the mass ratio of LiPO2F2 to vinyl sulfate in the electrolyte is (1.5-2.5):1; Preferably, the solvent includes one or more of ethylene carbonate, ethyl methyl carbonate, and diethyl carbonate.
3. The formation method of the soft-pack lithium-ion battery according to claim 1, characterized in that, In step (2), the segmented constant current charging formation includes the initial nucleation SEI stage of the negative electrode, the CEI film deposition stage on the NCM side, the pre-deposition stage of the protective CEI layer on the LMFP side, the completion stage of the CEI film deposition on the LMFP side, the overall shaping stage of the CEI film on the positive electrode side, and the first full charge stage of the battery.
4. The formation method of the soft-pack lithium-ion battery according to claim 3, characterized in that, The constant current charging current during the initial nucleation SEI stage of the negative electrode is 0.02C-0.03C, and the voltage range corresponding to the constant current charging is from the open circuit voltage to 3.55V. The constant current charging current during the NCM-side CEI film deposition stage is 0.04C-0.06C, and the corresponding voltage range for constant current charging is 3.55V to 3.85V; preferably, a first venting process is performed during this stage, and the first venting process takes 12-20 minutes. During the deposition of the protective CEI layer on the LMFP side, the constant current charging current is 0.04C-0.06C, and the voltage range corresponding to the constant current charging is 3.85V to 3.92V±0.02V; when the voltage reaches 3.92V±0.02V, the constant voltage charging is maintained until the current decays to 0.01-0.02C. The constant current charging current during the CEI film deposition completion stage on the LMFP side is 0.08C-0.12C, and the voltage range corresponding to the constant current charging is 3.92V-4.05V; preferably, a second venting process is performed at the end of this stage, more preferably, the venting negative pressure is -45 to -55kPa, and the time is 8-12min; The constant current charging current during the overall shaping of the CEI film on the positive electrode side and the first full charge stage of the battery is 0.15C-0.2C, and the voltage range corresponding to constant current charging is 4.05V to 4.25V. When the voltage reaches 4.25V, charge at a constant voltage until the current is ≤0.02C.
5. The formation method of a soft-pack lithium-ion battery according to claim 1, characterized in that, In step (3), the battery is discharged until the voltage reaches 2.8V, then the discharge is stopped. And / or, the secondary charge is activated to a voltage of 3.7V.
6. The formation method of a soft-pack lithium-ion battery according to claim 1, characterized in that, In step (4), the aging process includes an exhaust aging process, an interface reconstruction aging process, and a stabilization process.
7. The formation method of a soft-pack lithium-ion battery according to claim 6, characterized in that, The exhaust aging treatment stage is conducted at a temperature of 20-30℃, a pressure of 0.03-0.08MPa, and a time of 20-26h; exhaust treatment is performed during the exhaust aging treatment stage. Preferably, the exhaust treatment pressure is -90 kPa to -100 kPa, and the time is 3-8 min.
8. The formation method of a soft-pack lithium-ion battery according to claim 6, characterized in that, The interface reconstruction aging process is carried out at a temperature of 40-50℃, a pressure of 0.35-0.45MPa, and a charging voltage of 3.75V±0.02V. Under these conditions, the interface reconstruction aging process is completed by constant voltage charging until the microcurrent decays to below 0.002C. And / or, the stabilization treatment stage is performed at a temperature of 20-30°C, a pressure of 0.12-0.16 MPa, and a time of 20-26 h.
9. The formation method of a soft-pack lithium-ion battery according to claim 1, characterized in that, The positive electrode of the soft-pack lithium-ion battery comprises a composite system of lithium manganese iron phosphate (LMFP) and ternary material NCM. Preferably, the ternary material NCM is selected from one or more of the NCM523, NCM622, NCM811, NCM9, and NCM613 systems.
10. A soft-pack lithium-ion battery, characterized in that, Prepared by the formation method according to any one of claims 1-9; Preferably, the Mn in the SEI of the negative electrode of the soft-pack lithium-ion battery 2+ Deposition amount ≤25ppm; two-phase charge depth difference ΔSOC ≤5%; capacity retention ≥92% after 1000 cycles at 0.5C / 0.5C@25℃.