A method for recycling battery cores and a method for recycling batteries.

By combining short-circuit wetting treatment and ultrasonic treatment, the problems of cathode material contamination and separation difficulties in core recycling were solved, achieving efficient lithium recovery and material separation, and improving the overall effect of core recycling.

CN123120952APending Publication Date: 2026-11-17MIRATTERY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611387589.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-08
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the existing technology, the positive electrode material is easily contaminated during the core recycling process, resulting in poor separation effect. In particular, the tight adhesion between the separator and the electrode makes separation difficult, and excessive discharge may cause the ceramic layer to fall off or the positive and negative electrodes to break, affecting material repair.

Method used

A short-circuit wetting treatment method is adopted, in which the core is immersed in a wetting solution of non-flammable organic solvent and nonionic surfactant, combined with ultrasonic treatment, to achieve the precipitation of LiPF6 and the separation of the separator and the electrode, thus preventing impurities from entering the positive electrode material.

Benefits of technology

It significantly improves the efficiency of core disassembly, reduces the impurity content in the cathode material, increases the lithium recovery rate, and ensures smooth separation of the separator and electrode, avoiding overheating and gas bulging problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to a method for recycling battery cores and a method for recycling batteries, specifically in the field of battery recycling. The method includes: immersing a battery core discharged to 0% SOC in a wetting solution for short-circuit wetting treatment, separating LiPF6 solids and the electrolyte-removed core; the short-circuit wetting treatment includes: immersing the core in the wetting solution for a first preset time, followed by ultrasonication for a second preset time, during which the core is in a short-circuit state; the wetting solution includes: a non-flammable organic solvent and a nonionic surfactant, wherein the polarity of the non-flammable organic solvent is less than the polarity of the electrolyte solvent in the core. The recycling method provided by this application can precipitate LiPF6 in the electrolyte into crystals for direct recycling, avoiding impurities from entering the positive electrode material during recycling. Simultaneously, the wetting solution combined with ultrasonication significantly reduces the adhesion between the separator and the electrode, making it easier for the separator to start and separate from the positive and negative electrodes, thus improving the efficiency of core dismantling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery recycling, specifically to a method for recycling battery cores and a method for recycling batteries. Background Technology

[0002] The cells used in power battery packs or energy storage batteries are mainly divided into wound square aluminum shell, wound cylindrical and stacked blade batteries.

[0003] After these batteries are retired, they need to be recycled and disposed of. Currently, the commonly used disposal methods are cell crushing and pulverization and refined dismantling. Cell crushing and pulverization results in the positive and negative electrode materials being mixed together, and a lot of copper and aluminum impurities are mixed in, making direct repair impossible; while the positive and negative electrode sheets obtained from refined dismantling can be separated well, so the refined dismantling route has a better development prospect.

[0004] However, since laminated cells often use thermal bonding technology, the separator and electrode sheets adhere to each other, making disassembly difficult. Therefore, refined disassembly currently focuses on wound cells. The refined disassembly steps include: over-discharging to prevent fire during subsequent disassembly, then breaking open the outer casing, removing the core, drying the core, and then reversing the winding of the wound core (for laminated cells, separating the electrode sheets), separating the positive electrode sheet, negative electrode sheet, and separator.

[0005] For example, CN119231001A discloses a method for dismantling waste lithium batteries, including: step S1, discharging the waste lithium batteries; step S2, testing the voltage of the discharged lithium batteries; step S3, puncturing the lithium batteries that pass the voltage test; step S4, dismantling the punctured batteries to form waste materials and battery cells; step S5, recycling the waste materials generated during the dismantling process; step S6, pushing the dismantled lithium batteries into cores, recycling the shells and other waste materials removed from the dismantled lithium batteries and temporarily storing them in a shell storage box, and temporarily storing the dismantled cores in a core storage bin; step S7, the temporarily stored cores can be manually separated from the positive and negative electrode plates and the separator.

[0006] However, most battery cells now use ceramic separators, where the ceramic layer is made of alumina, boehmite, or silica coated onto a PE separator with binders such as PVDF. If the battery cell is over-discharged (continued to discharge after the battery voltage has fallen below a specified value), the internal temperature rises significantly. This causes the binders in the ceramic layer and the positive and negative electrode material layers to soften, resulting in the separator and certain areas of the positive and negative electrodes becoming too tightly bonded and unable to separate. In severe cases, this can lead to breakage of the positive and negative electrodes and failure to unwind; in milder cases, the ceramic layer may detach from the separator and enter the positive electrode material, introducing impurities and hindering material repair.

[0007] Over-discharge can also cause gas to be generated inside the battery cell, causing the outer casing to bulge and affecting the accuracy of subsequent casing breaking. Moreover, after over-discharge, the voltage will rebound after being left for a period of time, causing lithium ions to migrate to the negative electrode, resulting in a lack of lithium ions in the positive electrode material.

[0008] If the battery cell has a long service life and consumes a lot of internal electrolyte, then there will be insufficient lubrication between the separator and the positive and negative electrode plates. It will be difficult to start the separator during the unwinding process, resulting in poor separation between the separator and the positive and negative electrodes. The ceramic layer is easy to fall off and enter the positive electrode material.

[0009] In summary, current recycling solutions for battery cores still suffer from drawbacks such as easy contamination of the recycled cathode material and poor core disassembly efficiency. Summary of the Invention

[0010] In view of the problems existing in the prior art, the purpose of this application is to provide a method for recycling and processing battery cores and a method for recycling batteries, so as to solve the defects of the recycling scheme of battery cores, which are easy to contaminate the recycled positive electrode material and have poor battery core splitting effect.

[0011] To achieve this objective, the following technical solution is adopted in this application:

[0012] Firstly, this application provides a method for recycling and processing a winding core, the recycling and processing method comprising:

[0013] The core, which was discharged to 0% SOC, was immersed in the wetting solution for short-circuit wetting treatment. After separation, LiPF6 solid and the core with the electrolyte removed were obtained.

[0014] The short-circuit wetting process includes: immersing the core in the wetting liquid for a first preset time and then ultrasonicating it for a second preset time, during which the core is in a short-circuit state.

[0015] The wetting liquid includes: a non-flammable organic solvent and a non-ionic surfactant, wherein the polarity of the non-flammable organic solvent is less than the polarity of the solvent in the electrolyte in the core.

[0016] The recycling method provided in this application can precipitate LiPF6 in the electrolyte into crystals through a specific wetting solution treatment, thereby directly recycling it and avoiding impurities from entering the positive electrode material during recycling. Furthermore, the wetting solution combined with ultrasound can significantly reduce the adhesion between the separator and the electrode, making it easier for the separator to start and separate from the positive and negative electrodes, thus improving the efficiency of core disassembly.

[0017] As one technical solution of this application, the recycling method satisfies at least one of the following:

[0018] (1) The discharge rate of the discharge is ≤0.3C;

[0019] (2) The wetting solution comprises, by mass percentage: 0.05-1% nonionic surfactant, with the remainder being non-flammable organic solvent.

[0020] As one technical solution of this application, the recycling method satisfies at least one of the following:

[0021] (1) The wetting solution can be used in either method one or method two.

[0022] Method one includes: preparing a solution according to the formula for direct use;

[0023] Method 2 includes: obtaining non-flammable organic solvents and non-ionic surfactants according to the formula, impregnating the core with the non-flammable organic solvent for a first preset time, and then adding the non-ionic surfactant and supplementing with ultrasound for a second preset time.

[0024] (2) The nonionic surfactant includes: dehydrated sorbitan fatty acid ester and / or fatty alcohol polyoxyethylene ether;

[0025] (3) The non-flammable organic solvent includes one or a combination of at least two of carbon tetrachloride, dichloromethane, chloroform or pentafluoropropanol.

[0026] As one technical solution of this application, the recycling method satisfies at least one of the following:

[0027] (1) The dehydrated sorbitan fatty acid esters include: one or a combination of at least two of Span20, Span40, Span60 or Span80;

[0028] (2) The fatty alcohol polyoxyethylene ether includes one or a combination of at least two of AEO-1, AEO-2 or AEO-3.

[0029] As one technical solution of this application, the recycling method satisfies at least one of the following:

[0030] (1) The core used in the short-circuit impregnation treatment has had the tape and insulating film removed;

[0031] (2) In the short-circuit impregnation treatment, the impregnation liquid is 3-5 cm higher than the core;

[0032] (3) The temperature of the wetting liquid in the short-circuit wetting treatment is controlled to be 10-40℃.

[0033] As one technical solution of this application, the first preset time is 5-10 minutes.

[0034] As one technical solution of this application, the recycling method satisfies at least one of the following:

[0035] (1) The frequency of the ultrasound is 20-100 kHz;

[0036] (2) The power of the ultrasound is 0.1-5kW.

[0037] As one technical solution of this application, the second preset time is 5-10 minutes.

[0038] As one technical solution of this application, after the second preset time is reached, the electrolyte-removed core is sequentially drained, dried, and unwound.

[0039] Secondly, this application provides a method for recycling batteries, the method comprising: disassembling the battery to obtain a winding core, and processing the obtained winding core using the recycling method described in the first aspect.

[0040] Compared with existing technical solutions, this application has the following advantages:

[0041] (1) The recycling method provided in this application does not require the battery cell to be over-discharged before breaking the shell, and will not overheat or produce gas swelling. It can prevent impurities from entering the positive electrode material and improve the success rate of unwinding.

[0042] (2) The recycling method provided in this application allows most of the lithium to return to the cathode material without voltage rebound, which can significantly reduce the loss of lithium during the recycling process.

[0043] (3) The recycling method provided in this application makes it easy to separate the separator from the electrode, which facilitates the start-up and unwinding of the separator, while the ceramic layer on the separator will not stick to the positive electrode material.

[0044] The present application is described in further detail below. However, the examples below are merely simplified examples and do not represent or limit the scope of protection of the present application. The scope of protection of the present application shall be determined by the claims. Detailed Implementation

[0045] To better illustrate this application and facilitate understanding of its technical solutions, typical but non-limiting embodiments of this application are as follows:

[0046] I. This specific embodiment provides a method for recycling and processing a winding core, the recycling and processing method comprising:

[0047] The core, which was discharged to 0% SOC, was immersed in the wetting solution for short-circuit wetting treatment. After separation, LiPF6 solid and the core with the electrolyte removed were obtained.

[0048] The short-circuit wetting process includes: immersing the core in the wetting liquid for a first preset time and then ultrasonicating it for a second preset time, during which the core is in a short-circuit state.

[0049] The wetting liquid includes: a non-flammable organic solvent and a non-ionic surfactant, wherein the polarity of the non-flammable organic solvent is less than the polarity of the solvent in the electrolyte in the core.

[0050] In this application, "core" refers to a component obtained by removing the outer casing from the cell used in a power battery pack or energy storage battery, specifically formed by spiral winding of a positive electrode sheet, a negative electrode sheet, and a separator.

[0051] In this application, the cores are derived from defective cores generated during the manufacturing process, such as defective cores generated during the winding process, defective cores generated during battery assembly, cores removed from faulty batteries, cores removed from batteries that have reached the end of their service life, etc. However, qualified cores are not excluded, and even qualified cores can be processed using the recycling method of this application.

[0052] In this application, the positive electrode sheet in the core can be a ternary material coated with polyvinylidene fluoride as a binder onto an aluminum foil current collector, or a lithium iron phosphate material coated with polyvinylidene fluoride as a binder onto an aluminum foil or carbon-coated aluminum foil current collector.

[0053] In this application, the negative electrode sheet in the core can be an artificial graphite or natural graphite or a silicon-carbon negative electrode sheet coated on copper foil with carboxymethyl cellulose, styrene-butadiene rubber, etc. as binders.

[0054] In this application, the diaphragm in the core can be a PE diaphragm or a PE ceramic diaphragm, etc.

[0055] In this application, the active component of the electrolyte in the core includes lithium hexafluorophosphate. An exemplary composition is that the volume ratio of solvent ethylene carbonate EC: ethyl methyl carbonate EMC: dimethyl carbonate DMC is 1:1:1, the concentration of LiPF6 is 1 mol / L, and the proportion of additives is 1-2%.

[0056] In this application, during the impregnation process, the polarity of the lipid solvent in the electrolyte of the core is greater than that of the non-flammable organic solvent. At the same time, the concentration of lithium hexafluorophosphate in the electrolyte is high. When it encounters the non-flammable organic solvent in the narrow space between the cores, the solubility of lithium hexafluorophosphate in the mixed solvent of the non-flammable organic solvent and the lipid solvent in the electrolyte is greatly reduced, causing the lithium hexafluorophosphate to be partially precipitated, thereby realizing the recovery of lithium hexafluorophosphate.

[0057] In this application, non-flammable organic solvents refer to organic liquid solvents that cannot be ignited by an open flame under normal or high temperature conditions, or whose combustion reaction is extremely difficult to sustain. Corresponding to this application, non-flammable organic solvents are those that do not burn under the operating conditions of this application (temperature of core short circuit ≤200℃) and meet the corresponding limitations, so as to avoid possible combustion due to core short circuit during the impregnation process, while ensuring that LiPF6 can be precipitated as solid particles.

[0058] In some specific embodiments, the discharge rate is ≤0.3C, for example, it can be 0.3C, 0.29C, 0.28C, 0.27C, 0.26C, 0.25C, 0.24C, 0.23C, 0.22C, 0.21C, 0.2C, 0.19C, 0.18C, 0.17C, 0.16C, 0.15C, 0.14C, 0.13C, 0.12C, 0.11C, or 0.1C, but is not limited to the listed values. Other unlisted values ​​within this range also meet the requirements.

[0059] In some specific embodiments, the wetting solution comprises, by mass percentage: 0.05-1% nonionic surfactant, with the balance being a non-flammable organic solvent.

[0060] In this application, the nonionic surfactant in the wetting solution is 0.05-1% by mass, for example, it can be 0.05%, 0.0975%, 0.145%, 0.1925%, 0.24%, 0.2875%, 0.335%, 0.3825%, 0.43%, 0.4775%, 0.525%, 0.5725%, 0.62%, 0.6675%, 0.715%, 0.7625%, 0.81%, 0.8575%, 0.905%, 0.9525% or 1%, etc., but is not limited to the listed values. Other unlisted values ​​within this range are also acceptable.

[0061] In this application, the wetting solution, under the action of ultrasound, enters the pores between the positive electrode, negative electrode and the separator. Under the action of nonionic surfactant, the adhesion between the electrode and the separator is significantly reduced, causing the separator to start, thereby improving the separation effect between the separator and the electrode, and further enhancing the precipitation of LiPF6.

[0062] In some specific embodiments, the wetting liquid is used in either method one or method two.

[0063] In this application, method one includes: preparing a solution according to a formula for direct use.

[0064] In this application, the second method includes: obtaining a non-flammable organic solvent and a non-ionic surfactant according to the formula, impregnating the core with the non-flammable organic solvent for a first preset time, and then adding the non-ionic surfactant and supplementing it with ultrasound for a second preset time.

[0065] In some specific embodiments, the nonionic surfactant includes: dehydrated sorbitan fatty acid esters and / or fatty alcohol polyoxyethylene ethers.

[0066] In some specific embodiments, the non-flammable organic solvent includes one or a combination of at least two of carbon tetrachloride, dichloromethane, chloroform, or pentafluoropropanol.

[0067] In this application, the combination of non-flammable organic solvents may be selected as a combination of carbon tetrachloride and dichloromethane, a combination of dichloromethane and trichloromethane, a combination of trichloromethane and pentafluoropropanol, etc.

[0068] In some specific embodiments, the dehydrated sorbitan fatty acid ester includes one or a combination of at least two of Span20, Span40, Span60, or Span80.

[0069] In this application, the combination of dehydrated sorbitan fatty acid esters can be selected as a combination of Span20 and Span40, a combination of Span40 and Span60, a combination of Span20 and Span80, etc.

[0070] In some specific embodiments, the fatty alcohol polyoxyethylene ether includes one or a combination of at least two of AEO-1, AEO-2, or AEO-3.

[0071] In this application, the combination of fatty alcohol polyoxyethylene ethers can be selected as a combination of AEO-1 and AEO-2, a combination of AEO-2 and AEO-3, a combination of AEO-1 and AEO-3, etc.

[0072] In some specific embodiments, the core used in the short-circuit impregnation treatment has had the tape and insulating film removed.

[0073] In this application, the tape refers to the tape used to fix the structure of the battery cell after it has been wound, including: tape at the bottom, sides, top and winding end of the battery cell, and tape at the head, tail, welding tab and tab lead-out part of the electrode sheet.

[0074] In this application, the insulating film is used to achieve insulation between the battery cell and the battery casing. Removing the insulating film before impregnation can ensure that the impregnation liquid can fully contact the battery cell body, thereby achieving effective treatment of the core.

[0075] In some specific embodiments, the wetting liquid level in the short-circuit impregnation treatment is 3-5 cm higher than the core, for example, it can be 3 cm, 3.1 cm, 3.2 cm, 3.3 cm, 3.4 cm, 3.5 cm, 3.6 cm, 3.7 cm, 3.8 cm, 3.9 cm, 4 cm, 4.1 cm, 4.2 cm, 4.3 cm, 4.4 cm, 4.5 cm, 4.6 cm, 4.7 cm, 4.8 cm, 4.9 cm, or 5 cm, but is not limited to the listed values. Other unlisted values ​​within this range are also acceptable.

[0076] In this application, the short-circuit state is achieved by connecting the positive and negative electrodes of the core, such as by using graphite or aluminum to connect the positive and negative electrodes of the core to achieve a short circuit. By short-circuiting, it can be ensured that lithium returns to the positive electrode material, thereby improving the lithium recovery effect.

[0077] In some specific embodiments, the temperature of the wetting liquid in the short-circuit wetting treatment is controlled to be 10-40℃, for example, it can be 10℃, 11.5℃, 13℃, 14.5℃, 16℃, 17.5℃, 19℃, 20.5℃, 22℃, 23.5℃, 25℃, 26.5℃, 28℃, 29.5℃, 31℃, 32.5℃, 34℃, 35.5℃, 37℃, 38.5℃ or 40℃, but is not limited to the listed values, other unlisted values ​​within this range are also acceptable.

[0078] In some specific embodiments, the first preset time is 5-10 minutes, for example, it can be 5 minutes, 5.25 minutes, 5.5 minutes, 5.75 minutes, 6 minutes, 6.25 minutes, 6.5 minutes, 6.75 minutes, 7 minutes, 7.25 minutes, 7.5 minutes, 7.75 minutes, 8 minutes, 8.25 minutes, 8.5 minutes, 8.75 minutes, 9 minutes, 9.25 minutes, 9.5 minutes, 9.75 minutes, or 10 minutes, but is not limited to the listed values. Other unlisted values ​​within this range are also acceptable.

[0079] In some specific embodiments, the frequency of the ultrasound is 20-100kHz, for example, it can be 20kHz, 24kHz, 28kHz, 32kHz, 36kHz, 40kHz, 44kHz, 48kHz, 52kHz, 56kHz, 60kHz, 64kHz, 68kHz, 72kHz, 76kHz, 80kHz, 84kHz, 88kHz, 92kHz, 96kHz or 100kHz, but is not limited to the listed values, other unlisted values ​​within this range are also acceptable.

[0080] In some specific embodiments, the power of the ultrasound is 0.1-5kW, for example, it can be 0.1kW, 0.345kW, 0.59kW, 0.835kW, 1.08kW, 1.325kW, 1.57kW, 1.815kW, 2.06kW, 2.305kW, 2.55kW, 2.795kW, 3.04kW, 3.285kW, 3.53kW, 3.775kW, 4.02kW, 4.265kW, 4.51kW, 4.755kW, or 5kW, but is not limited to the listed values. Other unlisted values ​​within this range are also acceptable.

[0081] In some specific embodiments, the second preset time is 5-10 minutes, for example, it can be 5 minutes, 5.25 minutes, 5.5 minutes, 5.75 minutes, 6 minutes, 6.25 minutes, 6.5 minutes, 6.75 minutes, 7 minutes, 7.25 minutes, 7.5 minutes, 7.75 minutes, 8 minutes, 8.25 minutes, 8.5 minutes, 8.75 minutes, 9 minutes, 9.25 minutes, 9.5 minutes, 9.75 minutes, or 10 minutes, but is not limited to the listed values. Other unlisted values ​​within this range are also acceptable.

[0082] In this application, the short-circuit wetting treatment can be achieved by means of a tank. For example, the wetting tank can be designed in sections according to the structure of the core or battery, so that it can flexibly handle one or more cores or batteries. At the same time, multiple ultrasonic generators can be evenly arranged in the tank to achieve sufficient ultrasonic treatment.

[0083] In this application, separation refers to removing the core from the immersion liquid to obtain a core with the electrolyte removed, and then performing solid-liquid separation on the immersion liquid to obtain solid LiPF6.

[0084] In this application, the solid-liquid separation methods include: filtration, vacuum filtration, pressure filtration, centrifugation, etc.

[0085] In some specific embodiments, after the second preset time is reached, the electrolyte-removed core is sequentially drained, dried, and unwound.

[0086] In this application, "reverse unwinding" refers to separating the stacked electrode roll into positive electrode, negative electrode and separator.

[0087] II. This specific embodiment provides a battery recycling method, which includes: disassembling the battery to obtain a winding core, and processing the obtained winding core using the recycling method described above.

[0088] In this application, when recycling the battery, the battery can be discharged as a whole according to the discharge requirements of this application, and then disassembled to obtain the winding core for the subsequent short-circuit wetting treatment of this application. Alternatively, the battery can be disassembled to obtain the battery cell, and then the winding core can be obtained after discharge disassembly, and then the recycling method of this application can be carried out.

[0089] III. To illustrate the superior recycling effect achievable by the recycling method for the core provided in this application, the following example is used:

[0090] Example 1

[0091] This embodiment provides a method for recycling and processing a winding core, the recycling and processing method comprising:

[0092] Discharge the retired battery cell to 0% SOC at a normal rate, then break open the outer casing, cut the connection between the core and the top cover, remove the core, and obtain the discharged core.

[0093] The discharge core is immersed in the wetting solution for short-circuit wetting treatment. The core is then removed from the wetting solution to obtain a core with electrolyte removed. The wetting solution is then filtered to obtain solid LiPF6.

[0094] The short-circuit wetting process includes: immersing the discharge core in the wetting liquid for a first preset time and then ultrasonicating it for a second preset time, during which the discharge core is in a short-circuit state.

[0095] The core is a core removed from a battery that has reached the end of its service life, specifically including: a positive electrode of lithium iron phosphate, a negative electrode of artificial graphite, a PE ceramic separator, an electrolyte of 1 mol / L LiPF6 solution, and a solvent with a volume ratio of EC:EMC:DMC=1:1:1.

[0096] The discharge rate is 0.3C;

[0097] The wetting solution comprises, by weight percentage: 0.08% nonionic surfactant, with the balance being non-flammable organic solvent;

[0098] The wetting solution is prepared as a solution according to the formula and used directly.

[0099] The non-flammable organic solvent is carbon tetrachloride;

[0100] The nonionic surfactant is Span40;

[0101] The core used in the short-circuit impregnation treatment has had the tape and insulating film removed;

[0102] In the short-circuit immersion treatment, the immersion liquid level is 4 cm higher than the discharge core.

[0103] The short-circuit state of the discharge core in the short-circuit impregnation treatment is achieved by connecting the positive and negative poles of the core. Graphite is used to connect the positive and negative poles of the core to achieve a short circuit.

[0104] The temperature of the wetting solution is controlled at 25°C during the short-circuit wetting treatment.

[0105] The first preset time is 8 minutes;

[0106] The frequency of the ultrasound is 50 kHz; the power of the ultrasound is 3 kW.

[0107] The second preset time is 6 minutes;

[0108] After the second preset time is reached, the electrolyte-removed core will be drained, dried and reverse-wound in sequence; reverse-wound refers to separating the stacked electrode roll into positive electrode, negative electrode and separator.

[0109] Example 2

[0110] This embodiment provides a method for recycling and processing a winding core, the recycling and processing method comprising:

[0111] Discharge the retired battery cell to 0% SOC at a normal rate, then break open the outer casing, cut the connection between the core and the top cover, remove the core, and obtain the discharged core.

[0112] The discharge core is immersed in the wetting solution for short-circuit wetting treatment. The core is then removed from the wetting solution to obtain a core with electrolyte removed. The wetting solution is then filtered to obtain solid LiPF6.

[0113] The short-circuit wetting process includes: immersing the discharge core in the wetting liquid for a first preset time and then ultrasonicating it for a second preset time, during which the discharge core is in a short-circuit state.

[0114] The core is a core removed from a faulty battery, specifically including: a positive electrode of lithium iron phosphate, a negative electrode of artificial graphite, a PE ceramic separator, an electrolyte of 1 mol / L LiPF6 solution, and a solvent with a volume ratio of EC:EMC:DMC=1:1:1.

[0115] The discharge rate is 0.2C;

[0116] The wetting solution comprises, by weight percentage: 0.06% nonionic surfactant, with the balance being non-flammable organic solvent;

[0117] The method of using the wetting solution includes: obtaining a non-flammable organic solvent and a non-ionic surfactant according to the formula, wetting the discharge core with the non-flammable organic solvent for a first preset time, and then adding the non-ionic surfactant and supplementing it with ultrasound for a second preset time.

[0118] The non-flammable organic solvent is dichloromethane;

[0119] The nonionic surfactant is Span60;

[0120] The core used in the short-circuit impregnation treatment has had the tape and insulating film removed;

[0121] In the short-circuit immersion treatment, the immersion liquid level is 4 cm higher than the discharge core.

[0122] The short-circuit state of the discharge core in the short-circuit impregnation treatment is achieved by connecting the positive and negative electrodes of the core, specifically by using aluminum to connect the positive and negative electrodes of the core to achieve a short circuit.

[0123] The temperature of the wetting solution is controlled at 30°C during the short-circuit wetting treatment.

[0124] The first preset time is 6 minutes;

[0125] The frequency of the ultrasound is 70 kHz; the power of the ultrasound is 1 kW.

[0126] The second preset time is 8 minutes;

[0127] After the second preset time is reached, the electrolyte-removed core will be drained, dried and reverse-wound in sequence; reverse-wound refers to separating the stacked electrode roll into positive electrode, negative electrode and separator.

[0128] Example 3

[0129] This embodiment provides a method for recycling and processing a winding core, the recycling and processing method comprising:

[0130] Discharge the retired battery cell to 0% SOC at a normal rate, then break open the outer casing, cut the connection between the core and the top cover, remove the core, and obtain the discharged core.

[0131] The discharge core is immersed in the wetting solution for short-circuit wetting treatment. The core is then removed from the wetting solution to obtain a core with electrolyte removed. The wetting solution is then filtered to obtain solid LiPF6.

[0132] The short-circuit wetting process includes: immersing the discharge core in the wetting liquid for a first preset time and then ultrasonicating it for a second preset time, during which the discharge core is in a short-circuit state.

[0133] The core is a core removed from a battery that has reached the end of its service life, specifically including: a positive electrode of lithium iron phosphate, a negative electrode of artificial graphite, a PE ceramic separator, an electrolyte of 1 mol / L LiPF6 solution, and a solvent with a volume ratio of EC:EMC:DMC=1:1:1.

[0134] The discharge rate is 0.3C;

[0135] The wetting solution comprises, by mass percentage: 1% nonionic surfactant, with the remainder being a non-flammable organic solvent;

[0136] The method of using the wetting solution is to prepare it into a solution according to the formula and use it directly; the second method includes: obtaining a non-flammable organic solvent and a non-ionic surfactant according to the formula, wetting the discharge core with the non-flammable organic solvent for a first preset time, and then adding the non-ionic surfactant and supplementing it with ultrasound for a second preset time.

[0137] The non-flammable organic solvent is pentafluoropropanol;

[0138] The nonionic surfactant is AEO-3;

[0139] The core used in the short-circuit impregnation treatment has had the tape and insulating film removed;

[0140] In the short-circuit wetting treatment, the wetting liquid level is 5 cm higher than the discharge core.

[0141] In the short-circuit impregnation treatment, the discharge core is in a short-circuit state. The short-circuit state is achieved by connecting the positive and negative poles of the core, such as by using graphite or aluminum to connect the positive and negative poles of the core to achieve a short circuit.

[0142] The temperature of the wetting solution is controlled at 40°C during the short-circuit wetting treatment.

[0143] The first preset time is 5 minutes;

[0144] The frequency of the ultrasound is 20kHz; the power of the ultrasound is 5kW.

[0145] The second preset time is 5 minutes;

[0146] After the second preset time is reached, the electrolyte-removed core will be drained, dried and reverse-wound in sequence; reverse-wound refers to separating the stacked electrode roll into positive electrode, negative electrode and separator.

[0147] Example 4

[0148] This embodiment provides a method for recycling and processing a winding core, the recycling and processing method comprising:

[0149] Discharge the retired battery cell to 0% SOC at a normal rate, then break open the outer casing, cut the connection between the core and the top cover, remove the core, and obtain the discharged core.

[0150] The discharge core is immersed in the wetting solution for short-circuit wetting treatment. The core is then removed from the wetting solution to obtain a core with electrolyte removed. The wetting solution is then filtered to obtain solid LiPF6.

[0151] The short-circuit wetting process includes: immersing the discharge core in the wetting liquid for a first preset time and then ultrasonicating it for a second preset time, during which the discharge core is in a short-circuit state.

[0152] The core is a core removed from a battery that has reached the end of its service life, specifically including: a positive electrode of lithium iron phosphate, a negative electrode of artificial graphite, a PE ceramic separator, an electrolyte of 1 mol / L LiPF6 solution, and a solvent with a volume ratio of EC:EMC:DMC=1:1:1.

[0153] The discharge rate is 0.1C;

[0154] The wetting solution comprises, by weight percentage: 0.05% nonionic surfactant, with the balance being non-flammable organic solvent;

[0155] The wetting solution is prepared as a solution according to the formula and used directly.

[0156] The non-flammable organic solvent is chloroform;

[0157] The nonionic surfactant is AEO-1;

[0158] The core used in the short-circuit impregnation treatment has had the tape and insulating film removed;

[0159] In the short-circuit wetting treatment, the wetting liquid level is 3 cm above the discharge core.

[0160] The short-circuit state of the discharge core in the short-circuit impregnation treatment is achieved by connecting the positive and negative poles of the core, such as by using graphite or aluminum to connect the positive and negative poles of the core to achieve a short circuit.

[0161] The temperature of the wetting solution is controlled at 10°C during the short-circuit wetting treatment.

[0162] The first preset time is 10 minutes;

[0163] The frequency of the ultrasound is 100 kHz; the power of the ultrasound is 0.1 kW.

[0164] The second preset time is 10 minutes;

[0165] After the second preset time is reached, the electrolyte-removed core will be drained, dried and reverse-wound in sequence; reverse-wound refers to separating the stacked electrode roll into positive electrode, negative electrode and separator.

[0166] Example 5

[0167] The only difference from Example 1 is that the discharge core is in an open circuit state during the short-circuit impregnation treatment, that is, the positive and negative poles are not short-circuited.

[0168] Example 6

[0169] The only difference from Example 1 is that the wetting solution, by mass percentage, includes: 0.01% nonionic surfactant, with the balance being non-flammable organic solvent.

[0170] Example 7

[0171] The only difference from Example 1 is that the wetting solution, by mass percentage, includes: 5% nonionic surfactant and the remainder is non-flammable organic solvent.

[0172] Example 8

[0173] The only difference from Example 1 is that the frequency of the ultrasound is 10 kHz.

[0174] Example 9

[0175] The only difference from Example 1 is that the frequency of the ultrasound is 120 kHz.

[0176] Example 10

[0177] The only difference from Example 1 is that the ultrasonic power is 0.05kW.

[0178] Example 11

[0179] The only difference from Example 1 is that the ultrasonic power is 8kW.

[0180] Comparative Example 1

[0181] The only difference from Example 1 is that the non-flammable organic solvent is replaced with an equal amount of ethylene carbonate.

[0182] Comparative Example 2

[0183] The only difference from Example 1 is that the wetting solution is replaced with an equal amount of carbon tetrachloride, i.e. no surfactant is added.

[0184] Comparative Example 3

[0185] The only difference from Example 1 is that the waste core is over-discharged to a voltage of 0.5V.

[0186] Comparative Example 4

[0187] The only difference from Example 1 is that ultrasound is not used, but the infiltration is still guaranteed to last for the second preset time.

[0188] Comparative Example 5

[0189] The only difference from Example 1 is that ultrasound with the same parameters is also used during the first preset time of immersion.

[0190] The materials obtained from the reverse unwinding of the above embodiments and comparative examples were analyzed, and the analysis results are shown in Table 1 below.

[0191] Table 1

[0192]

[0193] In the table: LiPF6 recovery rate refers to the percentage of recovered LiPF6 solid relative to the original electrolyte in the core; the testing process for aluminum and lithium content in the cathode material includes: first dissolving the cathode material in aqua regia, then diluting it, and then using ICP (inductively coupled plasma) to detect the aluminum and lithium content.

[0194] As shown in Table 1:

[0195] As can be seen from the results of Examples 1-4, the recycling method provided in this application, through specific wetting solution treatment, can precipitate LiPF6 in the electrolyte into crystals for direct recovery, avoiding impurities from entering the positive electrode material during recycling. Furthermore, the wetting solution combined with ultrasound can significantly reduce the adhesion effect between the separator and the electrode, making it easier for the separator to start and separate from the positive and negative electrodes, improving the efficiency of core disassembly. The LiPF6 recovery rate is ≥34.5%, the aluminum content in the positive electrode material is ≤242.5ppm, and the lithium content in the positive electrode material is ≥4.162ppm.

[0196] A comparison of Examples 1 and 5 shows that the external short circuit between the positive and negative electrodes during wetting is an important way to cause most of the active lithium to return to the positive electrode material.

[0197] As can be seen from the comparison between Example 1 and Examples 6 and 7, the amount of nonionic surfactant added in the wetting agent of this application needs to be reasonably controlled in order to facilitate the efficient recovery of lithium in LiPF6 and cathode materials, while reducing the entry of impurity aluminum into the cathode material.

[0198] As can be seen from the comparison of Example 1 with Examples 8, 9, 10, 11 and Comparative Example 4, the ultrasonic conditions should not be too weak or too strong. If the conditions are too weak, the surfactant cannot enter the core to play a lubricating role, and if the conditions are too strong, the ceramic layer on the diaphragm will be directly shattered and enter the material.

[0199] As can be seen from the comparison between Example 1 and Comparative Example 1, the use of the specific non-flammable organic solvent of this application enables LiPF6 to precipitate out as solid particles and be recovered.

[0200] As can be seen from the comparison between Example 1 and Comparative Example 2, when no surfactant is added to the wetting solution of this application, the content of aluminum impurities in the recovered cathode material will be significantly increased, while the lithium recovery effect in the cathode material will be reduced.

[0201] As can be seen from the comparison between Example 1 and Comparative Example 3, when the core is over-discharged, it will affect the deposition effect of LiPF6 and reduce the recovery rate of LiPF6. At the same time, although it can improve the recovery effect of lithium in the cathode material, it will increase the content of aluminum impurities in the recovered cathode material, which will have an adverse effect on the subsequent utilization of the cathode material.

[0202] The embodiments of this application have been described in detail above. However, this application is not limited to the specific details of the above embodiments. Within the scope of the technical concept of this application, various simple modifications can be made to the technical solution of this application, and these simple modifications all fall within the protection scope of this application.

[0203] It should also be noted that the various specific technical features described in the above embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, this application will not describe the various possible combinations separately.

[0204] Furthermore, various different implementations of this application can be combined in any way, as long as they do not violate the spirit of this application, they should also be regarded as the content disclosed in this application.

Claims

1. A method for recycling and processing a winding core, characterized in that, The recycling process includes: The core, which was discharged to 0% SOC, was immersed in the wetting solution for short-circuit wetting treatment. After separation, LiPF6 solid and the core with the electrolyte removed were obtained. The short-circuit wetting process includes: immersing the core in the wetting liquid for a first preset time and then subjecting it to ultrasonication for a second preset time, during which the core is in a short-circuit state. The wetting liquid includes: a non-flammable organic solvent and a non-ionic surfactant, wherein the polarity of the non-flammable organic solvent is less than the polarity of the solvent in the electrolyte in the core.

2. The recycling method as described in claim 1, characterized in that, The recycling method satisfies at least one of the following: (1) The discharge rate of the discharge is ≤0.3C; (2) The wetting solution comprises, by mass percentage: 0.05-1% nonionic surfactant, with the remainder being non-flammable organic solvent.

3. The recycling method as described in claim 1, characterized in that, The recycling method satisfies at least one of the following: (1) The wetting solution can be used in either method one or method two. Method one includes: preparing a solution according to the formula for direct use; Method 2 includes: obtaining non-flammable organic solvents and non-ionic surfactants according to the formula, impregnating the core with the non-flammable organic solvent for a first preset time, and then adding the non-ionic surfactant and supplementing with ultrasound for a second preset time. (2) The nonionic surfactant includes: dehydrated sorbitan fatty acid ester and / or fatty alcohol polyoxyethylene ether; (3) The non-flammable organic solvent includes one or a combination of at least two of carbon tetrachloride, dichloromethane, chloroform or pentafluoropropanol.

4. The recycling method as described in claim 3, characterized in that, The recycling method satisfies at least one of the following: (1) The dehydrated sorbitan fatty acid esters include: one or a combination of at least two of Span20, Span40, Span60 or Span80; (2) The fatty alcohol polyoxyethylene ether includes one or a combination of at least two of AEO-1, AEO-2 or AEO-3.

5. The recycling method as described in claim 1, characterized in that, The recycling method satisfies at least one of the following: (1) The core used in the short-circuit impregnation treatment has had the tape and insulating film removed; (2) In the short-circuit impregnation treatment, the impregnation liquid is 3-5 cm higher than the core; (3) The temperature of the wetting liquid in the short-circuit wetting treatment is controlled to be 10-40℃.

6. The recycling method as described in claim 1, characterized in that, The first preset time is 5-10 minutes.

7. The recycling method as described in claim 1, characterized in that, The recycling method satisfies at least one of the following: (1) The frequency of the ultrasound is 20-100 kHz; (2) The power of the ultrasound is 0.1-5kW.

8. The recycling method as described in claim 1, characterized in that, The second preset time is 5-10 minutes.

9. The recycling method as described in claim 1, characterized in that, After the second preset time is reached, the electrolyte-removed core will be drained, dried, and unwound in sequence.

10. A method for recycling batteries, characterized in that, The recycling method includes: disassembling the battery to obtain the winding core, and processing the obtained winding core using the recycling method described in any one of claims 1-9.

Citation Information

Patent Citations

  • Waste lithium battery disassembling method

    CN119231001A