Corona-resistant modified insulation paper and automobile motor
By using polyimide matrix and mica composite fiber layer in insulating paper, and combining a fiber layer cladding layer without mica, the problem of insufficient corona resistance performance in existing insulating paper in high voltage environments is solved, and the problem of existing insulating paper is achieved. Longer corona life and higher local discharge start voltage while maintaining the overall strength of the material.
Patent Information
- Application Number
- CN202420270057.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2034-02-04
AI Technical Summary
The existing insulating paper for automotive motors has a low corona life and local discharge starting voltage level under a voltage environment of more than 700V, making it difficult to meet the corona performance requirements of high-voltage automotive motors.
A corona-resistant modified insulating paper, including a polyimide matrix, a composite fiber layer cladding layer containing polyaramide and mica in the middle, and a fiber layer cladding layer without mica, is added by appropriate amount of mica. and structural design to improve the corona life and local discharge starting voltage of insulating paper while reducing brittleness.
It significantly improves the corona life and local discharge starting voltage of insulating paper, meets the corona performance requirements of automotive motors above 700V, and maintains good tensile strength and elongation of break, avoiding the addition of mica Increased brittleness.
Smart Images

Figure CN222126150U_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of insulating materials, and in particular relates to a corona-resistant modified insulating paper and an automotive motor. Background Art
[0002] Insulating paper is an electrical insulating material used for various electrical equipment such as cables and coils. It has good insulating properties and mechanical strength. In the field of new energy vehicle manufacturing, insulating paper can be used as slot insulation, interturn insulation and interlayer insulation of motors. At present, typical insulating papers for automotive motors include aramid fiber paper and composite insulating paper. With the development of automotive technology, the design voltage of automotive motors is getting higher and higher, and the requirements for corona resistance of insulating paper for automotive motors are getting higher and higher. The corona resistance life and partial discharge inception voltage (PDIV) of existing insulating paper for automotive motors are relatively low, which makes it difficult to meet the requirements for corona resistance of automotive motors above 700V. Utility Model Content
[0003] The embodiments of the present application provide a corona-resistant modified insulating paper, which can effectively improve the corona resistance life and partial discharge starting voltage level of automobile motors.
[0004] In the first aspect, an embodiment of the present application provides a corona-resistant modified insulating paper, which includes a polyimide matrix, a first coating layer and a second coating layer; wherein the polyimide matrix is the middle layer of the insulating paper, the first coating layer is bonded to the outer surface of the polyimide matrix in a continuous layered form, the first coating layer is a composite fiber layer containing polyaramid and mica, the mica is filled in the interior of the polyaramid, and the content ratio of the mica to the polyaramid is positively correlated with the voltage value of the automobile motor, the second coating layer is stacked and connected to the side of the first coating layer away from the polyimide matrix, and the second coating layer is a fiber layer containing polyaramid.
[0005] According to a first aspect of an embodiment of the present application, in the first coating layer, the content of mica is 10%-15% of the mass of the polyaramid.
[0006] According to a first aspect of an embodiment of the present application, the content of the mica in the first coating layer is preferably 10% of the mass of the polyaramid.
[0007] According to a first aspect of the embodiment of the present application, the number of the first coating layers is two, and the two first coating layers are symmetrically distributed on both sides of the polyimide substrate.
[0008] According to a first aspect of the embodiment of the present application, the number of the second coating layers is two, and the two second coating layers are symmetrically distributed on both sides of the polyimide matrix.
[0009] According to a first aspect of the embodiment of the present application, the insulating paper further comprises a plurality of adhesive layers;
[0010] Any two adjacent to each other among the polyimide matrix, the first cladding layer, and the second cladding layer are connected to each other through the adhesive layer.
[0011] According to a first aspect of the embodiment of the present application, the bonding layer is an interlayer structure layer containing epoxy glue.
[0012] According to a first aspect of the embodiment of the present application, any one or more of the polyimide matrix, the first coating layer and the second coating layer has a dimension of 0.038 mm to 0.05 mm along its thickness direction.
[0013] According to the first aspect of the embodiment of the present application, any one or more of the polyimide matrix, the first coating layer and the second coating layer preferably has a dimension of 0.05 mm along its thickness direction.
[0014] In a second aspect, an embodiment of the present application provides an automotive motor, which includes any of the aforementioned corona-resistant modified insulating paper.
[0015] The corona-resistant modified insulating paper and automotive motor provided in the embodiments of the present application, in response to the corona-resistant requirements of automotive motors above 700V, can ensure that the insulating paper has a longer corona-resistant life and a higher partial discharge starting voltage by adding an appropriate amount of mica to the polyaromatic in the first coating layer; at the same time, in order to reduce the problem of increased brittleness of the insulating paper due to the addition of mica components, the side of the first coating layer away from the polyimide matrix is bonded with a second coating layer, and the second coating layer is a fiber layer containing polyaromatic, and does not contain mica components to reduce the overall brittleness of the insulating paper. Based on this, the present application can improve the corona-resistant life and partial discharge starting voltage level of the insulating paper while ensuring the tensile strength and elongation at break of the insulating paper, thereby meeting the requirements of automotive motors above 700V for corona resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The features, advantages and technical effects of exemplary embodiments of the present application will be described below with reference to the accompanying drawings.
[0017] Figure 1 is a partial cross-sectional view of the corona-resistant modified insulating paper provided in an embodiment of the present application;
[0018] Figure 2 yes Figure 1 Enlarged schematic diagram at point A in the middle.
[0019] In the drawings, the drawings are not necessarily drawn to scale.
[0020] Reference numerals: polyimide matrix 1; first covering layer 2; second covering layer 3; adhesive layer 4. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0022] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field of this application; the terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned drawings and any variations thereof are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship.
[0023] This application is based on the inventor's discovery and understanding of the following facts and problems:
[0024] Insulating paper is a general term for electrical insulating paper, which is also called insulating fiber cloth. Insulating paper can be used for motor insulation, capacitor paper, and cable protective lining. In the process of motor manufacturing, insulating paper can be used for slot wedge insulation, phase insulation, and end laminates. By setting insulating paper in the motor, the thermal insulation, mechanical properties, safety, and service life of the motor can be improved. In the related art, there is an electric field concentration phenomenon inside the insulation layer of the stator coil of the automobile motor, in the air gap between the surface of the insulation layer and the slot wall, and in the notch, which is prone to local discharge, that is, corona phenomenon. Corona will produce thermal effects, ozone, and nitrogen oxides, and increase the local temperature in the coil, which will lead to problems such as adhesive deterioration and carbonization and strand short circuit; therefore, when manufacturing automobile motors, insulating paper will be set at the position where the motor is prone to corona.
[0025] With the development of new energy vehicle technology, the voltage level of automotive motors is gradually increasing, and the voltage level of automotive motors can reach 700V-1140V. Automotive motors have higher requirements for the corona resistance of insulating paper. However, the corona resistance life and partial discharge inception voltage (PDIV) of insulating paper used in current automotive motors are relatively low. The corona resistance life of current automotive motor stators tested according to national standards generally does not exceed 200 hours. However, the ideal corona resistance life of automotive motor stators above 700V should be more than 1000 hours based on the results of national standard tests. The insulating paper materials currently used in automotive motors are difficult to meet the above requirements. The current insulating paper used in automotive motors cannot meet the use requirements of automotive motors above 700V for corona resistance performance.
[0026] In order to solve the above problems, the present application embodiment provides a corona resistant modified insulating paper. Figure 1 and Figure 2 The corona-resistant modified insulating paper of the embodiment of the present application is described in detail.
[0027] like Figure 1 As shown, an embodiment of the present application provides a corona-resistant modified insulating paper, which includes a polyimide substrate 1, a first coating layer 2 and a second coating layer 3, wherein the polyimide substrate 1 is the middle layer of the insulating paper. It can be understood that polyimide is an organic polymer material that can withstand a high temperature of 400°C and has excellent mechanical, dielectric, radiation resistance, wear resistance and insulation properties. In the modified insulating paper provided in the embodiment of the present application, the polyimide substrate 1 is constructed as a film and can be used as a modified substrate to paste other film layers with specific characteristics, and each film layer can be the first coating layer 2 and the second coating layer 3.
[0028] Specifically, the first coating layer 2 is bonded to the outer surface of the polyimide matrix 1 in a continuous layered form. The first coating layer 2 is a composite fiber layer containing polyaramid and mica. The mica is filled in the interior of the polyaramid, and the content ratio of mica to polyaramid is positively correlated with the voltage value of the automobile motor. The second coating layer 3 is laminated and connected to the side of the first coating layer 2 facing away from the polyimide matrix 1. The second coating layer 3 is a fiber layer containing polyaramid.
[0029] In the embodiments of this application, please refer to Figure 1During the molding process of the modified insulating paper, the polyimide matrix 1 is used as the intermediate matrix, and the first coating layer 2 and the second coating layer 3 are stacked outward in sequence, wherein the first coating layer 2 is made of polyaromatic amide as the main material and is doped with a predetermined proportion of mica. It can be understood that mica, as a natural inorganic material, has excellent properties of electrical insulation and high temperature resistance, but adding mica to polyaromatic amide will increase the overall brittleness of the material of the first coating layer 2. Based on this, in the process of making the first coating layer 2 in the embodiment of the present application, it is necessary to control the proportion of mica doped in polyaromatic amide.
[0030] It should also be emphasized that in order to weaken the negative effects of mica on the insulating paper, such as increased brittleness and reduced tensile strength, the modified insulating paper provided in the embodiment of the present application is also pasted with a second coating layer 3 on the outside of the first coating layer 2, wherein the second coating layer 3 is a fiber layer containing polyaramid, and no mica component is added to the second coating layer 3. It can be understood that the outermost layer of the modified insulating paper provided in the embodiment of the present application is a fiber layer containing polyaramid, which is beneficial to improve the overall tensile strength of the modified insulating paper.
[0031] In some embodiments, in the first coating layer 2, the content of mica is 10%-15% of the mass of the polyaramid.
[0032] It is understandable that, on the one hand, if the content of mica added to the first coating layer 2 is too high, it will greatly increase the brittleness of the insulating paper and reduce the tensile strength and elongation at break of the insulating paper; on the other hand, if the content of mica added to the first coating layer 2 is too low, it will affect the corona resistance of the insulating paper. Therefore, for the case where the design voltage of the automobile motor is between 700V-1140V, after multiple tests and demonstrations, the content of mica in the first coating layer 2 is preferably 10%-15% of the mass of the polyaramid. By setting a second coating layer 3 without mica components on the side of the first coating layer 2 away from the polyimide matrix 1, the insulating paper can meet the use requirements of automobile motor corona resistance while ensuring a certain tensile strength.
[0033] In one example, the mica content in the first coating layer 2 is preferably 10% of the mass of the polyaramid. It is understandable that for automotive motors above 700V, when the mica content accounts for 10% of the mass of the polyaramid, the corona resistance life and partial discharge starting voltage of the insulating paper can meet the use requirements of automotive motors, and the insulating paper will not be too brittle overall due to the addition of mica in the first coating layer 2.
[0034] In some embodiments, please refer to Figure 1 The number of the first coating layers 2 is two, and the two first coating layers 2 are symmetrically distributed on both sides of the polyimide substrate 1 .
[0035] In the embodiment of the present application, the polyimide substrate 1 is used as the intermediate substrate of the insulating paper, the first coating layer 2 is respectively arranged on both sides of the polyimide substrate 1, and two groups of second coating layers 2 wrap the polyimide substrate 1.
[0036] It should also be emphasized that in order to ensure the balance of the overall material of the insulating paper and the balance of the corona resistance performance, the mica contents in the two first coating layers 2 on both sides of the polyimide matrix 1 can be the same or relatively close.
[0037] In some embodiments, please refer to Figure 1 The number of the second coating layers 3 is two, and the two second coating layers 3 are symmetrically distributed on both sides of the polyimide substrate 1 .
[0038] It can be understood that the second coating layer 3 is the outermost structure of the entire insulating paper, and the second coating layer 3 is provided mainly to reduce the overall brittleness of the insulating paper.
[0039] In the embodiment of the present application, since the second covering layer 3 is bonded and fixed to the surface of the first covering layer 3 one by one, and the two first covering layers 2 are symmetrically distributed on both sides of the polyimide matrix 1, the two second covering layers 3 are symmetrically distributed on the outside of the polyimide matrix 1, and the insulating paper is arranged in a balanced and symmetrical manner in the overall structure, and the corona resistance of both sides of the insulating paper is the same. Based on this, during the installation of the insulating paper inside the automobile motor, the operator does not need to distinguish between the front and back sides of the insulating paper, and the installation process of the insulating paper is simpler and faster.
[0040] In some embodiments, please refer to Figure 1 and Figure 2 , the insulating paper further comprises a plurality of adhesive layers 4; any two adjacent to each other among the polyimide matrix 1, the first coating layer 2 and the second coating layer 3 are connected to each other through the adhesive layer 4, and the adhesive layer 4 is an interlayer structure layer containing epoxy glue. It can be understood that in the process of making one insulating paper, it is necessary to first prepare one polyimide matrix 1, two first coating layers 2, two second coating layers 3 and a certain amount of epoxy glue.
[0041] In one example, the production of an insulating paper can be carried out according to the following steps: first, epoxy glue is applied on both sides of the polyimide matrix 1, and a first coating layer 2 is pasted on each side; then, epoxy glue is applied on the sides of the two first coating layers 2 facing away from the polyimide matrix 1, and a second coating layer 3 is pasted to obtain an intermediate of the insulating paper; finally, the intermediate is subjected to hot rolling composite treatment to obtain a fully formed insulating paper. During the hot rolling composite treatment, the epoxy glue applied on both sides of the first coating layer 2 is gradually cured and formed into a bonding layer 4.
[0042] In another example, the production of an insulating paper can also be carried out according to the following steps: taking a second coating layer 3 as the starting point of lamination bonding, laying a first coating layer 2, a polyimide matrix 1, another first coating layer 2 and another second coating layer 3 on one side of the second coating layer 3 in sequence by epoxy glue bonding, thereby obtaining an intermediate of the insulating paper, and then subjecting the intermediate to hot rolling composite treatment to obtain a fully formed insulating paper, wherein the bonding layer 4 in the insulating paper is formed by curing the epoxy glue applied on both sides of the first coating layer 2.
[0043] In some embodiments, please refer to Figure 1 Any one or more of the polyimide substrate 1, the first coating layer 2 and the second coating layer 3 has a dimension of 0.038 mm to 0.05 mm along its thickness direction.
[0044] In the embodiment of the present application, when designing the modified insulating paper, it is necessary to design the thickness of the polyimide matrix 1, the first coating layer 2 and the second coating layer 3 respectively based on the design thickness of the insulating paper and considering the thickness of the adhesive layer 4 formed by epoxy glue. It can be understood that the thickness of each polyimide matrix 1, the first coating layer 2 and the second coating layer 3 can be the same, or different thicknesses can be set accordingly as needed. When designing the thickness of the polyimide matrix 1, the first coating layer 2 and the second coating layer 3, the design voltage of the automotive motor on which the corona-resistant modified insulating paper is assembled should be fully considered.
[0045] It can be understood that since the design voltage of automobile motors is generally between 700V and 1140V, the design voltage of each model of automobile motors is different. Therefore, each model of automobile motor has different requirements for the corona resistance and partial discharge starting voltage of the insulating paper. When preparing the corona-resistant modified insulating paper provided in the embodiment of the present application, the thickness of the polyimide matrix 1, the first coating layer 2 and the second coating layer 3 can be adjusted according to the actual needs of the automobile motor.
[0046] In one example, when the design voltage of the automobile motor is relatively high, after determining the proportion of mica in the first coating layer 2, the thickness of the first coating layer 2 can be appropriately increased. Based on the predetermined overall thickness of the insulating paper, when allocating the thickness of each structural layer of the insulating paper, the thickness of the first coating layer 2 containing mica can be made greater than the thickness of the second coating layer 3 not containing mica, thereby ensuring that the insulating paper has higher corona resistance and local discharge starting voltage level.
[0047] In another example, when the design voltage of the automobile motor is low, after determining the proportion of mica in the first coating layer 2, the thickness of the first coating layer 2 can be appropriately reduced. Based on the predetermined overall thickness of the insulating paper, when allocating the thickness of each structural layer of the insulating paper, the thickness of the first coating layer 2 containing mica can be made smaller than the thickness of the second coating layer 3, thereby ensuring that the brittleness of the insulation after molding is low and that the insulating paper has higher tensile strength and elongation at break.
[0048] It should be emphasized that no matter how the relative thickness size between the first coating layer 2 and the second coating layer 3 is defined, in order to ensure that the corona resistance performance on both sides of the formed insulating paper is the same, it is necessary to ensure that the thickness of the two first coating layers 2 arranged on both sides of the polyimide substrate 1 is the same, and the thickness of the two second coating layers 3 arranged on both sides of the polyimide substrate 1 is the same.
[0049] In one example, any one or more of the polyimide matrix 1, the first coating layer 2 and the second coating layer 3 may preferably have a dimension of 0.05 mm along its own thickness direction, that is, the thickness of each first coating layer 2 is 0.05 mm, the thickness of each second coating layer 3 is also 0.05 mm, and the thickness of the polyimide matrix 1 is also 0.05 mm.
[0050] For the case where the thickness of the polyimide matrix 1, each first coating layer 2, and each second coating layer 3 is 0.05 mm, after the corresponding insulating paper is actually produced, the data of multiple index parameters corresponding to the insulating paper are measured, and the multiple index parameters corresponding to the insulating paper are compared with those of the traditional NHN paper. The comparison results are shown in Table 1:
[0051] Table 1
[0052]
[0053] The NHN paper shown in Table 1 is a soft composite material composed of a middle layer of polyimide film and Nomex1 paper (DuPont paper) on both sides, with a heat resistance grade of H (180°C). The NHN paper has good mechanical properties, such as tensile strength and edge tear resistance and good electrical strength. The surface of the NHN paper is smooth. The NHN paper is mainly used for slot insulation, slot cover insulation and phase insulation of high heat resistance motors. In addition, it can also be used as interlayer insulation of transformers or other electrical appliances.
[0054] The overall thickness of the corona-resistant modified insulating paper shown in Table 1 is 0.28 mm, the thickness of the polyimide matrix 1, each first coating layer 2 and each second coating layer 3 is 0.05 mm, and the superimposed thickness of each adhesive layer 4 is 0.03 mm. From the data in Table 1, it can be seen that: due to the addition of an appropriate amount of mica component in the first coating layer 2 of the insulating paper, the partial discharge inception voltage (PDIV) level of the insulating paper is higher than that of NHN paper, and the insulating paper has better corona resistance than NHN paper. Although the insulating paper has increased brittleness due to the addition of an inorganic material such as mica, the insulating paper provided in the embodiment of the present application is further provided with a second coating layer 3 without mica components on the outside of the first coating layer 2, and the second coating layer 3 can offset the effect of increased brittleness of the insulating paper caused by mica to a certain extent. As can be seen from Table 1, the longitudinal elongation at break, transverse elongation at break, longitudinal tensile strength and transverse tensile strength of the corona-resistant modified insulating paper are only slightly reduced compared with those of NHN paper, and do not affect the overall strength of the corona-resistant modified insulating paper.
[0055] In addition, an embodiment of the present application also provides an automotive motor, which uses any of the aforementioned corona-resistant modified insulating papers during the manufacturing process. The corona-resistant modified insulating paper can be used for slot-to-slot insulation, slot cover insulation and phase-to-phase insulation of the automotive motor, meeting the use requirements of automotive motors above 700V for corona resistance performance.
[0056] In summary, the present application provides a corona-resistant modified insulating paper and an automotive motor. The automotive motor uses the corona-resistant modified insulating paper provided in the embodiment of the present application for insulation arrangement, which can meet the current demand for higher corona resistance of automotive motors used in new energy vehicles. For automotive motors with different design voltages, by adjusting the thickness of the first coating layer 2 of the insulating paper and the mica content, the corona resistance of the insulating paper can be adaptively changed to fully meet the needs of automotive motors of different models. In addition, since the outer surface of the first coating layer of the insulating paper is also provided with a second coating layer that does not contain mica, the overall strength of the insulating paper can be guaranteed in the process of adjusting the thickness of the first coating layer 2 and the mica content.
[0057] Reference to "embodiment" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present application. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments.
[0058] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "attached" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0059] In the embodiments of the present application, the same reference numerals represent the same components, and for the sake of brevity, detailed descriptions of the same components are omitted in different embodiments. It should be understood that the thickness, length, width and other dimensions of various components in the embodiments of the present application shown in the drawings, as well as the overall thickness, length, width and other dimensions of the integrated device are only exemplary descriptions and should not constitute any limitation to the present application.
[0060] The term "plurality" used in the present application refers to more than two, including two.
[0061] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A corona resistant modified insulating paper, It is characterized in that include: A polyimide matrix (1), which is the middle layer of the insulating paper; A first coating layer (2) is bonded to the outer surface of the polyimide matrix (1) in a continuous layered form, wherein the first coating layer (2) is a composite fiber layer containing polyaramid and mica, wherein the mica is filled inside the polyaramid, and the content ratio of the mica to the polyaramid is positively correlated with the voltage value of the automobile motor; and The second covering layer (3) is laminated and connected to the side of the first covering layer (2) facing away from the polyimide matrix (1), and the second covering layer (3) is a fiber layer containing polyaramid.
2. The corona-resistant modified insulating paper according to claim 1, It is characterized in that The number of the first coating layers (2) is two, and the two first coating layers (2) are symmetrically distributed on both sides of the polyimide matrix (1).
3. The corona-resistant modified insulating paper according to claim 1, It is characterized in that The number of the second coating layers (3) is two, and the two second coating layers (3) are symmetrically distributed on both sides of the polyimide matrix (1).
4. The corona-resistant modified insulating paper according to claim 1, It is characterized in that The insulating paper further comprises a plurality of adhesive layers (4); Any two adjacent to each other among the polyimide matrix (1), the first coating layer (2) and the second coating layer (3) are connected to each other via the adhesive layer (4).
5. The corona-resistant modified insulating paper according to claim 4, It is characterized in that The bonding layer (4) is an interlayer structure layer containing epoxy glue.
6. The corona-resistant modified insulating paper according to claim 1, It is characterized in that Any one or more of the polyimide matrix (1), the first coating layer (2) and the second coating layer (3) has a dimension of 0.038 mm to 0.05 mm along its thickness direction.
7. The corona-resistant modified insulating paper according to claim 6, It is characterized in that Any one or more of the polyimide matrix (1), the first coating layer (2) and the second coating layer (3) has a dimension of 0.05 mm along its thickness direction.
8. An automotive motor, It is characterized in that The corona-resistant modified insulating paper according to any one of claims 1 to 7 is used.