METHOD FOR WELDING PROFILE BARS

DE502017016540D1Active Publication Date: 2024-11-21URBAN GMBH & CO MASCHINENBAU KGAA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502017016540
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-07-29
Filing Date
2017-07-29
Publication Date
2024-11-21
Estimated Expiration
2037-07-29

AI Technical Summary

Technical Problem

Existing methods for welding profile bars, such as those used in window frames, often result in unsightly weld beads on visible surfaces, requiring post-processing to remove and affecting the appearance and quality of the finished product.

Method used

A method where profile bars with recesses formed on their ends, made of weldable and fusible material, are melted and joined without directly welding the visible surfaces, ensuring the melted material forms a connection inside the bars, avoiding visible weld beads and maintaining the surface integrity.

Benefits of technology

This approach eliminates the need for post-processing to remove weld beads, maintaining the original appearance and feel of the visible surfaces while achieving a strong, stable material-locking connection between the profile bars.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for welding profile bars.

[0002] Such a process can be used in particular to manufacture window frames. Typically, a number of profile bars, for example four, are welded together.

[0003] The butt joints between the profile bars should typically have a clean appearance even after welding. According to typical state-of-the-art methods, this requires post-processing to remove weld beads.

[0004] US Patent 2015 / 367568 A1 discloses a method for welding two profile bars, the method comprising the following steps: 1) providing the first profile bar and the second profile bar, 2) wherein each profile bar extends along its respective longitudinal axis, 3) wherein each profile bar has an inner part and a surrounding enclosure, a portion of the enclosure forming a visible surface, 4) wherein a first outer recess is formed at a first longitudinal end of the first profile bar, the first visible surface being set back axially with respect to the longitudinal axis of the first profile bar behind a first projecting portion of the first inner part, and a second outer recess is formed at a second longitudinal end of the second profile bar.at which the second visible surface is set back axially relative to the longitudinal axis of the second profile bar behind a second projecting portion of the second inner part, 5) wherein each projecting portion is formed from a weldable and / or meltable material, 6) melting the projecting portions by heating, 7) and bringing together the first longitudinal end and the second longitudinal end, so that the melted projecting portions form a material-locking connection between the first profile bar and the second profile bar on the inside, and the first visible surface and the second visible surface directly adjoin one another, so that together they form a common visible surface.

[0005] Methods for welding two profile bars are also known from the documents JP-H03176584 A, DE 3039733 A1, EP 0920978 A2 and EP 1679180 A2.

[0006] It is therefore an object of the invention to provide a method for welding profile bars which, compared to the prior art, is alternatively, for example better implemented.

[0007] This is achieved according to the invention by a method according to claim 1. Advantageous embodiments can be found, for example, in the dependent claims.

[0008] The invention relates to a method for welding a first profile bar and a second profile bar, wherein the method comprises the following steps: Providing the first profile bar and the second profile bar, each profile bar extending along its respective longitudinal axis, the first profile bar having a first inner part and a first enclosure surrounding it, a portion of the first enclosure forming a first visible surface, the second profile bar having a second inner part and a second enclosure surrounding it, a portion of the second enclosure forming a second visible surface, at least one first outer recess being formed at a first longitudinal end of the first profile bar, the first visible surface being set back axially with respect to the longitudinal axis of the first profile bar behind a first projecting section of the first inner part, and / or at least one second outer recess being formed at a second longitudinal end of the second profile bar.on which the second visible surface is set back axially with respect to the longitudinal axis of the second profile bar behind a second projecting section of the second inner part, each projecting section being formed from a weldable and / or meltable material, melting the projecting sections by heating, and bringing together the first longitudinal end and the second longitudinal end, so that the melted projecting sections form a material-locking connection between the first profile bar and the second profile bar on the inside, and the first visible surface and the second visible surface directly adjoin one another, so that together they form a common visible surface.

[0009] This method ensures that the visible surfaces are not affected by the process. In particular, the molten material is not located on the visible surface, so that post-processing can typically be avoided and any loss of quality in terms of feel and / or appearance is prevented.

[0010] The process is particularly preferably carried out in such a way that, after the formation of the material-bonded connection between the first and second visible surfaces, no molten material is present. The molten material is thus typically only located within the profile bars or only oozes out on surfaces that are not visible, and where the bead therefore does not cause any disturbance.

[0011] It is particularly advantageous that the first and second visible surfaces remain unchanged during the process. This allows for a particularly good appearance and / or feel, which is not affected by molten material.

[0012] The visible surfaces are advantageously not welded together, but rather border directly on each other without forming a material-bonded connection.

[0013] It has proven advantageous if the first outer recess has an axial length between 1 cm and 4 cm, preferably 1 cm to 3 cm, and particularly preferably 1 cm to 2 cm, and / or the second outer recess has an axial length between 1 cm and 4 cm, preferably 1 cm to 3 cm, and particularly preferably 1 cm to 2 cm. This allows sufficient material to be melted and used to create the bonded connection. A greater length of axial recess generally results in higher strength.

[0014] After the process, the molten material can be found particularly in cavities of the profile bars.

[0015] It should be understood that in a typical case, both the first profile bar and the second profile bar have a respective projecting section. However, it can also be provided that only one of the profile bars has such a projecting section.

[0016] Preferably, the first profile bar is made of a single material, in particular a thermoplastic material, and / or the second profile bar is made of a single material, in particular a thermoplastic material. This results in a simple design. A thermoplastic material is easy to melt and thus weld, but remains hard at normal room temperatures.

[0017] According to an advantageous embodiment, the first profile bar is designed as a hollow profile and / or the second profile bar is designed as a hollow profile. This allows for high stability with low weight. Furthermore, it can provide cavities for accommodating the molten material.

[0018] Cleverly, the first enclosure is formed by a plurality of first outer surfaces, one of which is the first visible surface, and / or the second enclosure is formed by a plurality of second outer surfaces, one of which is the second visible surface. The enclosure can be complete, in particular. However, it can also have openings.

[0019] According to one embodiment, the first inner part is formed from a plurality of first inner surfaces arranged at angles to each other, and / or the second inner part is formed from a plurality of second inner surfaces arranged at angles to each other. This allows for high stability.

[0020] According to one embodiment, the first profile bar and the second profile bar are mitered at the first longitudinal end and the second longitudinal end, so that the first profile bar and the second profile bar form an angle to each other after welding. For example, they may form a right angle. This can be particularly advantageous in the manufacture of a conventional window frame.

[0021] It should be understood that the method can be used, for example, for the production of window frames. Typically, angles of 90° are used between the profile bars. It can also be used, for example, for the production of transom windows. For example, straight stop edges can be used between the profile bars. In this case, the V-shaped connection area is provided with an external recess, particularly on the visible side.

[0022] The first profile bar can be designed to be mirror-symmetrical to the second profile bar, especially apart from their respective lengths.

[0023] It should be understood that a visible surface is, in particular, a surface that is visible in the finished product in a typical installed state. In the case of window frames, this particularly includes those surfaces facing an interior and an exterior. However, other surfaces can also be visible surfaces.

[0024] The first visible surface may have a smooth surface and / or the second visible surface may have a smooth surface. However, the visible surfaces may also be suitably processed, textured, colored, or otherwise designed to achieve a desired feel and / or appearance.

[0025] According to a further training it is planned that a part of the first enclosure forms a further first visible surface which is opposite the first visible surface, a part of the second enclosure forms a further second visible surface which is opposite the second visible surface, a further first outer recess is formed at the first longitudinal end of the first profile bar, in which the further first visible surface is set back axially with respect to the longitudinal axis of the first profile bar behind the first projecting section of the first inner part, and / or a further second outer recess is formed at the second longitudinal end of the second profile bar, in which the further second visible surface is set back axially with respect to the longitudinal axis of the second profile bar behind the second projecting section of the second inner part,and after the formation of the material-bonded connection, the further first visible surface and the further second visible surface directly adjoin each other, so that together they form another common visible surface.

[0026] This allows for the provision of an additional viewing surface. It should be understood that, in principle, any number of viewing surfaces can be used within the framework of the process. For example, one, two, three, or four viewing surfaces can be used. It is also possible for the entire enclosure to consist solely of viewing surfaces. Accordingly, each viewing surface is typically assigned a corresponding external recess.

[0027] The recesses can in particular be milled out.

[0028] Furthermore, the proposal advantageously provides that the respective recess at the longitudinal end of the first and / or second profile bar is made to the same material thickness as the enclosing. It has been found that it is sufficient to incorporate a recess into the outer wall of the profile, its enclosing, at least on the visible surface, for example, by milling or otherwise creating a corresponding recess. As described below, this incorporation of the recess leads to a targeted weakening of the outer wall, the enclosing of the profile bar. This advantageously causes the molten material to fold inwards when the two profile bars are joined, resulting in the weld bead forming inside the profile and not on the visible surface, where it would be disruptive.

[0029] The inventive proposal therefore comprises at least two variants, namely the first variant in which the outer web or enclosure is completely removed, as is the case, for example, in Figure 1 shown or where the enclosure in the end area is deliberately weakened, as is the case, for example, in the Figures 5b , 7 or 9 is shown.

[0030] In a preferred embodiment of the proposal, the recess is formed by a recess end surface consisting of at least one partial area. This definition of the recess applies to both of the aforementioned embodiments of the proposal, i.e., where the recesses remove the entire material thickness of the outer enclosure or are only incorporated into the material thickness of the enclosure.

[0031] Advantageously, it has been found that the first partial surface of the recess end face is arranged essentially perpendicular to the visible surface. This first, perpendicularly arranged partial surface then defines the visible surface and, when the joining process is complete, will butt-join the analogous partial surface on the second profile bar without a weld bead.

[0032] Furthermore, it is provided that a second surface adjoins the first at an obtuse angle, adjoining, directly or indirectly, the end-bounding surface of the projecting section. This design will advantageously result, as described below, in the formation of the weld bead on the inside during the joining process, and the two joined profile bars will butt against each other at the visible surface.

[0033] According to the invention, the recess is created by machining before melting. Several methods exist for achieving this. First, the profile bars can be prepared with the corresponding recess in a separate station. The machining process can be, for example, milling or sawing. However, a combination of milling and heating in the same setup is advantageous, as this leads to a faster and higher-quality result.

[0034] In principle, however, it is also possible for preheating to take place first, followed by machining the recess. This preheating process can be the melting process, or the melting process can follow as a second heating step.

[0035] The inventive proposal therefore does not specify the order of forming the recess and heating. All related variations are part of the disclosure of the invention.

[0036] It is cleverly designed that the first and second profile bars, after being provided, are each clamped by a clamping device movable along one direction of movement, and that this clamping remains unchanged during welding. This means, in particular, that each profile bar is firmly held in its clamping position and, of course, movable within its clamping device to, for example, carry out the joining process with the other profile bar, which is held in the same way. It is well known that the profile bar should be moved as automatically as possible, since several different feed movements are necessary during the production of a window frame sash, etc., which necessitate movement of the profile bar. These include, for example, positioning the profile bar against the heating element to melt the end section, as well as the subsequent joining movement with the second profile bar.The clever aspect here is that the profile bar remains in the clamping device as a workpiece during the machining of the recess, for example during a milling step, and is thus positioned with high precision during each machining step (milling, heating or heating, milling and joining), which has a very positive influence on the entire machining chain.

[0037] This proposal is accompanied by high efficiency of such a process, coupled with high corner strength and optimal optical design of the corner area, because the formation of an unsightly weld bead on the visible surface is reliably avoided.

[0038] According to the invention, after the profile bars have been provided, the end of the profile bar is pre-melted. This is also a very clever suggestion. The pre-melting is accompanied by an initial positioning movement of the profile bar against the heating mirror. The profile bar is pressed against the heating mirror with a corresponding force, and the heated, and thus plasticized, plastic material (preferably a thermoplastic such as PVC) yields in a transverse direction. In particular, the yielding material will also yield upwards or outwards, towards the visible surface, which is ultimately undesirable.The preheating process step is carried out in a suitable manner, then the profile bar is removed from the heating mirror, i.e. withdrawn, whereby a weld protrusion (the beginning of a weld bead, in conjunction with the second profile) has formed in a transverse direction, which is then milled off.

[0039] According to the invention, the milling unit, controlled by at least one, preferably several NC axes, mills away precisely the area of ​​the plastic material that could subsequently form a visible weld bead.

[0040] According to the invention, the following process sequence is provided: Clamping the unprocessed profile bars (cut to size and mitered, but without a recess) - machining the recess - pre-melting - removal of the weld protrusion by milling - melting - joining. Advantageously, it is provided that the respective visible surface of the profile bars is at least partially covered by a shell, preferably an aluminum shell, and that the end of the shell is flush with the first partial surface. Conveniently, the end of the aluminum shell is flush with the recess and conceals the corner joint after the joining process.

[0041] Furthermore, it is advantageously provided that the shell is supported on the visible surface by support elements, and an additional reduction is incorporated at the end of the profile bar in the area of ​​the support elements. The additional reduction is carried out precisely where the shell is supported on the visible surface by support elements. This reduction creates space where molten plastic material could potentially expand and otherwise push the aluminum shell up from the profile via the support elements in an unsightly manner. However, since the aluminum shell is provided precisely in the visible area, this additional reduction can be incorporated; it is concealed by the butt-fitting, gap-free abutment of the aluminum shells of the two profile bars forming the corner connection.

[0042] The invention presented in this application is highly variable and flexible in its implementation. It is expressly pointed out that all different aspects of the disclosure described in this application can be combined with one another.

[0043] In particular, the disclosure also includes the following combinations of the prescribed methods: removing the visible surface as in Figure 1 shown, with the described process of pre-melting.

[0044] Weaknesses of the enclosure, as in Figure 5b , 7, 8 and 9 shown, with the described process of pre-melting.

[0045] The invention further relates to a profile bar arrangement comprising a first profile bar and a second profile bar, which were welded together using a method according to the invention. All described embodiments and variants of the method can be used.

[0046] The invention is shown schematically in the drawing. It depicts: Fig. 1 a profile bar in perspective view for use in the method according to the invention, Fig. 2 two profile bars which are cut at a miter, in a top view, for use in the method according to the invention, Fig. 3 the profile bars of Figure 2 in a perspective view, Fig. 4 the profile bars of Figure 2 in a side view, Fig. 5a, 6je in a 3-dimensional view the incorporation of the recess into the profile bar according to the invention, Fig. 5b, 5cje in a schematic side view the situation of welding the two profile bars before the actual welding ( Figure 5b ) and after welding ( Figure 5c) according to a first embodiment of the invention, Fig. 7 in a schematic side view the situation of the welding of the two profile bars before the actual welding according to a second embodiment of the invention, Fig. 8, 9 each in a schematic side view further variants of embodiments of the method according to the invention.

[0047] In the figures, identical or corresponding elements are designated with the same reference numerals and are therefore not described again unless expedient. The disclosures contained in the entire description are transferable analogously to identical parts with the same reference numerals or component designations. Furthermore, the positional designations chosen in the description, such as top, bottom, side, etc., refer to the directly described and illustrated figure and are to be applied analogously to the new position if the position changes. Individual features or combinations of features from the different embodiments shown and described can also represent independent, inventive, or inventive solutions.

[0048] Figure 1shows a profile bar 100 in a perspective view. The profile bar 100 extends along a longitudinal axis (not shown but clearly visible) in the usual manner.

[0049] The profile bar 100 is designed to be used in a method for welding two profile bars according to an embodiment of the invention.

[0050] In subsequent figures, where two profile bars are shown, profile bar 100 will be referred to as the first profile bar. It will also be referred to as the first profile bar 100 in the following text.

[0051] The first profile bar 100 has a first inner part 110 and a first enclosure 120. Overall, the first profile bar is designed in the form of a hollow profile.

[0052] The first inner part 110 has a number of first inner surfaces 112. These are arranged at an angle to each other, as shown in Figure 1This is clearly visible. Essentially, the inner surfaces 112 are each oriented either parallel or perpendicular to another inner surface 112. They extend along the longitudinal axis of the first profile bar 100.

[0053] The first enclosure 120 is formed by a plurality of outer surfaces 122. These form an outer side of the first profile bar 100 in a direction transverse to the longitudinal axis.

[0054] One of the outer surfaces 122, namely the one which is in Figure 1 The surface facing upwards is designed as the first visible surface 130. This first visible surface 130 is designed in such a way that it forms an attractive area. This can, in particular, be one side of a window frame, which in a typical installation situation is located in an interior or exterior area. For this purpose, the first visible surface 130 is smooth and finished with a suitable color.

[0055] Opposite the first visible surface 130, an outer surface 122 facing in the opposite direction is formed as a further first visible surface 135. The properties of the further first visible surface 135 are similar to those described for the first visible surface 130.

[0056] Figure 1 shows the first profile bar 100 adjacent to a first axial end 102.

[0057] Immediately adjacent to the first axial end 102, a first outer recess 140 is formed at the top. This causes the first visible surface 130 to not extend completely to the first axial end 102, but to end before it. Correspondingly, another first outer recess 145 is formed at the bottom. This causes the second visible surface 135 to not extend completely to the first axial end 102, but to end before it.

[0058] The outer recesses 140, 145 form a first projecting section 114 in the first inner part 110. This section projects, in particular, along recognizable edges 132, 137, at which the first visible surface 130 and the further first visible surface 135 terminate. This section 114 has, for example, an axial length of 1, 2, 3, or 4 cm, as well as intermediate lengths. The section 114 terminates with the edge 132, which can have a height (perpendicular to the longitudinal extent of the section 114) of 0.3 cm, 0.5 cm, 0.7 cm, 1.0 cm, 1.2 cm, 1.5 cm, 1.7 cm, or 2.0 cm. The invention also encompasses all ratios of the axial length of the section 114 to the height of the edge 132 in the specified dimensions.

[0059] Like the rest of the first profile bar 100, the first protruding section 114 is made of a thermoplastic material. This means, in particular, that the first protruding section can be melted by heating. This can be used to weld the first profile bar 100 to a second profile bar 200, as will be described in more detail below.

[0060] The Figure 1 The first profile bar 100 shown is cut transversely to its longitudinal direction at the first axial end 102. A second profile bar 200, which represents an extension of the first profile bar 100, could therefore be welded to this end, provided that the second profile bar 200 is designed in the same or a similar way.

[0061] The following with reference to the Figures 2 to 4The described application, however, is designed such that each profile bar is not cut transversely at the axial end to be welded, but at a miter, i.e., at a 45° angle to the longitudinal axis. This allows two profile bars to be welded together so that they are arranged at a right angle to each other. This is used, for example, in the typical manufacture of a window frame.

[0062] Figure 2 shows the first profile bar 100, which is basically as in Figure 1 is formed, but in a modification thereof has a first axial end 102 which is mitred, i.e. cut at an angle of 45° to the longitudinal axis. In addition, Figure 2 a second profile bar 200.

[0063] The first profile bar 100 is designed as shown in Figure 1 can be seen and with reference to Figure 1 described. A repetition is omitted.

[0064] The second profile bar 200 is mirror-symmetrical to the first profile bar 100. Therefore, the description of the second profile bar 200 refers to the description of the first profile bar 100. It should only be noted that, compared to the first profile bar 100, all reference symbols used for the second profile bar 200 are increased by 100. Furthermore, all elements designated as "first" elements for the first profile bar 100 are designated as "second" elements for the second profile bar 200.

[0065] Thus, the second profile bar 200 has a second axial end 202, a second inner part 210 with second inner surfaces 212 and a second projecting section 214, a second enclosure 220 with second outer surfaces 222, including a second visible surface 230 and another second visible surface 235, edges 232, 237, a second outer recess 240 and another second outer recess 245.

[0066] Figure 2 is a plan view in which the first visible surface 130 and the second visible surface 230 are particularly visible. The first projecting section 114 and the second projecting section 214 protrude above their edges 132, 232, as can also be clearly seen. These face each other when the profile bars are arranged as shown.

[0067] Figure 3 shows the profile bars 100, 200 of Figure 2 in a perspective view, Figure 4 It shows a side view.

[0068] It is understood that for the sake of better presentation in the Figures 2 to 4 Not all reference symbols are shown.

[0069] Based on the Figures 2 to 4 In the state shown, it is now possible to weld the profile bars 100, 200 according to an embodiment of the method according to the invention. This will be described below.

[0070] For this purpose, a flat heating element (not shown) is first arranged between the protruding sections 114, 214. The heating element is heated, causing the protruding sections 114, 214 to heat up. Since, as already mentioned, these are made of a thermoplastic material, they melt in the process.

[0071] Then the first profile bar 100 and the second profile bar 200 are pressed together so that the two protruding sections 114, 214 come into contact with each other. Since both are molten and therefore fluid, they mix together, so that a material-bonded connection is formed after cooling.

[0072] The profile bars 100, 200 are moved towards each other until the edges 132, 232 of the first and second visible surfaces 130, 230 and the edges 137, 237 of the further first and further second visible surfaces 135, 235 touch. These come into contact with each other without the visible surfaces 130, 230 being altered during the process. The melting process only occurred between the visible surfaces 130, 230 and the further visible surfaces 135, 235, and molten material is only present within the profile bars 100, 200, but not on the visible surfaces 130, 135, 230, 235. Therefore, molten material does not affect the appearance of the visible surfaces 130, 135, 230, 235, so that post-processing can typically be omitted. Nevertheless, a stable, material-bonded connection is applied.

[0073] It should be understood that the method described here for welding two profile bars 100, 200 can also be applied to more profile bars. For example, a typical window frame can be constructed from four profile bars.

[0074] The inventive proposal, which is particularly in Figure 1 As described, in the exemplary embodiment according Figure 7 further developed. Is in Figure 1 If a recess 140 is provided which removes the entire material thickness of the enclosure 120 (which also includes the visible surface 130), then in the embodiment according to Figure 7 The recess 140 is only executed in the material thickness of the enclosure 120. In other words, the scale of Figure 1 and Figure 7 not comparable Figure 7 shows a significant magnification of part of the profile bar 100.

[0075] During the welding process, the ends of the profile bars 100 and 200 are heated so intensely that they become plasticized. The heating element required for this process is no longer visible, as it has already been removed from the area between the two profile bars 100 and 200. The two profile bars 100 and 200 are now joined together (see the corresponding oppositely oriented arrows 10 and 20) to achieve the weld.

[0076] The web thickness or material thickness of the enclosure 120 and 220 is indicated by the reference symbol SD. In reality, this is a few millimeters. Compared to the embodiment according to Figure 1Here, the recess 140, 240 is not L-shaped in view, but rather designed as a slope 162. The slope 162 forms an acute angle α with the mitered surface or section surface. The slope 162 is the first and, in this case, only partial surface of the recess end surface 14, which in turn defines the recess 140. For clarity, this recess end surface 14 is shown only on profile bar 100; the situation is analogous for the second profile bar 200.

[0077] This results in a partial weakening or reduction of the web thickness SD of the sheathing, particularly in the end region of the profile. This design is identical for the two profile bars 100 and 200 to be welded together.

[0078] The whistle of this embodiment of the invention (and also of the embodiment according to Figure 5bor 9) lies in the fact that it was found that the formation of a welding bead visible on the outside can be cleverly avoided if the material thickness SD or the material of the outermost web, the enclosure 120, is deliberately weakened in a suitable manner. Since in these exemplary embodiments the recess 140, 240 is only arranged in the material thickness SD of the outermost material web, the enclosure 120, 220, the overall strength of the welded connection, which is particularly required in the corner area, is only slightly reduced. This proposal of the invention therefore combines the need to weld without a welding bead with a high mechanical strength of the (corner) connection produced in this way. It should be emphasized that to achieve this goal, no hold-down device or pusher or punch is necessary on the recess 140, 240 (or groove) running parallel to the miter surface.

[0079] The specific design of the end region of the enclosure 120 is described by several parameters. Reference numerals 160 and 260 describe the boundary surface or overhang, or the area of ​​the profile bar that is heated most in terms of depth (in the axial direction), i.e., melted or "burned off" (as it is called in technical terminology).

[0080] In general, here, as in the other description of this invention, the first digit 1 in a three-digit reference numeral designates the respective element on the profile bar 100, and the first digit 2 in a three-digit reference numeral designates the respective element on the profile bar 200.

[0081] The bevel 162,262 forms an acute angle α with the boundary surface 160,260. Ideally, no welding occurs in the area of ​​the edge 161a,261a, meaning the two profile bar materials penetrate each other. The web thickness SD describes the thickness of the material of the enclosure 120,220. The reference symbol S60 describes the height of the end boundary surface 160,260 of the web or enclosure 120,220. The quotient of the height S60 to the web thickness SD lies in the range of 0-80%, preferably 10-70%, particularly preferably 20-60%.

[0082] For this parameter, an interval is specified, defined by an upper and lower limit. For example, the following values ​​are provided as upper limits: 90%, 80%, 70%, 60%, 50%, 40%, 30%. For example, the following values ​​are provided as lower limits: 70%, 60%, 50%, 40%, 30%, 20%, 10%. The disclosure of this application comprises the set of all intervals resulting from all possible, technically correct combinations of the aforementioned upper and lower limits.

[0083] Both in Figure 7 , but especially in Figure 5b the reference numerals 161 and 261 are used, these reference numerals in Figure 7 describe only one edge 161a, 261a, whereas in Figure 5b a substantially rectangularly oriented surface 161b, 261b. It is clear that the position of these elements is the same in both figures, whereby in Figure 7The edge 161a,261a has no height, but defines the transition to the slope 162,262 and determines at least the axial position of the theoretical joining endpoint on the profile bar.

[0084] In Figure 5b The situation shown is almost the same as in Figure 7 In addition to the design according to Figure 7 shows the Figure 5b A (further) partial surface 161c, 261c of the recess end surface 14, which is arranged substantially perpendicular to the visible surface 135, 235. In the embodiment shown here, the recess end surface 14 is formed by two partial surfaces 161c, 162b. The first partial surface 161c described above, which is oriented substantially perpendicular to the visible surface 135, 235, is then adjoined by the inclined surface 162 (as the second partial surface). The inclined surface 162 forms an obtuse angle β with the stepped first partial surface 161c.

[0085] The end region of the respective profile bars 100,200 is according to the exemplary embodiment according to Figure 5b The material thickness of the enclosure (120, 220 mm) is characterized by several parameters. These include the height S61 of the right-angled step 161d, the height S62 of the slope 262, and the height S60 of the end-face boundary 160, 260 mm of the web or enclosure (120, 200 mm). The height refers to a measurement perpendicular to the longitudinal extent of the profile bar.

[0086] With a web thickness SD of approximately 2.5 to 3 or 4 mm, the height S61 is 0.3, 0.5, or even 1 mm. Therefore, the ratio of the height S61 to the web thickness SD lies within a range of 5% to 60%, preferably 10% to 40%.

[0087] For this parameter (ratio of height S61 to web thickness SD), an interval is specified, which is described by an upper and lower limit. The following values ​​are provided as an upper limit, for example: 60%, 50%, 40%, 30%. The following values ​​are considered as a lower limit: 25%, 20%, 10%, 5%. The disclosure of this application encompasses the set of all intervals consisting of all possible, technically correct combinations of the aforementioned upper and lower limits.

[0088] For angle α, a typical interval of 30–60°, preferably 40–50°, and particularly 45°, is provided. For angle β, a typical interval of 120–150°, preferably 125–145°, and preferably 135°, is provided. Preferably, the axial projection of the end-face boundary 160 relative to paragraph 161d is a few millimeters to a few centimeters, for example, 0.5 mm, 1 cm, 1.5 cm, or 2 cm. This projection must be melted or burned off during joining, i.e., during welding.

[0089] It is clear that the larger this overhang, the more material is available to form the undesired weld bead. Therefore, the goal of welding is to melt (i.e., heat) only as little material as possible to create a minimal weld bead while maintaining maximum strength. For this reason, the ratio of the overhang to the web thickness SD is intended to be, for example, within a range of 150% to 400%.

[0090] For this parameter (the quotient of the projection and the web thickness SD), an interval is specified, which is described by an upper and lower limit. The following values ​​are provided as the upper limit, for example: 600%, 500%, 400%, and 300%. The following values ​​are considered as the lower limit: 100%, 150%, 200%, 250%, 300%, and 350%. The disclosure of this application encompasses the set of all intervals consisting of all possible, technically correct combinations of the aforementioned upper and lower limits.

[0091] It should be noted that in the end area of ​​the outer web of the profile bar 100, the enclosure 120, which is only a few millimeters thick, three different zones are formed which also fulfill completely different functions in the welding process.

[0092] This is achieved in particular with the help of Figure 5c Sure. Figure 5bIt was described that the two melted, i.e., heated, ends of the profile bars 100, 200 are moved towards each other during the joining process, as indicated by the opposing arrows 10, 20, and that the heated areas of the profile ends touch and penetrate each other, thus fusing together. In the transverse direction to the direction of movement, the material mixing here must yield and seeks the path of least mechanical resistance. This path is predetermined for the heated material. The inclined surface 162 is stiffer than the inner edge 170 of the enclosure 120, which runs parallel to the visible surface 135. As a result, the aforementioned protrusion preferentially yields to the interior of the profile, i.e., downwards, and forms the weld bead 63 there, as described in Figure 5CAs shown. In the area marked here 60, a good fusion, i.e., penetration, of the materials of the two profile bars 100 and 200 actually forms.

[0093] In the area above, 62, which is related to the bevels 162 and 262, the penetration is not quite as good, as there is a slightly larger surface area available to the volume, and therefore this area cools somewhat faster, resulting in somewhat poorer material penetration during welding. At the same time, however, this material is somewhat stiffer, which positively supports the downward folding effect of the weld bead.

[0094] The uppermost sector 61 communicates with the two sections 161d and 262d, which ideally have not come into contact with the heating mirror and have only been heated indirectly and slightly, and therefore do not exhibit any plasticity and butt against each other after joining. Ideally, these are not welded together.

[0095] Figure 5aFigure 1 shows the machining step of how the recess 140 is machined into the material thickness of the enclosure 120. A milling tool 5 is used for this purpose. The respective areas of the end-face boundary surface are marked 160, 161e, and 162, forming the projection 160 (area with normal wear), the chamfer 162 (area with reduced wear), and the (right-angled) shoulder 161d (area without wear). The milling tool 5 has multiple cutting edges 50, each with a chamfer 51 at its corners, thus machining the chamfer 162 into the profile end of the profile bar 100. It is clear that the milling tool 5 performs a machining operation involving chip removal.Depending on the position of the milling tool 5 relative to the visible surface 135, i.e., the distance of the milling tool's axis of rotation to this visible surface 135, a larger or smaller chamfer 162 is formed, ultimately defining the shape of the profile end. This chamfer is then heated with the heating mirror and subsequently welded—that is, mechanically bonded—to the second profile bar 200, which is ideally prepared in the same way. The milling cutter 5 is moved along the mitered surface at an acute angle to the longitudinal axis of the profile bar. The milling cutter 5 is arranged on an NC axis that is movable and positionable along at least one spatial direction.

[0096] In Figure 6 The position of the milling tool 5 relative to the visible surface 135 is slightly different in such a way that only the protruding surface 160 (surface with normal wear) and the shoulder 161d (surface without wear) are formed.

[0097] A particular advantage of the proposal lies in the exemplary embodiment according to Figure 8 . It is now known to arrange metal shells, for example aluminum, on plastic profiles, thus combining the appearance of a metal window with the advantages of a plastic window. In particular, the use of aluminum shells 19, 29 poses no problem for the milling cutters used to machine the mitered surfaces, as these cutters cut the relatively soft aluminum metal in the same way as plastic. The arrangement is selected such that the end edge of the aluminum shell 19, 29 is aligned with the shoulder surface 161f, which runs perpendicular to the visible surface 135. The remaining process steps are described in Figure 8 analogous to that in Figure 5b or 7. It is also clear, of course, that at the end of a profile, as is the case, for example, in Figure 5b or 7It is shown that an aluminum shell can be attached in the same way and the same advantages are achieved as in the embodiment shown here.

[0098] It was explained above that reducing the web thickness SD at the end of the profile bar has the beneficial effect that the weld bead forms itself inside the profile bar and does not bulge upwards. The reduction in web thickness leads to a weakening of the profile at its end, more precisely of the outer web or the enclosure 120. Such a weakening, which leads to a preferential folding of the weld bead inwards, is in Figure 9 shown. For this purpose, a notch is provided in the end region of the enclosure 120, perpendicular to the longitudinal extent of the profile bar 100, which performs exactly the same function as the embodiment according to Figure 5b .

[0099] A process that leads to a processing result according to Figure 9The process would be structured as follows: The method is used to weld a first profile bar and a second profile bar, and the process comprises the following steps: Providing the first profile bar and the second profile bar, each profile bar extending along its respective longitudinal axis, the first profile bar having a first inner part and a first enclosure surrounding it, a part of the first enclosure forming a first visible surface, the second profile bar having a second inner part and a second enclosure surrounding it, a part of the second enclosure forming a second visible surface, at least one first weakening oriented substantially parallel to the mitered surface of the profile bar, such as a groove or notch (e.g. milled), is arranged at a first end region of the first profile bar, and / or at least one second weakening oriented substantially parallel to the mitered surface of the profile bar, such as a groove or notch, is arranged at a first end region of the second profile bar (e.g.milled) wherein each end region is formed from a weldable and / or meltable material, melting the end region by heating, and bringing together the first longitudinal end and the second longitudinal end, so that the melted end region forms a material-locking connection between the first profile bar and the second profile bar on the inside, and the first visible surface and the second visible surface are directly adjacent to one another, so that together they form a common visible surface.

[0100] With the help of the Figures 2 to 4 The further joining process was described. It is clear that the steps described here also apply analogously to the embodiments according to Figure 5b , 7, 8 and 9 are realized, the expert will be aware of this procedure.

Claims

1. Method of welding a first profiled bar (100) and a second profiled bar (200), the method comprising the following steps: ▪ providing the first profiled bar (100) and the second profiled bar (200), ▪ wherein each profile bar (100, 200) extends along its respective longitudinal axis, ▪ wherein the first profiled bar (100) has a first inner part (110) and a first enclosure (120) surrounding it, wherein a part of the first enclosure (120) forms a first visible surface (130, 135), ▪ wherein the second profiled bar (200) has a second inner part (210) and a second enclosure (220) surrounding it, wherein a part of the second enclosure (220) forms a second visible surface (230, 235), ▪ wherein at least one first external recess (140, 145) is formed at a first longitudinal end of the first profiled bar (100), at which recess the first visible surface (130, 135) is set back axially with respect to the longitudinal axis of the first profiled bar (100) behind a first projecting section (114) of the first inner part (110), and / or at least one second external recess (240, 245) is formed at a second longitudinal end of the second profiled bar (200), at which recess the second visible surface (230, 235) is set back axially in relation to the longitudinal axis of the second profiled bar (200) behind a second projecting section (214) of the second inner part (210), ▪ wherein each projecting portion (114, 214) is formed from a weldable and / or fusible material, ▪ melting of the protruding sections (114, 214) by heating, and ▪ bringing the first longitudinal end and the second longitudinal end together so that the fused-on projecting sections (114, 214) form a material-locking connection on the inside between the first profiled bar (100) and the second profiled bar (200), and the first visible surface (130, 135) and the second visible surface (230, 235) directly adjoin one another so that together they form a common visible surface, ▪ wherein the recess (140, 145, 240, 245) is formed by machining prior to melting and, after the profiled bars (100, 200) have been provided, the end side of the profiled bar (100, 200) is pre-melted, wherein during pre-melting the profiled bar (100, 200) is pressed against a heating surface in a first adjusting movement and is then withdrawn again from the heating surface, ▪ wherein the method is characterised by the process sequence ∘ clamping of unmachined profile bars (100, 200), cut to size and mitred, but without recess (140, 145, 240, 245), ∘ incorporating the recess (140, 145, 240, 245), ∘ pre-melting, whereby the heated, plasticised plastic material evaporates in a transverse direction, in particular towards the visible surface (130, 135, 230, 235) and a weld protrusion is formed, ∘ removing of the welding protrusion by milling, whereby a milling unit controlled by at least one, preferably several NC axes mills away precisely the area of the plastic material that could subsequently form a visible welding bead (63), ∘ melting, ∘ joining.

2. Method according to claim 1, characterised in that no molten material is present between the first visible surface (130, 135) and the second visible surface (230, 235) after the positive connection has been formed.

3. Method according to one of the preceding claims, characterised in that the respective recess (140, 145, 240, 245) at the longitudinal end of the first and / or second profiled bar (100, 200) is / are designed in the material thickness of the enclosure (120, 220).

4. Method according to one of the preceding claims, characterised in that the recess (140, 145, 240, 245) is formed by a recess end surface (14) consisting of at least one partial surface (161c, 261c).

5. Method according to one of the preceding claims, characterised in that the first partial surface (161c, 261c) of the recess end surface (14) is arranged substantially at right angles to the visible surface (130, 135, 230, 235).

6. Method according to one of the preceding claims, characterised in that the first partial surface (161c, 261c) is adjoined at an obtuse angle by a second partial surface which adjoins, directly or indirectly, the end boundary surface (160, 260) of the projecting portion (114, 214).

7. Method according to one of the preceding claims, characterised in that the first and second profiled bars (100, 200) are each clamped by a clamping device movable along a direction of movement after they have been provided and this clamping is not changed during welding.

8. Method according to one of the preceding claims, characterised in that the respective visible surface (130, 135, 230, 235) of the profiled bars (100, 200) is at least partially covered by a shell, preferably an aluminium shell (19, 29), and the end of the shell is aligned with the first partial surface (161c, 261c).

9. Method according to claim 8, characterised in that the shell is supported on the visible surface (130, 135, 230, 235) via support elements and an additional ablation is incorporated at the end of the profile bar in the region of the support elements.

10. Method according to one of the preceding claims, characterised in that the first visible surface (130, 135) and the second visible surface (230, 235) remain unchanged during the method.

11. Method according to one of the preceding claims, characterised in that the first external recess (140, 145) has an axial length of between 1 mm and 4 mm and / or the second external recess (240, 245) has an axial length of between 1 mm and 4 mm.

12. Method according to one of claims 1 to 10, characterised in that the end region of the profiled bars (100, 200) has a right-angled shoulder (161d) and the axial projection of the end boundary surface (160) relative to the shoulder (161d) is a few millimetres to a few centimetres, for example 0.5 mm, 1 cm, 1.5 cm, 2 cm.

13. Method according to one of the preceding claims, characterised in that the first inner part (110) is formed from a plurality of first inner surfaces (112) arranged at an angle to one another, and / or the second inner part (210) is formed from a plurality of second inner surfaces (212) arranged at an angle to one another.

14. Method according to one of the preceding claims, characterised in that ▪ a part of the first enclosure (120) forms a further first viewing surface (130, 135) which is opposite the first viewing surface (130, 135), ▪ a part of the second enclosure (220) forms a further second viewing surface (230, 235) which is opposite the second viewing surface (230, 235), ▪ a further first external recess (140, 145) is formed at the first longitudinal end of the first profiled bar (100), at which recess the further first visible surface (130, 135) is set back axially with respect to the longitudinal axis of the first profiled bar (100) behind the first projecting section (114) of the first inner part (110), and / or a further second external recess (240, 245) is formed at the second longitudinal end of the second profiled bar (200), at which the further second visible surface (230, 235) is set back axially in relation to the longitudinal axis of the second profiled bar (200) behind a second projecting section (214) of the second inner part (210), and after the formation of the material-locking connection, the further first visible surface (130, 135) and the further second visible surface (230, 235) directly adjoin one another, so that together they form a further common visible surface.